Hydraulic composition, method for producing hydraulic composition, method for producing hardened body, and method for suppressing fluctuation of compression strength

A hydraulic composition with controlled alkali stimulant production and specific component ratios stabilizes compressive strength in high blast furnace slag mixes, addressing strength fluctuations and reducing CO2 emissions.

JP2024144247APending Publication Date: 2024-10-11MITSUBISHI UBE CEMENT CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024044527
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing hydraulic compositions with a high proportion of blast furnace slag face significant fluctuations in compressive strength due to low formulation accuracy and deviations in component composition, making them unsuitable for practical use.

Method used

A hydraulic composition comprising a binder made of granulated blast furnace slag, gypsum, and an accelerator, with specific ratios of calcium oxide, gypsum, and an admixture, which controls the production rate of alkali stimulants to ensure stable hardening and suppress strength fluctuations.

Benefits of technology

The composition achieves stable and excellent compressive strength even with low mixing precision, allowing for the use of high blast furnace slag content without significant strength variations, reducing CO2 emissions by minimizing cement clinker usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144247000001
    Figure 2024144247000001
  • Figure 2024144247000002
    Figure 2024144247000002
Patent Text Reader

Abstract

To provide a hydraulic composition capable of stably exhibiting excellent compression strength, by curing, even when, in a region where a quantity of a blast furnace slag is very large. a blending accuracy of the hydraulic composition is low and a composition of each component deviates from a designed composition.SOLUTION: The present disclosure provides a hydraulic composition comprising an admixture, water-granulated blast furnace slag, and a binder made of gypsum, and an accelerator, the admixture containing 20 mass% or more of CaO, and based on 100 mass% of the binder, the content of the admixture is 0.5 to 20.0 mass%, the content of the granulated blast furnace slag is 70.0 to 95.5 mass%, and the content of the gypsum is 4 to 10.0 mass% in terms of SO3, and the content of the accelerator is 0.5 to 8.0 pts.mass relative to 100 pts.mass of the binder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a hydraulic composition, a method for producing a hydraulic composition, a method for producing a hardened body, and a method for suppressing fluctuations in compressive strength. [Background technology]

[0002] In cement production, large amounts of CO2 are generated from fuel combustion and from decarbonation of raw materials, and as demands for global warming countermeasures increase, there is a demand to reduce the amount of CO2 generated in cement production.Since a large amount of CO2 is generated during the preparation of cement clinker, the raw material, cement in which part of the cement clinker is replaced with an admixture is being widely studied from the perspective of reducing CO2 emissions.

[0003] It is generally believed that when the amount of admixture is increased, the compressive strength of the hardened body obtained by hardening of cement decreases, and therefore it is important to achieve the desired performance, such as compressive strength, that can be used in practical applications while mixing the admixtures. Among the admixtures, steel slag such as blast furnace slag is expected to increase the long-term strength of concrete and improve its salt shielding effect. For this reason, research is being conducted on cement that uses steel slag as an admixture and has a higher mixture ratio of it.

[0004] Blast-furnace cement, in which part of the cement clinker is replaced with granulated blast-furnace slag (BFS), is classified according to the replacement ratio. JIS R 5211:2019 specifies type B blast-furnace cement, which contains more than 30% by mass and not more than 60% by mass of blast-furnace slag, and type C blast-furnace cement, which contains more than 60% by mass and not more than 70% by mass of blast-furnace slag. However, there are no regulations for cement with a blast-furnace slag content of more than 70% by mass. At present, it is considered difficult to use in practice when the cement content is less than 30%, because the compressive strength exhibited when hardened into a hardened body is unstable (Non-Patent Document 1).

[0005] On the other hand, from the viewpoint of reducing the amount of CO2 generated, research is being conducted on cement compositions in which the amount of blast furnace slag is further increased than that of blast furnace cement type C (for example, Non-Patent Document 1). In Non-Patent Document 1, it has been confirmed that the cement composition hardens even in a composition in which the amount of cement clinker is as small as 1 mass% or less and the amount of blast furnace slag is extremely large. However, it is known that the amount needs to be strictly controlled from the viewpoint of strength development of the hardened body. For example, in the example described in Non-Patent Document 1, it has been confirmed that when the amount of cement clinker exceeds 1 mass% and is about 3 to 5 mass%, the hardening reaction of the cement composition does not proceed, and the compressive strength of the obtained hardened body is extremely reduced. That is, in the region in which the amount of blast furnace slag is extremely large, even a slight change in the composition of the cement composition causes a large fluctuation in the developed strength. Specifically, the strength of 55 N / mm 2 The strength of the concrete can be increased by 10N / mm depending on the amount of cement clinker mixed. 2 It has been confirmed that the compressive strength decreases significantly until it reaches a strength below 1000 kPa.

[0006] In general, the measurement accuracy in preparing cement compositions at an industrial level is said to be at most 1 to 2% by mass, and it is not realistic to control the amount of cement clinker to 1% by mass as described above. This is also one of the reasons why cement compositions containing a very large amount of blast furnace slag have not been commercialized. From this perspective, it is practically appropriate to adjust the composition of blast furnace cement so that the amount of cement clinker is at least 30% by mass, as specified by the JIS, and this is common sense in the industry. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] Tokyo Institute of Technology et al., "ECM Cement: A low-carbon cement that can reduce energy consumption and CO2 emissions by more than 60%", Figure 6, [online], May 2017, NEDO Practical Application Document, [Retrieved January 4, 2022], Internet<URL:https: / / www.nedo.go.jp / hyoukabu / articles / 201705ecm / index.html> [Non-Patent Document 2] Toshio Yonezawa et al., "Energy-CO2-Minimum (ECM) Cement-Concrete System", Concrete Engineering, Japan Concrete Institute, 2010, Vol. 48, No. 9, pp. 69-73 Summary of the Invention [Problem to be solved by the invention]

[0008] It would be useful to have a technology that can prevent the compressive strength of the hardened hydraulic composition from fluctuating significantly from the expected value or falling significantly below the expected value due to slight differences in the amount of hydraulic composition in a region where the amount of blast furnace slag is extremely large (for example, a region where blast furnace slag is 70 mass% or more), and that can produce a hydraulic composition that can exhibit stable quality even with industrial-level measuring accuracy.

[0009] The present disclosure aims to provide a hydraulic composition that can stably exhibit excellent compressive strength upon hardening, even when the blending precision of the hydraulic composition is low and the composition of each component deviates from the designed composition in the region where the amount of blast furnace slag is extremely large, and a method for producing the same. The present disclosure also aims to provide a method for producing a hardened body using the above-mentioned hydraulic composition. The present disclosure also aims to provide a method for suppressing fluctuations in compressive strength, even when a large amount of granulated blast furnace slag is included. [Means for solving the problem]

[0010] One aspect of the present disclosure provides the following [1] to

[12] .

[0011] [1] A binder comprising an admixture, granulated blast furnace slag, and gypsum, and an accelerator; The admixture contains 20% by mass or more of CaO, Based on 100% by mass of the binder, the content of the admixture is 0.5 to 20.0% by mass, the content of the granulated blast furnace slag is 70.0 to 95.5% by mass, and the content of the gypsum is 4.0 to 10.0% by mass in terms of SO3; A hydraulic composition, wherein the content of the accelerator is 0.5 to 8.0 parts by mass based on 100 parts by mass of the binder. [2] The hydraulic composition according to [1], wherein the content of free lime in the admixture is 0.2 to 5.0 mass %. [3] The hydraulic composition according to [1] or [2], wherein the admixture contains at least one selected from the group consisting of electric furnace reduction slag, converter slag, ready mixed concrete sludge, and waste concrete. [4] The hydraulic composition according to any one of [1] to [3], wherein the accelerator contains at least one monovalent anion selected from the group consisting of nitrite ions, nitrate ions, chloride ions, formate ions, and acetate ions. [5] The hydraulic composition according to any one of [1] to [4], wherein the accelerator contains at least one selected from the group consisting of alkali metal salts and alkaline earth metal salts. [6] The hydraulic composition according to any one of [1] to [5], wherein the accelerator contains a calcium salt. [7] The hydraulic composition according to any one of [1] to [6], wherein the gypsum contains at least one selected from the group consisting of gypsum dihydrate and gypsum hemihydrate. [8] The hydraulic composition according to any one of [1] to [7], wherein the basicity of the granulated blast furnace slag is 1.60 to 1.95. [9] The hydraulic composition according to any one of [1] to [8], wherein the content of aluminum oxide in the granulated blast furnace slag is 10.0 mass% or more.

[10] A first step of preparing a binder by mixing raw materials including an admixture, granulated blast furnace slag, and gypsum; A second step of mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder, The admixture contains 20% by mass or more of CaO, The first step comprises: Based on a total of 100% by mass of the binder, the amount of the admixture is adjusted to 0.5 to 20.0% by mass, and the amount of the granulated blast furnace slag is adjusted to 70.0 to 95.5% by mass. The amount of the gypsum is adjusted to be 4.0 to 10.0 mass% in terms of SO3, based on 100 mass% of the total of the binders. A method for producing a hydraulic composition comprising the steps of:

[11] A first step of preparing a binder by mixing raw materials including a mineral admixture, granulated blast furnace slag, and gypsum; A second step of obtaining a hydraulic composition by mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder; and a third step of mixing 50 parts by mass of water with respect to 100 parts by mass of the hydraulic composition, The admixture contains 20% by mass or more of CaO, The first step comprises: Based on a total of 100% by mass of the binder, the amount of the admixture is adjusted to 0.5 to 20.0% by mass, and the amount of the granulated blast furnace slag is adjusted to 70.0 to 95.5% by mass. The amount of the gypsum is adjusted to be 4.0 to 10.0 mass% in terms of SO3, based on 100 mass% of the total of the binders. A method for producing a cured body, comprising:

[12] For a composition containing a binder consisting of a mineral admixture, granulated blast furnace slag, and gypsum, The content of gypsum is adjusted to be 4.0 to 10.0 mass% in terms of SO3, with the total amount of the binder being 100 mass%; and The accelerator is blended in an amount of 0.5 to 8.0 parts by mass relative to 100 parts by mass of the binder, The method for suppressing fluctuations in compressive strength, wherein the admixture contains 20 mass% or more of CaO. Effect of the Invention

[0012] According to the present disclosure, it is possible to provide a hydraulic composition that can stably exhibit excellent compressive strength by hardening, even when the blending accuracy of the hydraulic composition is low and the composition of each component deviates from the designed composition in the region where the amount of blast furnace slag is extremely large, and a manufacturing method thereof. According to the present disclosure, it is also possible to provide a manufacturing method of a hardened body using the above-mentioned hydraulic composition. According to the present disclosure, it is also possible to provide a method for suppressing fluctuations in compressive strength, even when a large amount of granulated blast furnace slag is included. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the following description, when it is written "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified.

[0014] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0015] [Hydraulic composition] The hydraulic composition of the present disclosure is obtained by replacing a part of the binder made of granulated blast furnace slag and gypsum with a specified admixture and blending an accelerator therein.

[0016] The hydraulic composition of the present disclosure does not contain alkaline irritants used in conventional hydraulic compositions, such as Portland cement clinker, hydrated lime, and quicklime.

[0017] One embodiment of the hydraulic composition includes a binder made of an admixture, granulated blast furnace slag, and gypsum, and an accelerator. The admixture in the hydraulic composition contains 20% by mass or more of CaO. In the hydraulic composition, the content of the admixture is 0.5 to 20% by mass, and the content of the granulated blast furnace slag is 70.0 to 95.5% by mass, based on 100% by mass of the binder. The content of the gypsum is 4.0 to 10.0% by mass in terms of SO3. The content of the accelerator is 0.5 to 8.0 parts by mass relative to 100 parts by mass of the binder.

[0018] The hydraulic composition is obtained by replacing a part of the granulated blast furnace slag with an admixture containing a predetermined amount of calcium oxide, and adjusting the amount of gypsum, the content of the accelerator, and the amount of each component. This allows the composition to harden and exhibit sufficient compressive strength even if it does not contain an alkaline activator such as cement clinker. Furthermore, in the region where the amount of granulated blast furnace slag is extremely large, even if the content of the admixture deviates from the design composition due to the measurement when preparing the hydraulic composition, the compressive strength is prevented from fluctuating extremely from the expected value. The reason why the above-mentioned effect is obtained is unclear, but the inventors speculate as follows.

[0019] First, in conventional hydraulic compositions containing an alkaline stimulant such as cement clinker, it is believed that an alkaline stimulant such as calcium hydroxide (Ca(OH)2) eluted from the alkaline stimulant contributes to the initiation of the hardening reaction of granulated blast furnace slag. In hydraulic compositions containing an alkaline stimulant, the alkaline stimulant is generated at a high rate in the early stages of hydration, causing a rapid reaction with the granulated blast furnace slag. This rapid reaction is believed to form a dense hardening film on the surface of the granulated blast furnace slag, inhibiting the progress of the subsequent reaction (e.g., Non-Patent Document 2). In hydraulic compositions containing a very large amount of granulated blast furnace slag, when the rapid reaction of the granulated blast furnace slag occurs as described above, it is presumed that the partial progress and inhibition of the reaction occurs in the granulated blast furnace slag constituting the hydraulic composition, and unreacted blast furnace slag remains, resulting in cases where stable compressive strength is not exhibited.

[0020] On the other hand, in the hydraulic composition according to the present disclosure, the admixture containing a predetermined amount of calcium oxide serves as a supply source of the alkaline irritant, and the rate of production of the alkaline irritant is slower than that of the conventional alkaline irritant. This makes it possible for the hydraulic composition according to the present disclosure to cause the hardening reaction of the granulated blast furnace slag to proceed relatively slowly, and it is believed that the hardening reaction of the granulated blast furnace slag in the system can be made to proceed more uniformly by suppressing the formation of a dense hardened film on the surface of the granulated blast furnace slag that inhibits the hardening reaction.

[0021] Furthermore, the hydraulic composition according to the present disclosure contains an accelerator. When an accelerator is added, the hardening reaction of the hydraulic composition is accelerated. In this case, it is generally considered that the reaction is more difficult to control when an accelerator is added, and the compressive strength fluctuates, compared to the hydraulic composition without an accelerator, in which the reaction proceeds slowly. In light of such technical common knowledge of a person skilled in the art, it is a new finding that is difficult to imagine that the above-mentioned effects can be obtained by further adding an accelerator in a range in which the amount of granulated blast furnace slag is extremely large. It is presumed that the above-mentioned effects can be obtained by using an admixture that generates an alkaline irritant at a relatively slow rate without adding an alkaline irritant, and by adjusting the amount of each component including the accelerator.

[0022] In this specification, the binder refers to a material that reacts with water to produce a substance that contributes to the strength of concrete or mortar, and refers to a powder that contains granulated blast furnace slag as the main component and additives, etc. (in some cases, a powder that further contains gypsum).

[0023] (Calcium oxide-containing admixture) The admixture in the present disclosure contains 20% by mass or more of calcium oxide (CaO). The lower limit of the CaO content in the admixture may be, for example, 30% by mass or more, 40% by mass or more, or 50% by mass or more. When the lower limit of the CaO content in the admixture is within the above range, a more stable strength-enhancing effect of compressive strength can be obtained. The upper limit of the CaO content in the admixture may be, for example, 65% by mass or less, 60% by mass or less, or 55% by mass or less. When the upper limit of the CaO content in the admixture is within the above range, a significant decrease in compressive strength can be more sufficiently suppressed.

[0024] The calcium oxide content in this specification is a value expressed in terms of the amount of calcium present in the admixture as detected by fluorescent X-ray analysis, regardless of the form in which the calcium compound is present, expressed as an oxide equivalent value.

[0025] The content of free lime (f-CaO) in the admixture is preferably 0.2 to 5.0% by mass. The lower limit of the content of free lime in the admixture may be, for example, 0.5% by mass or more, 1.0% by mass or more, or 2.0% by mass or more. By the lower limit of the content of free lime in the admixture being within the above range, sufficient compressive strength at the initial age can be more sufficiently ensured. The upper limit of the content of free lime in the admixture may be, for example, 4.5% by mass or less, 4.0% by mass or less, or 3.0% by mass or less. By the upper limit of the content of free lime in the admixture being within the above range, initial rapid reaction can be suppressed, and the reactivity of the granulated blast furnace slag can be further sustained.

[0026] In this specification, the free lime content refers to the amount of calcium present in a free state (a single compound not bound to other substances, in the form of calcium oxide). The amount of free lime (f-CaO amount) is a value measured in accordance with the description in JCAS I-01-1997 "Method for determining free calcium oxide."

[0027] The admixture may contain at least one selected from the group consisting of electric furnace reduction slag, converter slag, ready-mixed concrete sludge, and waste concrete, for example, or may be at least one selected from the group consisting of electric furnace reduction slag, converter slag, ready-mixed concrete sludge, and waste concrete. Among the above-mentioned admixtures, from the viewpoint of further improving the long-term compressive strength, it is more preferable to include ready-mixed concrete sludge or waste concrete. In addition, since the amount of hexavalent chromium mixed in is small and there is no need to provide a process for removing hexavalent chromium during the production of the hydraulic composition, from the viewpoint of environmental consideration, it is preferable that the admixture is at least one of ready-mixed concrete sludge and waste concrete.

[0028] The electric furnace reduced slag is a slag produced by reduction refining among slags produced when iron scrap is melted and refined in an electric furnace. The form of the electric furnace reduced slag is preferably powdered from the viewpoint of preparing a hydraulic composition. The electric furnace reduced slag more preferably has a CaO content of 20.0 to 55.0 mass% and an f-CaO content of 0.2 to 5.0 mass%. The particle size of the powdered electric furnace reduced slag is preferably 90 μm or less. The particle size of the electric furnace reduced slag is a value specified based on the dry manual sieving method described in JIS Z 8815-1994 "General rules for sieving test method", and the above powder of 90 μm or less means a powder that has passed through a sieve with 90 μm openings.

[0029] Converter slag is slag generated when molten iron tapped from a blast furnace is treated in a molten iron pretreatment process, and slag generated when poured into a converter after the molten iron pretreatment process. Converter slag preferably has a CaO content of 20.0 to 55.0 mass% and an f-CaO content of 0.2 to 5.0 mass%. The particle size of powdered converter slag is preferably 90 μm or less. The particle size of converter slag is a value specified based on a dry manual sieving method described in JIS Z 8815-1994 "General rules for sieving test method", and the above powder of 90 μm or less means a powder that has passed through a sieve with 90 μm openings.

[0030] Ready-mixed concrete sludge is a powdery sludge consisting of the washing liquid from mixer equipment and mixer trucks in ready-mixed concrete plants, and the residual concrete and return concrete from concrete construction sites, and is strongly alkaline. Ready-mixed concrete sludge preferably has a CaO content of 20.0 to 55.0 mass% and an f-CaO content of 0.2 to 5.0 mass%. The particle size of the powdery ready-mixed concrete sludge is preferably 90 μm or less. The particle size of ready-mixed concrete sludge is a value specified based on the dry manual sieving method described in JIS Z 8815-1994 "General Rules for Sieving Test Methods", and the above powder of 90 μm or less means a powder that passes through a sieve with 90 μm openings.

[0031] Waste concrete is concrete rubble discharged during construction and demolition work. The waste concrete is preferably prepared by crushing waste concrete blocks. The waste concrete more preferably has a CaO content of 20.0 to 55.0 mass% and an f-CaO content of 0.2 to 5.0 mass%. The particle size of the powdered waste concrete is preferably 90 μm or less. The particle size of the waste concrete is a value specified based on the dry manual sieving method described in JIS Z 8815-1994 "General Rules for Sieving Test Methods", and the above powder of 90 μm or less means a powder that has passed through a sieve with 90 μm openings.

[0032] The content of the admixture is 0.5 to 20.0% by mass based on 100% by mass of the binder. The upper limit of the content of the admixture may be, for example, 20.0% by mass or less, 17.0% by mass or less, 16.0% by mass or less, 15.0% by mass or less, 14.0% by mass or less, 13.0% by mass or less, 12.0% by mass or less, 11.0% by mass or less, or 10.0% by mass or less based on 100% by mass of the binder. By the upper limit of the content of the admixture being within the above range, the strength enhancing effect mainly due to the reaction of the granulated blast furnace slag can be more fully obtained. The lower limit of the content of the admixture may be, for example, 1.0% by mass or more, 2.5% by mass or more, 5.0% by mass or more, or 10.0% by mass or more based on 100% by mass of the binder. By setting the lower limit of the content of the admixture within the above range, the reaction of the granulated blast furnace slag can be made more sufficient.

[0033] The content of the admixture in this specification means a value determined by the method described below. First, the granulated blast furnace slag and gypsum are determined by the following method. A hydraulic composition is heated at 900°C for 1 hour to crystallize the granulated blast furnace slag (glass), and the gypsum is converted into anhydrous gypsum to prepare a measurement sample. Then, X-ray diffraction measurement is performed on the measurement sample, and the content of the granulated blast furnace slag and gypsum is determined by quantifying each crystal phase (gehlenite, akermanite, mayenite, and anhydrite) in the measurement sample by Rietveld analysis. Next, the peak residuals other than the above-mentioned crystal phases become admixtures, and the peak residuals are identified using ICSD (Inorganic Crystal Structure Database) or ICDD PDF (International Center for Diffraction Data Powder Diffraction Database) to identify the minerals. The identified minerals are quantified by Rietveld analysis, and the quantitative values ​​of the identified minerals other than gehlenite, akermanite, mayenite, and anhydrite are used to determine the content of the admixtures. When preparing a hydraulic composition by oneself, the content of the admixture is the same as the mixing amount, so that the above-mentioned analysis is not required.

[0034] (granulated blast furnace slag) Granulated blast furnace slag has a high vitrification rate and is a sand-like slag made by injecting a large amount of pressurized water into the molten slag produced in a blast furnace to rapidly cool it.

[0035] The granulated blast furnace slag may be, for example, commercially available, or slag equivalent to the granulated blast furnace slag may be prepared by oneself and used.

[0036] The upper limit of the aluminum oxide content (also referred to as the Al2O3 amount) in the granulated blast furnace slag may be, for example, 14.5% by mass or less, or 14.3% by mass or less. When the Al2O3 amount in the granulated blast furnace slag is within the above range, the long-term strength development of the obtained hydraulic composition can be further suppressed from decreasing. The lower limit of the Al2O3 amount in the granulated blast furnace slag may be, for example, 10.0% by mass or more, 11.0% by mass or more, 12.0% by mass or more, or 13.0% by mass or more. When the lower limit of the Al2O3 amount in the granulated blast furnace slag is within the above range, the latent hydraulic property of the granulated blast furnace slag can be more fully exhibited. The latent hydraulic property means a property of starting a hydration reaction by adding an alkaline activator. The amount of Al2O3 in the granulated blast furnace slag may be adjusted within the above-mentioned range, and may be, for example, 10.0 to 14.5 mass%, 12.0 to 14.5 mass%, or 13.0 to 14.5 mass%.

[0037] The lower limit of the silicon dioxide content (also referred to as the SiO2 amount) in the granulated blast furnace slag may be, for example, 30.0 mass% or more, 33.0 mass% or more, 34.0 mass% or more, 34.5 mass% or more, or 35.0 mass% or more. When the lower limit of the SiO2 amount of the granulated blast furnace slag is within the above range, the initial and long-term strength development can be suppressed from decreasing. The upper limit of the SiO2 amount of the granulated blast furnace slag may be, for example, 40.0 mass% or less, 38.0 mass% or less, 36.5 mass% or less, or 35.5 mass% or less. When the upper limit of the SiO2 amount of the granulated blast furnace slag is within the above range, the initial strength development can be suppressed from decreasing. The SiO2 amount of the granulated blast furnace slag may be adjusted within the above range, and may be, for example, 33.0 to 40.0 mass% or 34.0 to 35.5 mass%.

[0038] The lower limit of the calcium oxide content (also referred to as the CaO content) in the granulated blast furnace slag may be, for example, 35.0 mass% or more, 38.5 mass% or more, or 40.0 mass% or more. When the lower limit of the CaO content of the granulated blast furnace slag is within the above range, the initial strength development can be further improved. The upper limit of the CaO content of the granulated blast furnace slag may be, for example, 45.0 mass% or less, 43.5 mass% or less, 43.0 mass% or less, 42.5 mass% or less, 42.0 mass% or less, or 41.5 mass% or less. When the upper limit of the CaO content of the granulated blast furnace slag is within the above range, the deterioration of the long-term strength development can be suppressed. The CaO content of the granulated blast furnace slag may be adjusted within the above range, and may be, for example, 38.5 to 45.0 mass% or 40.0 to 42.5 mass%.

[0039] The lower limit of the magnesium oxide content (also referred to as the MgO content) in the granulated blast furnace slag may be, for example, 4.0% by mass or more, 5.0% by mass or more, 5.5% by mass or more, 6.0% by mass or more, or 7.0% by mass or more. By setting the lower limit of the MgO content of the granulated blast furnace slag within the above range, it is possible to suppress a decrease in the initial and long-term strength development. The upper limit of the MgO content of the granulated blast furnace slag may be, for example, 10.0% by mass or less, 9.0% by mass or less, less than 7.5% by mass, less than 7.4% by mass, less than 7.2% by mass, or less than 7.1% by mass. By setting the upper limit of the MgO content of the granulated blast furnace slag within the above range, it is possible to suppress a decrease in the initial strength development. The MgO content of the granulated blast furnace slag may be adjusted within the above range, and may be, for example, 4.0 to 10.0% by mass, or 6.0% by mass or more and less than 7.4% by mass.

[0040] Granulated blast furnace slag may contain, as other components, for example, sulfur trioxide (SO3), sodium oxide (NaO2), potassium oxide (K2O), and titanium oxide (TiO2).

[0041] The chemical composition of the granulated blast furnace slag in this specification means a value measured in accordance with the description of JIS R 5202:2015 "Method of Chemical Analysis of Cement".

[0042] The reactivity of granulated blast furnace slag is evaluated by an index called basicity, which is expressed by the value of (CaO+MgO+Al2O3) / SiO2 (the ratio of the total content of calcium oxide, magnesium oxide, and aluminum oxide to the content of silicon dioxide in granulated blast furnace slag). As granulated blast furnace slag, either high basicity or low basicity can be used.

[0043] Granulated blast furnace slag having a basicity of, for example, 1.60 to 1.95 can be widely used. Granulated blast furnace slag having a basicity of less than 1.75 is generally considered to be a low-grade slag having a low basicity and low reactivity, but can be used as a component of the hydraulic composition of the present disclosure.

[0044] The upper limit of the basicity of the granulated blast furnace slag may be, for example, 1.95 or less, less than 1.95, less than 1.90, less than 1.85, or less than 1.80. The lower limit of the basicity of the granulated blast furnace slag, which has relatively excellent reactivity, may be, for example, more than 1.75, or 1.78 or more. When the lower limit of the basicity is within the above range, it is easier to improve the initial strength of the hydraulic composition. The basicity of the granulated blast furnace slag can be adjusted within the above range, and may be, for example, 1.75 to 1.95, or 1.75 or more and less than 1.80.

[0045] In the hydraulic composition according to the present disclosure, granulated blast furnace slag with low basicity can also be used. Granulated blast furnace slag with low basicity is often refrained from being used as low-grade slag because it is usually difficult to obtain sufficient compressive strength. However, in the hydraulic composition according to the present disclosure, the hardening reaction can be sufficiently promoted by blending a relatively large amount of gypsum and adjusting the content of the accelerator, so that even the above-mentioned low-grade slag can be used. The upper limit of basicity of such low-grade granulated blast furnace slag may be, for example, less than 1.75, less than 1.70, or less than 1.65. The lower limit of basicity of low-grade granulated blast furnace slag is not particularly limited, but may be, for example, 1.60 or more, or 1.65 or more. The basicity of low-grade granulated blast furnace slag may be adjusted within the above-mentioned range, and may be, for example, 1.60 or more and less than 1.75.

[0046] The basicity (JIS basicity) in this specification is a value measured in accordance with the description in JIS A 6206:2013 "Ground granulated blast furnace slag for concrete", and specifically means the value of (CaO+MgO+Al2O3) / SiO2 (the ratio of the total content of calcium oxide, magnesium oxide, and aluminum oxide to the content of silicon dioxide).

[0047] The specific surface area of ​​granulated blast furnace slag is, for example, 2500 to 10000 cm 2 / g, 2500~8000cm 2 / g, 2500-6000cm 2 / g, 2500~5000cm 2 / g, 3000-5000cm 2 / g, 4000-5000cm 2 / g, or 4000-4500cm 2 / g.

[0048] In this specification, the term "Blaine specific surface area" refers to a value measured in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement."

[0049] The content of the granulated blast furnace slag is 70.0 to 95.5% by mass based on 100% by mass of the binder. The upper limit of the content of the granulated blast furnace slag may be, for example, 95.0% by mass or less, 90.0% by mass or less, 85.0% by mass or less, or 80.0% by mass or less based on 100% by mass of the binder. When the upper limit of the content of the granulated blast furnace slag is within the above range, the reactivity of the granulated blast furnace slag can be more sufficient. The lower limit of the content of the granulated blast furnace slag may be, for example, 71.0% by mass or more, 72.5% by mass or more, 75.0% by mass or more, or 77.5% by mass or more based on 100% by mass of the binder. When the lower limit of the content of the granulated blast furnace slag is within the above range, the latent hydraulic property of the granulated blast furnace slag can be more fully exhibited.

[0050] The content of granulated blast furnace slag in this specification means a value determined by the method shown below. Specifically, a hydraulic composition is first heated at 900°C for 1 hour to crystallize the granulated blast furnace slag (glass) to prepare a measurement sample. Then, X-ray diffraction measurement is performed on the measurement sample, and each crystal phase in the measurement sample is quantified by Rietveld analysis to quantify gehlenite, akermanite, and merwinite as crystal phases formed by crystallization of the granulated blast furnace slag, and the total amount of these is the content of the granulated blast furnace slag. When a hydraulic composition is manufactured by oneself, the blending amount (measured value) of the granulated blast furnace slag added during the manufacturing process corresponds to the above content.

[0051] (plaster) The gypsum may be, for example, gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, etc. The gypsum may contain at least one selected from the group consisting of gypsum dihydrate and gypsum hemihydrate, or may be one selected from the group consisting of gypsum dihydrate and gypsum hemihydrate. The gypsum may be gypsum obtained by regenerating waste gypsum board.

[0052] The content of gypsum in the binder is relatively high from the viewpoint of making the hydraulic composition exhibit excellent compressive strength. The content of gypsum in the binder is 4.0 to 10.0 mass% in terms of SO3. By making the content of gypsum within the above range, it is possible to exhibit the effect of improving the compressive strength accompanying the hardening of the hydraulic composition by gypsum in a hydraulic composition containing a very large amount of blast furnace slag, and even if the composition of the hydraulic composition changes due to the addition of an accelerator or the like, it is possible to suppress extreme fluctuations in compressive strength.

[0053] The upper limit of the gypsum content may be, for example, 9.5% by mass or less, 9.0% by mass or less, 8.0% by mass or less, or 7.0% by mass or less in terms of SO3, based on 100% by mass of the binder. By setting the upper limit of the gypsum content within the above range, the initial and long-term strength development can be further improved. The lower limit of the gypsum content in the binder may be, for example, 4.2% by mass or more, 4.5% by mass or more, 5.0% by mass or more, 5.5% by mass or more, or 6.0% by mass or more in terms of SO3, based on 100% by mass of the binder. By setting the lower limit of the gypsum content within the above range, the hydration reaction of the granulated blast furnace slag is more favorable, the hardening of the hydraulic composition after mixing with water is promoted, and the initial strength development can be further improved. The content of gypsum in the binder may be adjusted within the above-mentioned range, and may be, for example, 4.2 to 9.5 mass % or 6.0 to 7.0 mass % in terms of SO3, based on 100 mass % of the binder.

[0054] The gypsum content in this specification means the total amount of the gypsum component that may be contained in the granulated blast furnace slag, as well as the gypsum component, etc., that is mixed with the binder. The gypsum content in this specification means a value determined by the method shown below. Specifically, the gypsum content is measured in accordance with the analysis method for SO3 specified in JIS R 5202:2015 "Methods for Chemical Analysis of Cement."

[0055] (Accelerator) The accelerator is a compound that accelerates the reaction of granulated blast furnace slag and improves its early strength.

[0056] The accelerator may contain a monovalent anion or a salt having a monovalent anion. The monovalent anion may be, for example, at least one anion selected from the group consisting of nitrite ion, nitrate ion, chloride ion, formate ion, and acetate ion. For example, when the accelerator contains a nitrite, the early strength of the hydraulic composition during hardening can be further improved. When the accelerator contains a nitrite, the amount of heat generated by hydration during hardening can also be reduced.

[0057] The accelerator may contain at least one selected from the group consisting of an alkali metal salt and an alkaline earth metal salt. By containing an alkali metal salt or an alkaline earth metal salt in the accelerator, the reactivity of the granulated blast furnace slag can be further improved.

[0058] The alkali metal may be, for example, sodium, potassium, etc., and the alkaline earth metal may be, for example, magnesium, calcium, etc. From the viewpoint of promoting the formation of hydrates and improving compressive strength, the alkaline earth metal preferably contains calcium, and more preferably is calcium. The accelerator may contain, for example, a calcium salt.

[0059] In conventional hydraulic compositions containing an alkaline stimulant such as cement clinker, it is believed that an alkaline stimulant such as calcium hydroxide (Ca(OH)2) eluted from the alkaline stimulant contributes to the initiation of the hardening reaction of the granulated blast furnace slag. Similarly, in the hydraulic composition according to the present disclosure, an alkaline stimulant such as calcium hydroxide is believed to contribute to the initiation of the hardening reaction of the granulated blast furnace slag, and it is expected that the hardening of the granulated blast furnace slag will be accelerated by the generation of calcium-containing eluted components from the admixture or accelerator containing calcium oxide. Although there is a difference in the elution rate of the alkaline stimulant depending on the type of the admixture, this can be dealt with by adjusting the hardening reaction time. Therefore, when the accelerator contains a calcium salt, even when it does not contain an alkaline stimulant, a sufficient hardening reaction of the granulated blast furnace slag can be expected. Due to such an action, it is possible to better tolerate fluctuations in the amount of each component in the hydraulic composition, making it easier to put the hydraulic composition according to the present disclosure into practical use.

[0060] Examples of the accelerator include calcium nitrite, calcium nitrate, calcium chloride, calcium hydroxide, sodium nitrite, potassium nitrite, sodium nitrate, potassium nitrate, sodium chloride, potassium chloride, etc. Among the above-mentioned compounds, the accelerator preferably contains an alkali metal nitrite, more preferably contains calcium nitrite, and further preferably is calcium nitrite.

[0061] The upper limit of the content of the accelerator is 8.0 parts by mass or less relative to 100 parts by mass of the binder, but may be, for example, 7.0 parts by mass or less, 6.0 parts by mass or less, 5.0 parts by mass or less, or 4.0 parts by mass or less. When the upper limit of the content of the accelerator is within the above range, the occurrence of abnormal coagulation when the reaction of granulated blast furnace slag or the like is excessively promoted can be more reliably suppressed. The lower limit of the content of the accelerator is 0.5 parts by mass or more relative to 100 parts by mass of the binder, but may be, for example, 0.8 parts by mass or more, 1.0 parts by mass or more, 1.5 parts by mass or more, or 2.0 parts by mass or more. When the lower limit of the content of the accelerator is within the above range, the reaction of granulated blast furnace slag can be further promoted. The content of the accelerator may be adjusted within the above range, and may be, for example, 0.5 to 8.0 parts by mass, or 2.0 to 4.0 parts by mass relative to 100 parts by mass of the cement.

[0062] The content of the accelerator in this specification is determined by subjecting the powdered composition to X-ray diffraction measurement and quantifying the content of the accelerator by Rietveld analysis. When the hydraulic composition is prepared by oneself, the content of the accelerator is the same as the blending amount, so the above-mentioned analysis is not required.

[0063] The hydraulic composition may further contain other components in addition to the binder and accelerator, such as silica powder, inorganic powder containing calcium (excluding the above admixture and granulated blast furnace slag), fly ash, silica fume, and inorganic minerals containing Si and Al (excluding aggregates).

[0064] [Method of manufacturing hydraulic composition] One embodiment of the method for producing a hydraulic composition includes a first step of preparing a binder by mixing raw materials including a mineral admixture, granulated blast furnace slag, and gypsum, and a second step of mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder. The mineral admixture contains 20% by mass or more of CaO. The binder and the accelerator can be applied to the contents described above regarding the hydraulic composition.

[0065] In the first step, each component constituting the raw material may be crushed. When crushing is performed in the first step, the order of mixing and crushing is not particularly limited. That is, the various components may be mixed and then crushed, or the various components may be crushed and then mixed, or the various components may be mixed and crushed simultaneously. The mixing of the various components in the first step may be performed using a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, or may be mixed and crushed using a crusher such as a ball mill, a vertical roller mill, or a roller press, or may be mixed using a mixer such as a mechanical mixer after crushing each of the various components.

[0066] The first step includes adjusting the amount of the admixture to be 0.5 to 20 mass% or less and the amount of the granulated blast furnace slag to be 70.0 to 95.5 mass% based on a total of 100 mass% of the binders, and adjusting the amount of the gypsum to be 4.0 to 10.0 mass% in terms of SO3 based on a total of 100 mass% of the binders.

[0067] In the second step, the binder and the accelerator are mixed. The mixing means may be the same as or different from that in the first step. In the second step or in a step other than the first and second steps, other components may be blended. Examples of other components include silica powder, inorganic powders containing calcium (excluding the above-mentioned admixtures and granulated blast furnace slag), fly ash, silica fume, and inorganic minerals containing Si and Al (excluding aggregates).

[0068] The method for producing a hydraulic composition may include other steps in addition to the first step and the second step. Examples of the other steps include a step of crushing a lump of admixture (crushing step), a step of heat-treating the admixture (heat-treatment step), and a step of adjusting the particle size of the admixture (particle size adjustment step). A ball mill or the like can be used for crushing in the crushing step. In the crushing step, the particle size of the admixture may be adjusted to 90 μm or less. In the heat treatment step, the amount of water adhering to the surface of the admixture is reduced. In the heat treatment step, a dryer or the like can be used, and the heating temperature can be 100° C. or more and may be 130° C. or less. The particle size adjustment step is, for example, a step of adjusting the particle size of the admixture using a sieve or the like.

[0069] [Method of manufacturing the hardened body] The hydraulic composition described above is suitable as a raw material for preparing a hardened body such as mortar and concrete. That is, one embodiment of the method for producing a hardened body includes a step of mixing 50 parts by mass of water with 100 parts by mass of the hydraulic composition described above. In the above-mentioned production method, in addition to water, for example, fine aggregate, coarse aggregate, admixture, etc. may be mixed to produce a hardened mortar body. In the above-mentioned method for producing a hardened body, it is preferable to ensure a relatively long hardening time. The hardening time may be, for example, 72 hours or more. During the above-mentioned hardening, it is preferable to maintain the shape of the mortar, etc. in a formwork or the like so as to maintain the shape of the target hardened body.

[0070] The hydraulic composition may be produced in the same manner as the hydraulic composition described above. That is, one embodiment of the method for producing the hardened body includes a first step of preparing a binder by mixing raw materials including a mineral admixture, granulated blast furnace slag, and gypsum, a second step of mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder to obtain a hydraulic composition, and a third step of mixing 50 parts by mass of water with respect to 100 parts by mass of the hydraulic composition. The mineral admixture contains 20% by mass or more of CaO.

[0071] The first step includes adjusting the amount of the admixture to be 0.5 to 20 mass% and the amount of the granulated blast furnace slag to be 70.0 to 95.5 mass% based on a total of 100 mass% of the binders, and adjusting the amount of the gypsum to be 4.0 to 10.0 mass% in terms of SO3 based on a total of 100 mass% of the binders.

[0072] Examples of water include tap water, distilled water, deionized water, etc. The amount of water used may be 20 to 100 parts by mass, or 40 to 70 parts by mass, based on 100 parts by mass of the hydraulic composition.

[0073] The fine aggregate may be one specified in JIS A 5005:2020 "Crushable stone and crushed sand for concrete". Examples of fine aggregate include river sand, land sand, sea sand, crushed sand, silica sand, copper slag fine aggregate, and electric furnace oxidized slag fine aggregate. When using fine aggregate, the amount of fine aggregate may be, for example, 50 to 500 parts by mass, 100 to 300 parts by mass, or 200 to 250 parts by mass relative to 100 parts by mass of the hydraulic composition.

[0074] The coarse aggregate may be one specified in JIS A 5005:2020 "Crushable stone and crushed sand for concrete". Examples of the coarse aggregate include gravel and crushed stone. When using a coarse aggregate, the amount of the coarse aggregate used may be, for example, 50 to 500 parts by mass, 100 to 300 parts by mass, or 200 to 250 parts by mass relative to 100 parts by mass of the hydraulic composition.

[0075] Fine aggregate and coarse aggregate can be used in combination. In this case, the total amount of fine aggregate and coarse aggregate used may be 100 to 300 parts by mass, or 200 to 250 parts by mass, per 100 parts by mass of the hydraulic composition.

[0076] Examples of the admixture include an AE agent, a water reducing agent, an AE water reducing agent, a high-performance water reducing agent, a high-performance AE water reducing agent, a superplasticizer, an antifoaming agent, a shrinkage reducing agent, a setting accelerator, a setting retarder, and a thickener. The amount of the admixture used may be, for example, 0.01 to 2 parts by mass relative to 100 parts by mass of the above-mentioned hydraulic composition.

[0077] [Method for suppressing variation in compressive strength in a composition containing a very large amount of blast furnace slag (e.g., a composition containing 70% or more by mass of blast furnace slag)] By applying the above-mentioned findings, it is possible to provide a method for suppressing the expected variation in compressive strength so that the compressive strength expected from the composition can be exhibited without strict measurement when preparing a hydraulic composition in the region where the amount of blast furnace slag is extremely large (for example, the region where blast furnace slag is 70 mass% or more). This method can also be said to be a method for suppressing the decrease in compressive strength caused by the deviation even if the content of each component deviates from the designed composition of the hydraulic composition. This method can also be said to be a method for suppressing the variation in the exhibited strength even if the composition of the hydraulic composition is changed in the region where the amount of granulated blast furnace slag is extremely large.

[0078] As shown in Non-Patent Document 1, in conventional hydraulic compositions using an alkaline activator such as Portland cement, when the amount of the alkaline activator used is extremely low, the compressive strength fluctuates when the amount of the alkaline activator is changed, resulting in a sudden increase or decrease in the compressive strength. In the present disclosure, by using a material having a composition specified in the present disclosure instead of a hydraulic composition containing an alkaline activator that was dominated by Portland cement, etc., it is possible to suppress the variation in the strength and stably exhibit high strength, even when the composition is changed in a region where the proportion of granulated blast furnace slag is extremely high.

[0079] One embodiment of the method for suppressing the variation of compressive strength includes adjusting the content of gypsum in a composition containing a binder made of a mineral admixture, granulated blast furnace slag, and gypsum to 4.0 to 10.0 mass% in terms of SO3, with the total amount of the binder being 100 mass%, and mixing an accelerator to 0.5 to 8.0 mass parts per 100 mass parts of the binder. The mineral admixture contains 20 mass% or more of CaO. By using this method, it is possible to provide a hydraulic composition that can exhibit a compressive strength that can be fully used in practical use, even if the hydraulic composition contains a very large amount of blast furnace slag, which could not be used at the actual machine level in the past. By applying this method, when a plurality of hydraulic compositions are prepared with a design composition that satisfies the above conditions, even if the compositions are slightly different from each other due to the limit of the weighing accuracy, each hydraulic composition can exhibit a compressive strength that can be expected from the design composition.

[0080] Although several embodiments have been described above, the present disclosure is not limited to the above-described embodiments. In addition, the descriptions of the above-described embodiments can be mutually applied. EXAMPLES

[0081] The present disclosure will be described in more detail below with reference to examples, comparative examples, and reference examples. However, the present disclosure is not limited to the following examples.

[0082] [Raw materials for hydraulic compositions] The following materials were used as raw materials for the hydraulic composition.

[0083] (Admixture) The admixtures used were waste concrete, fresh concrete sludge, converter slag, electric furnace reduced slag, and blast furnace slag. Each admixture was pulverized in a ball mill, dried in a dryer at 100°C until all adhering water was removed, and then sieved to select those with particles of 90 μm or less. The chemical compositions of the waste concrete, converter slag, electric furnace reduced slag, and blast furnace slag were measured using the FP method (fundamental parameter method) by fluorescent X-ray analysis. The results are shown in Table 1.

[0084] The waste concrete used was general waste concrete consisting of aggregate components such as pebbles and sand and cement components. The ready-mix concrete sludge used was dried powder obtained by evaporating water from a mixture of sludge water, and the residue of aggregate recovered from returned concrete and remaining concrete. The converter slag used was converter slag, which is generated as an impurity in the pig iron that is removed when molten pig iron is placed in a converter, auxiliary materials such as quicklime are added, and oxygen is blown into the converter. The electric furnace reduced slag used was electric furnace reduced slag generated during reduction refining in a ladle refining furnace during steel production. The blast furnace cooled slag used was crystalline blast furnace cooled slag, which was obtained by pouring molten slag generated in a blast furnace during steel production into a cooling yard and cooling it naturally or by moderate water spraying.

[0085] (granulated blast furnace slag) The granulated blast furnace slag used was ground granulated blast furnace slag without the addition of gypsum. The chemical composition of the ground granulated blast furnace slag was measured in accordance with the description in JIS R 5202:2015 "Methods for chemical analysis of cement." The results are shown in Table 1.

[0086] (Alkaline stimulant) As the alkali activator, cement clinker, which is commonly used when preparing ordinary Portland cement, was used. In Table 1, "OPC" stands for ordinary Portland cement clinker. The chemical composition of ordinary Portland cement clinker was measured in accordance with the description in JIS R 5202:2015 "Methods for chemical analysis of cement." The results are shown in Table 1.

[0087] [Table 1]

[0088] Table 1 also lists the chemical composition of ordinary Portland cement (OPC) for reference.

[0089] (plaster) The gypsum used was dehydrated gypsum, a by-product of coal-fired power plants, and reagent anhydrous gypsum. In Table 1, dehydrated gypsum is referred to as dihydrate gypsum. The chemical composition of the gypsum was measured in accordance with the description in JIS R 5202:2015 "Methods for chemical analysis of cement." The results are shown in Table 1.

[0090] (Accelerator) The accelerator used was an inorganic accelerator, calcium nitrite monohydrate (hereafter sometimes referred to as CN) manufactured by Kishida Chemical Co., Ltd.

[0091] [Example 1] The binder was prepared by mixing each component so that the granulated blast furnace slag was 84.0% by mass, the waste concrete as the admixture specified in the present disclosure was 1.0% by mass, and the dihydrate gypsum as gypsum was 15% by mass. The gypsum content in the binder was 6.9% in terms of SO3.

[0092] Next, calcium nitrite monohydrate was mixed as an accelerator so that the amount of the accelerator was 2.0 parts by mass per 100 parts by mass of the binder, thereby preparing the hydraulic composition of Example 1.

[0093] [Examples 2 to 14, Comparative Example 1] A hydraulic composition was prepared in the same manner as in Example 1, except that the components and amounts were changed as shown in Table 2.

[0094] [Reference examples 1 and 2] A hydraulic composition containing an alkaline activator, granulated blast furnace slag, gypsum and an accelerator was prepared based on the components and amounts shown in Table 2 without using any of the above-mentioned admixtures.

[0095] [Evaluation of hydraulic composition: compressive strength] The compressive strength of each of the hydraulic compositions prepared in Examples 1 to 14, Comparative Example 1, and Reference Examples 1 and 2 at ages of 7 and 28 days was measured according to the method described below. The results are shown in Table 2. The compressive strength was measured in accordance with the description of JIS R 5201:1992 "Physical Testing Methods for Cement" except that the demolding time of the hardened mortar was changed.

[0096] First, the compressive strength was evaluated using a mortar composition obtained by mixing a hydraulic composition, fine aggregate, and water. Specifically, for each of the hydraulic compositions prepared in the Examples, Comparative Examples, and Reference Examples, 200 parts by mass of sand (standard sand / manufactured by the Cement Association) as fine aggregate and 50 parts by mass of water were mixed with 100 parts by mass of the hydraulic composition to prepare a mortar composition for evaluation. The above-mentioned mixture was adjusted so that the ratio of hydraulic composition:sand:water was 100:300:50 (mass ratio, mixed according to the description of JIS R 5201:2015 "Physical Test Methods for Cement").

[0097] A mortar hardened body was prepared using each of the obtained mortar compositions. First, the above mortar composition was mixed as mortar in a constant temperature room at 20 ° C., and filled into a formwork of 4 cm × 4 cm × 16 cm (prepared according to the description of JIS R 5201: 2015 "Physical Test Methods for Cement"). The formwork was stored in a humidity box and cured for 72 hours. After curing for 72 hours, the formwork was removed to obtain a mortar hardened body. The obtained mortar hardened body was cured underwater in a constant temperature room at 20 ° C. for 7 days (age 7 days). The mortar hardened body after underwater curing was used as a test specimen to measure the compressive strength of the mortar hardened body at 7 days. In the same manner, the obtained mortar hardened body was cured underwater in a constant temperature room at 20 ° C. for 28 days (age 28 days), and the compressive strength of the mortar hardened body at 28 days was measured.

[0098] [Table 2] [Industrial Applicability]

[0099] According to the present disclosure, it is possible to provide a hydraulic composition that can stably exhibit excellent compressive strength by hardening, and a manufacturing method thereof, even when the blending accuracy of the hydraulic composition is low and the composition of each component deviates from the designed composition in the region where the amount of blast furnace slag is extremely large. According to the present disclosure, it is also possible to provide a manufacturing method of a hardened body using the above-mentioned hydraulic composition. According to the present disclosure, it is also possible to provide a method for suppressing the variation of compressive strength even when a large amount of granulated blast furnace slag is contained. According to the hydraulic composition of the present disclosure, it is possible to manufacture a hardened body that can exhibit compressive strength equal to or higher than that of conventional hydraulic compositions, without using cement clinker that emits a large amount of CO2 during preparation. Such a technology is useful because it can reduce the apparent amount of CO2 generated in the manufacture of a hardened body.

Claims

1. The present invention includes a binder including an admixture, granulated blast furnace slag, and gypsum, and an accelerator, The admixture contains 20% by mass or more of CaO, Based on 100% by mass of the binder, the content of the admixture is 0.5 to 20.0% by mass, the content of the granulated blast furnace slag is 70.0 to 95.5% by mass, and the content of the gypsum is SO 3 This is calculated as 4.0 to 10.0 mass%. The content of the accelerator is 0.5 to 8.0 parts by mass per 100 parts by mass of the binder.

2. The hydraulic composition according to claim 1, wherein the content of free lime in the admixture is 0.2 to 5.0 mass %.

3. 3. The hydraulic composition according to claim 1, wherein the admixture comprises at least one selected from the group consisting of electric furnace reduced slag, converter slag, ready mixed concrete sludge, and waste concrete.

4. 3. The hydraulic composition according to claim 1, wherein the accelerator contains at least one monovalent anion selected from the group consisting of nitrite ions, nitrate ions, chloride ions, formate ions, and acetate ions.

5. The hydraulic composition according to claim 1 or 2, wherein the accelerator contains at least one selected from the group consisting of alkali metal salts and alkaline earth metal salts.

6. The hydraulic composition according to claim 1 or 2, wherein the accelerator contains a calcium salt.

7. The hydraulic composition according to claim 1 or 2, wherein the gypsum contains at least one selected from the group consisting of gypsum dihydrate and gypsum hemihydrate.

8. 3. The hydraulic composition according to claim 1, wherein the basicity of the granulated blast furnace slag is 1.60 to 1.

95.

9. The hydraulic composition according to claim 1 or 2, wherein the content of aluminum oxide in the granulated blast furnace slag is 10.0 mass% or more.

10. A first step of preparing a binder by mixing raw materials including an admixture, granulated blast furnace slag, and gypsum; A second step of mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder, The admixture contains 20% by mass or more of CaO, The first step comprises: Based on a total of 100% by mass of the binder, the amount of the admixture is adjusted to 0.5 to 20.0% by mass, and the amount of the granulated blast furnace slag is adjusted to 70.0 to 95.5% by mass; The amount of the gypsum is SO 3 Adjust so that the content is 4.0 to 10.0 mass% in terms of mass conversion. A method for producing a hydraulic composition comprising the steps of:

11. A first step of preparing a binder by mixing raw materials including an admixture, granulated blast furnace slag, and gypsum; A second step of obtaining a hydraulic composition by mixing 0.5 to 8.0 parts by mass of an accelerator with respect to 100 parts by mass of the binder; and a third step of blending 50 parts by mass of water with respect to 100 parts by mass of the hydraulic composition, The admixture contains 20% by mass or more of CaO, The first step comprises: Based on a total of 100% by mass of the binder, the amount of the admixture is adjusted to 0.5 to 20.0% by mass, and the amount of the granulated blast furnace slag is adjusted to 70.0 to 95.5% by mass; The amount of the gypsum is SO 3 Adjust so that the content is 4.0 to 10.0 mass% in terms of mass conversion. A method for producing a cured body, comprising:

12. A composition including a binder made of admixture, granulated blast furnace slag, and gypsum, The content of gypsum is calculated by taking the total amount of the binder as 100% by mass, and 3 Adjust so that the content is 4.0 to 10.0 mass% in terms of mass conversion; and The accelerator is blended in an amount of 0.5 to 8.0 parts by mass relative to 100 parts by mass of the binder, The method for suppressing fluctuations in compressive strength, wherein the admixture contains 20 mass% or more of CaO.

Citation Information

Cited By

  • Cement admixture, cement composition, cement hardened body, and method for producing cement admixture

    WO2025243853A1