Gas diffusion electrode base material and fuel cell

The gas diffusion electrode base material with a microporous layer of spherical pores addresses the balance of moisture retention and drainage, enhancing power generation performance in polymer electrolyte fuel cells.

JP2024144202APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024036763
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing gas diffusion electrode base materials for polymer electrolyte fuel cells struggle to balance moisture retention and drainage properties, leading to poor power generation performance at both low and high current densities due to insufficient porosity, pore size, and durability issues.

Method used

A gas diffusion electrode base material with a microporous layer featuring spherical pores of 10 to 60 μm diameter, 10 to 50% cross-sectional porosity, 5 to 25% surface porosity, and a thickness of 5 to 55 μm, using carbon fibers and a water-repellent resin to enhance moisture retention and drainage.

Benefits of technology

The material achieves both moisture retention and drainage properties, resulting in improved power generation performance across low and high current densities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144202000001
    Figure 2024144202000001
  • Figure 2024144202000002
    Figure 2024144202000002
  • Figure 2024144202000003
    Figure 2024144202000003
Patent Text Reader

Abstract

To provide a gas diffusion electrode base material excellent in moisture retention and drainage and having good power generation performance at low current density and high current density in a fuel cell.SOLUTION: There is provided a gas diffusion electrode base material that has a microporous layer on at least one surface of a conductive porous base material. The gas diffusion electrode base material has spherical holes with an average diameter of 10-60 μm in the microporous layer. An area rate of holes formed over the entire cross section of the microporous layer is 10-50%, an area rate of holes formed over the entire surface of the microporous layer on a side where the conductive porous base material is not formed is 5-25%, and an average diameter of the spherical holes is greater than the thickness of the microporous layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas diffusion electrode substrate for use in a fuel cell, particularly a polymer electrolyte fuel cell, and to a fuel cell including said gas diffusion electrode substrate. [Background technology]

[0002] A polymer electrolyte fuel cell, which supplies a fuel gas containing hydrogen to the anode and an oxidizing gas containing oxygen to the cathode to obtain an electromotive force by an electrochemical reaction occurring at both electrodes, is generally constructed by stacking a separator, a gas diffusion electrode substrate, a catalyst layer, an electrolyte membrane, a catalyst layer, a gas diffusion electrode substrate, and a separator in this order. The gas diffusion electrode substrate needs to have high gas diffusivity to diffuse the gas supplied from the separator to the catalyst layer, high drainage to discharge water generated by the electrochemical reaction to the separator, and high conductivity to extract the generated current. For this reason, a gas diffusion electrode substrate in which a microporous layer is formed on the surface of a carbon sheet made of carbon fiber or the like as a substrate is widely used.

[0003] However, the problems with such a gas diffusion electrode substrate are: (1) when a solid polymer electrolyte fuel cell is operated in a low current density region, the amount of water produced is small, resulting in a dry condition, and the electrolyte membrane dries out, resulting in a decrease in proton conductivity, and as a result, power generation performance is decreased; and (2) when the solid polymer electrolyte fuel cell is operated in a high current density region, the amount of water produced is large, resulting in a wet condition, and the gas diffusion electrode substrate is clogged with the produced water, resulting in a shortage of gas supply, resulting in a decrease in power generation performance. Therefore, the gas diffusion electrode substrate is required to have both high moisture retention in a low current density region and high drainage in a high current density region. To solve this problem, a method is used in which a microporous layer is formed on the surface of the gas diffusion electrode substrate and pores are formed in the microporous layer to improve gas diffusion and drainage.

[0004] For example, a gas diffusion electrode substrate has been proposed in which pores larger than the thickness of a microporous layer are formed to have a high porosity (Patent Document 1).

[0005] Also, a gas diffusion electrode substrate has been proposed in which columnar pores are formed penetrating through the substrate in the thickness direction (Patent Document 2).

[0006] Also, a gas diffusion electrode substrate in which fibrous pores are formed in a microporous layer has been proposed (Patent Document 3). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-15226 A [Patent Document 2] JP 2007-179870 A [Patent Document 3] JP 2006-120506 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the technology described in Patent Document 1 can achieve high drainage, but the porosity is too high, so it is difficult to balance with moisture retention, and the durability of the microporous layer is also questionable. In addition, the technology described in Patent Document 2 can improve gas diffusion and drainage by using through holes, but is ineffective in terms of moisture retention. In addition, the technology described in Patent Document 3 has fibrous holes, so the pore size is small and sufficient drainage cannot be achieved.

[0009] In view of the above background of the prior art, an object of the present invention is to provide a gas diffusion electrode substrate which achieves both moisture retention and drainage properties, which have been difficult to achieve in the past, and which has excellent power generation performance at both low and high current densities. [Means for solving the problem]

[0010] The embodiments of the present invention are as follows. (1) A gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, the microporous layer having spherical pores with an average diameter of 10 to 60 μm, an area ratio of the pores formed in the entire cross section of the microporous layer being 10 to 50%, an area ratio of the pores formed in the entire surface of the microporous layer being 5 to 25%, and the average diameter of the spherical pores being greater than the thickness of the microporous layer. (2) The gas diffusion electrode substrate according to (1), wherein the microporous layer has an arithmetic mean surface roughness Sa of 6 to 20 μm. (3) The gas diffusion electrode substrate according to (1) or (2), wherein the F / C ratio of the surface of the microporous layer is 0.4 to 0.6. (4) The gas diffusion electrode substrate according to any one of (1) to (3), wherein the microporous layer has a contact angle of 5 to 50° on the surface. (5) The gas diffusion electrode substrate according to any one of (1) to (4), wherein the microporous layer has a thickness of 5 to 55 μm. (6) The gas diffusion electrode substrate according to any one of (1) to (5), wherein the conductive porous substrate is carbon paper. (7) A fuel cell comprising the gas diffusion electrode substrate according to any one of (1) to (6). Effect of the Invention

[0011] According to the present invention, it is possible to obtain a gas diffusion electrode substrate which has both moisture retention and drainage properties, which was previously difficult to achieve, and which has excellent power generation performance at both low and high current densities. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention is a gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, the microporous layer having spherical pores with an average diameter of 10 to 60 μm, an area ratio of pores formed in the entire cross section of the microporous layer being 10 to 50%, an area ratio of pores formed in the entire surface of the microporous layer on the side not having the conductive porous substrate being 5 to 25%, and the average diameter of the spherical pores being greater than the thickness of the microporous layer.

[0013] The conductive porous substrate, the microporous layer, and the fuel cell constituting the gas diffusion electrode substrate of the present invention will be described in detail below.

[0014] [Conductive porous base material] As the conductive porous substrate in the present invention, a porous substrate containing carbon fiber or a metal porous body is generally used. Among them, in the present invention, a porous substrate containing carbon fiber such as a carbon fiber fabric, a carbon fiber paper body, carbon felt, and carbon paper is preferably used. Here, carbon paper refers to a sheet obtained by binding a carbon fiber paper body with a binder such as a resin carbide. Among these, it is more preferable to use carbon paper because of its excellent corrosion resistance and its property of absorbing dimensional changes in the thickness direction of the electrolyte membrane, i.e., its excellent "springiness".

[0015] Examples of carbon fibers that can be preferably used for the conductive porous substrate include polyacrylonitrile (PAN)-based, pitch-based, and rayon-based carbon fibers. Among them, PAN-based carbon fibers and pitch-based carbon fibers are preferably used because of their excellent mechanical strength. In addition, natural fibers and synthetic fibers such as rayon fibers, acrylic fibers, and cellulose fibers may be mixed.

[0016] The average diameter of the carbon fiber single fibers is preferably 3 to 20 μm. When the average diameter is 3 μm or more, the pore size of the conductive porous substrate becomes large, and gas diffusion and drainage are improved, thereby improving the power generation performance of the fuel cell. On the other hand, when the average diameter is 20 μm or less, the water vapor diffusion is reduced, and it is possible to prevent the electrolyte membrane and catalyst layer from drying out and causing a decrease in performance. In other words, the moisture retention is improved. When the average diameter of the carbon fiber single fibers is 5 to 10 μm, these effects are enhanced, and this is more preferable.

[0017] When a carbon fiber paper sheet or carbon paper is used as the conductive porous substrate, the average length of the carbon fiber single fibers is preferably 3 to 20 mm. When the average length is 3 mm or more, the mechanical strength, electrical conductivity, and thermal conductivity of the conductive porous substrate are good. On the other hand, when the average length is 20 mm or less, the dispersion of the carbon fibers during papermaking is good, and a homogeneous conductive porous substrate is obtained. When the average length of the carbon fiber single fibers is 5 to 15 mm, these effects are enhanced, and therefore it is more preferable.

[0018] The mass per unit area of ​​the conductive porous substrate is 20 to 50 g / m 2 It is preferable that the basis weight is 20 g / m 2 When the weight per unit area is 50 g / m or more, the mechanical strength and electrical conductivity of the conductive porous substrate are improved. 2 When the weight per unit area of ​​the conductive porous substrate is 30 to 40 g / m or less, the gas diffusibility of the conductive porous substrate is good. 2 This is more preferable since it enhances these effects.

[0019] The weight per unit area of ​​the conductive porous substrate can be adjusted by controlling the amount of the carbon fiber, resin carbide, or the like, which are the constituent materials of the conductive porous substrate.

[0020] The conductive porous substrate is preferably one in which a water-repellent resin is attached to the inside by a water-repellent treatment. As the water-repellent resin, a fluororesin having a fluoroalkyl chain is preferable. Examples of the fluororesin include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkylvinylether copolymer), ETFE (tetrafluoroethylene-ethylene copolymer), PVDF (polyvinylidene fluoride), and PVF (polyvinyl fluoride), and PTFE or FEP that exhibits high water repellency are preferable.

[0021] The amount of the water-repellent resin is not particularly limited, but is preferably 0.1 to 20% by mass relative to 100% by mass of the entire conductive porous substrate. Within this range, the water-repellent resin can exhibit sufficient water repellency while preventing the water-repellent resin from blocking pores that serve as gas diffusion paths and from increasing electrical resistance.

[0022] In a solid polymer electrolyte fuel cell, the gas diffusion electrode substrate is required to have high gas diffusivity for diffusing the gas supplied from the separator to the catalyst and high drainage for discharging the water generated by the electrochemical reaction to the separator. For this reason, the conductive porous substrate preferably has a pore diameter peak at 10 to 100 μm. The pore diameter and its distribution can be obtained by pore diameter distribution measurement using a mercury porosimeter. To obtain the pore diameter of the conductive porous substrate, only the conductive porous substrate may be measured, or the gas diffusion electrode substrate after the microporous layer is formed may be measured. When measuring the gas diffusion electrode substrate, each layer structure is confirmed by observing a cross section parallel to the thickness direction of the gas diffusion electrode substrate with a scanning electron microscope (SEM), and the diameter of the pores of the conductive porous substrate is roughly obtained from the SEM image. Next, the pore diameter of the conductive porous substrate is determined while correlating the multiple pore diameter peaks obtained by the mercury porosimeter with the approximate values ​​from the SEM image.

[0023] In the present invention, the porosity of the conductive porous substrate is preferably 80 to 95%. When the porosity is 80% or more, gas diffusibility is increased and power generation performance is improved. On the other hand, when the porosity is 95% or less, the mechanical strength of the conductive porous substrate is increased and the conductivity is also improved. When the porosity of the conductive porous substrate is 85 to 90%, these effects are enhanced, and therefore it is more preferable. The porosity of the conductive porous substrate can be measured using a specific gravity meter or the like.

[0024] The thickness of the conductive porous substrate of the present invention is preferably 90 to 180 μm. Here, the thickness of the conductive porous substrate is the thickness when both surfaces are sandwiched under a pressure of 0.15 MPa. When the thickness is 90 μm or more, the mechanical strength is maintained and handling in the manufacturing process is easy. In addition, the spring property is increased, and the gas diffusion electrode substrate can absorb the dimensional change due to the expansion and contraction of the electrolyte membrane when used in a fuel cell, and the gas diffusion in the in-plane direction is improved, so that the power generation performance is improved. On the other hand, when the thickness of the conductive porous substrate is 180 μm or less, the gas diffusion in the thickness direction is increased, and the conductive path in the thickness direction is shortened, so that the conductivity is improved, so that the power generation performance is improved. When the thickness of the conductive porous substrate is 110 to 150 μm, these effects are enhanced, so that it is more preferable.

[0025] [Microporous layer] Next, the microporous layer will be described. The gas diffusion electrode substrate of the present invention has a microporous layer on at least one side of the conductive porous substrate, but it is preferable that the conductive porous substrate has a microporous layer only on one side. The role of the microporous layer includes water management such as keeping the electrolyte membrane or catalyst layer moist and draining generated water, reducing the interfacial electrical resistance between the catalyst layer and the gas diffusion electrode substrate, and suppressing damage to the electrolyte membrane caused by carbon fibers protruding from the conductive porous substrate. The microporous layer in the present invention has pores to improve moisture retention and drainage. In addition, the microporous layer in the present invention is preferably a layer containing carbon fine particles and a water-repellent resin.

[0026] The microporous layer of the present invention has spherical pores with an average diameter of 10 to 60 μm. The spherical pores maintain their shape against the pressure applied to the microporous layer in the fuel cell better than linear or flat pores, and therefore can trap more water vapor, leading to improved moisture retention. When the average diameter of the spherical pores is 10 μm or more, drainage is improved and power generation performance at high current density is improved. On the other hand, when the average diameter is 60 μm or less, moisture retention is improved and power generation performance at low current density is improved. When the average diameter is 30 to 50 μm, these effects are enhanced, and this is preferable.

[0027] In the present invention, a spherical pore refers to a pore having an aspect ratio, calculated as the ratio of the major axis to the minor axis, in the range of 1.0 to 1.3. Here, the major axis refers to the longest line segment connecting two points within the pore, and the minor axis refers to the longest line segment perpendicular to the major axis.

[0028] The method for measuring the aspect ratio is described below. Using an ion milling device, 10 samples for cross-section observation are randomly prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction. At this time, the cutting position of the gas diffusion electrode substrate is not particularly limited, and the size of the sample for cross-section observation is 5 mm (width of the cross-section cut part) × 12 mm. Next, using a scanning electron microscope, an image of the cross section of the microporous layer at any location of the sample is obtained by enlarging it 1,000 times, and the aspect ratio is obtained by measuring the long and short diameters of each pore present in the microporous layer in the image using the image analysis software "ImageJ", and the average value is calculated. The same procedure is performed for the images of 10 samples, and the overall arithmetic average value is taken as the aspect ratio of the pores.

[0029] In the present invention, the average diameter of spherical pores means the average value of the circle-equivalent diameter of spherical pores. As a measurement method, as described above, a gas diffusion electrode substrate is cut parallel to the thickness direction using an ion milling device, a cross section of the sample is magnified 1,000 times using a scanning electron microscope to obtain an image, and the area of ​​each spherical pore present in the microporous layer in the image is measured using the image analysis software "ImageJ", and the circle-equivalent diameter is calculated according to the following formula. The average value of the obtained circle-equivalent diameters of 1 μm or more is calculated. The same procedure is performed for the images of 10 samples, and the overall arithmetic average value is taken as the average diameter of the spherical pores.

[0030]

number

[0031] In the microporous layer of the present invention, the area ratio of the pores formed in the entire cross section of the microporous layer (hereinafter referred to as cross-sectional porosity) is 10 to 50%, and the area ratio of the pores formed in the entire surface of the microporous layer (hereinafter referred to as surface porosity) is 5 to 25%. If the cross-sectional porosity is 10% or more and the surface porosity is 5% or more, the drainage property is improved and the power generation performance at high current density is improved. On the other hand, if the cross-sectional porosity is 50% or less and the surface porosity is 25% or less, the moisture retention is improved and the power generation performance at low current density is improved. If the cross-sectional porosity is 15 to 30% and the surface porosity is 8 to 15%, these effects are enhanced, and therefore it is preferable.

[0032] The cross-sectional porosity is the area ratio of pores to the entire cross section of a sample cut parallel to the thickness direction of the microporous layer. The measurement method involves taking an image of the cross section magnified 1,000 times with a scanning electron microscope, measuring the area of ​​pores with a circle equivalent diameter of 1 μm or more using image analysis software "ImageJ," and determining the ratio of the area of ​​the pores to the entire cross-sectional area of ​​the microporous layer, which is the cross-sectional porosity. Ten samples are cut out, and the arithmetic average of the cross-sectional porosity of each of the ten samples is taken as the cross-sectional porosity of the microporous layer.

[0033] The surface porosity is the area ratio of pores to the entire surface of the microporous layer on the side not having the conductive porous substrate. The measurement method is to obtain an image of the microporous layer surface at any location of the sample by magnifying it 1,000 times with a scanning electron microscope, measure the area of ​​pores with a circle equivalent diameter of 1 μm or more in the image with the image analysis software "ImageJ", and calculate the ratio of the area of ​​the pores to the area of ​​the entire microporous layer, which is the surface porosity. Images are obtained at any 10 locations, and the arithmetic average value of the surface porosity at each of the 10 locations is the surface porosity of the microporous layer.

[0034] In the present invention, the average diameter of the spherical pores present in the microporous layer is larger than the thickness of the microporous layer. This allows many pores to be formed penetrating the microporous layer, improving drainage and power generation performance at high current density. The thickness of the microporous layer here refers to the value obtained by subtracting the thickness of the conductive porous substrate from the thickness of the gas diffusion electrode substrate, i.e., the thickness of the microporous layer that is permeated into the conductive porous substrate is not taken into consideration.

[0035] The thickness of the microporous layer can be measured by placing the conductive porous substrate on a smooth surface plate, measuring the thickness of the conductive porous substrate under a pressure of 0.15 MPa, and then measuring the thickness of the gas diffusion electrode substrate on which the microporous layer is formed in the same manner, and subtracting the thickness of the conductive porous substrate from the thickness of the gas diffusion electrode substrate. When measuring the thickness from the gas diffusion electrode substrate, the microporous layer is heated in air at 500°C for 1 hour and then removed by rubbing, and only the conductive porous substrate is taken out, and the thickness can be calculated from the difference between the thickness before and after removing the microporous layer.

[0036] As a method for forming pores in the present invention, a method can be used in which a pore-forming agent is mixed with a carbon coating liquid described below, the carbon coating liquid is applied to a conductive porous substrate, and then the substrate is sintered to burn off the pore-forming agent.

[0037] The shape of the pore former is preferably spherical, like the shape of the pores. The material of the pore former is not particularly limited as long as it is a material that burns or shrinks under the sintering conditions of the gas diffusion electrode substrate to form pores in the microporous layer, and for example, acrylic resin, styrene resin, starch, polylactic acid resin, sublimable low molecular weight substance, microballoons, etc. can be used. Here, the sublimable low molecular weight substance is a low molecular weight organic powder having a molecular weight of 1,000 or less, which sublimes and burns at the sintering temperature. Examples of the sublimable low molecular weight substance include anthracene, pentacene, and phenanthrene. In addition, microballoons are hollow particles that expand greatly when heated, forming pores around them, and finally the resin part is thermally decomposed or shrinks, leaving only the pores, and various materials are commercially available. Examples include "Matsumoto Sphere (registered trademark)" (manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) and "Expancel (registered trademark)" (manufactured by Nippon Phillite Co., Ltd.). In the case of a pore-forming agent that expands when heated, such as microballoons, the maximum diameter of expansion when heated is regarded as the diameter of the pore-forming agent in the present invention.

[0038] As the pore-forming agent, a material with a carbonization yield of 20% or less at 380°C, which is a general sintering condition, is preferable. If a pore-forming agent with a carbonization yield of more than 20% is used, hydrophilic carbonized material remains after sintering, and water may accumulate in the pores themselves and inhibit discharge. An example of a material that satisfies this condition is polymethylmethacrylate (PMMA). The carbonization yield can be measured using a TGA device such as EXTRA TGA6200 manufactured by SII. Specifically, using this device, the temperature is raised from 50°C to 380°C at a heating rate of 2°C / min in the atmosphere and held at 380°C for 10 minutes. The mass after being held at 380°C is then divided by the original mass and multiplied by 100 to obtain the carbonization yield at 380°C.

[0039] The amount of the pore-forming agent in the carbon coating liquid is preferably 10 to 500 parts by mass, and more preferably 30 to 200 parts by mass, when the amount of carbon fine particles is 100 parts by mass. If the amount of the pore-forming agent is less than 10 parts by mass, sufficient pores may not be obtained, and drainage may be insufficient. If the amount of the pore-forming agent is more than 500 parts by mass, the porosity becomes excessive, the mechanical strength, electrical conductivity, and thermal conductivity of the microporous layer decrease, and sufficient power generation performance may not be obtained.

[0040] Specific examples of the carbon fine particles preferably contained in the microporous layer include carbon black, carbon nanofibers, carbon nanotubes, graphene, etc. Among these, inexpensive carbon black is preferably used.

[0041] The specific surface area of ​​the above carbon particles is 20 to 40 m 2 / g is preferable. The method for measuring the specific surface area is not particularly limited, but it can be determined, for example, by the nitrogen adsorption method. The nitrogen adsorption method is a technique in which degassed carbon fine particles are sealed together with nitrogen in a container cooled to liquid nitrogen temperature, the amount of nitrogen adsorbed on the surface of the carbon fine particles at equilibrium is measured, and the specific surface area is calculated from this value. 2 When the specific surface area of ​​the carbon particles is 40 m / g or more, the dispersibility of the carbon particles in the carbon coating liquid described below is increased, and a uniform microporous layer can be formed. In addition, the moisture retention and drainage properties of the microporous layer are improved, and power generation performance is improved. 2 When the carbon content is 1.0 to 1.0 ppm, the oxidation and corrosion reaction of carbon is suppressed, thereby improving the durability of the fuel cell.

[0042] The contents of the water-repellent resin and carbon fine particles in the microporous layer can be measured by mass spectrometry. The content of the water-repellent resin can be measured by analyzing the degassed components when the microporous layer is heated to 1,000°C in a helium atmosphere to decompose and remove the resin components. The content of the carbon fine particles can be measured from the mass of the residue from the above-mentioned thermal decomposition treatment.

[0043] Furthermore, fibrous carbon particles such as carbon nanofibers and carbon nanotubes form conductive paths within the microporous layer, and are therefore effective in reducing the electrical resistance of the microporous layer.

[0044] The water-repellent resin preferably contained in the microporous layer is a fluororesin having a fluoroalkyl chain from the viewpoints of chemical stability, water repellency, etc., and examples thereof include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), ETFE (tetrafluoroethylene-ethylene copolymer), etc., similar to the fluororesins preferably used in the water-repellent treatment of conductive porous substrates.

[0045] Generally, fluororesins are insoluble in water or organic solvents, so when producing a carbon coating liquid, it is preferable to use a dispersion of water-repellent resin processed into fine particles. Examples of dispersions of fine water-repellent resin include "Polyflon (registered trademark)" D-210C, ND-110 (both manufactured by Daikin Industries, Ltd.), 120-JRB, and 31-JR (both manufactured by Mitsui-Chemours Fluoroproducts, Inc.).

[0046] Silicone having a siloxane bond can also be used as the water-repellent resin.

[0047] In addition to the water-repellent resin, the layer may contain a thermosetting resin, such as a phenol resin, an epoxy resin, an acrylate resin, or a furan resin.

[0048] Furthermore, the microporous layer may contain hydrophilic particles to enhance moisture retention. As the hydrophilic particle component, organic polymers such as phenolic resin, acrylic resin, ester resin, and ether resin are preferred, and phenolic resin particles with a high carbonization yield are more preferred to maintain electrical conductivity. In addition, the microporous layer may contain fine particles such as iridium oxide, ruthenium oxide, and titanium oxide that promote the electrolysis of water in a reverse potential state when hydrogen is insufficient. Furthermore, the microporous layer may contain fine particles such as cerium oxide and manganese oxide to inactivate hydroxide radicals generated at the anode electrode.

[0049] The microporous layer of the present invention has a basis weight of 5 to 35 g / m 2 It is preferable that the microporous layer has a basis weight of 5 g / m 2 When the thickness is more than 35 g / m, the carbon fibers protruding from the surface of the conductive porous substrate are covered, so that the carbon fibers can be prevented from damaging the electrolyte membrane. In addition, the contact resistance between the gas diffusion electrode substrate and the catalyst layer can be reduced, and the electrolyte membrane can be prevented from drying out. In addition, when the basis weight of the microporous layer is 35 g / m or more, the carbon fibers protruding from the surface of the conductive porous substrate are covered, so that the carbon fibers can be prevented from damaging the electrolyte 2 When the weight of the microporous layer is 10 to 25 g / m or less, the drainage property is good. 2 This is more preferable since it enhances these effects.

[0050] The thickness of the microporous layer is preferably 5 to 55 μm. If the thickness is 5 μm or more, the carbon fibers protruding from the surface of the conductive porous substrate are covered, so that the carbon fibers are prevented from damaging the electrolyte membrane, and moisture retention is further improved. On the other hand, if the thickness is 55 μm or less, the conductivity of the gas diffusion electrode substrate is increased, and drainage is further improved. If the thickness is 15 to 40 μm, these effects are enhanced, and therefore it is more preferable.

[0051] The thickness of the microporous layer can be measured by placing the conductive porous substrate on a smooth surface plate, measuring the thickness of the conductive porous substrate under a pressure of 0.15 MPa, and then measuring the thickness of the gas diffusion electrode substrate on which the microporous layer is formed in the same manner, and subtracting the thickness of the conductive porous substrate from the thickness of the gas diffusion electrode substrate. When measuring the thickness from the gas diffusion electrode substrate, the microporous layer is heated in air at 500°C for 1 hour and then removed by rubbing, and only the conductive porous substrate is taken out, and the thickness can be calculated from the difference between the thickness before and after removing the microporous layer.

[0052] The arithmetic mean roughness Sa of the surface of the microporous layer of the present invention is preferably 6 to 20 μm. When Sa is 6 μm or more, the surface has large unevenness, water vapor is more likely to remain, moisture retention is increased, and power generation performance at low current density is improved. On the other hand, when Sa is 20 μm or less, adhesion between the microporous layer and the catalyst layer is improved, and the mechanical properties and durability of the microporous layer itself are improved. When Sa is 7 to 15 μm, these effects are enhanced, and this is more preferable.

[0053] The fluorine atom / carbon atom ratio (F / C ratio) on the surface of the microporous layer of the present invention is preferably 0.4 to 0.6. When the F / C ratio is 0.4 or more, the water repellency of the surface is increased and drainage is improved. On the other hand, when the F / C ratio is 0.6 or less, moisture retention is improved.

[0054] The contact angle of the surface of the microporous layer of the present invention is preferably 5 to 50°. When the contact angle is 5° or more, the water repellency of the surface is increased and drainage is improved. On the other hand, when the contact angle is 50° or less, the moisture retention is improved. When the contact angle is 10 to 30°, these effects are enhanced, and therefore it is more preferable.

[0055] The microporous layer can be formed by, for example, applying the above-mentioned pore-forming agent and a carbon coating liquid containing carbon fine particles to at least one surface of the conductive porous substrate.

[0056] The carbon coating liquid may contain a dispersion medium such as water or an organic solvent, and may also contain a dispersion aid such as a surfactant. The dispersion medium is preferably water, and the dispersion aid is preferably a nonionic surfactant.

[0057] The carbon coating liquid can be applied to the conductive porous substrate using various commercially available coating devices. Coating methods that can be used include screen printing, rotary screen printing, spray atomization, intaglio printing, gravure printing, die coater coating, bar coating, and blade coating. The coating methods are merely examples and are not necessarily limited to these.

[0058] After the carbon coating liquid is applied to the conductive porous substrate, it is preferable to dry the coating liquid at a temperature of 80 to 180°C. That is, it is preferable to put the conductive porous substrate on which the microporous layer precursor is formed into a dryer set at a temperature of 80 to 180°C and dry it for 2 to 30 minutes. The amount of drying air can be appropriately determined, but rapid drying may induce microcracks on the surface. After the drying, it is preferable to put it into a muffle furnace, a baking furnace, or a high-temperature dryer and sinter it at a temperature of preferably 300 to 380°C for 5 to 20 minutes to melt the water-repellent resin and form a microporous layer by using it as a binder between carbon fine particles. In addition, in the sintering, it is preferable that the pore-forming agent is burned away by thermal decomposition, melting and volatilization, or sublimation to form pores. The pores become pores that maintain the shape of the burned particles.

[0059] [Gas diffusion electrode substrate] The thickness of the gas diffusion electrode substrate of the present invention is preferably 130 to 190 μm. Here, the thickness of the gas diffusion electrode is the thickness when both surfaces are sandwiched under a pressure of 0.15 MPa. When the thickness of the gas diffusion electrode substrate is 130 μm or more, the mechanical strength is maintained and handling in the manufacturing process is easy. On the other hand, when the thickness of the gas diffusion electrode substrate is 190 μm or less, the gas diffusibility is increased and the electric resistance is reduced, so that the power generation performance of the fuel cell is improved. The thickness of the gas diffusion electrode substrate can be adjusted by appropriately adjusting the thickness of the conductive porous substrate and the microporous layer.

[0060] [Membrane electrode assembly] In the present invention, the gas diffusion electrode substrate described above is bonded to at least one side of a solid polymer electrolyte membrane having catalyst layers on both sides to form a membrane electrode assembly. The solid polymer electrolyte membrane is preferably one having high proton conductivity and oxidation resistance and small gas crossover, and examples of such membranes include those made of fluorine-based polymers and hydrocarbon-based polymers. The catalyst layer is preferably one made of a mixture of catalyst-supported carbon particles, in which catalyst fine particles made of precious metals such as platinum, palladium, ruthenium, iridium, and rhodium, or oxides thereof, are supported on carbon particles, and a proton-conducting polymer.

[0061] When the gas diffusion electrode substrate is joined to a solid polymer electrolyte membrane having a catalyst layer, by arranging the microporous layer side of the gas diffusion electrode substrate on the catalyst layer side, various effects are achieved, such as water management, such as keeping the electrolyte membrane and catalyst layer moist and draining generated water, reducing the interfacial electrical resistance between the catalyst layer and the gas diffusion electrode substrate, and suppressing damage to the electrolyte membrane due to carbon fibers protruding from the conductive porous substrate.

[0062] [Fuel cell] The fuel cell of the present invention includes the gas diffusion electrode substrate of the present invention. That is, the fuel cell of the present invention has separators on both sides of the above-mentioned membrane electrode assembly. That is, a fuel cell is constructed by disposing separators on both sides of the above-mentioned membrane electrode assembly. Usually, a solid polymer fuel cell is constructed by stacking a plurality of such membrane electrode assemblies sandwiched between separators via gaskets (fuel cell units). For example, by preparing 200 to 500 fuel cell units and connecting them in series, a high voltage of 40 to 200 kV can be generated, and such a fuel cell stack can be used as a power source for a fuel cell vehicle or the like. EXAMPLES

[0063] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description.

[0064] [Raw material] Porosity-forming agent PMMA beads MBX-40 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 40 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-12 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 12 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-60 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 60 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-8 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 8 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-80 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 80 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-20 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 20 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) PMMA beads MBX-5 spherical (manufactured by Sekisui Chemical Co., Ltd., average particle size (catalog value): 5 μm, aspect ratio: 1.0, carbonization yield after heating at 380°C for 10 minutes: 0.5% or less) ADCA "Vinihole (registered trademark)" amorphous (manufactured by Eiwa Chemical Industry Co., Ltd., particle length: 30 μm (catalog value), aspect ratio 1.5, carbonization yield after heating at 380°C for 10 minutes is 0.5% or less) <Measurement of basis weight of microporous layer> The mass [g] of the conductive porous substrate was measured using a precision balance in a 10 cm square shape. Next, the mass [g] of the gas diffusion electrode substrate on which the microporous layer was formed was similarly measured in a 10 cm square shape. The mass of the conductive porous substrate was subtracted from the mass of the gas diffusion electrode substrate to obtain the sample area (0.01 m 2 ) is the basis weight [g / m 2 ].

[0065] <Measurement of microporous layer thickness> The conductive porous substrate was placed on a smooth surface plate, and the height difference between the case where the object to be measured (conductive porous substrate) was present and the case where the object was not present under a pressure of 0.15 MPa was measured. Sampling was performed at 10 different locations, and the average of the measured height differences was taken as the thickness, which was the thickness of the conductive porous substrate. Next, the thickness of the gas diffusion electrode substrate on which the microporous layer was formed was measured in the same manner. The thickness of the conductive porous substrate was subtracted from the thickness of the gas diffusion electrode substrate to obtain the thickness [μm] of the microporous layer.

[0066] <Measurement of the average diameter of spherical pores> First, 10 samples for cross-sectional observation were randomly prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction using an ion milling device IM4000 (Hitachi High-Tech Corporation). At this time, the cutting position of the gas diffusion electrode substrate was not particularly limited, and the size of the above-mentioned cross-sectional observation sample was 5 mm (width of the cross-sectional cut part) × 12 mm. Next, a scanning electron microscope SU8010 (Hitachi High-Tech Corporation) was used to obtain an image of the cross section of the microporous layer at any location of the sample enlarged 1,000 times, and the area of ​​each spherical pore present in the microporous layer in the image was measured using the image analysis software "ImageJ", and the circle equivalent diameter was calculated from the following formula. The average value of the obtained circle equivalent diameters of 1 μm or more was calculated. The same was performed for the images of 10 samples, and the overall arithmetic average value was taken as the average diameter of the spherical pores.

[0067]

number

[0068] <Measurement of cross-sectional porosity> As in the above <Measurement of the average diameter of spherical pores>, 10 samples for cross-sectional observation were randomly prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction, and images of the cross section of the microporous layer at any location on each sample were obtained at 1,000 times magnification using a scanning electron microscope SU8010 (Hitachi High-Tech Corporation). At this time, the area of ​​the pores with a circle equivalent diameter of 1 μm or more shown in <Measurement of the average diameter of pores> was measured using the image analysis software "ImageJ", and the ratio of the area of ​​the pores to the area of ​​the entire microporous layer was calculated. The same procedure was performed on the images of the 10 samples, and the overall arithmetic average was calculated to obtain the cross-sectional porosity [%].

[0069] <Measurement of surface porosity> First, 10 locations were randomly selected from a 300mm x 300mm sample of the gas diffusion electrode substrate, and images of the microporous layer surface were taken at 1,000 times magnification using a scanning electron microscope SU8010 (Hitachi High-Tech Corporation). Next, the area of ​​the pores with a circle equivalent diameter of 1μm or more shown in <Measurement of the average diameter of pores> was measured using the image analysis software "ImageJ", and the ratio of the area of ​​the pores to the area of ​​the entire microporous layer was calculated. The same procedure was carried out for the images of the 10 locations, and the overall arithmetic average was calculated to obtain the surface porosity [%].

[0070] <Measurement of the arithmetic mean roughness Sa of the surface> The arithmetic mean roughness (Sa) of the microporous layer side surface of the gas diffusion electrode substrate in an area of ​​8.4 mm × 6.0 mm was measured using a laser microscope VK-X100 (manufactured by Keyence Corporation). Sa was measured at any four points on a 30 mm × 30 mm sample, and the average value was calculated.

[0071] <Measurement of surface F / C ratio> An X-ray photoelectron spectrometer (XPS) Model 5400 (ULVAC-PHI, Inc.) was used to perform elemental analysis at five random locations on the surface of the microporous layer of the gas diffusion electrode substrate. The elemental concentrations [%] of fluorine (F) and carbon (C) were quantified, the F / C ratio was calculated, and the average value of the five locations was calculated.

[0072] <Contact angle measurement> In an environment of 23°C and 50% humidity, 5 μL droplets of a mixture of ethanol and water in a mass ratio of 75:25 were dropped onto 10 randomly selected locations on the surface of the microporous layer of the gas diffusion electrode substrate, and the average value measured using an automatic contact angle meter DM-501 (Kyowa Interface Science Co., Ltd.) was taken as the contact angle [°].

[0073] <Evaluation of power generation characteristics> A catalyst solution was prepared by adding, in order, 1.00 g of platinum-supported carbon (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd., platinum loading: 50% by mass), 1.00 g of purified water, 8.00 g of Nafion (registered trademark) solution (Sigma-Aldrich Corporation's Nafion (registered trademark) 5.0% by mass), and 18.00 g of isopropyl alcohol (manufactured by Nacalai Tesque, Inc.).

[0074] Next, the catalyst solution was sprayed onto "Naflon (registered trademark)" PTFE tape "TOMBO (registered trademark)" No. 9001 (manufactured by Nichias Corporation) cut to 50 mm x 50 mm, and then dried at room temperature to obtain a platinum content of 0.3 mg / cm. 2 A PTFE sheet with a catalyst layer was produced. Next, a solid polymer electrolyte membrane (thickness: 10 μm) was produced using a 10 mass% dispersion of "Nafion (registered trademark)" (manufactured by Sigma-Aldrich Corporation) and cut into a size of 80 mm x 80 mm. The obtained solid polymer electrolyte membrane was sandwiched between two PTFE sheets with a catalyst layer, and pressed at a temperature of 130°C for 5 minutes while applying a pressure of 5 MPa with a flat plate press, thereby transferring the catalyst layer to the solid polymer electrolyte membrane. After pressing, the PTFE sheet was peeled off to produce a solid polymer electrolyte membrane with a catalyst layer.

[0075] Next, the solid polymer electrolyte membrane with the catalyst layer was sandwiched between two gas diffusion electrode substrates cut to 50 mm × 50 mm, and pressed at 130°C for 5 minutes while applying a pressure of 3 MPa with a flat press to produce a membrane electrode assembly. The gas diffusion electrode substrate was placed so that the surface having the microporous layer was in contact with the catalyst layer side.

[0076] The obtained membrane electrode assembly was assembled into a single cell for fuel cell evaluation, and the voltage was measured when the current density was changed. In addition, unpressurized hydrogen was supplied to the anode side, and unpressurized air was supplied to the cathode side, and the evaluation was performed.

[0077] The cell temperature was set to 65°C, and the hydrogen and air supplied were both humidified using a humidifier pot set to a temperature of 60°C, so that the humidity inside the cell was 80%, and the utilization rates of the oxygen in the hydrogen and air were 70% and 40%, respectively. Current density: 0.5A / cm 2 or 2.0A / cm 2 The output voltage was measured and used as an index of dry performance (moisture retention) and wet performance (drainage).

[0078] <Method of manufacturing conductive porous substrate> Polyacrylonitrile carbon fiber "TORAYCA (registered trademark)" T300 (average fiber diameter: 7 μm) manufactured by Toray Industries, Inc. was cut to a length of 6 mm, dispersed in water, and continuously made into paper. The paper was then spray-coated with a 10% by mass aqueous solution of polyvinyl alcohol, dried, and made into a paper with a basis weight of 30 g / m. 2 A long paper body made of carbon fibers was obtained. The amount of polyvinyl alcohol adhered was 15 parts by mass per 100 parts by mass of the paper body.

[0079] Next, a resin composition solution was prepared by mixing flake graphite (average particle size: 5 μm), phenol resin (a mixture of resol-type phenol resin and novolac-type phenol resin in a mass ratio of 1:1), and methanol in a mass ratio of 5:10:85. The resin composition solution was continuously applied onto the paper body by spray coating so that the total amount of the phenol resin and the flake graphite was 130 parts by mass per 100 parts by mass of the carbon fibers in the conductive porous substrate, and then dried at 100° C. for 5 minutes.

[0080] Next, the paper sheet with the resin composition attached was sandwiched between the upper and lower hot plates in a press molding machine and heat-compressed at 180°C for 5 minutes. Here, release paper was placed between the paper sheet and the hot plates to prevent the hot plates from adhering to the paper sheet substrate, and spacers were placed around the edges of the upper and lower hot plates to adjust the thickness of the conductive porous substrate after heat compression. After that, the paper sheet was heated to 2,400°C in a nitrogen atmosphere in a heating furnace and carbonized.

[0081] Furthermore, a water-repellent resin dispersion liquid obtained by mixing 5 parts by mass of FEP resin ("Neoflon (registered trademark)" FEP Dispersion ND-110 (manufactured by Daikin Industries, Ltd.)) and 95 parts by mass of ion-exchanged water was spray-coated, and dried at 100°C for 5 minutes to obtain a thickness of 150 μm at 0.15 MPa and a basis weight of 40 g / m. 2 Thus, a conductive porous substrate of 1000 g was obtained.

[0082] Example 1 A carbon coating liquid was prepared by mixing spherical PMMA beads MBX-40 as a pore-forming agent, powdered "Denka Black (registered trademark)" (manufactured by Denka Co., Ltd.) as carbon fine particles, fluororesin PTFE as a water-repellent resin, "TRITON (registered trademark)" X-100 (manufactured by Nacalai Tesque, Inc.) as a dispersing agent, and water as a dispersing medium in the blending ratio shown in Table 1. In this case, a dispersion of PTFE particles dispersed in water, "Polyflon (registered trademark)" D-210C (manufactured by Daikin Industries, Ltd.), was used as a supply source of PTFE. In addition, when preparing the coating liquid, a planetary mixer was used to disperse the raw materials so that the coating liquid composition was uniform.

[0083] The carbon coating liquid was applied to the conductive porous substrate manufactured according to the above-mentioned <Manufacturing method of conductive porous substrate> using a die coater, dried at 120°C for 10 minutes, and then heated at 380°C for 10 minutes to promote adhesion between the water-repellent resin and carbon microparticles, decompose and remove the dispersant, and burn and remove the pore-forming agent, to produce a gas diffusion electrode substrate. Here, the basis weight of the microporous layer after heating was 19 g / m 2The coating amount was adjusted so that the thickness of the obtained gas diffusion electrode substrate was 180 μm. The results of the evaluations of the above-mentioned <measurement of basis weight of microporous layer>, <measurement of thickness of microporous layer>, <measurement of average diameter of spherical pores>, <measurement of cross-sectional porosity>, <measurement of surface porosity>, <measurement of arithmetic mean roughness Sa of surface>, <measurement of surface F / C ratio>, and <measurement of contact angle> are shown in Table 1.

[0084] Next, the power generation performance was evaluated as described above in <Evaluation of power generation characteristics>. The power generation performance was good, as shown in Table 1.

[0085] Example 2 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that spherical PMMA beads MBX-12 were used as the pore-forming agent and the basis weight and thickness were as shown in Table 1, and various evaluations were carried out.

[0086] Example 3 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that spherical PMMA beads MBX-60 were used as the pore-forming agent, and various evaluations were carried out.

[0087] (Examples 4 and 5) A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that the coating solution composition for the microporous layer was as shown in Table 1, and various evaluations were carried out.

[0088] Example 6 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that spherical PMMA beads MBX-60 were used as the pore-forming agent and the basis weight and thickness were as shown in Table 1, and various evaluations were carried out.

[0089] Example 7 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that spherical PMMA beads MBX-12 were used as the pore-forming agent and the basis weight and thickness were as shown in Table 1, and various evaluations were carried out.

[0090] Comparative Example 1 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that PMMA beads MBX-8 spherical were used as a pore-forming agent and the basis weight and thickness were set as shown in Table 2. This gas diffusion electrode substrate had a small average pore diameter of 7 μm, insufficient drainage, and the power generation characteristics, especially on the high current density side, were deteriorated.

[0091] Comparative Example 2 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that PMMA beads MBX-80 spherical were used as the pore-forming agent. This gas diffusion electrode substrate had a large average pore diameter of 76 μm, insufficient moisture retention, and the power generation characteristics, especially on the low current density side, were deteriorated.

[0092] (Comparative Examples 3 and 4) A gas diffusion electrode substrate was prepared and various evaluations were performed in the same manner as in Example 1, except that the composition of the carbon coating liquid was as shown in Table 2. The gas diffusion electrode substrate of Comparative Example 3 had a small cross-sectional porosity and surface porosity, and the drainage was insufficient, and the power generation characteristics were particularly deteriorated on the high current density side. The gas diffusion electrode substrate of Comparative Example 4 had a large cross-sectional porosity and surface porosity, and the moisture retention was insufficient, and the power generation characteristics were particularly deteriorated on the low current density side.

[0093] Comparative Example 5 A gas diffusion electrode substrate was prepared and evaluated in the same manner as in Example 1, except that PMMA MBX-20 spherical beads were used as the pore-forming agent. This gas diffusion electrode substrate had an average pore diameter of 19 μm, while the microporous layer was as thick as 30 μm, making it difficult to form through-holes, resulting in insufficient drainage and reduced power generation characteristics, especially on the high current density side.

[0094] Comparative Example 6 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that PMMA beads MBX-5 spherical were used as a pore-forming agent and the basis weight and thickness were set as shown in Table 2. This gas diffusion electrode substrate had a small average pore diameter of 5 μm, insufficient drainage, and the power generation characteristics, especially on the high current density side, were significantly reduced.

[0095] Comparative Example 7 A gas diffusion electrode substrate was prepared and evaluated in the same manner as in Example 1, except that spherical PMMA beads MBX-80 were used as the pore-forming agent and the basis weight and thickness were as shown in Table 2. This gas diffusion electrode substrate had a large average pore diameter of 76 μm, insufficient moisture retention, and the power generation characteristics, especially on the low current density side, were deteriorated.

[0096] Comparative Example 8 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that ADCA "Vinihole (registered trademark)" amorphous was used as a pore-forming agent and the thickness was set as shown in Table 2. This gas diffusion electrode substrate had non-spherical pores, insufficient moisture retention, and through-holes were difficult to form, resulting in insufficient drainage, and the power generation characteristics were reduced on both the low current density side and the high current density side.

[0097] Comparative Example 9 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that no pore-forming agent was added and the coating liquid composition for the microporous layer was as shown in Table 2. Since no pores were formed by the pore-forming agent in this gas diffusion electrode substrate, both moisture retention and drainage were insufficient, and the power generation characteristics were reduced on both the low current density side and the high current density side.

[0098] [Table 1]

[0099] [Table 2] [Industrial Applicability]

[0100] The gas diffusion electrode substrate of the present invention is excellent in moisture retention and drainage properties, and a fuel cell using the same has good power generation performance at both low and high current densities, making it useful.

Claims

1. A gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, the microporous layer having spherical pores with an average diameter of 10 to 60 μm, an area ratio of pores formed in the entire cross section of the microporous layer being 10 to 50%, an area ratio of pores formed in the entire surface of the microporous layer on the side not having the conductive porous substrate being 5 to 25%, and an average diameter of the spherical pores being greater than a thickness of the microporous layer.

2. 2. The gas diffusion electrode substrate according to claim 1, wherein the microporous layer has a surface with an arithmetic mean roughness Sa of 6 to 20 μm.

3. 3. The gas diffusion electrode substrate according to claim 1, wherein the F / C ratio of the surface of the microporous layer is 0.4 to 0.

6.

4. 3. The gas diffusion electrode substrate according to claim 1, wherein the contact angle of the surface of the microporous layer is from 5 to 50°.

5. 3. The gas diffusion electrode substrate according to claim 1, wherein the microporous layer has a thickness of 5 to 55 μm.

6. 3. The gas diffusion electrode substrate according to claim 1, wherein the conductive porous substrate is carbon paper.

7. A fuel cell comprising the gas diffusion electrode substrate according to claim 1 or 2.

Citation Information

Patent Citations

  • Solid polymer fuel cell

    JP2006120506A

  • Gas diffusion electrode, membrane-electrolyte assembly, polymer electrolyte fuel cell and methods for producing them

    JP2007179870A

  • Gas-diffusion electrode base material for fuel cell and method for producing the same

    JP2015015226A