Manufacturing method of board unit and board unit
A protective film covering the substrate's back and side surfaces addresses the issue of substrate damage during etching, enabling repeated use of laminated substrates for semiconductor functional layer growth.
Patent Information
- Application Number
- JP2024006066
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional methods of protecting the crystal growth surface of a substrate during etching treatment are insufficient, leading to damage and preventing the reuse of laminated substrates for subsequent semiconductor functional layer growth.
A protective film is formed to cover the back and side surfaces of the substrate and semiconductor laminate, including a sacrificial layer, to prevent damage during etching and enable reuse.
The protective film reduces substrate damage, allowing for increased reuse of the substrate and semiconductor stack by preventing corrosion during etching processes.
Smart Images

Figure 2024144108000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a substrate unit and a substrate unit. [Background technology]
[0002] 2. Description of the Related Art There has been proposed a technique relating to a manufacturing method for a semiconductor device that enables reuse of a substrate for crystal growth of a semiconductor thin film as a semiconductor functional layer (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-019590 A (see, for example, paragraphs 0030 and 0040) Summary of the Invention [Problem to be solved by the invention]
[0004] However, simply protecting the crystal growth surface of the substrate as in the above-mentioned conventional technology is not enough to prevent the substrate from being damaged by the etching process, and therefore, the laminated substrate including the substrate and the semiconductor laminate formed thereon cannot be reused for the crystal growth of the next semiconductor functional layer in many cases.
[0005] An object of the present disclosure is to provide a substrate unit manufacturing method and a substrate unit that can reduce damage to a substrate for growing a semiconductor functional layer. [Means for solving the problem]
[0006] The method for manufacturing a substrate unit disclosed herein is characterized in that a semiconductor laminate is formed on a substrate, a sacrificial layer is formed on the semiconductor laminate, a semiconductor functional layer is formed on the sacrificial layer, and a protective film is formed to cover at least a back surface of the substrate different from a formation surface on which the semiconductor laminate is formed, a side surface of the substrate, and a side surface of the semiconductor laminate.
[0007] The substrate unit of the present disclosure is characterized by having a substrate, a semiconductor laminate formed on the substrate, and a protective film that covers at least a back surface of the substrate different from a formation surface on which the semiconductor laminate is formed, a side surface of the substrate, and a side surface of the semiconductor laminate. Effect of the Invention
[0008] According to the present disclosure, damage to a substrate for growing a semiconductor functional layer can be reduced, and the number of times the substrate and semiconductor laminate can be reused can be increased. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2A is a schematic diagram showing a cross section of a substrate unit according to the first embodiment, and FIG. 2B is a schematic diagram showing an upper surface of the substrate unit according to the first embodiment. [Diagram 2] 5 is a flowchart showing a method for manufacturing a substrate unit according to the first embodiment. [Diagram 3] 5 is a schematic cross-sectional view showing a manufacturing process (part 1) of the substrate unit according to the first embodiment. FIG. [Figure 4] 5 is a schematic cross-sectional view showing a second manufacturing process of the substrate unit according to the first embodiment. FIG. [Diagram 5] 5 is a schematic cross-sectional view showing a third manufacturing process of the substrate unit according to the first embodiment. FIG. [Figure 6] 1(A) and 1(B) are a schematic cross-sectional view and a schematic plan view showing a peeling step (part 1) of a semiconductor functional layer. [Figure 7] 13(A) and 13(B) are a schematic cross-sectional view and a schematic plan view showing a peeling step (part 2) of a semiconductor functional layer. [Figure 8] 13(A) and 13(B) are a schematic cross-sectional view and a schematic plan view showing a peeling step (part 3) of a semiconductor functional layer. [Figure 9] FIG. 4 is a schematic cross-sectional view showing a peeling step (part 4) of the semiconductor functional layer. [Figure 10]5 is a schematic cross-sectional view showing a first step of recycling the substrate unit according to the first embodiment. FIG. [Figure 11] 5 is a schematic cross-sectional view showing a second recycling process of the substrate unit according to the first embodiment. FIG. [Figure 12] 6 is a schematic cross-sectional view showing a third recycling process of the substrate unit according to the first embodiment. FIG. [Figure 13] 11 is a schematic cross-sectional view showing a fourth step of recycling the substrate unit according to the first embodiment. FIG. [Figure 14] 5 is a schematic cross-sectional view showing a mechanical polishing step (part 1) of the substrate unit according to the first embodiment. FIG. [Figure 15] 5 is a schematic cross-sectional view showing a second mechanical polishing step of the substrate unit according to the first embodiment. FIG. [Figure 16] 11 is a schematic cross-sectional view showing a fifth step of reusing the substrate unit according to the first embodiment. FIG. [Figure 17] 11 is a schematic diagram showing a laminated substrate that is the basis of a substrate unit according to a second embodiment. FIG. [Figure 18] 11 is a schematic diagram showing a cross section of a substrate unit according to a second embodiment. FIG. [Figure 19] 10 is a flowchart showing a method for manufacturing a substrate unit according to a second embodiment. [Figure 20] 10 is a schematic cross-sectional view showing a first manufacturing process of the substrate unit according to the second embodiment. [Figure 21] 10 is a schematic cross-sectional view showing a second manufacturing process of the substrate unit according to the second embodiment. [Figure 22] 13(A) and 13(B) are a schematic cross-sectional view and a schematic plan view showing a third manufacturing process of the substrate unit according to the second embodiment. [Diagram 23] 13(A) and 13(B) are a schematic cross-sectional view and a schematic plan view showing a fourth manufacturing process of the substrate unit according to the second embodiment. [Figure 24] 13(A) and 13(B) are a schematic cross-sectional view and a schematic plan view illustrating a fifth manufacturing process of the substrate unit according to the second embodiment. [Diagram 25]13 is a schematic cross-sectional view showing a sixth manufacturing process of the substrate unit according to the second embodiment. FIG. [Figure 26] 13 is a schematic cross-sectional view showing a seventh step of manufacturing the substrate unit according to the second embodiment. FIG. [Figure 27] 11 is a schematic cross-sectional view showing a first step of recycling a substrate unit according to the second embodiment. FIG. [Figure 28] 11 is a schematic cross-sectional view showing a second recycling process of the substrate unit according to the second embodiment. FIG. [Figure 29] 11 is a schematic cross-sectional view showing a third recycling process of the substrate unit according to the second embodiment. FIG. [Diagram 30] FIG. 11 is a schematic cross-sectional view showing a fourth recycling process of the substrate unit according to the second embodiment. [Diagram 31] FIG. 11 is a schematic cross-sectional view showing a fifth step of reusing the substrate unit according to the second embodiment. [Diagram 32] FIG. 11 is a schematic cross-sectional view showing a sixth step of reusing the substrate unit according to the second embodiment. [Diagram 33] 11 is a schematic diagram showing a cross section of a laminated substrate that is the base of a substrate unit according to a second modification of the first embodiment. FIG. [Diagram 34] 11 is a schematic diagram showing a cross section of a substrate unit according to a second modification of the first embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a method for manufacturing a substrate unit and a substrate unit according to an embodiment of the present disclosure will be described with reference to the drawings. The following embodiment is merely an example, and various modifications are possible within the scope of the present disclosure.
[0011] 1. First embodiment 1-1 Overview of the First Embodiment FIG. 1(A) is a schematic diagram showing a cross section of a substrate unit 1 according to the first embodiment, and FIG. 1(B) is a schematic diagram showing the top surface of the substrate unit 1. As shown in FIG.
[0012] The substrate unit 1 includes a laminated substrate 100 having a plurality of laminated semiconductor layers, and a protective film 109 covering the entire laminated substrate 100. The laminated substrate 100 includes a substrate 101 which is a semiconductor substrate (e.g., a semiconductor wafer), a semiconductor laminate 110 provided on the substrate 101, a sacrificial layer 105 provided on the semiconductor laminate 110, and a semiconductor functional layer 120 provided on the sacrificial layer 105.
[0013] The semiconductor stack 110 has one or more semiconductor layers formed by epitaxial growth as crystal growth on the substrate 101. Specific examples of the semiconductor stack 110 will be described later.
[0014] The sacrificial layer 105 is a semiconductor layer formed on the semiconductor laminate 110 by epitaxial growth as crystal growth. The sacrificial layer 105 is made of a material that is easily etched by the etchant material used (i.e., has a faster etching rate than other layers). Specific examples of the sacrificial layer 105 will be described later.
[0015] The semiconductor functional layer 120 is a semiconductor layer in which a semiconductor element is formed. The semiconductor functional layer 120 shown in FIG. 1(A) is divided by processing to form a plurality of semiconductor elements (i.e., a plurality of divided semiconductor functional layers 120) arranged two-dimensionally on the substrate 101. By etching the sacrificial layer 105, each of the plurality of semiconductor elements (i.e., each of the plurality of divided semiconductor functional layers 120) can be separated (i.e., peeled off) from the semiconductor laminate 110. Each semiconductor functional layer 120 has a function as a semiconductor device (e.g., a light source, a photodetector, an image sensor, etc.) or a semiconductor element (e.g., a light emitting element, a light receiving element, a piezoelectric element, etc.). The separated semiconductor functional layer 120 is lifted and carried by a moving device (not shown) and is attached to a mounting substrate (not shown) by, for example, intermolecular forces. A specific example of the semiconductor functional layer 120 will be described later.
[0016] In FIG. 1, the protective film 109 covers the entire laminated substrate 100, but the protective film 109 does not necessarily need to cover the entire laminated substrate 100. The protective film 109 may have a structure that covers a portion that is repeatedly used for forming the semiconductor functional layer 120. For example, it is preferable that the protective film 109 at least covers the back surface 101b, which is different from the formation surface 101a of the substrate 101 on which the semiconductor laminated body 110 is formed, the side surface 101c of the substrate 101, and the side surface 110c of the semiconductor laminated body 110 in the substrate unit 1. In other words, the substrate unit 1 may have the protective film 109 formed from the back surface 101b to the side surface of the buffer layer 104 (shown in FIGS. 4 to 9 described later). With such a substrate unit 1, the substrate 1 and the buffer layer 104 are not eroded by the etching process after the formation and separation of the semiconductor functional layer 120, and the substrate 101 and the buffer layer 102 (shown in FIGS. 4 to 16 described later) can be repeatedly reused.
[0017] 1-2 Details of the First Embodiment <Manufacturing of circuit board units> Fig. 2 is a flowchart showing a method for manufacturing a substrate unit according to embodiment 1. Figs. 3, 4, and 5 are schematic cross-sectional views showing manufacturing steps (parts 1, 2, and 3) of the substrate unit according to embodiment 1.
[0018] 3 and 4, in the method for manufacturing the substrate unit according to the first embodiment, a semiconductor laminate 110 is grown by epitaxial growth on a substrate 101 as a semiconductor substrate (step S101 in FIG. 2), a sacrificial layer 105 is grown on the semiconductor laminate 110 (step S102 in FIG. 2), and a semiconductor functional layer 120 is grown on the sacrificial layer 105 (step S103 in FIG. 2). The substrate 101 is, for example, an indium phosphide (InP) substrate.
[0019] As shown in Fig. 4, the semiconductor laminate 110 grown on the substrate 101 has a buffer layer 102 as a first layer made of InP, an etching stop layer 103 as a second layer made of indium gallium arsenide (InGaAs) formed on the buffer layer 102, a buffer layer 104 as a third layer made of InP formed on the etching stop layer 103, and a sacrificial layer 105 made of indium gallium arsenide (InGaAs). The sacrificial layer 105 may be a single layer made of InGaAs only. The sacrificial layer 105 may also be a multilayer structure made of multiple layers of materials, such as a layer made of InGaAs and a layer made of indium gallium arsenide phosphide (InGaAsP). The first etchant material for the buffer layer 104 is hydrochloric acid, and the second etchant material for the etching stop layer 103 is a mixture of phosphoric acid and hydrogen peroxide, or a mixture of citric acid and hydrogen peroxide, or a mixture of sulfuric acid and hydrogen peroxide. The sacrificial layer 105 is also a mixture of phosphoric acid and hydrogen peroxide, or a mixture of citric acid and hydrogen peroxide, or a mixture of sulfuric acid and hydrogen peroxide.
[0020] By forming the buffer layer 102 from the same material as the substrate 101, the total thickness of the substrate 101 and the buffer layer 102 can be increased, and by providing the buffer layer 102, it is possible to prevent the thickness of the substrate 101 from being reduced when the upper layer is removed in a reuse (i.e., recycling) process described below. The etching stop layer 103 may be formed from other materials such as aluminum gallium arsenide (AlGaAs). The semiconductor laminate 110 is not limited to the configuration shown in FIG.
[0021] 4, the semiconductor functional layer 120 grown on the sacrificial layer 105 has an n-type cladding layer 106 made of InP, an active layer 107 as an InGaAs light absorption layer, and a p-type cladding layer 108 made of InP. In the first embodiment, the n-type cladding layer 106 and the p-type cladding layer 108 are formed of the same material as the substrate 101.
[0022] Next, as shown in FIG. 5, a protective film 109 is formed to cover the entire laminated substrate 100 (step S104 in FIG. 2). The protective film 109 is formed of, for example, an organic metal material. The protective film 109 is formed by, for example, ALD (Atomic Layer Deposition). The protective film 109 may be formed by other methods such as CVD (Chemical Vapor Deposition). The protective film 109 is formed so as to cover at least the rear surface 101b of the semiconductor laminated body 110 in the substrate 101, the side surface 101c of the substrate 101, and the side surface 110c of the semiconductor laminated body 110, which are portions to be reused for forming the semiconductor functional layer 120. When ALD is used, the thickness of the protective film 109 can be made uniform.
[0023] Next, when depositing alumina, an aluminum oxide film, as protective film 109 all around the periphery of laminated substrate 100 by ALD processing, trimethylaluminum (TMA) covers the surface when it is poured onto a flat material, but once one layer of TMA covers the entire surface, no further deposition takes place. At this point, if nitrogen is poured, the excess TMA can be removed, and then if water or ozone is poured, the methyl groups of TMA are separated and the aluminum is oxidized, resulting in one layer of alumina film.
[0024] Next, the remaining water and ozone are removed, and then TMA is supplied again. By repeating this operation, alumina is deposited in multiple atomic layers. In the first embodiment, trimethylaluminum is used, but other organic metals, such as (CH3)3Ga (trimethylgallium), may also be used.
[0025] The protective film 109 may be another organic protective film such as a resist.
[0026] Peeling off of semiconductor functional layer 6(A) and (B), 7(A) and (B), and 8(A) and (B) are schematic cross-sectional views and schematic plan views showing the peeling steps (parts 1, 2, and 3) of the semiconductor functional layer 120. Fig. 9 is a schematic cross-sectional view showing the peeling step (part 4) of the semiconductor functional layer. In these figures, the planar shape of the substrate 101 is illustrated as a square, but the planar shape is not limited to the examples shown.
[0027] Next, as shown in Figures 6(A) and (B), the semiconductor functional layer 120 and the sacrificial layer 105 are patterned by dry etching, and as shown in Figures 7(A) and (B), the p-type cladding layer 108 made of InP and the active layer 107 made of InGaAs are patterned by dry etching (step S105 in Figure 2).
[0028] 8(A) and (B), a functional layer protective film 121 is formed so as to cover the side surface of the active layer 107 and the upper surface and side surface of the p-type cladding layer 108 (step S106 in FIG. 2). The functional layer protective film 121 is formed of, for example, Al2O3, Si3N4, or SiO2.
[0029] 9, the sacrificial layer 105 is etched with an etchant material for wet etching, and the semiconductor functional layer 120 is lifted by a moving device (not shown) to separate (i.e., peel) the semiconductor functional layer 120 from the semiconductor laminate 110 (step S107 in FIG. 2). The peeled semiconductor functional layer 120 (e.g., an individual piece of the semiconductor functional layer 120) is attached (i.e., transferred) onto a desired mounting substrate (not shown), provided with wiring, and functions as a semiconductor element (e.g., a light-emitting element, a light-receiving element, a piezoelectric element, etc.).
[0030] <Reusing the circuit board unit> 10 to 13 are schematic cross-sectional views showing steps (parts 1 to 4) of recycling a substrate unit according to embodiment 1. In these figures, the planar shape of substrate 101 is illustrated as a square, but the planar shape is not limited to the illustrated example.
[0031] After the semiconductor functional layer 120 is peeled off from the semiconductor laminate 110, as shown in FIG. 10, the buffer layer 104 is wet-etched to leave the substrate 101, the buffer layer 102, the etching stop layer 103, and a part of the protective film 109. Next, as shown in FIG. 11, the protective film 109 is etched. It is also possible not to remove the protective film 109 in FIGS. 11 and 12. Next, as shown in FIG. 12, the etching stop layer 103 is wet-etched. At this time, since the exposed upper surface of the buffer layer 102 is rough and has a low smoothness, a treatment for smoothing is performed by a polishing process (lapping) (step S108 in FIG. 2). FIG. 13 shows a laminate substrate having a smoothed upper surface.
[0032] Figures 14 and 15 are schematic cross-sectional views showing mechanical polishing steps (parts 1 and 2) of the substrate unit according to the first embodiment. Figures 14 and 15 show modified examples of the steps shown in Figures 10 to 12. That is, the steps shown in Figures 10 to 12 may be replaced with mechanical polishing steps using a polishing apparatus 150 shown in Figures 14 and 15. For example, CMP (Chemical Mechanical Polishing) is used as the mechanical polishing. A laminated substrate having a smoothed upper surface is obtained by the mechanical polishing steps shown in Figures 14 and 15.
[0033] Fig. 16 is a schematic cross-sectional view showing a reuse process (part 5) of the substrate unit according to the first embodiment. As shown in Fig. 16, a buffer layer is additionally formed on the buffer layer 102 in Fig. 15 (the surface protruding above the protective film 109), and the remaining layers of the semiconductor laminate 110, that is, the etching stop layer 103 and the buffer layer 104, the sacrificial layer 105, and the semiconductor functional layer 120, are grown in order (step S109 in Fig. 2). Also, a buffer layer is additionally formed on the buffer layer 102 in Fig. 13, and each layer is formed again as shown in Fig. 4.
[0034] Next, as shown in Figures 6(A) and (B), the semiconductor functional layer 120 and the sacrificial layer 105 are patterned by dry etching, and as shown in Figures 7(A) and (B), the p-type cladding layer 108 made of InP and the active layer 107 made of InGaAs are patterned by dry etching (step S110 in Figure 2).
[0035] Next, as shown in FIGS. 8(A) and 8(B), a functional layer protective film 121 is formed so as to cover the side surfaces of the active layer 107 and the upper surface and side surfaces of the p-type cladding layer .
[0036] Next, as shown in FIG. 9, the semiconductor functional layer 120 is peeled off from the semiconductor laminate 110 (Step S111 in FIG. 2).
[0037] In the process of reusing the substrate unit, the processes from step S108 to S111 (i.e., the processes for forming the semiconductor functional layer) can be repeated. In addition, in the process of reusing the substrate unit, the substrate unit of FIG. 5 can be obtained again by performing an ALD process.
[0038] 1-3. Advantages of the First Embodiment As described above, by using the manufacturing method or substrate unit 1 of the first embodiment, damage to the substrate 101 made of InP can be reduced by providing the protective film 109. Furthermore, it becomes possible to repeatedly reuse the substrate 101 and the buffer layer 102, including the buffer layer 102 made of InP, without erosion. Therefore, the number of times that the substrate 101 and the semiconductor laminate 110 for growing the semiconductor functional layer 120 can be reused can be increased. Furthermore, by forming the protective film 109 after forming the semiconductor functional layer 120 of the first embodiment, damage to the substrate 101 during etching of the sacrificial layer 105 can be further suppressed, and the number of times that the substrate 101 can be reused can be further increased.
[0039] 2. Second embodiment 2-1 Overview of the Second Embodiment Fig. 17 is a schematic diagram showing a laminated substrate that is the basis of a substrate unit according to embodiment 2. Fig. 18 is a schematic diagram showing a cross section of a substrate unit 2 according to embodiment 2. The substrate unit 2 in Fig. 18 is used to grow the semiconductor functional layer 220 in Fig. 17. Alternatively, the substrate unit 2 in Fig. 18 is formed by reusing the substrate 201 and the semiconductor laminated body 210 after the semiconductor functional layer 220 in Fig. 17 has been peeled off.
[0040] The substrate unit 2 includes a laminated substrate 200 having a plurality of laminated semiconductor layers, and a protective film 209 that covers the entire laminated substrate 200. The laminated substrate 200 includes a substrate 201 that is a semiconductor substrate (e.g., a semiconductor wafer), and a semiconductor laminate 210 provided on the substrate 201.
[0041] The semiconductor stack 210 has one or more semiconductor layers formed by epitaxial growth as crystal growth on the substrate 201. Specific examples of the semiconductor stack 210 will be described later.
[0042] The sacrificial layer 205 shown in Fig. 17 is a semiconductor layer formed on the semiconductor laminate 210 by epitaxial growth as crystal growth. The sacrificial layer 205 is made of a material that is easily etched by the etchant material used (i.e., has a faster etching rate than other layers). Specific examples of the sacrificial layer 205 will be described later.
[0043] The semiconductor functional layer 220 shown in FIG. 17 is a semiconductor layer in which a semiconductor element is formed. As in the first embodiment, the semiconductor functional layer 220 is divided by processing and arranged two-dimensionally on a semiconductor wafer. By etching the sacrificial layer 205, each of the multiple semiconductor elements (i.e., each of the multiple divided semiconductor functional layers 220) can be separated (i.e., peeled off) from the semiconductor laminate 210. Each semiconductor functional layer 220 has a function as a semiconductor device (e.g., a light source, a photodetector, an image sensor, etc.) or a semiconductor element (e.g., a light emitting element, a light receiving element, a piezoelectric element, etc.). The separated semiconductor functional layer 220 is lifted and carried by a moving device (not shown) and is attached to a mounting substrate (not shown) by, for example, intermolecular forces. A specific example of the semiconductor functional layer 220 will be described later.
[0044] 18, the protective film 209 covers the entire laminated substrate 200, but the protective film 209 does not necessarily need to cover the entire laminated substrate 200. The protective film 209 may have a structure that covers a portion that is repeatedly used for forming the semiconductor functional layer 220. For example, it is desirable that the protective film 209 covers at least a back surface 201b of the substrate 201, which is different from a formation surface 201a on which the semiconductor laminated body 210 is formed, a side surface 201c of the substrate 201, and a side surface 210c of the semiconductor laminated body 110 in the substrate unit 2.
[0045] 2-2 Details of the second embodiment <Manufacturing of circuit board units> Fig. 19 is a flowchart showing a method for manufacturing a substrate unit according to embodiment 2. Figs. 20 and 21 are schematic cross-sectional views showing manufacturing steps (parts 1 and 2) of the substrate unit according to embodiment 2.
[0046] 20 and 21, in the method for manufacturing a substrate unit according to the second embodiment, a semiconductor laminate 210 is grown by epitaxial growth on a substrate 201 as a semiconductor substrate, a sacrificial layer 205 is grown on the semiconductor laminate 210, and a semiconductor functional layer 220 is grown on the sacrificial layer 105 (step S201 in FIG. 19). The substrate 201 is, for example, an InP substrate. The sacrificial layer 205 may be a single layer made of only InGaAs, as in the case of the sacrificial layer 105 in the first embodiment. The sacrificial layer 205 may also be a multilayer structure made of layers of multiple materials, such as a layer made of InGaAs and a layer made of InGaAsP.
[0047] As shown in FIG. 21, a semiconductor laminate 210 grown on a substrate 201 has a buffer layer 202 as a first layer made of InP, an etching stop layer 203 as a second layer made of InGaAs formed on the buffer layer 202, and a buffer layer 204 as a third layer made of InP formed on the etching stop layer 203.
[0048] The buffer layer 202 is formed of the same material as the substrate 201, so that the total thickness of the substrate 201 and the buffer layer 202 can be increased. Furthermore, by providing the buffer layer 202, it is possible to prevent the thickness of the substrate 201 from being reduced when removing the upper layer in the reuse process described later. The etching stop layer 203 may be formed of other materials such as InGaAsP. The semiconductor laminate 210 is not limited to the configuration shown in FIG. 21. Here, in the second embodiment, it is preferable that the sacrificial layer 205 is InGaAs and the etching stop layer 203 is InGaAsP. This reduces the etching selectivity of the etching stop layer 203 to the sacrificial layer 205, so that damage to the etching stop layer 203 when removing the sacrificial layer 205 can be reduced.
[0049] 21, the semiconductor functional layer 220 grown on the sacrificial layer 205 has an n-type cladding layer 206 made of InP, an active layer 207 as an InGaAs light absorption layer, and a p-type cladding layer 208 made of InP. In the first embodiment, the n-type cladding layer 206 and the p-type cladding layer 208 are formed of the same material as the substrate 201.
[0050] 22(A) and (B), 23(A) and (B), and 24(A) and (B) are schematic cross-sectional views and schematic plan views showing manufacturing steps (parts 3, 4, and 5) of a substrate unit according to embodiment 2. In these figures, the planar shape of substrate 201 is illustrated as a square, but the planar shape is not limited to the example illustrated.
[0051] Next, as shown in Figures 22(A) and (B), the semiconductor functional layer 220 and the sacrificial layer 205 are patterned by dry etching, and as shown in Figures 23(A) and (B), the p-type cladding layer 208 made of InP and the active layer 207 made of InGaAs are patterned by dry etching (step S202 in Figure 19).
[0052] 24(A) and (B), a functional layer protective film 221 is formed so as to cover the side surfaces of the active layer 207 and the upper surface and side surfaces of the p-type cladding layer 208. The functional layer protective film 221 is formed of, for example, Al2O3, Si3N4, or SiO2.
[0053] Fig. 25 is a schematic cross-sectional view showing a manufacturing process (part 7) of the substrate unit according to the second embodiment. As shown in Fig. 25, the sacrificial layer 205 is etched with an etchant material for wet etching, and the semiconductor functional layer 220 is lifted by a moving device (not shown), thereby separating (i.e., peeling) the semiconductor functional layer 220 from the semiconductor laminate 210 (step S203 in Fig. 19). The peeled semiconductor functional layer 220 (e.g., an individual piece of the semiconductor functional layer 220) is attached (i.e., transferred) onto a desired mounting substrate (not shown), provided with wiring, and functions as a semiconductor element (e.g., a light-emitting element, a light-receiving element, a piezoelectric element, etc.).
[0054] FIG. 26 is a schematic cross-sectional view showing a manufacturing process (part 8) of the substrate unit according to the second embodiment. As shown in FIG. 26, a protective film 209 is formed to cover the entire laminated substrate 200 including the substrate 201 and the semiconductor laminated body 210 (step S204 in FIG. 19). The protective film 209 is formed of, for example, an organometallic material. The protective film 209 is formed by, for example, ALD. The protective film 209 may be formed by other methods such as CVD. The protective film 209 does not necessarily cover the entire laminated substrate 200. The protective film 209 is formed so as to cover at least the back surface 201b of the semiconductor laminated body 210 in the substrate 201, the side surface 201c of the substrate 201, and the side surface 210c of the semiconductor laminated body 210, which are portions to be reused for forming the semiconductor functional layer 220. The protective film 209 is the same as the protective film in the first embodiment.
[0055] <Reusing the circuit board unit> 27 to 31 are schematic cross-sectional views showing steps (parts 1 to 5) of reusing a substrate unit according to the second embodiment.
[0056] After the semiconductor functional layer 220 is peeled off from the semiconductor laminate 210, as shown in FIG. 27 and FIG. 28, the buffer layer 204 is wet-etched to leave the substrate 201, the buffer layer 202, the etching stop layer 203, and a part of the protective film 209. Next, as shown in FIG. 29, the protective film 209 is etched. It is also possible not to remove the protective film 209 in FIG. 29. Next, as shown in FIG. 30, the etching stop layer 303 is wet-etched. At this time, since the upper surface of the exposed buffer layer 302 is rough and has a low smoothness, a polishing process (lapping) is performed to smooth it (step S205 in FIG. 19). FIG. 31 shows a laminate substrate having a smoothed upper surface. As in the case of the first embodiment, CMP may be used for the smoothing process.
[0057] Fig. 32 is a schematic cross-sectional view showing a sixth reuse step of the substrate unit according to the embodiment 1. As shown in Fig. 32, the remaining layers of the semiconductor laminate 210, that is, the etching stop layer 203 and the buffer layer 204, are grown in this order on the buffer layer 202 in Fig. 31 to form the laminate substrate 200 (Step S206 in Fig. 19).
[0058] Next, as shown in Fig. 26, a protective film 209 is formed to cover the entire laminated substrate 200 (step S207 in Fig. 19). The protective film 209 is formed so as to cover at least the rear surface 201b of the semiconductor laminated body 210 in the substrate 201, the side surface 201c of the substrate 201, and the side surface 210c of the semiconductor laminated body 210, which are portions to be reused for forming the semiconductor functional layer 220. Through this process, the substrate unit 2 shown in Fig. 26 is formed.
[0059] 2-3. Advantages of the Second Embodiment As described above, by using the manufacturing method or substrate unit 2 of the second embodiment, it becomes possible to repeatedly reuse not only the substrate 201 made of InP but also the buffer layer 202 made of InP without any erosion due to the provision of the protective film 209. Therefore, the number of times that the substrate 201 and the semiconductor laminate 210 for growing the semiconductor functional layer 220 can be reused can be increased. In addition, since the protective film 209 is formed after the process of separating the semiconductor functional layer 220 from the semiconductor laminate 210, the occurrence of scratches on the protective film 209 that may occur during the separation process can be reduced. Therefore, in the process of reusing the substrate unit, the intrusion of an etching solution (etchant) through scratches on the protective film 209 can be prevented, and the yield in reuse can be improved.
[0060] <3> Variation 1 In the above-mentioned first and second embodiments, the substrate 101, 201 as the growth source, the semiconductor laminate 110, 210, and the semiconductor functional layer 120, 220 grown on the sacrificial layer 105, 205 are shown as examples, but an additional layer may be provided on the semiconductor laminate 110, 210, an additional layer may be provided on the sacrificial layer 105, 205, or an additional upper layer may be provided on the semiconductor functional layer 120, 220. In addition, the semiconductor laminate 110 (210) is composed of the buffer layer 102 (202), the etching stop layer 103 (203), and the buffer layer 104 (204), but it may be composed of only one layer. For example, the semiconductor laminate may be composed of only the buffer layer 104 (204).
[0061] In the above-mentioned first and second embodiments, the laminated substrates 100, 200 are formed using an InP-based material, but the laminated substrates 100, 200 may be formed using a GaAs-based material or a GaN-based material. For example, the substrates 101, 201 may be made of GaAs, the buffer layers 102, 202 may be made of GaAs, the etching stop layers 103, 203 may be made of InGaP, the buffer layers 104, 204 may be made of AlGaAs or GaAs, and the sacrificial layers 105, 205 may be made of AlAs.
[0062] 4. Variation 2 In the above-mentioned embodiment 1, an example has been described in which a substrate unit is manufactured using a laminate substrate 100 in which the semiconductor laminate 110 is composed of a buffer layer 102, an etching stop layer 103 made of InGaAs formed on the buffer layer 102, and a buffer layer 104 made of InP formed on the etching stop layer 103, the sacrificial layer 105 is made of InGaAs, and the semiconductor functional layer 120 is composed of an n-type cladding layer 106 made of InP formed on the sacrificial layer 105, an active layer (AC) 107, and a p-type cladding layer 108 made of InGaAs. However, as shown in FIG. 33, a substrate unit relating to variant example 2 can also be manufactured using a laminate substrate 1100 in which a semiconductor laminate 1110 is composed of a buffer layer 1102 made of InP and an etching stop layer 1103 made of InGaAs, a sacrificial layer 1105 is made of InP, and a semiconductor functional layer 1120 is composed of an n-type cladding layer 1106 made of InGaAs, an active layer (AC) 1107, and a p-type cladding layer 1108 made of InGaAs.
[0063] In the second modification, as shown in FIG. 34, a semiconductor laminate 1110, a sacrificial layer 1105, and a semiconductor functional layer 1120 are laminated in this order on a substrate 1101, and then a protective film 1109 is formed. The material, shape, and forming method of the protective film 1109 are the same as those of the protective film 109 in the first embodiment. In the subsequent steps, the sacrificial layer 1105 is removed and the semiconductor functional layer 1120 is separated from the semiconductor laminate 1110, as in the first or second embodiment. Thereafter, as in the examples shown in FIG. 14 and FIG. 15, the etching stop layer 1103 is removed by polishing by CMP, and the upper surface of the buffer layer 1102 is smoothed, thereby obtaining a substrate unit having the substrate 1101, the buffer layer 1102 having a smoothed upper surface on the substrate 1101, and the protective film 1109 formed to cover from the back surface 1101b of the substrate 1101 to the side surface 1102c of the buffer layer 1102 (the side surface of the semiconductor laminate 1110).
[0064] In this way, even if the substrate 1101 and the sacrificial layer 1105 are made of the same material (e.g., InP), the protective film 1109 is formed after the semiconductor functional layer 1120 is formed and before the sacrificial layer 105 is removed, so that the back surface 1101b and side surface 1101c of the substrate 1101, and the side surface 1102c of the buffer layer 1102 (the side surfaces 1101c and 1102c form the side surfaces of the semiconductor laminate 1110) can be protected from damage caused by the etchant used to remove the sacrificial layer 1105.
[0065] The multilayer substrate 1100 of the second modification may be formed using a GaAs-based material or a GaN-based material, as in the first modification. [Explanation of symbols]
[0066] 1, 2 Substrate unit, 100, 200, 1100 Laminated substrate, 101, 201, 1101 Substrate, 101a, 201a Formation surface, 101b, 201b, 1101b Back surface, 101c, 201c, 1101c Side surface of substrate, 102, 202, 1102 Buffer layer (first layer), 1102c Side surface of buffer layer, 103, 203, 1103 Etching stop layer (second layer), 104, 204 Buffer layer (third layer), 105, 205, 1105 Sacrificial layer, 106, 206, 1106 n-type cladding layer, 107, 207, 1107 Active layer, 108, 208, 1108 p-type cladding layer, 109, 209, 1109 protective film; 110, 210, 1110 semiconductor laminate; 110c, 210c side surface of semiconductor laminate; 120, 220, 1120 semiconductor functional layer.
Claims
1. forming a semiconductor laminate on a substrate; forming a sacrificial layer on the semiconductor laminate; forming a semiconductor functional layer on the sacrificial layer; A protective film is formed to cover at least a rear surface of the substrate different from a surface on which the semiconductor laminate is formed, a side surface of the substrate, and a side surface of the semiconductor laminate. A method for manufacturing a substrate unit comprising the steps of:
2. The protective film is formed after the semiconductor functional layer is formed. The method for manufacturing a substrate unit according to claim 1 .
3. The protective film is formed so as to entirely cover the substrate, the semiconductor laminate, the sacrificial layer, and the semiconductor functional layer. The method for manufacturing a substrate unit according to claim 2 .
4. The protective film is formed after the semiconductor functional layer is separated from the semiconductor laminate by etching the sacrificial layer. The method for manufacturing a substrate unit according to claim 1 .
5. The protective film is formed so as to cover the entire substrate and the semiconductor laminate. The method for manufacturing a substrate unit according to claim 4 .
6. The formation of the semiconductor laminate includes: forming a first layer on the substrate; forming a second layer on the first layer, the second layer being made of a material different from that of the first layer; This is carried out by The method for manufacturing a substrate unit according to claim 1 .
7. After forming the protective film, the second layer is etched with an etchant material. The method for manufacturing a substrate unit according to claim 6 .
8. After the second layer is etched, the surface of the first layer on which the second layer is to be formed is smoothed by mechanical polishing. The method for manufacturing a substrate unit according to claim 7 .
9. The formation of the semiconductor laminate includes: forming a first layer on the substrate; forming a second layer on the first layer, the second layer being made of a material different from that of the first layer; forming a third layer on the second layer, the third layer being made of the same material as the first layer; This is carried out by The method for manufacturing a substrate unit according to claim 1 .
10. A protective film is formed on a laminate substrate having a substrate and a semiconductor laminate formed on the substrate, the protective film covering at least a rear surface of the substrate different from a surface on which the semiconductor laminate is formed, a side surface of the substrate, and a side surface of the semiconductor laminate. A method for manufacturing a substrate unit comprising the steps of:
11. A substrate; A semiconductor laminate formed on the substrate; a protective film that covers at least a rear surface of the substrate different from a surface on which the semiconductor laminate is formed, a side surface of the substrate, and a side surface of the semiconductor laminate; A substrate unit comprising:
12. The protective film covers the entire substrate and the semiconductor laminate. The substrate unit according to claim 11 .
13. a sacrificial layer formed on the semiconductor laminate; A semiconductor functional layer formed on the sacrificial layer and separable from the semiconductor laminate by etching the sacrificial layer; The substrate unit according to claim 11, further comprising:
14. The protective film covers the entirety of the substrate, the semiconductor laminate, the sacrificial layer, and the semiconductor functional layer. The substrate unit according to claim 13 .
15. The semiconductor laminate is a buffer layer formed of the same material as the substrate. The substrate unit according to claim 11 .
Citation Information
Patent Citations
Method of manufacturing semiconductor device
JP2005019590A
Cited By
Semiconductor structure, method for manufacturing semiconductor structure, and method for manufacturing electronic device