Resin composition, resin sheet, laminate, sheet cured product and circuit board material
The resin composition with styrenic and olefinic thermoplastic elastomers and a crosslinking agent addresses high-frequency dielectric loss and heat resistance issues in circuit boards by forming a crosslinked structure with improved crosslinking density, achieving low dielectric and heat-resistant properties.
Patent Information
- Application Number
- JP2024033314
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-11
AI Technical Summary
Existing thermosetting resins and polymer compositions do not adequately address high-frequency dielectric loss and heat resistance issues in circuit board materials, particularly in the GHz range, and struggle with forming a mesh structure for improved heat resistance.
A resin composition incorporating styrenic thermoplastic elastomer, olefinic thermoplastic elastomer, and ethylene polymer, along with a specific crosslinking agent, forms a crosslinked structure with enhanced crosslinking density, improving heat resistance and maintaining low dielectric properties.
The composition achieves low dielectric properties and heat resistance, suitable for high-frequency applications, by forming a pseudo-higher crosslinking density through entangled molecular chains, enhancing elastic modulus and heat resistance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a resin sheet, a laminate, a cured sheet, and a circuit board material. [Background technology]
[0002] In recent years, with the increasing performance and functionality of electrical and electronic devices, the speed of communication and the amount of information transmitted have increased. To this end, communication frequencies are becoming higher and higher. When a digital signal is sent to a circuit board, part of the transmitted digital signal undergoes thermal transformation within the circuit board. The amount of transmission loss is expressed as the product of the dielectric constant and the dielectric loss tangent, To achieve low-loss communication, materials with low dielectric constant and dielectric loss tangent, i.e., low dielectric properties, are required. In particular, transmission signals in the high frequency range are more easily converted into heat. Due to these trends, there is a demand for materials with lower dielectric properties. On the other hand, as the circuits in electrical and electronic equipment become more highly integrated, the amount of heat generated inside the electrical and electronic equipment also increases. Therefore, circuit board materials are also required to have heat resistance.
[0003] For example, Patent Document 1 describes a material that has low moisture absorption, excellent heat resistance, mechanical properties, electrical properties, etc. Polyimide containing unsaturated groups is a thermosetting resin suitable for sealing and bonding electronic parts. It is characterized by being composed of phenylene ether resin and a compound containing a benzocyclobutene group. The thermosetting resin is disclosed as a compound containing a benzocyclobutene group. Vinylsiloxane bisbenzocyclobutene (CYCLOTENE® 3022, (manufactured by The Dow Chemical Company) is disclosed. Patent Document 2 describes copolymerized alkyl, heteroatom-containing alkyl, aryl, and heptane. one or more groups selected from the group consisting of aryl containing a heteroatom, and aryloxy containing a heteroatom; One or more addition-polymerizable arylcyclobutene-containing monomers having as cyclobutene ring substituents a monomer A, one or more second aromatic addition polymerizable monomers, and a third addition polymerizable nitrogen heterocyclic monomer. a ring-containing monomer, a fourth addition polymerizable monomer, or one or more of said third monomers, and one or more other addition-polymerizable monomers selected from both of the one or more fourth monomers; A polymer composition is disclosed that includes a monomer mixture of: [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-194549 [Patent Document 2] JP 2019-085562 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the thermosetting resin described in Patent Document 1 has a high frequency range (GHz order) The dielectric tangent of the material was insufficient and further improvement was required. In addition, the polymer composition described in Patent Document 2 has a low crosslink density in the cured product, and a network is formed during crosslinking. It was difficult to form a mesh structure, and the improvement in heat resistance was sometimes insufficient.
[0006] Therefore, an object of the present invention is to provide a sheet cured product and a circular molded product having low dielectric properties and heat resistance. A substrate material, and a cured sheet having low dielectric properties and heat resistance. The present invention provides a resin composition, a resin sheet, and a laminate that can be used to produce a circuit board material. [Means for solving the problem]
[0007] As a result of intensive research into solving the above problems, the present inventors have found that a specific crosslinking agent is added to a thermoplastic resin. It has been found that the above problems can be solved by adding
[0008] The gist of the present invention is as follows.
[0009] [1] Styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers and ethylene At least one thermoplastic resin (A1) selected from the group consisting of olefin-based polymers and the following general A resin composition comprising a polymer compound (B) having a repeating unit represented by formula (1). .
[0010] [ka]
[0011] (In formula (1), R 11 ~R 13 each independently represents a hydrogen atom or an alkyl group; R 14 each independently represents an oxygen atom, an alkylene group which may have a substituent, or Ar represents an aromatic hydrocarbon ring group. 11 Each of the groups may independently have a substituent. represents an aromatic hydrocarbon ring group; 11 each independently represents one of the following groups which may have a substituent: A bridging group represented by the general formula (2). Subscript n 11 is an integer between 0 and 10, n 12 teeth, n, an integer between 0 and 5 13 is an integer between 1 and 2.)
[0012] [ka]
[0013] (In formula (2), ring Ar 21 represents an aromatic hydrocarbon ring, and the symbol * represents the Ar 11 The bond to formula (2) is Ar 21 )
[0014] [2] The above-mentioned thermoplastic resin (A1) contains a styrene-based thermoplastic elastomer. The resin composition according to [1]. [3] The styrene content of the styrene-based thermoplastic elastomer is 10% by mass or more and 70% by mass or less. % or less. [4] R of the polymer compound (B) 11 ~R 13 are all hydrogen atoms, as shown in [1] above. The resin composition according to any one of items [3] to [3]. [5] n of the polymer compound (B) 11 and n 12 are all 0, and n 13 is 1 The resin composition according to any one of the above [1] to [4]. [6] The resin according to any one of the above [1] to [5], which is substantially free of a polymerization initiator. composition. [7] Any of the above [1] to [6], which contains a cyclic polyolefin resin copolymer (A2). 1. The resin composition described in Item 1. [8] The cyclic polyolefin resin copolymer (A2) has an alicyclic group in a side chain of the polyolefin. The resin composition according to [7], which is a copolymer having a structure. [9] A resin sheet comprising the resin composition according to any one of the above [1] to [8].
[10] A laminate having a release film on one or both sides of the resin sheet according to [9] above. Layered body.
[11] A sheet cured product obtained by curing the resin sheet described in [9] above.
[12] A circuit board comprising an insulating layer made of the resin sheet according to the above item [9] and a conductor laminated thereon. board material. Effect of the Invention
[0015] According to the present invention, a sheet cured product and a circuit board material having low dielectric properties and heat resistance are provided. and a cured sheet and a circuit board having low dielectric properties and heat resistance. It is possible to obtain a resin composition from which materials can be manufactured, a resin sheet and a laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below. The following description is an example of the embodiment of the present invention. The present invention is not limited to the following description unless it deviates from the gist of the present invention. In the following, when the expression "~" is used, it means that the numerical values or physical properties before and after it are included. shall be used as such.
[0017] [Resin composition] The resin composition of the present invention (hereinafter also referred to as "the composition") is a styrene-based thermoplastic elastomer. Thermoplastic elastomers, olefin-based thermoplastic elastomers, and ethylene-based polymers. At least one thermoplastic resin (A1) having a specific structure and a polymer compound (B) having a specific structure. Contains: The reason why the heat resistance of the sheet cured product and the circuit board material made of this composition is good is unclear. However, when the composition is cured, the amount of the polymer compound (B) in the thermoplastic resin (A1) increases. A crosslinked structure is formed from the reaction points, or a polymer compound is reacted with the thermoplastic resin (A1). This is thought to be because the molecular chains of substance (B) become entangled, resulting in a pseudo-high cross-link density. In particular, the polymer compound (B) has a higher molecular weight than the benzocyclobutene compound described in Patent Document 2. Since there are many crosslinking points, the crosslinking density is higher, the elastic modulus at high temperatures is improved, and heat resistance is improved. It is considered to be favorable. Each component of the composition will now be described.
[0018] 1.Thermoplastic resin (A1) The thermoplastic resin (A1) of the present composition is a styrene-based thermoplastic elastomer, an olefin-based At least one selected from the group consisting of thermoplastic elastomers and ethylene polymers. do.
[0019] The styrene-based thermoplastic elastomer is, for example, styrene-butadiene-styrene. styrene-isoprene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer ( SIS) and hydrogenated styrene-ethylene-butadiene-styrene block copolymers Styrene-ethylene-propylene-styrene block copolymer (SEBS), PS), styrene-isobutylene-styrene block copolymer (SIBS), etc. can be.
[0020] The above olefin-based thermoplastic elastomer contains polyolefin as the hard segment. and contains a rubber component as a soft segment. The olefin-based thermoplastic elastomer is a mixture of polyolefin and rubber components (polyolefin). A crosslinked product obtained by crosslinking a polyolefin with a rubber component may be used. Alternatively, it may be a polymer obtained by polymerizing a polyolefin and a rubber component. The polyolefin includes polypropylene, polyethylene, and the like. The rubber component may be isoprene rubber, butadiene rubber, butyl rubber, propylene- Butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-isoprene rubber Diene rubbers such as ethylene-propylene non-conjugated diene rubbers, ethylene-butadiene co-rubbers, etc. Polymer rubber and the like.
[0021] The ethylene polymer includes a homopolymer of ethylene and a polymer of ethylene and another monomer. Copolymers of the above are also included. The copolymer of ethylene and another monomer preferably contains ethylene as a main component. Here, "mainly composed of ethylene" means that the copolymer contains 50 ethylene structural units. % or more, preferably 60 mol % or more. In addition, the other monomers copolymerized with ethylene are preferably any monomers copolymerizable with ethylene. Not limited to. Preferred examples of the ethylene polymer include low density polyethylene (LDPE), linear Low density polyethylene (LLDPE), a polyethylene obtained by polymerization using a metallocene catalyst. Among them, linear low density polyethylene ( It is preferable to use LLDPE.
[0022] Among the thermoplastic resins (A1) exemplified above, the thermoplastic resin (A1) is particularly preferred as a polymerizable resin. When a combination that reacts with the thermoplastic resin (A1) and the polymer compound (B) is selected, It is believed that (B) and (C) form a crosslinked structure with each other, which can further improve heat resistance. From this point of view, among the above thermoplastic resins (A1), those having more unsaturated double bonds are preferred. This is preferable, but the balance with low dielectric properties must be considered.
[0023] On the other hand, among the above-mentioned thermoplastic resins (A1), the thermoplastic resin (A1) itself is particularly When a combination is selected in which the polymer compound (B) is unlikely to react with the thermoplastic resin (C), The polymer (A1) and the polymer compound (B) form an interpenetrating polymer network structure (hereinafter referred to as "semi-IPN structure"). It is believed that this will improve the low dielectric properties and heat resistance. In the PN structure, a thermoplastic resin (A1) and a polymer compound (B) form a chemical bond. The molecular chains of the thermoplastic resin (A1) and the polymer compound (B) are mutually partially and physically bonded to each other. By forming this semi-IPN structure, the thermoplastic resin (A 1) While maintaining the low dielectric properties, it has a pseudo crosslink density compared to the thermoplastic resin (A1) alone. Therefore, it is considered that the elastic modulus is improved and the heat resistance is good. Among the above thermoplastic resins (A1), styrene-based thermoplastic elastomers are preferred. Styrene-isobutylene-styrene block copolymer (SIBS) or styrene- Ethylene-butadiene-styrene block copolymer (SEBS) is more preferred, and styrene More preferred is styrene-ethylene-butadiene-styrene block copolymer (SEBS).
[0024] When a styrene-based thermoplastic elastomer is used as the thermoplastic resin (A1), the styrene The styrene content of the styrene-based thermoplastic elastomer is preferably 10% by mass or more, and more preferably 15% by mass or more. More preferably, the content is 70% by mass or less, and more preferably 60% by mass or less. It is more preferably 50% by mass or less, and even more preferably 40% by mass or less. When the styrene content is within the above range, the thermoplastic resin (A1) has a low dielectric tangent and a low elasticity. The modulus is also moderate, so it is possible to achieve both low dielectric properties and heat resistance, and it is also easy to handle. .
[0025] The weight average molecular weight (Mw) of the thermoplastic resin (A1) is such that the resulting resin sheet has tackiness. From the viewpoint of preventing this from occurring, 30,000 or more is preferable, and 40,000 or more is more preferable. It is preferable that the molecular weight is 50,000 or more, and more preferable that the molecular weight is 50,000 or more. Preferably, it is 300,000 or less, more preferably 250,000 or less, and more preferably 200,000 or less. It is more preferable that the value is 0 or less. In the present invention, the weight average molecular weight (Mw) is measured by gel permeation chromatography. This is a polystyrene equivalent value determined by the calculation.
[0026] The thermoplastic resin (A1) may be modified by a known method. For example, the above-mentioned thermoplastic resin (A1) and an unsaturated carboxylic acid and / or anhydride thereof may be used. The reaction products include: By modifying the thermoplastic resin (A1), the polarity of the polymer increases, so that it is possible to apply the resin to copper foil, etc. This is expected to improve adhesion to the metal layer.
[0027] Examples of the unsaturated carboxylic acid and / or its anhydride include acrylic acid, methacrylic acid, and the like. Acetic acid, α-ethylacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, methyl Tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, sodium Examples of the unsaturated carboxylic acid include unsaturated carboxylic acids such as carboxylic acids and their anhydrides. Specific examples of the acid anhydride include maleic anhydride, citraconic anhydride, sodium anhydride, and sodium tetrahydrofuran. Examples of such acids include carboxylic acids. As for nadic acids or their anhydrides, endo-cis-bicyclo[2.2.1]he but-2,3-dicarboxylic acid (nadic acid), methyl-endo-cis-bicyclo[2.2. 1] Hept-5-ene-2,3-dicarboxylic acid (methylnadic acid) and its anhydrides Some examples include:
[0028] Among these unsaturated carboxylic acids and / or their anhydrides, acrylic acid, maleic acid, Nadic acid, maleic anhydride, and nadic anhydride are preferred. The unsaturated carboxylic acid and / or anhydride thereof may be used alone or in combination of two or more. may be used.
[0029] The content of the thermoplastic resin (A1) in the present composition is set to be 0.01 to 0.1% by weight from the viewpoint of low dielectric properties. Of the resin components, 60% by mass or more is preferable, 70% by mass or more is more preferable, and 80% by mass or more is more preferable. % or more, more preferably 85% by mass or more, and even more preferably 85% by mass or more. However, the resin component of the present composition is not limited to the above, and may be only the thermoplastic resin (A1) (100 mass %). This is also fine. In the present invention, the term "resin component" refers to the thermoplastic resin (A1) contained in the present composition, Cyclic polyolefin resin copolymer (A2) and other resins added as necessary. (However, polymer compound (B) is excluded.)
[0030] The storage modulus of the thermoplastic resin (A1) at 24°C is preferably 0.1 MPa or more, More preferably, the pressure is 1 MPa or more. Also, the pressure is preferably less than 2000 MPa, and more preferably less than 1500 MPa. More preferably, it is less than 1000 MPa, and even more preferably, it is less than 500 MPa. is preferred, less than 300 MPa is particularly preferred, and less than 100 MPa is especially preferred. Most preferably, it is less than 50 MPa. By controlling the storage modulus to be less than the above upper limit, the flexibility of the obtained sheet cured product is good. In addition, by setting the storage modulus to be equal to or greater than the above lower limit, the heat resistance of the obtained cured sheet is improved. The durability and handling properties are improved. The storage modulus was measured using a resin sheet having a thickness of 300 μm and made of a thermoplastic resin (A1). The test piece was made of the sheet cured product obtained by heat pressing for 30 minutes at 250°C and 0.2 MPa. This value was determined by measuring the dynamic viscoelasticity.
[0031] The density of the thermoplastic resin (A1) measured by the immersion method (ISO 1183) is 0. 98g / cm 3 Less than 0.95 g / cm is preferred. 3 Less than 0.91g / is more preferable. cm 3 On the other hand, the lower limit is not particularly limited, but is preferably 0.80 g / cm 3 Below Above is preferred. When the density is equal to or less than the above value, the flexibility of the obtained cured sheet is good.
[0032] The dielectric tangent of the thermoplastic resin (A1) is preferably less than 0.003 at 10 GHz, and more preferably less than 0.003 at 10 GHz. It is more preferably less than 0.002, and even more preferably less than 0.0015. It is not set, but should be 0 or greater. The smaller the dielectric tangent, the smaller the dielectric loss. This results in higher efficiency and speed in the transmission of electrical signals. The above dielectric tangent was measured using a 300 μm thick resin sheet made of thermoplastic resin (A1). The test pieces were heat-pressed at 250°C and 0.2 MPa for 30 minutes to obtain hardened sheets. The dielectric constant and dielectric loss tangent of the cured sheet in the in-plane direction were measured using a cavity resonator (manufactured by AET Co., Ltd.). The measurements were performed in TE mode using a network analyzer MS46 122B (manufactured by Anritsu). This is the value obtained.
[0033] 2. Cyclic polyolefin resin copolymer (A2) The present composition is a cyclic ... The resin composition may contain a fibrous polyolefin resin copolymer (A2). The reason for the improvement in heat resistance, linear thermal expansion coefficient, and tackiness is unclear, but it is believed that the thermoplastic By containing the cyclic polyolefin resin copolymer (A2) together with the soluble resin (A1), This is thought to be because a rigid skeleton is adopted by the fetus. The cyclic polyolefin resin copolymer (A2) is a copolymer having an alicyclic structure. Specifically, it is a copolymer having an alicyclic structure in the side chain of a polyolefin. Suitable examples of the structure include cycloalkanes, bicycloalkanes, polycyclic compounds, etc. Among these, cycloalkanes are preferred, and cyclohexane is more preferred. The alicyclic structure is a hydrogenated aromatic vinyl polymer block unit described below. More preferably, it is an alicyclic structure generated by hydrogenation of an aromatic ring.
[0034] The cyclic polyolefin resin copolymer (A2) has a crystal melting peak temperature of less than 100° C. It is preferable to do so. The crystalline melting peak temperature of the cyclic polyolefin resin copolymer (A2) is preferably 50° C. or higher. The temperature is preferably 60° C. or higher, more preferably 65° C. or higher. The crystalline melting peak temperature of the copolymer is preferably 90°C or less, more preferably 85°C or less. I wish. The crystal melting peak temperature in the present invention is the differential scanning calorimetry measured at a heating rate of 10° C. / min. This is the temperature at which a crystal melting peak is detected in the differential scanning calorimetry (DSC). The cyclic polyolefin resin copolymer (A2) used in the product has a crystal melting peak of less than 100°C. For example, the crystal melting point exists at two points, below 100℃ and above 100℃. This includes cases where a peak exists.
[0035] The known cyclic polyolefins include monocyclic norbornene monomers or polycyclic norbornene monomers. Hydrogenated ring-opening polymers having repeating units derived from triboroylene monomers (e.g., International Publication No. 2012 / 046443, International Publication No. 2012 / 033076, etc. This cyclic polyolefin has an alicyclic structure in the polymer main chain, and The solution peak temperature does not exist below 100°C, or the material is amorphous. The crystallinity of a polymer usually changes due to the regularity of the molecular structure and steric hindrance. Polymers that have an alicyclic structure in the chain or main chain are difficult to crystallize due to large steric hindrance, and remain amorphous. It's easy to become. On the other hand, the cyclic polyolefin resin copolymer (A2) of the present resin composition is a hydrogenated copolymer described later. The copolymer has a structure of diphenylene polymer block units, which gives it crystallinity and also gives it a polyolefin structure. The alicyclic structure in the side chain of the polyolefin reduces the crystal melting peak temperature to less than 100°C. can be present in its entirety.
[0036] The melt flow rate (MFR) of the cyclic polyolefin resin copolymer (A2) is particularly Although not limited, it is usually 0.1 g / 10 min or more, and from the viewpoint of the molding method and the appearance of the molded product, Preferably, the melt flow rate (MFR) is 0.5 g / 10 min or more. is usually 200g / 10min or less, and from the viewpoint of material strength, preferably 100g / 1 0 minutes or less, more preferably 90.0 g / 10 minutes or less. This improves compatibility with the thermoplastic resin. The MFR is based on ISO R1133, with a measurement temperature of 230°C and a measurement load of 2.16 kg. It can be determined by measuring under certain conditions.
[0037] The cyclic polyolefin resin copolymer (A2) used in the present resin composition has low dielectric properties. In view of the above, at least one hydrogenated aromatic vinyl polymer block unit and at least Cyclic polyolefins containing one type of hydrogenated conjugated diene polymer block unit (hereinafter referred to as "cyclic polyolefins") Polyolefin (a) or the unsaturated carboxylate of said cyclic polyolefin (a) Preferred are those modified with at least one of carboxylic acid and its anhydride.
[0038] In the present invention, a "block" refers to a structurally or compositionally distinct polymer segment of a copolymer. Microphase separation refers to polymerized segments of a copolymer that exhibit microphase separation from the lamina. It results from the immiscibility of polymerized segments in block copolymers. For more information on microphase separation and block copolymers, see the 1999 issue of PHYSICS TODAY. “Block Copolymers-Designer So” on pages 32-38 of the February issue This is discussed extensively in the paper “Fiber-Based Materials.”
[0039] The cyclic polyolefin (a) is a hydrogenated aromatic vinyl polymer block unit (hereinafter referred to as "block unit"). Block A) and hydrogenated conjugated diene polymer block units (hereinafter referred to as "Block B"). A diblock copolymer consisting of at least one of block A and block B. Triblock copolymers, tetrablock copolymers, pentablock copolymers containing 2 or more Marr et al. The cyclic polyolefin (a) preferably contains at least two blocks A, for example Suitable examples include the ABA type, ABAB type, and ABABA type.
[0040] The cyclic polyolefin (a) is a cyclic polyolefin having an aromatic vinyl polymer at each end. It is preferable that the hydrogenated block copolymer of the present resin composition contains a segment. has at least two hydrogenated vinyl aromatic polymer block units (block A), Between the two hydrogenated aromatic vinyl polymer block units (block A), at least It is preferable that the copolymer has one or more hydrogenated conjugated diene polymer block units (Block B). From these viewpoints, the cyclic polyolefin (a) is an ABA type or an ABAB type. Type A is more preferred.
[0041] Hydrogenated aromatic vinyl polymer block units (blocks) in the cyclic polyolefin (a) The content of (A) is preferably 30 to 99 mol%, more preferably 40 to 90 mol%. Among them, more preferably 50 mol % or more, and even more preferably 60 mol % or more. It is. If the ratio of hydrogenated aromatic vinyl polymer block units (block A) is equal to or greater than the above lower limit, If the ratio is high, the rigidity will not decrease and the heat resistance and linear thermal expansion coefficient will be good. If it is equal to or less than the upper limit, the flexibility is good.
[0042] In addition, the hydrogenated conjugated diene polymer block unit (block unit) in the cyclic polyolefin (a) The content of block B) is preferably 1 to 70 mol %, more preferably 10 to 60 mol %. Among them, it is more preferable that the content is 50 mol % or less, and even more preferable that the content is 40 mol % or less. Below. If the ratio of hydrogenated conjugated diene polymer block units (block B) is equal to or greater than the lower limit above, On the other hand, if the ratio is equal to or less than the upper limit, the rigidity is not decreased. The heat resistance and linear thermal expansion coefficient are also good.
[0043] Hydrogenated aromatic vinyl polymer block units constituting the cyclic polyolefin (a) and water The halogenated conjugated diene polymer block units are each formed of an aromatic vinyl monomer and a The polymer block is composed of conjugated diene monomers such as butadiene and 1,3-butadiene. This can be obtained by The cyclic polyolefin (a) is preferably a block copolymer having no functional groups. "No functional group" means that no functional group is present in the block copolymer, i.e. That is, it means that there are no groups containing atoms other than carbon and hydrogen atoms.
[0044] The aromatic vinyl polymer block units and the conjugated diene polymer block units before hydrogenation are described below. The monomers for forming the block units will now be described.
[0045] (Aromatic vinyl monomer) The aromatic vinyl monomers used as raw materials for the aromatic vinyl polymer block units before hydrogenation are It is a monomer represented by the following general formula (1).
[0046] [ka]
[0047] In the above general formula (1), R is hydrogen or an alkyl group, and Ar is a phenyl group, a halo group, Phenyl group, alkylphenyl group, alkylhalophenyl group, naphthyl group, pyridinyl group Or an anthracenyl group.
[0048] When R is an alkyl group, the number of carbon atoms is preferably 1 to 6. Halo groups, nitro groups, amino groups, hydroxy groups, cyano groups, carbonyl groups and carboxyl groups. The aryl group may be mono- or polysubstituted with functional groups such as a group. Moreover, the above Ar is preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group. preferable.
[0049] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, vinyltoluene, and the like. styrene (including all isomers, especially p-vinyltoluene), ethylstyrene, propyl styrene, butyl styrene, vinyl biphenyl, vinyl naphthalene, vinyl ant Helices (including all isomers), and mixtures thereof. Among these, Styrene is preferred.
[0050] (Conjugated Diene Monomer) The conjugated diene monomers that serve as the raw material for the conjugated diene polymer block units before hydrogenation are two units. There are no particular limitations on the monomer as long as it has a conjugated double bond. Conjugated diene monomers include, for example, 1,3-butadiene, 2-methyl-1,3-butadiene, isoprene, 2-methyl-1,3-pentadiene and its analogues, Among these, bromine, which has a high structural regularity and is easily crystallized, is particularly preferred. From the viewpoint of obtaining a copolymer, 1,3-butadiene is preferred.
[0051] In addition, when 1,3-butadiene is used as the conjugated diene monomer, its polymer is Polybutadiene consists of 1,4-bonded units ([-CH2-CH=CH-CH2-]) and 1,2 -bond unit ([-CH2-CH(CH=CH2)-]), hydrogenation The former gives a structure similar to the repeating unit of polyethylene (ethylene structure), and the latter gives a 1- It gives a structure similar to the repeating unit when butene is polymerized (1-butene structure). The hydrogenated conjugated diene polymer block in the resin composition has an ethylene structure and a 1- It is preferable that the copolymer contains at least one of the butene structures. In addition, when isoprene is used as the conjugated diene monomer, the polymer polyiso Prene is a 1,4-bond unit ([-CH2-C(CH3)=CH-CH2-]), 3,4 -bond unit ([-CH2-CH(C(CH3)=CH2)-]) and 1,2-bond unit ( [-CH2-C(CH3)(CH=CH2)-]), which can be obtained by hydrogenation. The repeating unit of the present invention is at least one of the repeating units.
[0052] (Block structure) Cyclic polyolefin (a) is SBS, SBSB, SBSBS, SBSBSB, SIS , SISIS, and SISBS (where S is polystyrene, B is polybutadiene, and I is Polyisoprene means a triblock copolymer, a tetrablock copolymer, etc. It is produced by hydrogenation of multiblock copolymers such as mers, pentablock copolymers, etc. The blocks may be linear or branched. The polymerization chains, if any, may be attached at any position along the backbone of the copolymer. In addition to linear blocks, the blocks may be tapered blocks or star blocks. It is also possible.
[0053] The block copolymer constituting the cyclic polyolefin (a) before hydrogenation is an aromatic vinyl One or more additional blocks other than the polymer block unit and the conjugated diene polymer block unit. For example, in the case of a triblock copolymer, these additional The triblock units may be attached at any position on the triblock polymer backbone.
[0054] A preferred example of the hydrogenated aromatic vinyl polymer block unit is hydrogenated polystyrene. Preferred examples of the hydrogenated conjugated diene polymer block units include Examples of the polybutadiene include hydrogenated polybutadiene and hydrogenated polyisoprene. Butadiene is more preferred. A preferred embodiment of the cyclic polyolefin (a) is a mixture of styrene and butadiene. and hydrogenated triblock or pentablock copolymers of the formula: Triblock copolymers are more preferred.
[0055] (Hydrogenation level) Cyclic polyolefin (a) contains double bonds derived from conjugated dienes such as butadiene, as well as In addition, aromatic rings derived from styrene, etc. are also hydrogenated, and the resulting product is essentially completely hydrogenated. Specifically, it refers to those that have achieved the following hydrogenation levels. The hydrogenation level of the hydrogenated aromatic vinyl polymer block units is preferably 90% or more. More preferably, the content is 95% or more, even more preferably 98% or more, and particularly preferably 99.5%. That's all. The hydrogenation level of the hydrogenated conjugated diene polymer block unit is preferably 95% or more. , more preferably 99% or more, and even more preferably 99.5% or more. This high level of hydrogenation reduces dielectric loss and provides rigidity. The adhesiveness and heat resistance are also improved. The hydrogenation level of the hydrogenated aromatic vinyl polymer block unit is The percentage of the polymer block units that are saturated by hydrogenation is shown. Hydrogenated Conjugated Diene Polymer The hydrogenation level of the block unit refers to the degree to which the conjugated diene polymer block unit is saturated by hydrogenation. The ratio of the sum is shown. The hydrogenation level of each block unit is determined using proton NMR.
[0056] The cyclic polyolefin resin copolymer (A2) may be used alone or in combination of two or more. They may be used in combination. The cyclic polyolefin resin copolymer (A2) in the resin composition is a commercially available product. Specifically, TEFABLOC (registered trademark) manufactured by Mitsubishi Chemical Corporation can be used. can be done.
[0057] When the present composition contains a cyclic polyolefin resin copolymer (A2), the content thereof is From the viewpoint of reducing the expansion rate and tackiness, 10% by mass or more of the resin component of the present composition is The upper limit is preferably 15% by mass or more, more preferably 20% by mass or more. From the viewpoint of flexibility and adhesion to the substrate, the content is preferably 40% by mass or less, and more preferably 38% by mass or less. It is more preferable that the content is 35 mass % or less, and further more preferable that the content is 35 mass % or less.
[0058] 3.High molecular compound (B) The polymer compound (B) of the present composition has a repeating unit represented by the following general formula (1): It is a compound.
[0059] [ka]
[0060] (In formula (1), R 11 ~R 13 each independently represents a hydrogen atom or an alkyl group; R 14 each independently represents an oxygen atom, an alkylene group which may have a substituent, or Ar represents an aromatic hydrocarbon ring group. 11 Each of the groups may independently have a substituent. represents an aromatic hydrocarbon ring group; 11 each independently represents one of the following groups which may have a substituent: A bridging group represented by the general formula (2). Subscript n 11 is an integer between 0 and 10, n 12 teeth, n, an integer between 0 and 5 13 is an integer between 1 and 2.)
[0061] [ka]
[0062] (In formula (2), ring Ar 21 represents an aromatic hydrocarbon ring, and the symbol * represents the Ar 11 The bond to formula (2) is Ar 21 )
[0063] In addition, n in the general formula (1) 11 is 2 or more, and R 14 , Ar 11 , Q 11 , n 12 Reach Bin 13 If there are two or more, R 14 , Ar 11 , Q 11 , n 12 and n 13 That They may be the same or different. 12 and n 13 Even if is 2 or more Same here.
[0064] <Definition> In the following, in describing the polymer compound (B) according to the present invention in detail, the common partial structure Unless otherwise specified, it has the following structure:
[0065] (Aromatic hydrocarbon ring group) The aromatic hydrocarbon ring group is a group that can be aromatic depending on the bonding state in the structure of the polymer compound (B). The term "aryl" refers to a monovalent, divalent, or trivalent or higher aromatic hydrocarbon ring structure. In the aromatic hydrocarbon ring structure, the number of carbon atoms is not usually limited, but is preferably The carbon number is preferably 6 or more and 60 or less, and more preferably 48 or less. More preferably, the number of carbon atoms is 30 or less. tetracene ring, phenanthrene ring, perylene ring, tetracene ring, pyrene ring, benzpyrene ring, chrysene ring, triphenylene ring, acenaphthene ring, fluoranthene ring, fluorene ring or a group having a 6-membered monocyclic ring or 2 to 5 condensed rings, or a group having a plurality of groups selected from these When multiple aromatic hydrocarbon rings are linked, the number of linked rings is usually 2 to 1. A structure in which 0 is linked is exemplified, and a structure in which 2 to 5 is linked is preferable. When a plurality of rings are linked, the same structures may be linked or different structures may be linked. . The aromatic hydrocarbon ring structure is preferably a benzene ring, a biphenyl ring, i.e., a benzene A structure in which two rings are connected, a structure in which three terphenyl rings are connected, or a structure in which three benzene rings are connected, Phenylene rings, i.e., structures in which four benzene rings are linked together, naphthalene rings, and fluorene rings. .
[0066] (Aromatic heterocyclic group) The aromatic heterocyclic group is an aromatic heterocyclic group that can be bonded to any of the following compounds depending on the bonding state in the structure of the polymer compound (B). It refers to a monovalent, divalent, or trivalent or higher valent ring structure. In the aromatic heterocyclic structure, the number of carbon atoms is not usually limited, but preferably The carbon number is preferably 3 or more and 60 or less, and more preferably 48 or less. More preferably, the number of carbon atoms is 30 or less. Specifically, a furan ring, a benzofuran ring, a thio Phenyl ring, benzothiophene ring, pyrrole ring, pyrazole ring, imidazole ring, oxazine ring Azole ring, indole ring, carbazole ring, pyrroloimidazole ring, pyrrolopyrazole ring, pyrrolopyrrole ring, thienopyrrole ring, thienothiophene ring, furopyrrole ring, furo Furan ring, thienofuran ring, benzisoxazole ring, benzisothiazole ring, benzyl Zoimidazole ring, pyridine ring, pyrazine ring, pyridazine ring, pyrimidine ring, triazine ring, quinoline ring, isoquinoline ring, cinnoline ring, quinoxaline ring, phenanthridine ring , benzimidazole ring, perimidine ring, quinazoline ring, quinazolinone ring, azulene ring, etc. and a divalent group having a 5- or 6-membered monocyclic ring or 2- to 4-condensed ring, or a group having a plurality of these linked together. When a plurality of aromatic heterocycles are linked, they may be linked to the same structure or to different structures. When a plurality of aromatic heterocycles are linked, the number of linked aromatic heterocycles is usually 2 to 10. A structure in which 2 to 5 are linked together is preferred. The aromatic heterocyclic structure is preferably a thiophene ring, a benzothiophene ring, or a pyrimidine ring. ring, triazine ring, carbazole ring, dibenzofuran ring, and dibenzothiophene ring.
[0067] (substituent) In the following description of the structure of the polymer compound (B), unless otherwise specified, the substituents are arbitrary. It is an arbitrary group, including a crosslinking group. It is preferably a group selected from the following substituent group Z: In addition, in the description of the structure of the polymer compound (B) of the present invention, the substituents that may be present are It is preferred that the substituents which are or may be present are selected from the group Z. In the case where "a" is described as "a", preferred substituents are also as described in Substituent Group Z below.
[0068] (Substituent group Z) The substituent group Z is an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an aryl group, oxy group, heteroaryloxy group, alkoxycarbonyl group, dialkylamino group, di Arylamino group, arylalkylamino group, acyl group, halogen atom, haloalkyl group , alkylthio group, arylthio group, silyl group, siloxy group, cyano group, aromatic hydrocarbon The group consisting of aromatic heterocyclic groups, aromatic ring groups, and aromatic heterocyclic groups. These substituents may be linear, branched, or cyclic. It may include any of the structures.
[0069] The substituent group Z preferably has the following structure. Alkyl groups with 1 to 24 carbon atoms, alkenyl groups with 2 to 24 carbon atoms, Alkynyl groups with 1 to 24 carbon atoms, alkoxy groups with 4 to 36 carbon atoms, The following aryloxy or heteroaryloxy groups: alkoxy groups having 2 to 24 carbon atoms: Dicarbonyl group, dialkylamino group having 2 to 24 carbon atoms, and dialkylamino group having 10 to 36 carbon atoms arylalkylamino groups having 7 to 36 carbon atoms; Acyl groups with 24 or less carbon atoms, halogen atoms, haloalkyl groups with 1 to 12 carbon atoms, Alkylthio groups having 1 to 24 carbon atoms, arylthio groups having 4 to 36 carbon atoms, and Silyl groups with 36 or less carbon atoms, siloxy groups with 2 to 36 carbon atoms, cyano groups, an aromatic hydrocarbon ring group having 0 or less carbon atoms, and an aromatic heterocyclic group having 4 to 30 carbon atoms.
[0070] The above-mentioned substituent may have any of a linear, branched or cyclic structure, and the above-mentioned substituent may be When adjacent, the adjacent substituents may be bonded to each other to form a ring.
[0071] More specifically, the substituent group Z includes the following structures.
[0072] The alkyl group may be linear, branched, or cyclic and may have 1 or more and 24 or less carbon atoms. , preferably 12 or less, more preferably 8 or less, and even more preferably 6 or less. Specific examples include methyl, ethyl, n-propyl, i-propyl, and n-butyl groups. butyl group, i-butyl group, sec-butyl group, tert-butyl group, n-hexyl group, cyclohexyl group Examples of the alkyl group include dihexyl and dodecyl groups.
[0073] The alkenyl group is linear, branched, or cyclic and has 2 or more carbon atoms, and usually has 2 It is equal to or less than 4, and preferably equal to or less than 12. A specific example is a vinyl group.
[0074] The alkynyl group is linear or branched and has 2 or more and 24 or less carbon atoms, preferably. or less than 12. A specific example is an ethynyl group.
[0075] The alkoxy group has 1 or more and 24 or less, preferably 12 or less, carbon atoms. Examples of the alkyl group include a methoxy group and an ethoxy group.
[0076] The aryloxy group and the heteroaryloxy group have 4 or more carbon atoms, preferably 5 The alkyl group is 36 or less, and preferably 24 or less. Specific examples include a phenoxy group, a naphthalene group, and the like. butoxy group, pyridyloxy group, etc.
[0077] The alkoxycarbonyl group has 2 or more and 24 or less, preferably 12 or less, carbon atoms. Specific examples include a methoxycarbonyl group and an ethoxycarbonyl group.
[0078] The dialkylamino group has 2 or more and 24 or less, and preferably 12 or less, carbon atoms. Specific examples include a dimethylamino group and a diethylamino group.
[0079] The diarylamino group has 10 or more, preferably 12 or more and 36 or less carbon atoms. , preferably 24 or less. Specific examples include a diphenylamino group and a ditolylamino group. , and N-carbazolyl group.
[0080] The arylalkylamino group has 7 or more and 36 or less, preferably 24 or less, carbon atoms. A specific example is a phenylmethylamino group.
[0081] The acyl group has 2 or more and 24 or less, preferably 12 or less, carbon atoms. Examples of the alkyl group include an acetyl group and a benzoyl group.
[0082] The halogen atom is a fluorine atom, a chlorine atom, etc., and is preferably a fluorine atom. .
[0083] The haloalkyl group has 1 or more and 12 or less carbon atoms, and preferably 6 or less carbon atoms. Examples of the aryl groups include trichloromethyl, trifluoromethyl, pentafluoroethyl, and nonafluoromethyl. A fluorobutyl group and the like are particularly preferred, and an alkyl group substituted with fluorine is particularly preferred. Most preferably, it is a trifluoromethyl group.
[0084] The alkylthio group has 1 or more carbon atoms and usually 24 or less, preferably 12 or less. Specific examples include a methylthio group and an ethylthio group.
[0085] The arylthio group has 4 or more carbon atoms, preferably 5 or more carbon atoms, and 36 or less carbon atoms, preferably The number of carbon atoms is preferably 24 or less. Specifically, phenylthio group, naphthylthio group, pyridylthio group, etc. Examples include:
[0086] The silyl group has usually 2 or more, preferably 3 or more, and usually 36 or less, preferably 36 or less. Preferably, it is 24 or less. Specific examples include a trimethylsilyl group and a triphenylsilyl group. etc.
[0087] The siloxy group has 2 or more carbon atoms, preferably 3 or more carbon atoms, and usually has 36 or less carbon atoms, preferably The number is 24 or less. Specific examples include trimethylsiloxy groups and triphenylsiloxy groups. etc.
[0088] The aromatic hydrocarbon group has 6 or more and 36 or less, preferably 24 or less, carbon atoms. Examples of the aryl group include a phenyl group, a naphthyl group, and a group in which multiple phenyl groups are linked together. do.
[0089] The aromatic heterocyclic group has 3 or more carbon atoms, preferably 4 or more carbon atoms, and 36 or less carbon atoms, preferably The number is preferably 24 or less. Specific examples include a thienyl group, a pyridyl group, and the like.
[0090] The above-mentioned substituents may have any of a straight-chain, branched or cyclic structure. When the above-mentioned substituents are adjacent to each other, the adjacent substituents may be bonded to each other to form a ring. The preferred ring sizes are 4-, 5-, and 6-membered rings. Specific examples include cyclobutane rings. Cyclopentane ring, cyclohexane ring.
[0091] Among the above-mentioned substituent group Z, alkyl groups, aliphatic groups, and the like are preferable in order to reduce the dielectric tangent. alkoxy group, halogen atom, aromatic hydrocarbon group, more preferably alkyl group, halogen atom, aromatic hydrocarbon group, A halogen atom or an aromatic hydrocarbon group is particularly preferred. An alkyl group or an aromatic hydrocarbon group is particularly preferred. A fluorine atom is preferred, and an alkyl group or an aromatic hydrocarbon group is most preferred.
[0092] Each of the substituents in the above-mentioned substituent group Z may further have a substituent. Examples of the substituents include the same as those in the above-mentioned group Z of substituents or bridging groups. is absent, is an alkyl group having 8 or less carbon atoms, or is a halogen atom.
[0093] <R 11 ~R 13 > R in general formula (1) 11 ~R 13 are each independently a hydrogen atom or an alkyl group. . Specific examples of the alkyl group include the alkyl groups exemplified above as the substituent group Z. , preferably an alkyl group having 1 to 10 carbon atoms, and particularly preferably a methyl group. . In order to improve crosslinking and film handling properties, 11 is a hydrogen atom or carbon It is preferably an alkyl group having a number of 1 to 10, more preferably a hydrogen atom or a methyl group. A hydrogen atom is particularly preferred. For the same reason, R 12 and R 13 is a hydrogen atom It is preferable that the parent is a child.
[0094] <R 14 > R in general formula (1) 14 each independently represents an oxygen atom, an alkylene group, or an aromatic carbon atom; These represent hydrogen ring groups, and may have a substituent. Q is a bridging group 11 To keep away from the main chain, R 14 exists and tends to move away from the main chain. However, it is believed that the crosslink density increases, which can improve the handling properties of the cured film. Preferred are aromatic hydrocarbon ring groups and alkylene groups.
[0095] The alkylene group is preferably linear, branched, or cyclic and has one or more carbon atoms. The number is preferably 4 or more and 24 or less, more preferably 12 or less, and even more preferably 8 or less. More preferably, it is 6 or less. Specific examples include methane, ethane, propane, and butane. Examples of the divalent groups include those derived from isobutane, hexane, cyclohexane, and dodecane. It is preferably an alkylene group having 1 to 10 carbon atoms, and more preferably ethylene. A propylene group is preferred, and an ethylene group is particularly preferred. As the substituent of the alkylene group, the substituent group Z is preferable, and a fluorine atom is particularly preferable. It is.
[0096] Specific examples of the aromatic hydrocarbon ring group include the aromatic hydrocarbons exemplified above as the substituent group Z. As the substituent of the aromatic hydrocarbon ring group, the substituent group Z is preferable, and more preferably More preferably, it is an alkyl group having 1 to 10 carbon atoms.
[0097] <Ar 11 > Ar in general formula (1) 11 each independently represents an aromatic carbonyl group which may have a substituent; Represents a hydrogen ring group. Specific examples of the aromatic hydrocarbon ring group which may have a substituent include the above-mentioned substituent group Z and Examples of the substituent of the aromatic hydrocarbon ring group include the aromatic hydrocarbon ring groups listed above. From the viewpoint of film stability, the substituent group Z is preferred, and from the viewpoint of reducing the dielectric loss tangent, Preferably, it is an alkyl group having 1 to 10 carbon atoms.
[0098] <n 11 , n 12 and n 13 > Subscript n in general formula (1) 11 is an integer between 0 and 10. The resulting sheet hardness From the viewpoint of the heat resistance of the compound, the value is preferably 0 to 4, and particularly preferably 0. Subscript n in general formula (1) 12 is an integer from 0 to 5. From the viewpoint of the heat resistance of the product, it is preferably 0 or 1, and particularly preferably 0. Subscript n in general formula (1) 13 is an integer from 1 to 2. From the viewpoint of the heat resistance of the product, 1 is preferable.
[0099] 11 > Q in general formula (1) 11 is a structure represented by general formula (2) which may have a substituent. It is made of. Q 11 The substituent of is preferably a substituent group Z, more preferably a substituent having 1 to 10 carbon atoms. is an alkyl group up to
[0100] General formula (2) is an aromatic hydrocarbon ring group having a condensed cyclobutane ring, and is represented by the following formula: can be.
[0101] [ka]
[0102] (In formula (2), ring Ar 21 represents an aromatic hydrocarbon ring, and the symbol * represents the Ar 11 The bond to formula (2) is Ar 21 )
[0103] <Ar 21 > Ar in general formula (2) 21 represents an aromatic hydrocarbon ring. Specific examples of the aromatic hydrocarbon ring include the aromatic hydrocarbons exemplified above as the substituent group Z. Preferred are benzene ring, naphthalene ring, anthracene ring, and phenanthrene ring. From the viewpoint of solubility in the coating process, A benzene ring or a naphthalene ring is preferred.
[0104] <Specific examples of general formula (1)> The repeating unit represented by the general formula (1) in the polymer compound (B) of the present invention is Specific examples are given below, but the present invention is not limited to these.
[0105] [ka]
[0106] <Copolymerization component> The polymer compound (B) may contain any copolymer other than the repeating unit represented by the general formula (1). It may contain repeating units derived from synthetic components. The copolymerization component is not particularly limited, but may be any copolymer containing an aromatic hydrocarbon ring group which may have a substituent. It is preferable to do so. When the polymer compound (B) contains any copolymerization component, the arrangement state is random copolymerization. The copolymer may be any of a copolymer, an alternating copolymer, a block copolymer, a graft copolymer, etc. From the viewpoint of thermal resistance, a random copolymer or an alternating copolymer is preferred.
[0107] When the polymer compound (B) contains an optional copolymerization component, from the viewpoint of heat resistance, it is preferable that the polymer compound (B) contains an optional copolymerization component represented by the general formula (1) and a repeating unit derived from any copolymer component is 10:90 or more Preferably, the ratio is 97:3, more preferably 20:80 to 95:5, and more preferably 30:7 A ratio of 0 to 90:10 is even more preferable.
[0108] <Preferred specific examples of polymer compound (B)> More preferred specific examples of the polymer compound (B) of the present invention are shown below. The present invention is not limited to these. It is not something that can be determined.
[0109] [ka]
[0110] <Method for producing polymer compound (B)> The polymer compound (B) is, for example, a vinyl derivative and a vinyl aryl group described in the following documents 1-3. It can be obtained by a general synthetic method by reacting with a cyclobutene derivative in the presence of a catalyst. can be done. Document 1: Journal of Polymer Science: Part A: Polymer Chemistry, Vol. 46, 2799-280 6 (2008) Reference 2: J. Polymer Sci., 61,31 (1962) Reference 3: J. Am.Chem. Soc., 84, 2508 (1962) The vinyl derivatives include styrene, p-chlorostyrene, p-methylstyrene, distyrene, Styrene derivatives such as vinylbenzene, alkyl vinyl derivatives such as butadiene and pentadiene Examples include the body. Vinylarylcyclobutene derivatives include 4-vinylbenzocyclobutene, 1,2 -dihydro-4-vinylcyclobuta[a]naphthalene, etc. The catalyst is a radical polymerization catalyst such as benzoyl peroxide or azobisisobutyronitrile. Synthesis catalyst, methyllithium, phenyllithium, n-butyllithium, naphthylnaphthalene and cationic polymerization catalysts such as sulfuric acid and tin chloride. The reaction solvents include no solvent, halogenated solvents such as methylene chloride and carbon tetrachloride. Aromatic solvents such as toluene and xylene, and hydrocarbon solvents such as cyclohexane and decalin Examples of ether solvents include tetrahydrofuran, cyclopentyl methyl ether, and other ether solvents. Can be obtained.
[0111] <Content of polymer compound (B)> The content of the polymer compound (B) in the present composition is 100 parts by mass of the thermoplastic resin (A1). Preferably, the amount is 1 part by mass or more and less than 500 parts by mass, and more preferably 3 parts by mass or more and less than 450 parts by mass. The amount is preferably 5 parts by mass or less and 400 parts by mass or less, more preferably 7 parts by mass or more and 30 parts by mass or less. 0 parts by mass or less is more preferable, 10 parts by mass or more and 200 parts by mass or less is particularly preferable, and 12 Parts by weight or more and 100 parts by weight or less are most preferable. When the content of the polymer compound (B) is within the above range, crosslinking can be performed while maintaining low dielectric properties. It is possible to achieve high density while still maintaining a good balance with copper adhesion.
[0112] <Weight average molecular weight of polymer compound (B)> The weight average molecular weight of the polymer compound (B) is preferably 2,000 or more, more preferably 5,000 or more, more preferably 10,000 or more, and preferably 2,000,0 00 or less, more preferably 1,000,000 or less, and even more preferably 500,000 or less. It is particularly preferably 200,000 or less. By setting the weight average molecular weight to the above lower limit, the fluidity is not too high, so that the flowability is improved. In addition, by setting the weight average molecular weight to the above upper limit or less, the heat This makes it easier to mix uniformly with plastic resin.
[0113] The weight average molecular weight and number average molecular weight of the polymer compound (B) in the present invention are determined by SEC (Sequence Index). The SEC measurement is performed using a chromatographic method. The elution time is short, and the lower the molecular weight component, the longer the elution time. The elution time of the sample is converted to molecular weight using a calibration curve calculated from the elution time of the reference sample. By this, the weight average molecular weight, number average molecular weight, and molecular weight distribution (M w / M n ) is calculated It will be. w / M n is preferably 1.0 or more, preferably 10 or less, more preferably It is preferably 5 or less, and more preferably 3 or less. M w / M n By making it equal to or greater than the lower limit above, compatibility with the thermoplastic resin (A1) is good. Also, M w / M n By making the above upper limit value or less, a more uniform crosslinked structure is formed. This results in good mechanical and mechanical properties.
[0114] 4. Solvent (C) When a resin sheet is produced from the present composition through a coating process, the composition may contain a solvent (C). good. The solvent (C) is one in which the thermoplastic resin (A1) and the polymer compound (B) can be dissolved uniformly. Examples of suitable solvents include, but are not limited to, toluene, cyclohexane, tetrahydrofuran, and xylene. etc.
[0115] The solvent (C) must have a boiling point of 200°C or less so that it evaporates when the resin sheet is dried. is preferred.
[0116] The content of the solvent (C) in the present composition is set to 1 / 1 of the thermoplastic resin (A1) from the viewpoint of film-forming property. Preferably, the amount is 100 parts by mass or more and 500 parts by mass or less, and more preferably 200 parts by mass or more and 400 parts by mass or less. 00 parts by mass or less is more preferable.
[0117] 5. Other Ingredients The composition further comprises, as a component other than the above, a thermoplastic elastomer other than the thermoplastic resin (A1). -, crosslinking agents other than polymer compound (B), polymerization initiators, crosslinking catalysts, UV absorbers, antistatic agents agents, antioxidants, coupling agents, plasticizers, flame retardants, colorants, dispersants, emulsifiers, elasticity reducing agents agents, diluents, defoamers, ion trapping agents, thickeners, leveling agents, inorganic particles, organic particles, etc. may also contain
[0118] Examples of crosslinking agents other than the polymer compound (B) include bismaleimide compounds and epoxy compounds. Compounds and the like.
[0119] Examples of the polymerization initiator include hydroperoxides, dialkyl peroxides, Organic peroxides such as diacyl peroxides, peroxy esters, and ketone peroxides Examples include: More specifically, cumene hydroperoxide, t-butyl hydroperoxide Hydroperoxides such as dicumyl peroxide, di-t-butyl peroxide , 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-bis(t Dialkyl peroxy such as ert-butylperoxy-2,5-dimethyl-3-hexyne Side: Diacyl peroxides such as lauryl peroxide and benzoyl peroxide t-Butyl peroxyacetate, t-Butyl peroxybenzoate, t-Butyl Peroxy esters such as peroxyisopropyl carbonate; cyclohexanone peroxy Examples of suitable peroxides include ketone peroxides such as ketone peroxides.
[0120] The content of the polymerization initiator is set to 100 parts by mass of the thermoplastic resin (A1) in order to promote the curing reaction. Preferably, the amount is 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and more preferably 1 part by mass or more. On the other hand, in terms of keeping the dielectric properties low, the amount is preferably 5 parts by mass or less. It is preferably 1 part by mass or less, more preferably 0.1 part by mass or less, and is substantially contained. It is most preferable that this not occur. The above phrase "substantially does not contain" means that it is not intentionally contained, and The content of the polymerization initiator is 0 parts by mass or more relative to 100 parts by mass of the thermoplastic resin (A1). It means 0.05 parts by mass or less, and more preferably 0 parts by mass or more and 0.01 parts by mass or less.
[0121] Examples of inorganic particles include calcium carbonate, magnesium carbonate, barium carbonate, and sulfuric acid. Magnesium, barium sulfate, calcium sulfate, zinc oxide, magnesium oxide, calcium oxide Sium, titanium oxide, aluminum oxide, zinc oxide, alumina, aluminum hydroxide, Hydroxyapatite, Silica, Magnesium Silicate, Mica, Talc, Kaolin, Chloride Examples of the inorganic fillers include clay, glass powder, asbestos powder, zeolite, and clay silicate. Examples of organic particles include (meth)acrylate-based resin particles, styrene-based resin particles, Silicone resin particles, nylon resin particles, polyethylene resin particles, benzoguanamine Examples of the resin particles include polyurethane resin particles, polyurethane resin particles, and fluorine resin particles. When inorganic particles or organic particles are contained, the content thereof is determined based on 100 mass of the resin component of the present composition. The amount is preferably 1 part by weight or more and 500 parts by weight or less, and more preferably 5 parts by weight or more and 350 parts by weight or less. More preferably, the content is from 10 parts by mass to 200 parts by mass. When the content of the molecule is equal to or more than the lower limit, the dielectric properties of the cured sheet can be further reduced. In addition, the linear thermal expansion coefficient of the cured sheet can be reduced, and when the sheet is used as a circuit board material, On the other hand, when the content of inorganic particles or organic particles is equal to or less than the upper limit, peeling is unlikely to occur. In this case, the formability of the cured sheet product is improved.
[0122] <Resin sheet> The resin sheet of the present invention (hereinafter also referred to as "the present resin sheet") is a resin sheet comprising the present composition in an uncured state. The material is molded into a sheet in a state similar to that described above.
[0123] The thickness of the resin sheet after curing is preferably 1 to 300 μm, more preferably 2 to 250 μm. It is more preferable, and further more preferable is 5 to 200 μm. When the thickness of the resin sheet after curing is equal to or greater than the above lower limit, the sheet has good handleability. If the thickness is equal to or less than the upper limit, the resin sheet may be used as a circuit board material. In this case, conformability to steps on the substrate is excellent. The above thickness was measured by heat pressing the resin sheet at 250°C and 0.2 MPa for 30 minutes. The values were measured using a micrometer on the obtained sheet cured product.
[0124] The resin sheet has a relative dielectric constant of preferably 4 or less, more preferably 3 or less after curing. More preferably, the ratio is 2.5 or less. On the other hand, the lower limit is not particularly limited, and it is sufficient that the ratio is 1 or more. . The dielectric loss tangent of the resin sheet after curing is preferably 0.003 or less, and more preferably 0.0 It is more preferable that the ratio is 0.02 or less, and even more preferable that the ratio is 0.0015 or less. It is not set, but should be 0 or greater. The above dielectric constant and dielectric tangent were measured at 250°C and 0.2 MPa for the resin sheet. The sheet cured product obtained by heat pressing for 30 minutes was used as a test piece, and the ratio of the in-plane direction of the sheet cured product was The dielectric constant and dielectric loss tangent were measured using a cavity resonator (manufactured by AET) and a network analyzer MS46 The value was obtained by measuring in TE mode using a 122B (manufactured by Anritsu Corporation).
[0125] The storage modulus (130°C) of this resin sheet after curing is 0.0 from the viewpoint of heat resistance. Preferably, the pressure is 1 MPa or more, more preferably, 0.05 MPa or more, and even more preferably, 0.1 MPa or more. From the viewpoint of flexibility, the upper limit is preferably 10,000 MPa or less, and more preferably 1,000 MPa or less. Less than or equal to a is more preferable. The storage modulus was measured by heating the resin sheet at 250°C and 0.2 MPa for 30 minutes. The sheet cured product obtained by pressing was used as a test piece, and the dynamic viscoelasticity was measured. This is the value.
[0126] The linear thermal expansion coefficient of the resin sheet after curing is preferably 1000 ppm / K or less, 750 ppm / K or less is more preferable, 500 ppm / K or less is even more preferable, and 400 It is even more preferable that the linear thermal expansion coefficient is not more than ppm / K. , 0 ppm / K or more is preferable. If the linear thermal expansion coefficient is equal to or less than the upper limit, the resin sheet may be used as a circuit board material. In this case, warping during bonding with the conductor can be suppressed, and high reliability can be obtained. The linear thermal expansion coefficient was measured by subjecting the resin sheet to 250°C and 0.2 MPa for 30 minutes. The sheet cured product obtained by heat pressing was used as a test piece, and it was heated at 0 to 120°C by the method described in the Examples. This is the average value.
[0127] <Laminate> The resin sheet has a release film on one or both sides for easy handling. It is preferable to provide a laminate. Examples of the release film include polyolefins such as polyethylene and polypropylene; Polyesters such as polyethylene terephthalate and polyethylene naphthalate; polyimides; A resin film mainly composed of polycarbonate or the like can be used. The peel strength may be adjusted by applying a silicone resin release agent or the like. The thickness of the release film is preferably 1 μm or more and 300 μm or less, and more preferably 5 μm or more and 200 μm or less. More preferably, the thickness is 10 μm or more and 150 μm or less, and even more preferably, the thickness is 20 μm or more and 120 μm or less. Even more preferably, the thickness is 0 μm or less. The release film has a matte finish, corona treatment, and antistatic treatment on the surface that comes into contact with the resin sheet. It may be possible to carry out
[0128] The laminate may be wound around a core to form a wound body. In this wound body, the length of the laminate is preferably 10 m or more, and more preferably The length of the laminate is 10 m or more. For example, the resin sheet When used as a flexible or stretchable laminate, the electronic components are continuously It is possible to produce the film in a continuous manner, and the film can be easily produced. However, a distance of 1000m or less is preferable. The material of the core is not particularly limited, but may be, for example, paper, resin-impregnated paper, acrylonitrile / butadiene Diene / styrene copolymer (ABS resin), fiber reinforced plastic (FRP), phenol Examples of the resin include polyvinyl chloride resin, resin containing inorganic substance, etc. An adhesive may be used for the core.
[0129] <Method of manufacturing resin sheet> The method for producing the resin sheet will be described below. It is not limited to the law.
[0130] [First manufacturing method] The first method for producing the resin sheet includes a coating liquid preparation step of preparing a coating liquid comprising the composition. and a forming step of forming the coating liquid into a sheet. In the first method, the thermoplastic resin (A1) and the polymer compound (B) are appropriately compatible with each other and are cured. This is preferable in that an optimal semi-IPN structure can be constructed later, resulting in good low dielectric properties.
[0131] (1) Coating fluid preparation process In the coating liquid preparation process, a thermoplastic resin (A1), a polymer compound (B), and optionally The cyclic polyolefin resin copolymer (A2), the solvent (C) and other ingredients are stirred. The mixture is stirred to mix uniformly to obtain a coating liquid. For mixing, for example, a mixer, a blender, a three-roll kneading device, a ball mill, a kneader, A general mixing / stirring device such as a single-shaft or twin-shaft kneader can be used for mixing. may be heated if necessary.
[0132] (2) Molding process In the forming step, the coating liquid is formed into a sheet to obtain a resin sheet. The coating liquid can be formed into a sheet by any known method. For example, the doctor blade method, the solvent casting method, the extrusion film forming method, etc. may be used. A new molding method includes the following (2-1) coating step and (2-2) drying step. Examples include the law.
[0133] (2-1) Coating process In the coating step, a coating liquid is applied to the surface of a release film to form a coating film. The coating method is a common method such as dip coating, spin coating, spray coating, blade coating, etc. The coating may be performed by a method such as a spin coater, a slit coater, a die coater, or a brushless coater. A coating device such as a radar coater can be used, and a desired coating material can be applied to the release film. It is possible to form a coating film of uniform thickness.
[0134] (2-2) Drying process In the drying step, the solvent is removed from the coating film formed above. The drying temperature is not particularly limited, but is usually 10° C. or higher and 150° C. or lower, preferably 25° C. or higher. The drying temperature is preferably 120° C. or less, more preferably 30° C. or more and 110° C. or less. By keeping the drying temperature below 100°C, the crosslinking reaction of the polymer compound (B) in the coating film is suppressed. By making the amount of the solvent equal to or more than the lower limit, foaming of the resin sheet can be suppressed and the solvent can be effectively removed. This allows for improved productivity. The drying time can be appropriately adjusted depending on the state of the coating film, the drying environment, etc. It is preferably 1 minute or more, more preferably 2 minutes or more, even more preferably 5 minutes or more, and even more preferably Preferably, the time is 10 minutes or more, more preferably 20 minutes or more, and most preferably 30 minutes or more. , preferably 4 hours or less, more preferably 3 hours or less, and even more preferably 2 hours or less. Less than an hour. When the drying time is equal to or longer than the lower limit, the solvent can be sufficiently removed. By satisfying the above, productivity can be improved and manufacturing costs can be reduced. The solvent in the resin composition is heated on a hot plate, a hot air oven, an IR heating oven, a vacuum dryer, or a high-frequency oven. The removal can be performed by a known heating method such as a heating machine.
[0135] In addition, from the viewpoint of preventing contamination of the resin sheet surface and ease of handling, after the above drying step, A release film may be laminated on the resin sheet.
[0136] [Second manufacturing method] The second method for producing the resin sheet comprises melt-kneading the composition and forming it into a sheet-like film. Includes the process. The second manufacturing method does not require the use of a solvent, and is therefore advantageous in terms of cost and facilitating the formation of multiple layers. This is preferable in that it is possible to reduce the amount of the solvent and that problems caused by residual solvent are unlikely to occur.
[0137] In the film-forming process, a thermoplastic resin (A1), a polymer compound (B), and an optionally added The cyclic polyolefin resin copolymer (A2) and other components are mixed in a single-screw or twin-screw extruder. The temperature is equal to or higher than the melting point of the thermoplastic resin (A1) and lower than the crosslinking temperature of the polymer compound (B). The resin composition is extruded onto a release film using an extruder or the like under the above conditions to form a film. The method is not particularly limited, but more specifically, T-die molding is mentioned.
[0138] <Cured sheet> The sheet cured product of the present invention (hereinafter also referred to as the "main cured product") is obtained by curing the above-mentioned resin sheet. This is what was done.
[0139] The curing temperature is set so that the thermoplastic resin (A1) does not flow and the crosslinking reaction of the polymer compound (B) occurs. Specifically, the temperature is usually 80°C or higher, which accelerates the crosslinking rate. In order to achieve this, the temperature is preferably 120° C. or higher, more preferably 150° C. or higher, and even more preferably 1 It is over 80°C. In order to prevent the resin from decomposing, the temperature is usually 350° C. or lower, and preferably 310° C. or lower. °C or less, more preferably 300 °C or less, and further preferably 270 °C or less. The curing time is not particularly limited, but is usually 5 minutes or more. , 10 minutes or more, preferably 20 minutes or more, and more preferably 30 minutes or more. In order to suppress decomposition of the resin, the time is usually 3 hours or less, preferably 2 hours or less. More preferably, it is 1 hour or less.
[0140] <Applications of the resin composition, resin sheet, and cured sheet> An example of the application of the resin composition, resin sheet, and cured sheet of the present invention is a copper foil laminate. , stretchable boards, flexible printed circuit boards, multi-layer printed wiring boards, capacitors Circuit board materials for electric and electronic equipment such as inverters, underfill materials, inter-layer insulating materials for 3D-LSI Top fill, insulating sheet, vibration damping material, adhesive, solder resist, semiconductor encapsulation material, hole filling material Examples of the material include, but are not limited to, greases, resins for embedding parts, etc.
[0141] <Circuit board materials> The resin sheet of the present invention can be used as a circuit board material by laminating it with a conductor.
[0142] Conductors are made of conductive metals such as copper and aluminum, and alloys containing these metals. For example, a metal foil or a metal layer formed by plating or sputtering can be used.
[0143] When used as a circuit board material for electrical and electronic equipment, the resin sheet thickness must be 10 μm or more. The thickness of the conductor is preferably 0.2 μm or more and 70 μm or less. .
[0144] <Method of manufacturing circuit board materials> The circuit board material of the present invention can be produced, for example, by the following method. After the resin sheet of the present invention is laminated on a conductor, the resin sheet is thermally cured to form an insulating layer. A conductor is layered on top of the insulating layer, and as many such layers as necessary.
[0145] The curing temperature of the resin sheet is set at a temperature at which the thermoplastic resin (A1) does not flow and the polymer compound (B Specifically, the temperature is usually 80° C. or higher, and the crosslinking reaction proceeds more easily. In order to accelerate the crosslinking rate, the temperature is preferably 120° C. or higher, more preferably 150° C. or higher, and The temperature is preferably 180° C. or higher. In order to prevent the resin from decomposing, the temperature is usually 350° C. or lower, and preferably 310° C. or lower. °C or less, more preferably 300 °C or less, and further preferably 270 °C or less. The curing time is not particularly limited, but is usually 5 minutes or more. , 10 minutes or more, preferably 20 minutes or more, and more preferably 30 minutes or more. In order to suppress decomposition of the resin, the time is usually 3 hours or less, preferably 2 hours or less. More preferably, it is 1 hour or less.
[0146] Lamination of the resin sheet and the conductor is a method of directly overlapping a conductive metal foil on the resin sheet. Alternatively, a method in which the resin sheet and the conductive metal foil are bonded together using an adhesive may be used. Alternatively, a method of forming a conductive metal layer by plating or sputtering may be used. These methods may be combined. In addition, a process of drilling holes in the insulating layer to form via holes and a process of roughening the surface of the insulating layer are also performed. The method may include a step of: EXAMPLES
[0147] The present invention will be described in more detail below with reference to examples. Not limited to this.
[0148] <Raw materials> [Thermoplastic resin (A1)] a1-1: Styrene-ethylene-butadiene-styrene block copolymer (SEBS: Asahi Kasei "Tuftec H1052", styrene content = 20% by mass, storage modulus (24 ℃)=6.2MPa, density=890g / cm 3 , Dielectric loss tangent (10GH2) = 0.0004 ) was used.
[0149] [Cyclic polyolefin resin copolymer (A2)] a2-1: Cyclic polyolefin copolymer (HSEBS: Mitsubishi Chemical Corporation, "Tefab Block CP CP402, hydrogenated aromatic vinyl polymer block unit: content 67 moles %, hydrogenated polystyrene with hydrogenation level of 99% or more, hydrogenated conjugated diene polymer block Unit: Hydrogenated polybutadiene with a content of 33 mol%, hydrogenation level of 99% or more, block structure Construction: Block structure: Pentablock structure, Total hydrogenation level: 99% or more, Crystal fusion peak The test specimens were subjected to a test at a temperature of 75°C and a MFR (230°C, 2.16 kg): 85 g / 10 min.
[0150] [High molecular compound (B)] b-1: Compound b-1 prepared by the following method was used.
[0151] [Synthesis of compound b-1] Styrene (70 g) and 4-vinylbenzocyclobutene (30 g) were dissolved in toluol under a nitrogen atmosphere. Benzoyl peroxide (0.372 g) was added to the benzene solution (100 mL). The mixture was stirred at 84°C for 7 hours, then at 89°C for 3 hours. After cooling to room temperature, 600 mL of The toluene solution was added dropwise to methanol, and the precipitated polymer was filtered. The polymer was washed with methanol to obtain the target product (63 g). Yield: 63%, Mw=86,000. , Mw / Mn=2.0.
[0152] [ka]
[0153] b-2: Compound b-2 prepared by the following method was used.
[0154] [Synthesis of compound b-2] Styrene (40 g) and 4-vinylbenzocyclobutene (40 g) were dissolved in toluol under a nitrogen atmosphere. Benzoyl peroxide (0.170 g) was added to the benzene solution (100 mL). The mixture was stirred at 84°C for 7 hours, then at 89°C for 3 hours. After cooling to room temperature, 600 mL of The toluene solution was added dropwise to methanol, and the precipitated polymer was filtered. The polymer was washed with methanol to obtain the desired product (30 g). Yield: 37%, Mw: 11. 0 million, and Mw / Mn = 1.79.
[0155] [ka]
[0156] [Crosslinking agent (B')] b'-1: As a non-high molecular weight crosslinking agent, divinylbenzene 57%, ethylvinylbenzene A mixture of 40% benzene and 3% diethylbenzene (manufactured by Nippon Steel Chemical & Material Co., Ltd., "DV B570, mass average molecular weight (Mw): 131) was used.
[0157] [Example 1] The raw materials are mixed in the ratio shown in Table 1, heated to about 80°C, and completely dissolved to form a resin composition. The prepared resin composition was applied to a 50 μm-thick release film treated with silicone release agent. The resin is spread out in a sheet on the release-treated surface of a film (PET film manufactured by Mitsubishi Chemical Corporation). The thickness of the resin sheet was adjusted so that the thickness of the sheet after curing was about 300 μm. Adjusted. The resin sheet spread on the release film was dried in an oven at 100°C for 1 hour, and then the resin A 75μm-thick release film (Chukoh Chemical Industry Co., Ltd., TSUKO FLOW G type) is placed on top of the sheet. Then, remove the PET film and apply the same release film to this side. The laminate was heated to about 0° C. in a heat press at 250° C. Hold the resin sheet at a pressure of .2MPa for 30 minutes to completely harden it, then The release film was peeled off to obtain a sheet cured product. The dielectric properties, storage modulus, and linear thermal expansion coefficient were measured by the methods shown below. The results are shown in Table 1.
[0158] [Examples 2 to 9, Comparative Examples 1 and 2] The sheet was cured in the same manner as in Example 1, except that the raw materials were mixed according to the ratio shown in Table 1. The obtained cured sheet was subjected to the following measurement methods to measure the dielectric properties and storage elasticity. The elastic modulus and linear thermal expansion coefficient were measured, and the results are shown in Table 1.
[0159] [Measurement method] (1) Dielectric properties The dielectric constant and dielectric loss tangent in the in-plane direction of the cured sheet were measured using a cavity resonator (manufactured by AET Co., Ltd.). The measurements were taken in TE mode using a network analyzer MS46 122B (manufactured by Anritsu). The measurement frequency was 10 GHz.
[0160] (2) Storage modulus The dynamic viscoelasticity of the cured sheet was measured using a viscoelasticity spectrometer DVA-200 (IT Measurements were performed under the following conditions using a thermocouple (manufactured by Keisoku Seigyo Co., Ltd.). The elastic modulus value was taken as the storage elastic modulus of each sheet cured product. <Measurement conditions> Vibration frequency: 10Hz Distortion: 0.1% Heating rate: 3℃ / min Measurement temperature: -100℃~300℃
[0161] (3) Coefficient of linear thermal expansion The dimensional change of the cured sheet was measured using a thermomechanical analyzer TMA7100 (Hitachi High-Tech Science Corporation). The measurement was performed under the following conditions using a 3rd step 0 to 100 The average value of the dimensional change rate at ° C. was taken as the linear thermal expansion coefficient of each cured sheet. <Measurement conditions> Measurement mode: Tensile mode Atmosphere: 200mL / min nitrogen flow Heating rate: 5℃ / min Measurement temperature: 1st step: 0~100℃ 2nd step: 100~0℃ 3rd step: 0~120℃
[0162] [Table 1]
[0163] From Examples 1 to 9 and Comparative Example 1, it can be seen that the thermoplastic resin (A1) has a specific structure. By adding compound (B), the thermoplastic resin (A1) alone can be used while maintaining low dielectric properties. The heat ray can suppress the deformation (flow) of the resin composition even at a temperature where the resin composition would flow (130°C), and It was shown that the coefficient of expansion was reduced and heat resistance was improved. In Comparative Example 2, the crosslinking agent (B') does not have a benzocyclobutene crosslinking group in its molecule, so crosslinking It is difficult for density to increase, has a low storage modulus at 130℃, a high linear expansion coefficient, and has improved heat resistance. It is believed that the figure did not increase.
[0164] In the above examples, the thermoplastic resin (A1) was an olefin-based thermoplastic elastomer. Although there is no example of using an ethylene polymer, a polymer having a structure with a thermoplastic resin (A1) is The mechanism by which the molecular chains of the crosslinked compound (B) become entangled with each other improves heat resistance. From the viewpoint of structure, the same effect as that of styrene-based thermoplastic elastomers can be expected.
Claims
1. Styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers and ethylene-based At least one thermoplastic resin (A1) selected from the group consisting of polymers and a copolymer represented by the following general formula ( and a polymer compound (B) having a repeating unit represented by the formula: 【Chemistry 1】 (In formula (1), R 11 ~R 13 each independently represents a hydrogen atom or an alkyl group; R 14 each independently represents an oxygen atom, an alkylene group which may have a substituent, or Ar represents an aromatic hydrocarbon ring group. 11 Each of the groups may independently have a substituent. represents an aromatic hydrocarbon ring group; 11 each independently represents one of the following groups which may have a substituent: The bridging group is represented by the general formula (2). 11 is an integer from 0 to 10, n 12 teeth, n is an integer from 0 to 5 13 is an integer between 1 and 2.) 【Chemistry 2】 (In formula (2), ring Ar 21 represents an aromatic hydrocarbon ring, and the symbol * represents Ar in formula (1). 11 The bond to formula (2) is Ar 21 Binds to.)
2. 2. The thermoplastic resin (A1) according to claim 1, wherein the thermoplastic resin (A1) comprises a styrene-based thermoplastic elastomer. The resin composition according to claim 1.
3. The styrene content of the styrene-based thermoplastic elastomer is 10% by mass or more and 70% by mass or less. The resin composition according to claim 2, wherein
4. R of the polymer compound (B) 11 ~R 13 are hydrogen atoms according to claim 1 . A resin composition.
5. The n of the polymer compound (B) 11 and n 12 are all 0, and n 13 is 1, The resin composition according to claim 1.
6. The resin composition according to claim 1 , which is substantially free of a polymerization initiator.
7. The resin composition according to claim 1, comprising a cyclic polyolefin resin copolymer (A2).
8. The cyclic polyolefin resin copolymer (A2) has an alicyclic structure in a side chain of the polyolefin. The resin composition according to claim 7, which is a copolymer having the formula:
9. A resin sheet comprising the resin composition according to any one of claims 1 to 8.
10. A laminate comprising the resin sheet according to claim 9 and a release film on one or both surfaces thereof.
11. A sheet cured product obtained by curing the resin sheet according to claim 9.
12. A circuit board material obtained by laminating an insulating layer made of the resin sheet according to claim 9 and a conductor.
Citation Information
Patent Citations
Thermosetting resin
JP1997194549A
Low temperature curable addition polymers from vinyl arylcyclobutene-containing monomers and methods for making the same
JP2019085562A
Cited By
Resin composition, resin sheet, multilayer body, sheet cured product, and circuit board material
WO2026191993A1