Plated steel sheet, and method for manufacturing the same
The plated steel sheet with controlled composition and manufacturing process addresses variations in tensile strength and workability, achieving high strength, yield ratio, and uniformity, enhancing vehicle safety and weight reduction.
Patent Information
- Application Number
- JP2024022772
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing plated steel sheets used in automobile bodies exhibit variations in tensile strength along the sheet width direction, leading to potential reductions in collision safety and workability.
A plated steel sheet composition and manufacturing process that includes specific elements (C, Si, Mn, Al, Ti, P, S, N, and optional additives like Nb, V, Ni, Cr, Mo, B, Mg, REM, and Ca) and a controlled microstructure (ferrite, upper bainite, tempered martensite, MA, and retained austenite) to ensure uniform tensile strength and high workability, with a manufacturing process involving controlled heating, cooling, and plating.
The solution results in a plated steel sheet with high tensile strength, predetermined yield ratio, and enhanced workability, while suppressing variations in tensile strength across the sheet width, contributing to vehicle weight reduction and safety.
Smart Images

Figure 2024144149000005 
Figure 2024144149000001 
Figure 2024144149000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to plated steel sheets and methods for producing the same. [Background technology]
[0002] There has been a demand for improved safety for vehicle occupants, and for this purpose, the strength of the materials used in vehicle bodies has been improved. On the other hand, against the background of the worsening of global warming and other issues, there has been an accelerating movement to improve the fuel efficiency of automobiles. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.
[0003] Plated steel sheets used in automobile bodies are required to have greater strength in order to reduce the weight of the vehicle body while ensuring safety in the event of a collision, etc. For example, tensile strength and yield ratio are mechanical properties that have a large impact on safety in the event of a collision, etc.
[0004] On the other hand, excellent formability is also required for plated steel sheets to be used in components such as automobile bodies having complex shapes. Examples of mechanical properties that greatly contribute to formability include ductility and hole expandability.
[0005] As a technology for achieving both crashworthiness (high strength, specified yield ratio) and high workability, the use of retained austenite (utilizing the TRIP (Transformation induced plasticity) phenomenon) as well as soft ferrite (and upper bainite) has been proposed. Patent Document 1 discloses a plated steel sheet having a tensile strength of 980 MPa or more and good formability by including ferrite and controlling the structural ratio of MA and retained austenite. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2016-194139 Summary of the Invention [Problem to be solved by the invention]
[0007] If the tensile strength of a plated steel sheet varies in the sheet width direction, there is a risk that the collision safety of the plated steel sheet applied to, for example, an automobile body may be reduced due to preferential deformation of areas with low strength. However, in the conventional technology, the variation in tensile strength in the sheet width direction has not been taken into consideration, and there is room for further improvement.
[0008] The present invention has been made in view of the above circumstances, and one of its objectives is to provide a plated steel sheet that has high strength, can contribute to weight reduction of a vehicle body, has a predetermined yield ratio and high formability, and has reduced variation in tensile strength in the sheet width direction, and a manufacturing method thereof. [Means for solving the problem]
[0009] Aspect 1 of the present invention is A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet satisfying the following formulas (1) and (2): The steel sheet included in the plated steel sheet is C: 0.150~0.300% by mass, Si: 0.80~2.20% by mass, Mn: 1.60~2.80% by mass, Al: 0.300~0.800% by mass, Ti:0.010~0.050% by mass, P: 0.050% by mass or less (including 0% by mass), S: 0.0100% by mass or less (including 0% by mass), N: 0.0100% by mass or less (including 0% by mass), and The balance is composed of iron and inevitable impurities, and The metal structure has a total of 30-70 area % of ferrite and upper bainite, 10-45 area % of tempered martensite, 5-35 area % of MA, and 5-20 volume % of retained austenite. It is plated steel sheet. TS max -TS min <20MPa (1) TS min ≧980MPa (2) In equations (1) and (2), TS max is the maximum value of the tensile strength at five different points in the sheet width direction of the plated steel sheet, and TS min is the minimum value of the tensile strength at the five points, The five locations are, in the sheet width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the sheet width.
[0010] Aspect 2 of the present invention is The plated steel sheet according to aspect 1 further contains at least one selected from the group consisting of Nb: more than 0 mass % and 0.20 mass % or less and V: more than 0 mass % and 0.50 mass % or less.
[0011] Aspect 3 of the present invention is The plated steel sheet according to embodiment 1 or 2 further contains at least one selected from the group consisting of Ni: more than 0 mass% and not more than 2.0 mass%, Cr: more than 0 mass% and not more than 2.0 mass%, and Mo: more than 0 mass% and not more than 0.50 mass%.
[0012] A fourth aspect of the present invention is The plated steel sheet according to any one of Aspects 1 to 3 further contains B: more than 0 mass % and 0.0050 mass % or less.
[0013] A fifth aspect of the present invention is The plated steel sheet according to any one of aspects 1 to 4 further contains at least one selected from the group consisting of Mg: more than 0 mass% and not more than 0.040 mass%, REM: more than 0 mass% and not more than 0.040 mass%, and Ca: more than 0 mass% and not more than 0.040 mass%.
[0014] A sixth aspect of the present invention is In the plate thickness direction, In the plated steel sheet according to any one of Aspects 1 to 5, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
[0015] A seventh aspect of the present invention is The plated steel sheet according to any one of Aspects 1 to 6, wherein the maximum carbon concentration (mass %) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration.
[0016] Aspect 8 of the present invention is A step of hot rolling a steel having a composition according to any one of aspects 1 to 5 to obtain a rolled plate; A first heating step of heating the rolled plate to a first heating temperature of 850°C or more and 910°C or less; After the first heating step, a step of maintaining the first heating temperature for 5 to 1800 seconds; After the holding step, a first cooling step is performed to a first cooling stop temperature of 350 ° C. to 750 ° C. a retention step in which, after the first cooling step, from the first cooling stop temperature to a second cooling start temperature, which is 350° C. to the first cooling stop temperature, the average cooling rate is 10° C. / sec or less, which is slower than the average cooling rate in the first cooling step, and the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is 20 to 300 seconds; After the retention step, a second cooling step is performed in which the material is cooled from the second cooling start temperature to a second cooling stop temperature of 100 to 300° C. at an average cooling rate faster than that of the retention step. After the second cooling step, a second heating step is performed to a second heating temperature of 300 to 500 ° C.; After the second heating step, a step of obtaining a steel sheet by holding the steel sheet at the second heating temperature for 300 to 1800 seconds; forming a plating layer on the steel sheet; The method for producing the plated steel sheet according to any one of the first to seventh aspects includes the steps of:
[0017] A ninth aspect of the present invention is After the step of obtaining the rolled plate, an oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750 ° C., The method of the present invention is directed to an eighth aspect of the present invention, wherein the retaining step includes a first reduction treatment having a dew point of −35 to −15° C., followed by a second reduction treatment having a dew point of −25 to 0° C., which is higher than the dew point of the first reduction treatment. Effect of the Invention
[0018] According to the embodiments of the present invention, it is possible to provide a plated steel sheet having high strength, capable of contributing to weight reduction of a vehicle body, a predetermined yield ratio and high formability, and in which variation in tensile strength in the sheet width direction is suppressed, and a manufacturing method thereof. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a diagram showing an example of a carbon concentration profile obtained in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The inventors have conducted research from various angles in order to realize a plated steel sheet that has high strength (tensile strength TS 980 MPa or more) that can contribute to weight reduction of a vehicle body, has a specified yield ratio YR (0.55 to 0.75) and high formability (elongation EL 19% or more, hole expansion ratio λ 20% or more), and has reduced variation in tensile strength in the sheet width direction.
[0021] Usually, in order to sufficiently introduce soft ferrite and the like, it has been effective to carry out annealing after the hot rolling step (hereinafter also referred to as "first heating") at a relatively low temperature.
[0022] The present inventors have found that when soft ferrite or the like is introduced by the usual method as described above, the metal structure or the like in the steel sheet becomes non-uniform, which can result in variations in tensile strength in the sheet width direction. Therefore, the inventors have discovered that by adjusting the chemical composition to a predetermined one (in particular by adding a predetermined amount of Al, which can contribute to the formation of ferrite and upper bainite), carrying out annealing after the rolling process at a high temperature of 850°C or more to eliminate distortion and the like after rolling, and then retaining (or holding) the material at a predetermined temperature range for a certain period of time during subsequent cooling, it is possible to realize a predetermined metal structure containing a sufficient amount of ferrite, etc., and as a result, a plated steel sheet can be obtained that has high strength (high tensile strength), a predetermined yield ratio and high workability, and in which variation in tensile strength in the sheet width direction is suppressed. The following provides details of each requirement stipulated by the embodiment of the present invention.
[0023] <1. Plated steel sheet> The plated steel sheet according to the embodiment of the present invention includes a steel sheet and a plating layer disposed on the surface of the steel sheet. The plating layer may be a zinc-based plating layer such as a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer or an electrogalvanized layer, or an aluminum plating layer such as a hot-dip aluminum plating layer. The zinc-based plating layer may be a zinc-based alloy plating layer such as zinc-Ni, zinc-Fe, or zinc-Al. The plating layer may be formed on at least one surface (e.g., a rolled surface) of the steel sheet, may be formed on both opposing surfaces, or may be formed on the entire surface of the steel sheet. Specific examples of the plated steel sheet including the zinc-based plating layer include hot-dip galvanized steel sheet (GI), alloyed hot-dip galvanized steel sheet (GA), and electrogalvanized steel sheet (EG).
[0024] <2. Composition of steel sheets contained in plated steel sheets> The steel sheet included in the plated steel sheet according to the embodiment of the present invention (which may be, for example, a portion of the plated steel sheet excluding the plating layer) preferably contains C: 0.150 to 0.300 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.60 to 2.80 mass%, Al: 0.300 to 0.800 mass%, Ti: 0.010 to 0.050 mass%, P: 0.050 mass% or less (including 0 mass%), S: 0.0100 mass% or less (including 0 mass%), N: 0.0100 mass% or less (including 0 mass%), with the remainder being iron and unavoidable impurities. Each component will be described in detail below.
[0025] (C:0.150~0.300% by mass) C is an effective element for obtaining a desired structure such as residual austenite (hereinafter also referred to as "residual γ") and improving properties such as tensile strength TS and elongation EL. In order to exert this effect, the C content is 0.150 mass% or more, preferably 0.170 mass% or more, more preferably 0.180 mass% or more, and even more preferably 0.200 mass% or more. On the other hand, if the C content is excessive, MA (Martensite-Austenite constituent) and residual γ become coarse, the hole expandability λ decreases, and the weldability is also adversely affected. Therefore, the C content is 0.300 mass% or less, preferably 0.280 mass% or less, more preferably 0.260 mass% or less, and even more preferably 0.250 mass% or less.
[0026] (Si:0.80~2.20% by mass) Si suppresses the precipitation of cementite and promotes the formation of residual γ. In order to exert this effect, the Si content is set to 0.80 mass% or more, preferably 0.90 mass% or more, more preferably 1.00 mass% or more, and further preferably 1.20 mass% or more. On the other hand, if the Si content is excessive, MA and residual γ become coarse, and the hole expansion ratio λ decreases, and weldability also decreases. Therefore, the Si content is set to 2.20 mass% or less, preferably 2.10 mass% or less, and more preferably 2.00 mass% or less.
[0027] (Mn:1.60~2.80% by mass) Mn is an element that contributes to improving the strength of steel sheet by solid solution strengthening, and is an element necessary for ensuring high strength. In order to exert this effect, the Mn content is set to 1.60 mass% or more, preferably 1.80 mass% or more, and more preferably 2.00 mass% or more. On the other hand, if the Mn content is excessive, the formation of ferrite and upper bainite is suppressed in the manufacturing process, and soft structures that contribute to improving ductility cannot be sufficiently introduced, and as a result, high elongation EL cannot be realized. Therefore, the Mn content is set to 2.80 mass% or less, preferably 2.70 mass% or less, more preferably 2.60 mass% or less, and even more preferably 2.50 mass% or less.
[0028] (Al:0.300~0.800% by mass) Al has the effect of promoting the formation of ferrite and upper bainite, and is an important element for ensuring the desired area ratio of ferrite and upper bainite by short-time residence in a predetermined temperature range described later. In order to exert this effect, the Al content is 0.300 mass% or more, preferably 0.350 mass% or more, and more preferably 0.400 mass% or more. On the other hand, if the Al content is excessive, it may become difficult to eliminate the heterogeneity of the structure resulting from the manufacturing process, and as a result, there is a risk of the occurrence of strength variation in the steel sheet. For this reason, the Al content is 0.800 mass% or less, preferably 0.750 mass% or less, and more preferably 0.700 mass% or less.
[0029] (Ti:0.010~0.050% by mass) Ti is an element that exerts the effects of precipitation strengthening and refining the metal structure, and contributes to increasing the strength of the steel sheet. In order to exert this effect, the Ti content is set to 0.010 mass% or more, preferably 0.015 mass% or more, and more preferably 0.020 mass% or more. On the other hand, if the Ti content is excessive, Ti carbonitrides are excessively precipitated, and the workability of the steel sheet is reduced. Therefore, the Ti content is set to 0.050 mass% or less, preferably 0.045 mass% or less, and more preferably 0.040 mass% or less.
[0030] (P: 0.050 mass% or less (including 0 mass%)) P is an element that is inevitably present as an impurity element. If the P content is excessive, the elongation EL and the hole expansion ratio λ decrease. Therefore, the P content is set to 0.050 mass% or less, and preferably 0.030 mass% or less. In this specification, "including 0 mass%" means that it includes embodiments in which it is not added intentionally, i.e., the content is below the unavoidable impurity level (it does not exclude the case where it is added intentionally).
[0031] (S: 0.0100% by mass or less (including 0% by mass)) S is an element that is inevitably present as an impurity element. If the S content becomes excessive, sulfide-based inclusions such as MnS are formed, which become the starting point of cracks, and the hole expansion ratio λ decreases. Therefore, the S content is set to 0.0100 mass% or less, preferably 0.0050 mass% or less.
[0032] (N: 0.0100% by mass or less (including 0% by mass)) N is an element that is inevitably present as an impurity element. If the N content is excessive, it forms coarse nitrides, which deteriorates bendability and hole expandability, and causes blowholes during welding. For this reason, the N content is set to 0.0100 mass% or less. Note that reducing the N content is costly, and if an attempt is made to reduce the N content to less than 0.0005 mass%, the cost increases significantly. For this reason, the lower limit of the N content is preferably set to 0.0005 mass% or more.
[0033] The steel sheet included in the plated steel sheet according to the embodiment of the present invention preferably contains the above-mentioned composition, and in one embodiment of the present invention, the balance is preferably iron and inevitable impurities. As inevitable impurities, the inclusion of elements brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. Note that, for example, there are elements such as P, S, and N, which are usually preferable to have a lower content and therefore are inevitable impurities, but whose composition ranges are separately specified as above. For this reason, in this specification, when referring to "unavoidable impurities" constituting the balance, it is a concept excluding elements whose composition ranges are separately specified.
[0034] As a preferred embodiment of the present invention, in addition to the above elements, it is effective to further contain, as necessary, (a) at least one selected from the group consisting of Nb: more than 0% by mass and 0.20% by mass or less and V: more than 0% by mass and 0.50% by mass or less, (b) at least one selected from the group consisting of Ni: more than 0% by mass and 2.0% by mass or less, Cr: more than 0% by mass and 2.0% by mass or less, and Mo: more than 0% by mass and 0.50% by mass or less, (c) B: more than 0% by mass and 0.0050% by mass or less, (d) Mg: more than 0% by mass and 0.040% by mass or less, REM: more than 0% by mass and 0.040% by mass or less, and Ca: more than 0% by mass and 0.040% by mass or less, and the properties of the plated steel sheet are further improved depending on the type of element contained.
[0035] ((a) At least one selected from the group consisting of Nb: more than 0 mass% and 0.20 mass% or less and V: more than 0 mass% and 0.50 mass% or less) Nb is an element that exerts the effects of precipitation strengthening and refining the metal structure, and contributes to improving the strength of the steel sheet. Therefore, the Nb content is preferably more than 0 mass%. This effect increases as the Nb content increases, and the Nb content is more preferably 0.005 mass% or more, and even more preferably 0.010 mass% or more. On the other hand, if the Nb content is excessive, Nb carbonitrides may be excessively precipitated, which may reduce the workability of the steel sheet. Therefore, the Nb content is preferably 0.20 mass% or less, more preferably 0.10 mass% or less, and even more preferably 0.060 mass% or less. Like Nb, V is an element that exerts the effects of precipitation strengthening and metal structure refinement, and contributes to improving the strength of the steel sheet. Therefore, the V content is preferably more than 0 mass%. This effect increases as the V content increases, and the V content is more preferably 0.010 mass% or more, and even more preferably 0.020 mass% or more. On the other hand, if the V content is excessive, V carbonitrides may be excessively precipitated, which may reduce the workability of the steel sheet. Therefore, the V content is preferably 0.50 mass% or less, more preferably 0.40 mass% or less, even more preferably 0.30 mass% or less, and even more preferably 0.10 mass% or less.
[0036] ((b) at least one selected from the group consisting of Ni: more than 0 mass% and not more than 2.0 mass%, Cr: more than 0 mass% and not more than 2.0 mass%, and Mo: more than 0 mass% and not more than 0.50 mass%) Ni is an element that contributes to improving the strength of the steel sheet, and is effective in stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Ni content is preferably more than 0 mass%. This effect increases as the Ni content increases, and the Ni content is more preferably 0.001 mass% or more, and even more preferably 0.01 mass% or more. On the other hand, if the Ni content is excessive, there is a risk of reducing manufacturability during hot rolling. Therefore, the Ni content is preferably 2.0 mass% or less, and more preferably 1.0 mass% or less. Like Ni, Cr contributes to improving the strength of the steel sheet, and is an effective element for stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Cr content is preferably more than 0 mass%. This effect increases as the Cr content increases, and the Cr content is more preferably 0.001 mass% or more, and further preferably 0.02 mass% or more. On the other hand, if the Cr content is excessive, the manufacturability during hot rolling decreases. Therefore, the Cr content is preferably 2.0 mass% or less, and more preferably 1.0 mass% or less. Mo, like Ni and Cr, contributes to improving the strength of the steel sheet, and is an effective element for stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Mo content is preferably more than 0 mass%. This effect increases as the Mo content increases, and the Mo content is more preferably 0.001 mass% or more, and further preferably 0.01 mass% or more. On the other hand, if the Mo content is excessive, there is a risk of reducing manufacturability during hot rolling. Therefore, the Mo content is preferably 0.50 mass% or less, and more preferably 0.20 mass% or less. Each of Ni, Cr and Mo may be contained alone, or two or three of them may be contained in combination.
[0037] ((c)B: More than 0% by mass and 0.0050% by mass or less) B is an element that is effective in suppressing excessive ferrite transformation by increasing hardenability. Therefore, the B content is preferably more than 0 mass%. This effect increases as the B content increases, and the B content is more preferably 0.0001 mass% or more, even more preferably 0.0003 mass% or more, and even more preferably 0.0005 mass% or more. However, if the B content is excessive, the hardenability increases excessively, and there is a risk that it becomes difficult to introduce ferrite and upper bainite during cooling. Therefore, the B content is preferably 0.0050 mass% or less, more preferably 0.0030 mass% or less, and even more preferably 0.0020 mass% or less.
[0038] ((d) at least one selected from the group consisting of Mg: more than 0% by mass and 0.040% by mass or less, REM: more than 0% by mass and 0.040% by mass or less, and Ca: more than 0% by mass and 0.040% by mass or less) Mg, REM (rare earth elements), and Ca form fine oxides and / or sulfides, suppressing the decrease in hole expandability caused by coarse oxides and / or sulfides. Therefore, the contents of Mg, REM, and Ca are preferably each more than 0% by mass. This effect increases as the contents of these elements increase, but the contents of Mg, REM, and Ca are more preferably 0.0005% by mass or more, and even more preferably 0.0010% by mass or more. However, if the contents of Mg, REM, and Ca are excessive, the oxides and / or sulfides may become coarse, which may decrease the hole expandability. Therefore, the contents of Mg, REM, and Ca are preferably 0.040% by mass or less, and more preferably 0.010% by mass or less. In addition to Sc and Y, REM includes a total of 17 elements of lanthanoid series rare earth elements from La (atomic number 15) to Lu (atomic number 71), and the REM content means the total amount of these 17 elements.
[0039] <3. Metal structure of steel sheets contained in plated steel sheets> The metal structure of the steel sheet included in the plated steel sheet according to the embodiment of the present invention has a total area percentage of ferrite and upper bainite of 30 to 70%, tempered martensite of 10 to 45%, MA of 5 to 35%, and retained austenite of 5 to 20% by volume. Each structure will be described below.
[0040] (The total area of ferrite and upper bainite is 30-70%) Ferrite and upper bainite are important structures for improving workability (especially elongation EL). Therefore, the total of ferrite and upper bainite is 30 area% or more, preferably 35 area% or more, and more preferably 40 area% or more. On the other hand, since both ferrite and upper bainite have low strength, if the total area ratio of ferrite and upper bainite is excessive, the tensile strength TS and yield stress YS decrease. Therefore, the total of ferrite and upper bainite is 70 area% or less, preferably 65 area% or less, and more preferably 60 area% or less. The area ratios of ferrite and upper bainite can be determined by observing a nital-etched steel sheet with a scanning electron microscope (SEM) and measuring the black areas that do not contain carbide using a point counting method or the like.
[0041] (Tempered martensite: 10-45% area) Tempered martensite is an important metal structure for ensuring the desired tensile strength TS and yield ratio YR. Therefore, the tempered martensite is 10 area% or more, preferably 15 area% or more, more preferably 18 area% or more, and even more preferably 20 area% or more. On the other hand, if the tempered martensite is excessive, the elongation EL decreases. Therefore, the tempered martensite is 45 area% or less, preferably 40 area% or less, and more preferably 35 area% or less. The area ratio of tempered martensite can be determined as a portion excluding ferrite, upper bainite, MA, and the remaining structure including pearlite and cementite.
[0042] (MA is 5-35% area) MA is a composite structure of fresh martensite and residual γ. Since MA contains residual γ, increasing the amount of MA is effective in improving workability such as elongation (EL). For this reason, the amount of MA is set to 5 area% or more, preferably 7 area% or more, and more preferably 10 area% or more. However, since very hard fresh martensite is also contained in MA, an increase in the amount of MA increases the interface between fresh martensite and other structures, and the hole expansion ratio λ decreases. Therefore, the amount of MA is set to 35 area% or less, preferably 30 area% or less, and more preferably 25 area% or less. The area ratio of MA can be determined by observing a nital-etched steel sheet with a SEM and measuring the gray areas not containing carbide by a point counting method.
[0043] (Retained austenite is 5-20% by volume) Residual γ causes the TRIP (transformation induced plasticity) phenomenon in which it transforms into martensite during press working, etc., and contributes to improving elongation EL. Martensite formed by the TRIP phenomenon has high hardness, so residual γ is an effective structure for improving tensile strength TS and elongation EL. In order to achieve the desired strength and workability, the residual γ is 5 vol% or more, preferably 6 vol% or more, more preferably 8 vol% or more, and even more preferably 10 vol% or more. On the other hand, since residual γ is a structure with a low yield ratio, the volume fraction of residual γ to ensure the desired yield ratio is 20 vol% or less, preferably 19 vol% or less, more preferably 18 vol% or less, and even more preferably 16 vol% or less. The volume fraction of the residual γ can be measured, for example, by X-ray diffraction. In this method, for example, a portion from the surface of the steel sheet to ¼ of the thickness of the steel sheet is removed by mechanical polishing, chemical polishing, etc., and an X-ray diffraction pattern is obtained for the exposed surface using Co-Kα radiation as characteristic X-rays. The volume fraction of the residual γ can then be measured from the integrated intensity ratio of the diffraction peaks of the body-centered cubic lattice (bcc) phase, the body-centered tetragonal lattice (bct), and the face-centered cubic lattice (fcc).
[0044] The remaining structure of the metal structure includes pearlite, cementite, etc. The remaining structure may be contained in a total amount of 10 area % or less.
[0045] <4. Mechanical properties of plated steel sheets> The plated steel sheet according to this embodiment can exhibit high strength (high tensile strength), a predetermined yield ratio, and high formability (high elongation and high hole expansion ratio). In this specification, a high-strength plated steel sheet is defined as one having a tensile strength TS of 980 MPa or more, specifically, one satisfying the following formula (2). TS min ≧980MPa (2) In equation (2), TS min is the minimum value of tensile strength at five different locations in the width direction of the plated steel sheet, and the five locations are: two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the sheet width. The predetermined yield ratio YR is 0.55 to 0.75. By setting the tensile strength and yield ratio as described above, it is considered that sufficient collision safety can be ensured when applied to, for example, an automobile body. In addition, in this specification, a highly formable plated steel sheet is defined as one having an elongation EL of 19% or more and a hole expansion ratio λ of 20% or more. The left side of the above formula (2) is preferably 990 MPa or more, more preferably 1000 MPa or more. The yield ratio is preferably 0.57 to 0.72. The elongation EL is preferably 20% or more, more preferably 21% or more. The hole expansion ratio λ is preferably 23% or more, more preferably 25% or more, and even more preferably 30% or more. In order to ensure collision safety, the yield stress YS is preferably 550 MPa or more, more preferably 570 MPa or more, and even more preferably 600 MPa or more.
[0046] Furthermore, the plated steel sheet according to this embodiment has reduced variation in tensile strength in the sheet width direction (i.e., the direction perpendicular to the rolling direction and the sheet thickness direction), and specifically satisfies the following formula (1). TS max -TS min <20MPa (1) In formula (1), TS max is the maximum value of the tensile strength at five different points in the width direction of the plated steel sheet (i.e., the direction perpendicular to the rolling direction and the thickness direction), and TS min is the minimum value of the tensile strength at the five points, The five locations are, in the sheet width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the sheet width. The left side of the above formula (1) is preferably 18 MPa or less.
[0047] The thickness of the steel sheet included in the plated steel sheet according to the present embodiment is not particularly limited. The thickness of the steel sheet included in the plated steel sheet according to the present embodiment may be, for example, 0.8 mm or more and 2.3 mm or less. The coating weight of the plated steel sheet according to the present embodiment is not particularly limited, and may be, for example, 10 to 100 g / m per side. 2 The sheet width W of the plated steel sheet according to this embodiment (i.e., the length in the direction perpendicular to the rolling direction and the sheet thickness direction) is not particularly limited, but may be, for example, 800 mm or more and 1200 mm or less.
[0048] <5. Decarburized layer on the surface of plated steel sheets> The steel sheet included in the plated steel sheet according to this embodiment is (I) In the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is preferably in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet. The position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that the position is in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet and that the decarburized layer that contributes to bendability has a certain thickness or more, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be in a region of 0.5% or more, or even 1.0% or more of the sheet thickness from the surface of the steel sheet.
[0049] The steel sheet included in the plated steel sheet according to this embodiment is (II) The maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction is preferably less than 70% of the bulk carbon concentration. When the present inventors checked steel sheets included in conventional plated steel sheets, they first found that there is a region with a significantly high carbon concentration in the surface layer of the steel sheet, which is the cause of deterioration of bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be obtained by promoting decarburization of the surface layer of the steel sheet to suppress the carbon concentration in the surface layer of the steel sheet, specifically, by suppressing the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm in the sheet thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.
[0050] From the viewpoint of exhibiting excellent bendability, the plated steel sheet according to this embodiment preferably satisfies at least one of the above (I) and (II), and more preferably satisfies both of the above (I) and (II).
[0051] The "surface of the steel sheet" refers to the position of the interface between the plating layer and the steel sheet. In the case of a zinc-based plating, for example, the position of the interface between the plating layer and the steel sheet refers to the point where Zn constituting the plating layer is no longer detectable (the analytical value of Zn is 0) when Zn is analyzed from the surface of the plating layer in the thickness direction of the plating layer by GD-OES measured in the examples described later, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.
[0052] The plated steel sheet according to this embodiment exhibits high strength (high tensile strength), a predetermined yield ratio, and high workability (high elongation and high hole expansion ratio), satisfies the above formula (1), and further exhibits excellent bendability with a limit R / t of 2.0 or less when subjected to a bending test shown in the examples described later.
[0053] <6. Manufacturing method of plated steel sheets> A method for producing a plated steel sheet according to an embodiment of the present invention includes: (A) hot rolling a steel having the above-mentioned composition to obtain a rolled plate; (B) a first heating step of heating the rolled plate to a first heating temperature of 850°C or more and 910°C or less; (C) after the first heating step, maintaining the first heating temperature for 5 to 1800 seconds; (D) a first cooling step of cooling to a first cooling stop temperature of 350°C to 750°C after the holding step; (E) a retention step, after the first cooling step, from the first cooling stop temperature to a second cooling start temperature, which is 350° C. to the first cooling stop temperature, at an average cooling rate of 10° C. / sec or less, which is slower than that of the first cooling step, and a retention time in the temperature range from the first cooling stop temperature to the second cooling start temperature is 20 to 300 seconds; (F) a second cooling step in which, after the retention step, the material is cooled from the second cooling start temperature to a second cooling stop temperature of 100 to 300° C. at an average cooling rate faster than that of the retention step; (G) after the second cooling step, a second heating step of heating to a second heating temperature of 300 to 500°C; (H) after the second heating step, maintaining the steel sheet at the second heating temperature for 300 to 1800 seconds to obtain a steel sheet; (I) forming a plating layer on the steel sheet; Each step will be described in detail below.
[0054] (A) Process for obtaining rolled plate The steel having the above-mentioned composition is melted and cast by a commonly used method, and the steel (steel slab) is subjected to a hot rolling process by a commonly used method to obtain a rolled plate. As an example, the steel (steel slab) having the above-mentioned composition cast by a continuous casting method, an ingot method, a thin slab casting method, or the like may be reheated to about 1150 to 1300°C, hot rolled to a finish rolling temperature of about 850 to 950°C, and coiled at about 500 to 700°C to obtain a rolled plate.
[0055] If necessary, the rolled plate may be pickled by a conventional method to remove surface scale, and if necessary, the rolled plate may be further subjected to cold rolling by a conventional method.
[0056] (B) First heating step The rolled sheet is heated to a first heating temperature of 850°C or more and 910°C or less. If the first heating temperature is less than 850°C, the reverse transformation to austenite is insufficient, and processed structures including distortions due to rolling remain, resulting in strength variations in the sheet width direction of the plated steel sheet. For this reason, the first heating temperature is set to 850°C or more, preferably 860°C or more, and more preferably 870°C or more. On the other hand, if the first heating temperature is more than 910°C, the crystal grain size becomes coarse, which may result in a decrease in the amount of transformation of ferrite and upper bainite in the cooling process (as a result, the area ratio of tempered martensite may become excessive), and a decrease in workability such as the hole expansion ratio may occur. For this reason, the first heating temperature is set to 910°C or less, and preferably 900°C or less. The heating rate is not particularly limited, and the temperature may be raised at any heating rate. For example, the temperature may be raised from room temperature to the first heating temperature at an average heating rate of 1°C / sec or more and 100°C / sec or less.
[0057] (C) maintaining at the first heating temperature The rolled sheet is held at the first heating temperature for 5 to 1800 seconds. If the holding time is less than 5 seconds, the reverse transformation to austenite is insufficient, the processed structure cannot be sufficiently eliminated, and the strength of the plated steel sheet varies in the sheet width direction. Therefore, the holding time is set to 5 seconds or more, preferably 10 seconds or more, and more preferably 20 seconds or more. On the other hand, if the holding time exceeds 1800 seconds, in addition to lowering productivity, the grains of the steel sheet structure may become coarse, which may cause a decrease in workability such as the hole expansion ratio λ. Therefore, the holding time is set to 1800 seconds or less, preferably 1500 seconds or less, and more preferably 1000 seconds or less.
[0058] After step (A), the method preferably includes an oxidation treatment (hereinafter also referred to as "step (B1)") under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the method preferably includes a reduction treatment (hereinafter also referred to as "step (C1)") in which the first reduction treatment is performed at a dew point of -35 to -15°C, and then the second reduction treatment is performed at a dew point of -25 to 0°C, which is higher than the dew point of the first reduction treatment. For example, the oxidation treatment in step (B1) may be performed after step (A) and before step (B), or may be performed during the temperature rise to the first heating temperature in step (B) (i.e., step (B) may include the oxidation treatment in step (B1)). The reduction treatment in step (C1) may be performed during the holding at the first heating temperature in step (C).
[0059] By subjecting the surface of the steel sheet to the oxidation treatment in step (B1), an Fe oxide layer can be formed on the surface of the steel sheet. Then, by performing the reduction treatment in step (C1) in a reducing atmosphere, a decarburized layer can be formed on the surface of the steel sheet, while a reduced Fe layer capable of forming, for example, a good plating layer can be formed. The inventors have conducted research and found that, by performing the oxidation treatment as described above and, in the reduction treatment, determining the ranges of the dew points of the first reduction treatment and the second reduction treatment, and setting the dew point of the second reduction treatment higher than the dew point of the first reduction treatment, the decarburized state of the surface layer of the steel sheet described above, which can realize high tensile strength, a predetermined yield ratio, high elongation, high hole expansion ratio, and excellent bendability, can be easily secured. Each treatment of the oxidation treatment and the reduction treatment will be described below.
[0060] (B1) Oxidation treatment The oxidation treatment is preferably performed under conditions of an oxygen concentration of 0.1 to 2%. From the viewpoint of obtaining an excellent coating appearance, the oxygen concentration is preferably 0.1% or more, more preferably 0.15% or more, and even more preferably 0.2% or more. On the other hand, if the oxygen concentration is too high, excessive oxidation causes oxide scale to adhere to the rolls in the furnace, and the steel sheet is likely to develop a defect called pickup, in which a pressed mark is generated. From the viewpoint of suppressing the occurrence of such defects, the oxygen concentration is preferably 2% or less, more preferably 1.7% or less, and even more preferably 1.5% or less. The concentration of elements other than oxygen is not particularly limited, and for example, a gas atmosphere containing the above-mentioned concentration of oxygen, CO2, N2, H2O, and other unavoidable impurities can be used. For example, the oxidation treatment can be performed in a DFF (Direct Fired Furnace) type annealing furnace or the like, in a gas atmosphere in which the concentration of unburned O2 is controlled in combustion gas such as coke oven gas (COG) and liquefied petroleum gas (LPG). The oxidation treatment is preferably carried out under conditions of an ultimate temperature of 650 to 750° C. For example, heating may be carried out in an oxidation heating zone in a DFF-type annealing furnace to an ultimate temperature in the range of 650 to 750° C. By setting the ultimate temperature to 750° C. or less, it is possible to suppress the reaction between SiO2 and FeO generated by the oxidation treatment, particularly on the surface of the steel sheet in the vicinity of the edges in the sheet width direction, and it is possible to improve the adhesion between the steel sheet and the coating layer.
[0061] In this specification, the "achieved temperature" during heating in the oxidation treatment step means the maximum reached sheet temperature of the rolled sheet that is heat-controlled in the oxidation heating zone.
[0062] The temperature reached in the oxidation treatment is more preferably 730° C. or lower, further preferably 720° C. or lower, and even more preferably 700° C. or lower. On the other hand, the steel sheet temperature in the oxidation treatment is preferably 650° C. or higher from the viewpoint of forming an Fe oxide layer in the above gas atmosphere. The steel sheet temperature in the oxidation treatment is more preferably 670° C. or higher.
[0063] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so that the oxidation treatment is too long and does not form a fayalite layer that adversely affects, for example, plating. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted in consideration of the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Also, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. In the above, the case where the oxidation treatment is performed while increasing the temperature has been described, but the aspect of the oxidation treatment is not limited to this, and the oxidation treatment may be performed by increasing the temperature to the target temperature and holding the target temperature.
[0064] (C1) Reduction treatment In the reduction treatment, a decarburized layer is formed on the surface layer of the steel sheet, while a reduced Fe layer capable of favorably forming, for example, a plating layer is formed. In the manufacturing method according to this embodiment, the reduction treatment is preferably performed by first reduction treatment having a dew point of -35 to -15°C, followed by second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment. Hereinafter, the first reduction treatment and the second reduction treatment will be described respectively.
[0065] (C1a) First reduction treatment In the first reduction treatment, the dew point is preferably set in the range of -35 to -15°C. If the dew point exceeds -15°C, decarburization may proceed more than necessary, which may result in a decrease in strength. In addition, the reduction treatment may be difficult to proceed, and a defect called pickup may occur in which iron oxide produced in the oxidation treatment adheres to the rolls and causes pressure marks on the steel sheet. Therefore, the dew point is preferably set to -15°C or lower. The dew point is more preferably set to -20°C or lower. On the other hand, from the viewpoint of suppressing additional equipment and costs, the dew point in the first reduction treatment is preferably set to -35°C or higher. The dew point is more preferably set to -30°C or higher.
[0066] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in a furnace, or by bubbling the atmospheric gas to mix water vapor therein.
[0067] The atmosphere of the first reduction treatment may be an atmosphere that satisfies the above dew point and contains N2, H2, CO, H2O, O2, and other inevitable impurities. In the first reduction treatment, after the steel sheet reaches a temperature of 850°C in the atmosphere, the steel sheet is heated in a temperature range of 850 to 910°C for, for example, 60 to 240 seconds. The "holding" may be at a constant temperature or may be varied within the temperature range.
[0068] (C1b) Second reduction treatment Next, the dew point in the second reduction treatment will be described. In order to achieve excellent bendability with R / t less than 2.0, the dew point in the second reduction treatment is preferably -25°C or higher. On the other hand, the upper limit of the dew point in the second reduction treatment is preferably 0°C or lower from the viewpoint of exhibiting higher strength. The dew point in the second reduction treatment is more preferably -15°C or lower.
[0069] The atmosphere of the second reduction treatment may be an atmosphere that satisfies the above dew point and contains N2, H2, CO, H2O, O2, and other unavoidable impurities. In the second reduction treatment, the steel sheet may be heated in the above atmosphere for, for example, 60 to 240 seconds in a temperature range in which the steel sheet reaches a temperature of 850 to 910°C. The "holding" may be at a constant temperature or may be varied within the above temperature range.
[0070] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace may be provided for performing each of the first reduction treatment and the second reduction treatment. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided in the middle of the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.
[0071] Between the first reduction treatment and the second reduction treatment, a process such as a holding process for holding at least one of the conditions (dew point, etc.) of the first reduction treatment may be inserted as long as it does not adversely affect the decarburization state of the steel sheet according to the present embodiment. Preferably, the second reduction treatment is performed following the first reduction treatment.
[0072] The oxidation treatment and reduction treatment may be carried out using any one or more known facilities. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) facility is used. By using a continuous hot-dip galvanizing line, the oxidation treatment and reduction treatment by the oxidation-reduction method, and the hot-dip galvanizing treatment and alloying treatment when manufacturing, for example, a galvanized steel sheet as a steel sheet, can be carried out continuously in a series of production lines. More specifically, the oxidation treatment and reduction treatment by the oxidation-reduction method can be carried out using, for example, an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in the heating zone in a DFF-type annealing furnace as shown in the front vertical direction. The reduction treatment can be carried out, for example, in the soaking zone in a DFF-type annealing furnace.
[0073] (D) First cooling process After the step (C), the material is cooled to a first cooling stop temperature of 350°C to 750°C. If the first cooling stop temperature is less than 350°C, the ferrite and upper bainite cannot be sufficiently transformed (as a result, the area ratio of tempered martensite may become excessive), and the desired workability (high elongation EL, etc.) cannot be realized. For this reason, the first cooling stop temperature is set to 350°C or higher, preferably 360°C or higher, and more preferably 370°C or higher. On the other hand, if the first cooling stop temperature is more than 750°C, the transformation of ferrite and upper bainite does not occur, and the desired workability cannot be realized. For this reason, the first cooling stop temperature is set to 750°C or lower, preferably 720°C or lower, and more preferably 700°C or lower.
[0074] The cooling rate from the first heating temperature to the first cooling stop temperature is not particularly limited, and the average cooling rate may be, for example, 1° C. / sec or more and 50° C. / sec or less.
[0075] (E) Retention process After step (D), from the first cooling stop temperature to a second cooling start temperature of 350°C to the first cooling stop temperature, the average cooling rate is set to 10°C / sec or less, which is slower than that in step (D), and the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is set to 20 to 300 seconds. The transformation of ferrite and upper bainite can be promoted by steps (D) and (E).
[0076] If the average cooling rate from the first cooling stop temperature to the second cooling start temperature, which is 350°C to the first cooling stop temperature, exceeds 10°C / sec, or is equal to or greater than that in step (E), the ferrite and upper bainite cannot be sufficiently transformed, and the desired workability cannot be achieved. Therefore, the average cooling rate is 10°C / sec or less, preferably 8°C / sec or less, more preferably 5°C / sec or less, and even more preferably 3°C / sec or less. When the second cooling start temperature is the first cooling stop temperature, the average cooling rate is 0°C / sec.
[0077] If the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is less than 20 seconds, the ferrite and upper bainite cannot be sufficiently transformed, and the desired workability cannot be achieved. Therefore, the time is set to 20 seconds or more, preferably 25 seconds or more, and more preferably 30 seconds or more. On the other hand, if the time exceeds 300 seconds, ferrite and upper bainite are excessively formed, making it difficult to ensure a tensile strength of 980 MPa or more. Therefore, the time is set to 300 seconds or less, preferably 200 seconds or less, more preferably 150 seconds or less, and even more preferably 100 seconds or less.
[0078] (F)Second cooling process After step (E), the material is cooled from the second cooling start temperature to a second cooling stop temperature of 100 to 300° C. at an average cooling rate faster than that in step (E). This causes martensitic transformation to proceed, and tempered martensite is formed by carrying out a second heating step (tempering) described later.
[0079] If the second cooling stop temperature is less than 100°C, the martensite transformation will proceed excessively, the desired amount of residual γ will not be secured, and workability will decrease. Therefore, the second cooling stop temperature is set to 100°C or higher, preferably 120°C or higher, and more preferably 140°C or higher. On the other hand, if the second cooling stop temperature exceeds 300°C, the desired amount of martensite will not be secured, and the yield stress YS (and the yield ratio YR) will decrease. Therefore, the second cooling stop temperature is set to 300°C or lower, preferably 250°C or lower, and more preferably 200°C or lower.
[0080] The cooling rate from the second cooling start temperature to the second cooling stop temperature is set to an average cooling rate faster than that in step (E) from the viewpoint of productivity. The average cooling rate may be, for example, 1° C. / sec or more and 50° C. / sec or less.
[0081] In this step, the material may be held for a certain period of time after the cooling is stopped, or the second heating step described below may be performed without holding the temperature. Even if the holding time at the second cooling stop temperature is long, the properties are hardly affected, but from the viewpoint of productivity, it is preferable to hold the material for, for example, 600 seconds or less.
[0082] (G) Second heating step After step (F), the material is heated to a second heating temperature of 300 to 500°C. This step and the holding step (H) described below temper the martensite, and also transforms a part of the untransformed austenite into bainite. As a result, C is concentrated in the untransformed austenite, stabilizing it and allowing it to remain as retained γ.
[0083] If the second heating temperature is less than 300°C, the bainite formed with the tempered martensite becomes excessively hard, and the workability decreases. Therefore, the second heating temperature is set to 300°C or higher, preferably 320°C or higher, and more preferably 340°C or higher. On the other hand, if the second heating temperature exceeds 500°C, the bainite formed with the tempered martensite becomes excessively soft, and the tensile strength TS decreases. Therefore, the second heating temperature is set to 500°C or lower, preferably 480°C or lower, and more preferably 450°C or lower.
[0084] The heating rate from the second cooling stop temperature of 300° C. or less to the second heating temperature is not particularly limited, and may be, for example, an average heating rate of 1° C. / sec or more and 100° C. / sec or less.
[0085] (H) A process of obtaining a steel sheet by holding at the second heating temperature for 300 to 1800 seconds. After step (G), the steel sheet is held at the second heating temperature for 300 to 1800 seconds to obtain a steel sheet included in the plated steel sheet according to this embodiment. If the holding time is less than 300 seconds, the bainite transformation does not proceed sufficiently, C concentration in the untransformed γ becomes insufficient, and the amount of residual γ decreases. For this reason, the holding time is set to 300 seconds or more, preferably 350 seconds or more, and more preferably 400 seconds or more. On the other hand, if the holding time exceeds 1800 seconds, the mechanical properties are hardly affected, but the productivity decreases. For this reason, the holding time is set to 1800 seconds or less, preferably 1200 seconds or less, and more preferably 600 seconds or less.
[0086] (I) A step of forming a plating layer on the steel sheet The above-mentioned plating layer is formed on the surface of the steel sheet. The conditions for forming the plating layer are not particularly limited, and a conventional plating process can be adopted. For example, when forming a hot-dip galvanized layer, the hot-dip galvanizing process may be performed by immersing the steel sheet in a hot-dip galvanizing bath at 300°C or more and 550°C or less. The plating time may be appropriately adjusted so as to ensure a desired coating weight, and is preferably, for example, 1 to 10 seconds.
[0087] In the case of alloying hot-dip galvanizing, alloying treatment may be performed after the above-mentioned hot-dip galvanizing. The alloying temperature is not particularly limited, but if the alloying temperature is too low, alloying does not proceed sufficiently, so it is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 480°C or higher. However, if the alloying temperature is too high, alloying proceeds excessively, the Fe concentration in the plating layer becomes excessive, and plating adhesion deteriorates. From this viewpoint, the alloying temperature is preferably 550°C or lower, more preferably 540°C or lower, and even more preferably 530°C or lower. The alloying time is not particularly limited, and may be adjusted so that the hot-dip galvanizing is alloyed. The alloying time is, for example, 10 to 60 seconds.
[0088] The method for producing a plated steel sheet according to the embodiment of the present invention may include other processes without departing from the scope of the present disclosure. EXAMPLES
[0089] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.
[0090] Steel having the chemical composition shown in Table 1 was cast, cooled to room temperature after casting, and then heated to 1200 to 1350°C. Then, hot rolling including rough rolling at a temperature of 1100°C or higher and finish rolling at a temperature of 920°C or higher was performed, followed by cooling after finish rolling, and coiling at a temperature of 600°C or higher to obtain a rolled sheet. This rolled sheet was pickled to remove surface scale, and then cold rolled at a rolling ratio of 40 to 50% to reduce the sheet thickness to 1.0 to 1.6 mm.
[0091] [Table 1]
[0092] The above-mentioned rolled sheet was subjected to the above-mentioned step (B1) and steps (B) to (I) under the conditions shown in Table 2 to obtain plated steel sheets of Test Nos. 1 to 10 (however, for Test Nos. 8 to 10, as described later, the steel sheet was not plated, and only the temperature history of step (I) for forming the plated layer was given). In Table 2, "-" indicates that the measurement was not performed. Although not shown in Table 2, in Test Nos. 1 to 10, step (B1) was performed during the temperature rise to the first heating temperature in step (B), the oxygen concentration at each reached temperature was 0.1 to 2%, and the temperature rise time in the oxidation treatment was 10 seconds or more and 120 seconds or less. In addition, the heating time (retention time) of the first reduction treatment (step (C1a)) and the second reduction treatment (step (C1b)) was 60 seconds or more, respectively. In addition, in step (E), the steel sheet was held at the first cooling stop temperature (i.e., the first cooling stop temperature and the second cooling start temperature were equivalent), and the "time in the temperature range from the first cooling stop temperature to the second cooling start temperature" corresponds to the holding time at the first cooling stop temperature, and the average cooling rate from the first cooling stop temperature to the second cooling start temperature was 0°C / sec. In step (F), the steel sheet was cooled to the second cooling stop temperature at an average cooling rate faster than that in step (E). In addition, in step (I), the steel sheet was immersed in a hot-dip galvanizing bath at 300°C to 550°C to perform hot-dip galvanizing treatment (plating time 1 to 10 seconds) and then alloying treatment was performed, and the alloying treatment time was 10 to 60 seconds. In Test Nos. 8 to 10, only the temperature history was given for step (I). Specifically, the steel sheet was heated to 300°C to 550°C and held for 1 to 10 seconds, and then held at the "alloying treatment temperature" shown in Table 2 for 10 to 60 seconds.
[0093] [Table 2]
[0094] The plated steel sheets of Test Nos. 1 to 10 described above were subjected to the following evaluations.
[0095] <Metal structure evaluation> For the plated steel sheets of Test Nos. 1 to 10, test pieces were taken from the end toward the center in the sheet width direction (perpendicular to the rolling direction and sheet thickness direction) so as to include a position of W (sheet width) / 4, and a cross section parallel to the rolling direction and sheet width direction and located at 1 / 4 of the sheet thickness from the steel sheet surface included in the plated steel sheet was exposed by nital etching. The cross section was observed by SEM, and the sum of the area ratio of ferrite and the area ratio of upper bainite, the area ratio of tempered martensite, and the area ratio of MA were obtained by the above-mentioned method. In addition, an X-ray diffraction pattern was obtained from the cross section using Co-Kα rays as characteristic X-rays, and the volume ratio of retained γ was obtained by the above-mentioned method. Note that no structure other than pearlite and cementite was observed in the remaining structure, and the total of the remaining structure was 10 area % or less.
[0096] <Method for measuring decarburization behavior: Carbon profile measurement by GD-OES> As described below, the carbon profile was measured by GD-OES (glow discharge optical emission spectrometry) to investigate the decarburization behavior.
[0097] (Sample Preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. After that, samples were prepared by degreasing in the usual manner. Then, using the samples, the mass% concentration of each element was measured by GD-OES under the following conditions.
[0098] (Measurement conditions) Equipment used: Horiba, Ltd. Marcus type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler2 Sputtering method: Normal sputtering Measurement range: φ4mm Gas type: Ar Analyzed elements: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this embodiment, the evaluation was performed on these elements, but if elements other than the above are contained in, for example, the plating layer and / or the steel sheet, the elements other than the above will also be analyzed.)
[0099] (Measurement method) GD-OES measurements were performed on the plated surface of the sample up to a depth of 150 μm in the plate thickness direction.
[0100] (Analysis method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample after the analysis was completed was measured, and the value (sputtering depth) was plotted on the horizontal axis.
[0101] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below.
[0102] Sputter weight of element i per unit time W i (g / sec) and luminescence intensity I i The relationship is expressed by the following formula (3) using the slope a and intercept b of the calibration curve. W i =aI i +b...Formula (3) The sputter weight W of the above element i per unit time i is the concentration C i (wt.%), density ρ(g / cm 3 ), and the sputtering rate Δd (cm / sec) of the reference sample are known. 2 ) and is calculated using the following formula (4). W i =C i ×ρ×Δd×S...Equation (4)
[0103] W i Using two or more reference samples with known emission intensities I i was measured, the slope a and intercept b of the above formula (3) were determined, and a calibration curve was created with the emission intensity on the horizontal axis and the sputter weight on the vertical axis. The reference materials used are shown in Table 3 below. Using the created calibration curve, the sputter weight was determined from the emission intensity of each target element, and the concentration was converted from the weight ratio. Note that the calibration curve used to convert the O concentration was corrected using SiO2 so that the concentration ratio of Si to O was 1:2.
[0104] [Table 3]
[0105] Then, the carbon analysis results were used to obtain a carbon profile, an example of which is shown in Figure 1. Figure 1 shows the carbon profiles of Test No. 5 and Test No. 7. In Figure 1 above, the carbon profiles of all materials have a carbon concentration peak within the surface layer of 20 μm (more specifically, in the internal oxide layer). However, in Test No. 7, the carbon concentration is higher than the bulk carbon concentration, whereas in Test No. 5, the carbon concentration is kept sufficiently lower than the bulk carbon concentration.
[0106] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were obtained. The bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by normal steel analysis. For example, when the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.
[0107] <Evaluation of tensile strength, yield stress, yield ratio, elongation and tensile strength variation in the plate width direction> JIS No. 5 test pieces (plate-shaped test pieces) were taken so that the longitudinal direction of the test pieces was the sheet width direction in a plane parallel to the cold-rolled rolling surface of the steel sheet. As for the sampling positions, assuming the sheet width to be W, the test pieces were taken from five locations: two locations at W / 8 from both ends toward the center in the sheet width direction, two locations at W / 4 from both ends toward the center, and one location in the center. Using the test pieces, tensile tests were conducted in accordance with JIS Z 2241:2011 to measure the tensile strength TS, yield stress YS, and elongation EL. The yield ratio YR was calculated as YS / TS. The minimum tensile strength TS at the above five locations was calculated. minExamples where the yield ratio was 980 MPa or more were evaluated as sufficient, and examples where the yield ratio was less than 980 MPa were evaluated as insufficient. Examples where the yield ratio was 0.55 to 0.75 were evaluated as sufficient, and examples where the yield ratio was outside the range of 0.55 to 0.75 were evaluated as insufficient. Examples where the elongation EL was 19% or more were evaluated as sufficient, and examples where the elongation EL was less than 19% were evaluated as insufficient. Note that for each physical property value other than tensile strength, the value measured using a test piece taken from a single location at a position W / 4 from both ends toward the center in the sheet width direction was used.
[0108] <Hole expansion ratio evaluation> For Test Nos. 1 to 10, a hole expanding test specified in JIS Z 2256:2010 was performed to measure the hole expanding ratio λ. Examples with a hole expanding ratio λ of 20% or more were evaluated as sufficient, and examples with a hole expanding ratio λ of less than 20% were evaluated as insufficient.
[0109] <Evaluation of limit bending strength (R / t)> The bendability of test Nos. 1 to 10 was evaluated by the following procedure. A test piece with a width of 40 mm and a length of 100 mm was prepared by taking the major axis in the plate width direction, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. The bending radius was changed from 0 to 7 mm to obtain the minimum bending radius at which the material could be bent without breaking, and this was taken as the limit bending radius R (mm). The limit bending radius R (mm) / plate thickness t (mm) was calculated. Then, examples with a limit bending radius R (mm) / plate thickness t (mm) of 2.0 or less were evaluated as having excellent bendability, and examples with a limit bending radius R (mm) / plate thickness t (mm) of more than 2.0 were evaluated as having poor bendability.
[0110] The results are shown in Table 4. In Table 4, "-" indicates that the measurement was not performed. In addition, in Table 4, "F+UB" is the sum of the area ratios of ferrite and upper bainite, "M" is the area ratio of tempered martensite, "MA" is the area ratio of MA, "residual γ" is the volume ratio of retained austenite, and "maximum carbon concentration of surface layer" is the maximum carbon concentration (mass%) in the region from the surface of the steel sheet to 20 μm in the sheet thickness direction.
[0111] [Table 4]
[0112] From the results in Table 4, the following can be considered. Test Nos. 1 to 4 in Table 4 all satisfied the requirements stipulated in the embodiment of the present invention, exhibited high strength, a predetermined yield ratio, and high workability, and satisfied formula (1). Furthermore, Test Nos. 1 to 4 satisfied the requirements for exhibiting excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and were excellent in bendability. On the other hand, all of Test Nos. 5 to 7 in Table 4 did not satisfy the requirements defined in the embodiment of the present invention, and were unsatisfactory in the evaluation of the variation in strength, yield ratio, workability and / or tensile strength in the sheet width direction.
[0113] In Test No. 5, the first heating temperature in step (B) was less than 850° C., so that the variation in the tensile strength in the sheet width direction became large. However, Test No. 5 met the requirements for exhibiting excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and was excellent in bendability.
[0114] In Test No. 6, since the first heating temperature exceeded 910°C, the total of ferrite and upper bainite was less than 30 area % and tempered martensite exceeded 45 area %, resulting in a yield ratio YR exceeding 0.75. However, Test No. 6 met the requirements for exhibiting excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and was excellent in bendability.
[0115] In Test No. 7, the first heating temperature in step (B) was less than 850° C., so the variation in tensile strength in the sheet width direction was large. In addition, the dew point in step (C1b) was less than −25° C. and lower than the dew point in step (C1a), so the requirement for excellent bendability (satisfying at least one of the above-mentioned (I) and (II)) was not met, and therefore the bendability was poor.
[0116] In Test No. 8, the C content exceeded 0.300 mass%, the Al content was less than 0.300 mass%, and the first heating temperature in step (B) exceeded 910°C, so the total of ferrite and upper bainite was less than 30 area%, tempered martensite was more than 45 area%, and MA was less than 5 area%, the yield ratio YR exceeded 0.75, and the elongation EL was less than 19%.
[0117] In test No. 9, the Ti content was less than 0.010 mass%, the first cooling stop temperature in step (D) was less than 350°C, and the holding time in the second heating in step (H) was less than 300 seconds, so the total of ferrite and upper bainite was less than 30 area%, tempered martensite was more than 45 area%, and MA was less than 5 area%, and the yield ratio YR was more than 0.75 and the elongation EL was less than 19%.
[0118] In Test No. 10, the first heating temperature in step (B) exceeded 910°C and the second cooling stop temperature in step (F) exceeded 300°C, so that the tempered martensite was less than 10 area % and the MA was more than 35 area %, the yield ratio YR was less than 0.55, the elongation EL was less than 19%, and the hole expansion ratio λ was less than 20%.
Claims
1. A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet satisfying the following formulas (1) and (2): The steel sheet included in the plated steel sheet is C: 0.150 to 0.300% by mass, Si: 0.80 to 2.20% by mass, Mn: 1.60 to 2.80% by mass, Al: 0.300 to 0.800% by mass, Ti: 0.010 to 0.050% by mass, P: 0.050% by mass or less (including 0% by mass), S: 0.0100% by mass or less (including 0% by mass), N: 0.0100% by mass or less (including 0% by mass), and The balance is composed of iron and inevitable impurities, and The metal structure has a total of ferrite and upper bainite of 30 to 70 area %, tempered martensite of 10 to 45 area %, MA of 5 to 35 area %, and retained austenite of 5 to 20 volume %. Galvanized steel sheet. T.S. max -DS min <20MPa ・・・(1) TS min ≧980MPa ・・・(2) In formulas (1) and (2), T.S. max is the maximum value of the tensile strength at five different points in the sheet width direction of the plated steel sheet, and TS min is the minimum value of the tensile strength at the five points, The five locations are, in the plate width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the plate width.
2. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Nb: more than 0 mass % and 0.20 mass % or less and V: more than 0 mass % and 0.50 mass % or less.
3. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Ni: more than 0 mass% and 2.0 mass% or less, Cr: more than 0 mass% and 2.0 mass% or less, and Mo: more than 0 mass% and 0.50 mass% or less.
4. The plated steel sheet according to claim 1 , further comprising B: more than 0 mass % and 0.0050 mass % or less.
5. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Mg: more than 0 mass% and 0.040 mass% or less, REM: more than 0 mass% and 0.040 mass% or less, and Ca: more than 0 mass% and 0.040 mass% or less.
6. In the plate thickness direction, 2. The plated steel sheet according to claim 1, wherein a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
7. 2. The plated steel sheet according to claim 1, wherein a maximum carbon concentration (mass%) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of a bulk carbon concentration.
8. A step of hot rolling a steel having a component composition according to any one of claims 1 to 5 to obtain a rolled plate; A first heating step of heating the rolled plate to a first heating temperature of 850° C. or more and 910° C. or less; After the first heating step, a step of maintaining the first heating temperature for 5 to 1800 seconds; After the holding step, a first cooling step of cooling to a first cooling stop temperature of 350 ° C. to 750 ° C.; a retention step in which, after the first cooling step, from the first cooling stop temperature to a second cooling start temperature which is 350° C. to the first cooling stop temperature, the average cooling rate is 10° C. / sec or less, which is slower than the average cooling rate in the first cooling step, and the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is 20 to 300 seconds; After the retention step, a second cooling step is performed in which the steel sheet is cooled from the second cooling start temperature to a second cooling stop temperature of 100 to 300° C. at an average cooling rate faster than that of the retention step; After the second cooling step, a second heating step of heating to a second heating temperature of 300 to 500° C.; After the second heating step, a step of obtaining a steel sheet by holding the steel sheet at the second heating temperature for 300 to 1800 seconds; forming a plating layer on the steel sheet; The method for producing a plated steel sheet according to any one of claims 1 to 7, comprising:
9. After the step of obtaining the rolled plate, an oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750° C., The holding step includes a first reduction treatment having a dew point of −35 to −15° C., followed by a second reduction treatment having a dew point of −25 to 0° C., which is higher than the dew point of the first reduction treatment. The manufacturing method according to claim 8.
Citation Information
Patent Citations
HIGH STRENGTH COLD ROLLED STEEL SHEET EXCELLENT IN PROCESSABILITY AND COLLISION CHARACTERISTICS AND HAVING TENSILE STRENGTH OF 980 MPa OR MORE, AND MANUFACTURING METHOD THEREFOR
JP2016194139A