Corrosion prevention method and corrosion prevention tape
The anticorrosion tape with a surface protection film and controlled tensile properties addresses wrinkling and adherence issues, providing effective corrosion prevention on large and curved surfaces.
Patent Information
- Application Number
- JP2024049076
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
AI Technical Summary
Existing anticorrosion tapes with high followability tend to develop wrinkles when applied over large areas, while reducing flexibility to prevent wrinkles results in poor adherence to curved surfaces.
The anticorrosion tape consists of a base material with an adhesive layer and a surface protection film, allowing the tape to be applied with the protection film peeled off first for large areas and then attached to curved surfaces, with specific tensile load and peeling force conditions to minimize wrinkling and enhance adherence.
The tape effectively suppresses wrinkling during large-area application and maintains excellent curved surface followability, ensuring strong adhesion and durability.
Smart Images

Figure 2024144303000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a corrosion protection method for a structure and an anticorrosion tape. [Background technology]
[0002] In order to prevent corrosion of iron or alloys containing iron, such as steel, anticorrosive paints containing a large amount of zinc are widely used. Zinc is a metal with a lower potential than iron and has a sacrificial anticorrosive effect, so it is known to have high anticorrosive properties. However, corrosion prevention using paint requires a drying process after application, which takes time, and the work efficiency decreases when performing localized repairs in civil engineering and architectural applications such as bridges. In addition, corrosion prevention using paint is prone to uneven work.
[0003] In view of the above situation, efforts have been made to impart corrosion resistance to tapes and improve workability. For example, a tape is provided with a base film and an adhesive layer provided on one side of the base film, and the compressive stress when the adhesive layer is compressed by 25% in the thickness direction is 5 to 50 N / cm 2 An anti-rust adhesive film having a breaking elongation of 100% or more is known as a conventional technique (see Patent Document 1). This anti-rust adhesive film has excellent conformability, so it can be easily attached to an adherend having a curved surface or corners. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-187017 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the anticorrosive adhesive film of Patent Document 1 has a problem that wrinkles are easily generated when the anticorrosive adhesive film is applied to a large area due to its excellent conformability. In addition, if the flexibility of the anticorrosive adhesive film is reduced in order to suppress the generation of wrinkles when applied to a large area, a problem occurs in that the conformability is deteriorated. Therefore, an object of the present invention is to provide an anticorrosion tape that has excellent curved surface conformability and can suppress the occurrence of wrinkles when applied over a large area, and a corrosion prevention method using the anticorrosion tape. [Means for solving the problem]
[0006] As a result of extensive investigations, the present inventors have found that the above problems can be solved by using a surface protection film, and have completed the present invention. The present invention provides the following [1] to
[17] . [1] A corrosion prevention method comprising: a first step of preparing an anti-corrosion tape comprising a substrate, an adhesive layer provided on one side of the substrate, and a surface protective film provided on the other side of the substrate for protecting the other side of the substrate; and a second step of peeling the surface protective film from the anti-corrosion tape and then attaching the anti-corrosion tape to an adherend, or attaching the anti-corrosion tape to an adherend and then peeling the surface protective film from the anti-corrosion tape. [2] The second step is a step of peeling off the surface protective film from the corrosion protection tape and then attaching the corrosion protection tape to the adherend, wherein the adherend has a curved shape. The corrosion protection method described in [1] above. [3] The area of the anticorrosive tape to be applied is 0.5 m 2 The corrosion prevention method according to the above [2], wherein the corrosion prevention method is less than [4] The second step is a step of attaching the anticorrosion tape to the adherend and then peeling off the surface protective film from the anticorrosion tape, and the adhesion area of the anticorrosion tape on the adherend is 0.5 m 2 The corrosion prevention method described in [1] above. [5] The corrosion prevention method according to any one of the above [1] to [4], wherein the adherend is a concrete structure or a steel structure. [6] An anticorrosion tape comprising a substrate, an adhesive layer provided on one side of the substrate, and a surface protective film provided on the other side of the substrate for protecting the other side of the substrate. [7] A corrosion-protective tape as described in [6] above, wherein the difference between the tensile load when elongated by 2.5% and the tensile load when elongated by 0.5% in a laminate consisting of the substrate and the surface protective film is 2.5 N / mm or more and 6.0 N / mm or less, and the difference between the tensile load when elongated by 2.5% and the tensile load when elongated by 0.5% in the substrate is 1.3 N / mm or less. [8] The T-shaped peeling force when peeling off the surface protective film is 0.1N / 30mm or more. The anticorrosion tape according to [6] or [7] above, having a strength of 2.6N / 30mm or less. [9] The anticorrosion tape according to any one of the above [6] to [8], wherein the material of the surface protective film is at least one resin selected from the group consisting of polyester-based resins and polypropylene-based resins.
[10] The anticorrosion tape according to any one of the above [6] to [9], wherein the thickness of the surface protective film is from 25 μm to 200 μm.
[11] The corrosion-protective tape according to any one of the above [6] to
[10] , wherein the material of the substrate is at least one resin selected from the group consisting of polyethylene-based resins, polypropylene-based resins, acrylic-based resins, fluorine-based resins, and polyvinyl chloride-based resins.
[12] The corrosion-protective tape according to any one of the above [6] to
[11] , wherein the thickness of the substrate is 20 μm or more and 400 μm or less.
[13] The anticorrosion tape according to any one of the above [6] to
[12] , wherein after the surface protective film is peeled off and an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 is performed for 500 hours, the total light transmittance of the anticorrosion tape is 50% or more, after the surface protective film is peeled off and an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 is performed for 500 hours, the substrate is not broken, and after the surface protective film is peeled off and an adhesive strength of the anticorrosion tape is 20 N / 25 mm or more, after the surface protective film is peeled off and an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 is performed for 500 hours.
[14] The anticorrosion tape according to any one of the above [6] to
[13] , wherein the pressure-sensitive adhesive layer has a thickness of 50 to 2500 μm.
[15] The anticorrosion tape according to any one of the above [6] to
[14] , wherein the pressure-sensitive adhesive layer contains a photocurable resin.
[16] The anticorrosion tape according to any one of the above [6] to
[15] , wherein the pressure-sensitive adhesive layer has a storage modulus of 50,000 to 1,000,000 Pa at a temperature of 23°C.
[17] The corrosion-preventive tape according to any one of the above [6] to
[16] , wherein the pressure-sensitive adhesive layer is formed from an acrylic pressure-sensitive adhesive. Effect of the Invention
[0007] According to the present invention, there are provided an anticorrosion tape that has excellent curved surface conformability and can suppress the occurrence of wrinkles when applied over a large area, and a corrosion prevention method using the anticorrosion tape. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic diagram showing an example of the configuration of an anticorrosive tape of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a method for evaluating the convex portion-following ability of an anticorrosive tape. [Diagram 3] FIG. 1 is a diagram for explaining the evaluation of the large-area applicability of anticorrosion tape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Anti-corrosion tape] The anticorrosion tape of the present invention comprises a substrate, a pressure-sensitive adhesive layer provided on one side of the substrate, and a surface protective film provided on the other side of the substrate for protecting the other side of the substrate. The anticorrosion tape of the present invention can suppress the occurrence of wrinkles during application over a large area by the surface protective film, and the anticorrosion tape has excellent curved surface conformability by peeling off the surface protective film.
[0010] (Difference in tensile load) In the anticorrosive tape of the present invention, the difference between the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 2.5% and the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 0.5% is preferably 2.5 N / mm or more and 6.0 N / mm or less. When the difference between the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 2.5% and the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 0.5%, the occurrence of wrinkles in the anticorrosive tape during large-area application can be further suppressed by attaching the anticorrosive tape to the adherend without peeling off the surface protective film. When the difference between the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 2.5% and the tensile load when the laminate consisting of the substrate and the surface protective film is elongated by 0.5%, the anticorrosive tape can be attached to the adherend more easily when the surface protective film is not peeled off. From this viewpoint, the difference between the tensile load when elongated by 2.5% and the tensile load when elongated by 0.5% in a laminate consisting of a substrate and a surface protective film is more preferably 3.0 N / mm to 5.8 N / mm, and even more preferably 3.2 N / mm to 5.5 N / mm. The difference between the tensile load when elongated by 2.5% and the tensile load when elongated by 0.5% in a laminate consisting of a substrate and a surface protective film can be measured by the method described in the Examples below. The difference between the tensile load when elongated by 2.5% and the tensile load when elongated by 0.5% in a laminate consisting of a substrate and a surface protective film can be adjusted by the material and thickness of the surface protective film and the material and thickness of the substrate.
[0011] In the anticorrosion tape of the present invention, the difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate is preferably 1.3 N / mm or less. When the difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate is 1.3 N / mm or less, the curved surface conformability of the anticorrosion tape after peeling off the surface protective film can be further improved. From this viewpoint, the difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate is more preferably 1.0 N / mm or less, and even more preferably 0.5 N / mm or less. The lower limit of the range of the difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate is not particularly limited, but is usually 0.01 N / mm. The difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate can be measured by the method described in the Examples below. The difference between the tensile load when the substrate is elongated by 2.5% and the tensile load when the substrate is elongated by 0.5% can be adjusted by adjusting the material and thickness of the substrate.
[0012] (T-type peeling force) The T-type peeling force when peeling the surface protective film from the anticorrosive tape of the present invention is preferably 0.1 N / 30 mm or more and 2.6 N / 30 mm or less. When the T-type peeling force when peeling the surface protective film from the substrate is 0.1 N / 30 mm or more, when the anticorrosive tape is attached to the adherend without peeling the surface protective film, the occurrence of unintended peeling of the surface protective film can be further suppressed. When the T-type peeling force when peeling the surface protective film from the anticorrosive tape is 2.6 N / 30 mm or less, the surface protective film can be quickly peeled from the anticorrosive tape, and the workability is further improved. From this viewpoint, the T-type peeling force when peeling the surface protective film from the substrate is more preferably 0.1 N / 30 mm or more and 1.0 N / 30 mm or less, even more preferably 0.1 N / 30 mm or more and 0.5 N / 30 mm or less, and even more preferably 0.1 N / 30 mm or more and 0.3 N / 30 mm or less. The T-type peel force when peeling the surface protective film from the substrate can be measured by the method described in the Examples below. The T-type peel force when peeling the surface protective film from the substrate can be appropriately adjusted depending on the conditions of the laminating method and the material of the adhesive layer between the substrate and the surface protective film, as described below.
[0013] (Total light transmittance) After peeling off the surface protective film, the total light transmittance of the anticorrosive tape of the present invention from which the surface protective film has been peeled off is preferably 50% or more after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours. If the total light transmittance of the anticorrosive tape from which the surface protective film has been peeled off is 50% or more after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours after peeling off the surface protective film, the anticorrosive tape has sufficient weather resistance when exposed to the outdoors. From this perspective, the total light transmittance of the anticorrosive tape from which the surface protective film has been peeled off after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours after peeling off the surface protective film is more preferably 60% or more, and even more preferably 70% or more. The upper limit of the range of the total light transmittance of the anticorrosive tape from which the surface protective film has been peeled off after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours after peeling off the surface protective film is not particularly limited, but is usually 100%. The total light transmittance of the anticorrosive tape from which the surface protective film has been peeled off after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours after peeling off the surface protective film can be measured by the method described in the examples below. The total light transmittance of the anticorrosive tape from which the surface protective film has been peeled off after performing an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours after peeling off the surface protective film can be adjusted by the material and thickness of the substrate.
[0014] (Fracture of the substrate) It is preferable that the substrate does not break after 500 hours of accelerated weather resistance testing according to cycle A in JIS K5600-7-7 after peeling off the surface protective film. If the substrate does not break after 500 hours of accelerated weather resistance testing according to cycle A in JIS K5600-7-7 after peeling off the surface protective film, the anticorrosive tape has sufficient weather resistance when exposed to the outdoors. Note that breakage here includes not only complete breakage of the substrate, but also so-called cracks in which the substrate breaks partially.
[0015] (Adhesive strength) The adhesive strength of the anticorrosion tape of the present invention is preferably 20N / 25mm or more. When the adhesive strength of the anticorrosion tape is 20N / 25mm or more, the anticorrosion tape has sufficient adhesive strength for use in anticorrosion of concrete structures and steel structures. From this viewpoint, the adhesive strength of the anticorrosion tape of the present invention is more preferably 30N / 25mm or more, and even more preferably 40N / 25mm or more. The upper limit of the range of the adhesive strength of the anticorrosion tape of the present invention is not particularly limited, but is usually 100N / 25mm. The adhesive strength of the anticorrosion tape can be measured by the method described in the Examples below. The adhesive strength of the anticorrosion tape can be adjusted by the type of adhesive contained in the adhesive layer and the thickness of the adhesive layer.
[0016] In the anticorrosion tape of the present invention, the adhesive strength of the anticorrosion tape after peeling off the surface protective film and carrying out an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours is preferably 20N / 25mm or more. If the adhesive strength of the anticorrosion tape after peeling off the surface protective film and carrying out an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours is 20N / 25mm or more, the anticorrosion tape will have sufficient weather resistance when exposed to the outdoors. From this perspective, the adhesive strength of the anticorrosion tape after peeling off the surface protective film and carrying out an accelerated weather resistance test according to cycle A in JIS K5600-7-7 for 500 hours is more preferably 30N / 25mm or more, and even more preferably 40N / 25mm or more. The upper limit of the range of the adhesive strength of the anticorrosion tape of the present invention is not particularly limited, but is usually 100N / 25mm. The adhesive strength of the anticorrosion tape after peeling off the surface protective film and carrying out an accelerated weather resistance test for 500 hours in accordance with cycle A of JIS K5600-7-7 can be measured by the method described in the Examples below. The adhesive strength of the anticorrosion tape can be adjusted by the material and thickness of the substrate, and the type of adhesive contained in the adhesive layer and the thickness of the adhesive layer.
[0017] (Adhesive layer) The adhesive layer of the anticorrosive tape of the present invention may contain a metal having a lower potential than iron. When the adhesive layer contains a metal having a lower potential than iron, the anticorrosive tape has sacrificial anticorrosive properties, and when the adherend is a metal material, the anticorrosive properties of the anticorrosive tape are further improved. The metal having a lower potential than iron is preferably dispersed in the adhesive constituting the adhesive layer.
[0018] <Metals with a lower potential than iron> Examples of metals with a lower potential than iron (hereinafter also referred to as "sacrificial corrosion protection metals") include cadmium, chromium, zinc, manganese, and aluminum, among which zinc and aluminum are preferred, and zinc is particularly preferred. Use of zinc provides excellent sacrificial corrosion protection.
[0019] The sacrificial metal for corrosion protection may be dispersed in the pressure-sensitive adhesive as a filler in any form, such as a particulate form, a scale form, a spindle form, etc., but is preferably in a particulate form. By making the sacrificial metal for corrosion protection into a particulate form, it becomes easy to disperse in the pressure-sensitive adhesive layer without substantially decreasing the adhesiveness of the pressure-sensitive adhesive layer. In this specification, the particle shape refers to a particle shape having a small ratio of the length in the long axis direction to the length in the short axis direction (aspect ratio), for example, an aspect ratio of 3 or less, preferably 2 or less. The lower limit of the aspect ratio is 1. The particle shape is not particularly limited, and may be spherical or amorphous such as powder.
[0020] The specific surface area per unit volume of the sacrificial metal is preferably 0.15 m 2 / cm 3 The specific surface area per unit volume of the sacrificial corrosion protection metal is 0.15 m 2 / cm 3 If the specific surface area per unit volume of the sacrificial protection metal is more preferably 0.16 m or less, the electron transfer is less likely to be uneven, and the sacrificial protection property of the anticorrosive tape is less uneven. 2 / cm 3 The specific surface area per unit volume of the sacrificial corrosion protection metal is 0.16 m 2 / cm 3 From these viewpoints, the specific surface area per unit volume of the sacrificial anticorrosive metal is more preferably 0.25 m or more. 2 / cm 3 More preferably, it is 0.35 m or more. 2 / cm 3 More preferably, it is 1.0 m or more. 2 / cm 3 The upper limit of the range of the specific surface area per unit volume of the sacrificial corrosion protection metal is not particularly limited, but is, for example, 1.6 m 2 / cm 3 and preferably 1.45 m 2 / cm 3 and more preferably 1.2 m 2 / cm 3It is.
[0021] The content of the sacrificial metal for corrosion protection in the adhesive layer is preferably 40% by mass or less based on the total amount of the adhesive layer. When the content of the sacrificial metal for corrosion protection in the adhesive layer is 40% by mass or less, the adhesiveness of the anticorrosive tape is further improved. From this viewpoint, the content of the sacrificial metal for corrosion protection in the adhesive layer is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and even more preferably 12% by mass or less. In addition, from the viewpoint of the sacrificial anticorrosive properties of the anticorrosive tape, the content of the sacrificial metal for corrosion protection in the adhesive layer is, for example, 4.5% by mass or more, preferably 5% by mass or more, more preferably 6% by mass or more, and even more preferably 8% by mass or more.
[0022] The average particle size of the sacrificial metal is preferably 1 μm or more and 100 μm or less. When the average particle size of the sacrificial metal is 1 μm or more and 100 μm or less, the adhesiveness of the anticorrosive tape can be further improved while the unevenness of the sacrificial protection of the anticorrosive tape can be further reduced. From this viewpoint, the average particle size of the sacrificial metal is more preferably 10 μm or more and 80 μm or less, even more preferably 25 μm or more and 60 μm or less, and even more preferably 35 μm or more and 50 μm or less. The average particle size of the sacrificial metal can be measured by the method described in the examples below.
[0023] <Conductive materials> In addition to the sacrificial metal, the adhesive layer preferably further contains a conductive material other than the sacrificial metal. When the conductive material is contained, the electrons released when the sacrificial metal is ionized can be easily transferred to the adherend, and the sacrificial protection property can be easily improved. In addition, when the specific surface area per unit volume of the sacrificial metal is 0.16 m, the adhesive layer preferably contains a conductive material other than the sacrificial metal. 2 / cm 3 By making the specific surface area per unit volume of the sacrificial protection metal 0.16 m or more, the sacrificial protection metal can be more easily brought into contact with the conductive material, and the sacrificial protection property can be more easily improved. 2 / cm 3By doing so, it is possible to suppress local interruption of the movement of electrons between the sacrificial protection metal and the conductive material, and as a result, it is possible to further reduce unevenness in the sacrificial protection properties. The conductive material may be one or more selected from carbon-based materials, metal-based materials, metal oxide-based materials, ionic polymers, and conductive polymers. Examples of carbon-based materials include carbon black, graphite, graphene, carbon nanotubes, and acetylene black. Examples of metal-based materials include metals with a more noble potential than iron, such as gold, silver, copper, nickel, or alloys containing these metals, or iron. Examples of metal oxide materials include indium tin oxide (ITO), antimony trioxide (ATO), fluorine-doped tin oxide (FTO), and zinc oxide. Examples of conductive polymers include polyacetylene, polypyrrole, PEDOT (polyethylenedioxythiophene), PEDOT / PSS (a composite of polyethylenedioxythiophene and polystyrene sulfonic acid), polythiophene, polyaniline, poly(p-phenylene), polyfluorene, polycarbazole, polysilane, or derivatives thereof. Examples of ionic polymers include sodium polyacrylate and potassium polyacrylate. The conductive materials may be used alone or in combination of two or more. Among the above, the conductive material is preferably a carbon-based material, and more preferably a carbon nanotube.
[0024] <Carbon nanotubes> The adhesive layer preferably contains carbon nanotubes. By containing carbon nanotubes, the sacrificial corrosion protection of the adhesive layer is improved and the adhesive strength can be maintained at a high level, making it easier to obtain an anticorrosive tape with good adhesion, sacrificial corrosion protection, and sacrificial corrosion stability. This is presumably because, although carbon nanotubes are a conductive material, the amount required to exhibit a certain level of sacrificial corrosion protection is small compared to other types of conductive materials, so the degree of decrease in adhesive strength is small.
[0025] Carbon nanotubes are tubular materials made from carbon. Carbon nanotubes have excellent electrical properties, and when combined with resins, they can be used to form highly conductive sheets. Carbon nanotubes are made of graphite sheets with a hexagonal mesh of carbon atoms rolled into a cylinder. Carbon nanotubes rolled in one layer are called single-wall carbon nanotubes, and those rolled in multiple layers are called multi-wall carbon nanotubes. In the anticorrosive tape according to one embodiment of the present invention, the type of carbon nanotube is not particularly limited, and may be any of single-wall carbon nanotubes, multi-wall carbon nanotubes, and mixtures containing these in any ratio. Carbon nanotubes manufactured by various methods such as arc discharge, laser evaporation, and chemical vapor deposition (CVD) can also be used.
[0026] The average diameter of the carbon nanotubes is preferably 1 μm to 100 nm, more preferably 2 μm to 15 nm. The average length of the carbon nanotubes is preferably 0.1 μm to 1000 μm, more preferably 10 μm to 500 μm. The aspect ratio of the carbon nanotubes (average length / average diameter) is preferably 10 to 100,000, more preferably 500 to 30,000. The diameter of a carbon nanotube refers to the outer diameter in the case of a single-wall carbon nanotube, and the outer diameter of the outermost tube in the case of a multi-wall carbon nanotube. The diameter and length of a carbon nanotube may be measured, for example, in an image obtained by observation with a transmission electron microscope (TEM), and the average diameter and average length may be calculated as the arithmetic mean of any 50 nanotubes.
[0027] From the viewpoint of the sacrificial corrosion resistance and adhesive strength of the adhesive layer, the content of the conductive material in the adhesive layer is preferably 0.005 mass% or more and 10 mass% or less, more preferably 0.007 mass% or more and 5 mass% or less, and even more preferably 0.01 mass% or more and 3 mass% or less, based on the total amount of the adhesive layer.
[0028] When the conductive material is carbon nanotubes, the content of the carbon nanotubes in the adhesive layer is preferably 0.005 mass% or more and 0.1 mass% or less, more preferably 0.007 mass% or more and 0.05 mass% or less, and even more preferably 0.01 mass% or more and 0.03 mass% or less, based on the total amount of the adhesive layer. When the carbon nanotube content is equal to or greater than these lower limits, the sacrificial corrosion resistance is likely to be enhanced, whereas when the carbon nanotube content is equal to or less than these upper limits, the adhesive strength is likely to be improved.
[0029] <Adhesive> The adhesive layer is preferably formed of an adhesive. The type of adhesive is not particularly limited, but examples thereof include acrylic adhesives, rubber adhesives, urethane adhesives, and silicone adhesives. These may be used alone or in combination. Among these, the pressure-sensitive adhesive layer is preferably formed from an acrylic pressure-sensitive adhesive. The pressure-sensitive adhesive layer may contain a photocurable resin so that the pressure-sensitive adhesive layer can be obtained by irradiating the pressure-sensitive adhesive composition with light to polymerize the polymerizable monomer.
[0030] <Acrylic adhesive> The acrylic pressure-sensitive adhesive is a pressure-sensitive adhesive containing an acrylic polymer obtained by polymerizing a polymerizable monomer including a (meth)acrylic acid alkyl ester monomer (A). In this specification, the term "(meth)acrylic acid alkyl ester" refers to a concept including both acrylic acid alkyl ester and methacrylic acid alkyl ester, and the same applies to other similar terms. In addition, the term "polymerizable monomer" refers to a concept that can include not only a compound having no repeating unit, but also a monomer itself having a repeating unit, such as the olefin polymer (C) described later, as long as it is a compound that copolymerizes with the (meth)acrylic acid alkyl ester monomer (A).
[0031] ((Meth)acrylic acid alkyl ester monomer (A)) The (meth)acrylic acid alkyl ester monomer (A) is an ester of (meth)acrylic acid and an aliphatic alcohol, and is preferably an alkyl ester derived from an aliphatic alcohol in which the carbon number of the alkyl group of the aliphatic alcohol is preferably 2 to 14, more preferably 4 to 10. When the carbon number of the alkyl group is within this range, the adhesive strength is easily increased, and the storage modulus at 23°C of the adhesive described below is easily adjusted to a predetermined range.
[0032] Specific examples of the (meth)acrylic acid alkyl ester monomer (A) include ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, and tetradecyl (meth)acrylate. Among these, n-butyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate are preferred, and n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or a combination thereof is more preferred. The (meth)acrylic acid alkyl ester monomers may be used alone or in combination of two or more kinds.
[0033] The constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) constitutes the main component in the adhesive layer, and its content is generally 30% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more based on the total amount of the adhesive layer. In this way, by increasing the content of the (meth)acrylic acid alkyl ester monomer (A), it is possible to impart the desired adhesive strength to the adhesive layer. In addition, the content of the constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) is, for example, 97% by mass or less, preferably 95% by mass or less, more preferably 90% by mass or less in order to contain a certain amount or more of other components. The content of the constituent unit derived from the (meth)acrylic acid alkyl ester monomer (A) in the pressure-sensitive adhesive layer is substantially the same as the content of the (meth)acrylic acid alkyl ester monomer (A) in the pressure-sensitive adhesive composition described below, and can be expressed interchangeably. The same applies to components other than the component (A), such as the components (B) and (C) described below.
[0034] <Polar group-containing vinyl monomer (B)> The polymerizable monomer preferably contains a polar group-containing vinyl monomer (B) in addition to the (meth)acrylic acid alkyl ester monomer (A). The polar group-containing vinyl monomer (B) has a polar group and a vinyl group. By using the polar group-containing monomer (B), the adhesive strength to the adherend is easily improved. Examples of the polar group-containing vinyl monomer (B) include carboxylic acid vinyl esters such as vinyl acetate, carboxylic acids containing a vinyl group such as (meth)acrylic acid and itaconic acid, and their anhydrides, vinyl monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyoxyethylene (meth)acrylate, and polyoxypropylene (meth)acrylate, and nitrogen-containing vinyl monomers such as (meth)acrylonitrile, N-vinylpyrrolidone, N-vinylcaprolactam, N-vinyllaurolactam, (meth)acryloylmorpholine, (meth)acrylamide, dimethyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and dimethylaminomethyl(meth)acrylate. Among these, (meth)acrylic acid, itaconic acid, and other vinyl group-containing carboxylic acids and their anhydrides are preferred, (meth)acrylic acid is more preferred, and acrylic acid is even more preferred. These polar group-containing vinyl monomers (B) may be used alone or in combination of two or more.
[0035] When the polar group-containing vinyl monomer (B) is used, the content of the structural unit derived from the polar group-containing vinyl monomer (B) in the adhesive layer is preferably 1 to 15 parts by mass, more preferably 2 to 12 parts by mass, and even more preferably 3 to 10 parts by mass, relative to 100 parts by mass of the structural unit derived from the (meth)acrylic acid alkyl ester monomer (A). By setting the content of the polar group-containing vinyl monomer (B) within such a range, the adhesive strength of the anticorrosion tape is easily improved.
[0036] <Olefin polymer (C)> The polymerizable monomer preferably further contains an olefin polymer (C) having a polymerizable bond at one end. By using such an olefin polymer (C), the adhesive strength of the anticorrosion tape can be easily improved. The polymerizable bond means an unsaturated carbon-carbon bond capable of polymerizing with a polymerizable monomer, and examples thereof include an unsaturated double bond, and preferably a (meth)acryloyl group. The olefin polymer (C) may be a polyolefin having a (meth)acryloyl group at one end. The polyolefin is a polymer of an aliphatic hydrocarbon compound having a double bond, such as ethylene, propylene, butane, butadiene, isoprene, or the like, or a hydrogenated product thereof.
[0037] Examples of polyolefins having a (meth)acryloyl group at one end include polyethylene having a (meth)acryloyl group at one end, which is prepared by reacting polyethylene having an epoxy group at one end with (meth)acrylic acid. In addition, examples include polybutadiene having a (meth)acryloyl group at one end or a hydrogenated product thereof, and examples of commercially available products thereof include "L-1253" manufactured by Kuraray Co., Ltd.
[0038] The number average molecular weight of the olefin polymer (C) is preferably from 500 to 20000, more preferably from 1000 to 10000. The number average molecular weight may be measured by gel permeation chromatography (GPC) and calculated using a calibration curve of standard polystyrene. In addition, the content of the structural units derived from the olefin polymer (C) in the pressure-sensitive adhesive layer is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 2 parts by mass or more and 15 parts by mass or less, and even more preferably 4 parts by mass or more and 12 parts by mass or less, per 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0039] <Crosslinking agent (D)> The polymerizable monomer preferably further contains a crosslinking agent. Examples of the crosslinking agent include a polyfunctional monomer having two or more vinyl groups, and preferably a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups. The use of a polyfunctional monomer makes it easier to adjust the adhesive strength of the adhesive layer to an appropriate range. The polyfunctional (meth)acrylate is not particularly limited, and examples thereof include bifunctional alkyl (meth)acrylates such as hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, proxied trimethylolpropane triacrylate, proxied glyceryl triacrylate, neopentyl glycol adipate diacrylate, and the like, as well as polymers such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and liquid hydrogenated 1,2-polybutadiene di(meth)acrylate. Among these polyfunctional (meth)acrylates, polymers are preferred, and liquid hydrogenated 1,2-polybutadiene diacrylate is more preferred. Commercially available liquid hydrogenated 1,2-polybutadiene diacrylates include "TEAI-1000" manufactured by Nippon Soda Co., Ltd. In addition, bifunctional alkyl (meth)acrylates are also preferred, and commercially available products include A-HD-N of the NK Ester series manufactured by Shin-Nakamura Chemical Co., Ltd. In addition, the content of the structural units derived from the crosslinking agent in the pressure-sensitive adhesive layer is preferably 0.005 parts by mass or more and 3 parts by mass or less, more preferably 0.01 parts by mass or more and 2.0 parts by mass or less, and even more preferably 0.02 parts by mass or more and 1.5 parts by mass or less, relative to 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0040] <Tackifier resin> The acrylic adhesive may contain a tackifier resin from the viewpoint of improving adhesive strength. As the tackifier resin, a tackifier resin having low polymerization inhibition properties, such as hydrogenated terpene resin, hydrogenated rosin, disproportionated rosin resin, petroleum resin, etc., is preferable. Among these, hydrogenated tackifier resins are preferable because tackifier resins having many double bonds inhibit polymerization reactions, and hydrogenated petroleum resins are particularly preferable. From the viewpoint of improving the cohesive strength and adhesive strength of the adhesive, the softening point of the tackifier resin may be about 95° C. or higher, but preferably includes one that is 120° C. or higher, and for example, one that is 95° C. or higher and lower than 120° C. may be used in combination with one that is 120° C. or higher and 150° C. or lower. The softening point may be measured by the ring and ball method specified in JIS K2207. The content of the tackifier resin in the acrylic adhesive is preferably 3 parts by mass or more and 40 parts by mass or less, more preferably 4 parts by mass or more and 35 parts by mass or less, and even more preferably 5 parts by mass or more and 25 parts by mass or less, relative to 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0041] <Fine particles> The acrylic adhesive may contain fine particles, which can improve the adhesive strength. Examples of the fine particles include inorganic hollow particles such as glass balloons, shirasu balloons, and fly ash balloons; organic hollow particles made of polymethyl methacrylate, acrylonitrile-vinylidene chloride copolymers, polystyrene, and phenolic resins; inorganic fine particles such as glass beads, silica beads, and synthetic mica; and organic fine particles such as ethyl polyacrylate, polyurethane, polyethylene, and polypropylene. The content of the microparticles in the acrylic adhesive is preferably 0.1 parts by mass or more and 15 parts by mass or less, more preferably 0.3 parts by mass or more and 10 parts by mass or less, and even more preferably 0.5 parts by mass or more and 7 parts by mass or less, relative to 100 parts by mass of the structural units derived from the (meth)acrylic acid alkyl ester monomer (A).
[0042] <Other ingredients> The acrylic adhesive used in the adhesive layer may contain, in addition to the components described above, various additives conventionally used in adhesives, such as plasticizers, softeners, pigments, dyes, photopolymerization initiators, flame retardants, and thickeners.
[0043] <Method of manufacturing acrylic adhesive and adhesive layer> The acrylic adhesive can be obtained by irradiating a pressure-sensitive adhesive composition containing the above-mentioned polymerizable monomer, and optionally a sacrificial anticorrosive metal and a conductive material with light to polymerize the polymerizable monomer. The pressure-sensitive adhesive composition may also contain at least one of the above-mentioned tackifier resin, fine particles, and other components as required. More specifically, first, the polymerizable monomer, the sacrificial corrosion protection metal and conductive material which are blended as necessary, and further the tackifier resin, fine particles, and other components which are blended as necessary are placed in a reaction vessel such as a glass vessel and mixed to obtain a pressure-sensitive adhesive composition. Next, in order to remove dissolved oxygen in the pressure-sensitive adhesive composition, an inert gas such as nitrogen gas is generally supplied to purge the oxygen. Then, the pressure-sensitive adhesive composition is applied onto a release sheet, or onto a support such as a resin film, woven fabric, or nonwoven fabric, and then irradiated with light to polymerize the polymerizable monomer, thereby obtaining a pressure-sensitive adhesive layer. The steps from coating or impregnation with the pressure-sensitive adhesive composition to the step of irradiating with light are preferably carried out in an inert gas atmosphere or in a state in which oxygen is blocked by a film or the like. In the present production method, the pressure-sensitive adhesive composition obtained by mixing the components may be pre-polymerized before being applied to a release sheet, a support or the like in order to increase the viscosity.
[0044] <Rubber-based adhesive> Next, the rubber-based adhesive used in the adhesive layer will be described. The rubber-based adhesive contains a rubber component and a tackifier resin, and it is preferable to use a styrene-isoprene block copolymer as the rubber component. The styrene-isoprene block copolymer has a diblock ratio of preferably 25 to 70% by mass, more preferably 30 to 65% by mass, and even more preferably 45 to 60% by weight. Here, the diblock refers to a diblock consisting of styrene and isoprene. By setting the diblock ratio within the above range, it becomes easier to increase the adhesive strength. In addition to the diblock, the styrene-isoprene block copolymer also contains one having three or more blocks, such as a triblock consisting of a styrene, isoprene, and styrene block.
[0045] The amount of styrene in the styrene-isoprene block copolymer is not particularly limited, but is preferably 14 to 24% by mass, and more preferably 15 to 18% by mass. If the amount of styrene is 14% by mass or more, the adhesive tends to have high cohesiveness. If the amount of styrene is 24% by mass or less, the cohesive strength becomes moderate and adhesive strength is easily expressed. The molecular weight of the styrene-isoprene block copolymer is not particularly limited, but the mass average molecular weight is preferably 100,000 to 400,000, and more preferably 150,000 to 250,000. The mass average molecular weight here refers to the molecular weight measured in terms of polystyrene by a GPC (gel permeation chromatography) method.
[0046] The tackifier resin used in the rubber-based adhesive can be any of various types, but is preferably a petroleum-based resin, a terpene resin, or a coumarone resin. The tackifier resin may be used alone or in combination of two or more types, but it is preferable to use a petroleum-based resin in combination with at least one selected from a terpene resin and a coumarone resin. Such a combination of tackifier resins makes it easier to improve the adhesive strength. Examples of the petroleum resin include aliphatic petroleum resin (C5 petroleum resin), alicyclic petroleum resin, aromatic petroleum resin, etc., and from the viewpoint of compatibility with the styrene-isoprene block copolymer, aliphatic petroleum resin is preferred. In addition, it is preferable to use a petroleum resin having a softening point of about 90 to 120°C. The terpene resin may have a softening point of about 80 to 120° C., but from the viewpoint of ensuring adhesive strength, it is preferable that the softening point is less than 100° C. The coumarone resin used has a softening point of preferably 110 to 130° C., more preferably 115 to 125° C., in order to ensure cohesive strength.
[0047] The amount of the tackifier resin is preferably 60 to 250 parts by mass, more preferably 100 to 200 parts by mass, and even more preferably 110 to 180 parts by mass, per 100 parts by mass of the rubber component. By setting the amount of the tackifier resin within the above range, it is possible to improve the cohesive force and impart appropriate adhesive strength. When a petroleum-based resin is used in combination with at least one selected from a terpene resin and a coumarone resin, the amount of the petroleum-based resin is preferably 50 to 200 parts by mass, more preferably 60 to 150 parts by mass, and more preferably 60 to 110 parts by mass, relative to 100 parts by mass of the rubber component. On the other hand, the amount of the terpene resin is preferably 10 to 70 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 30 to 50 parts by mass, relative to 100 parts by mass of the rubber component. Furthermore, the amount of the coumarone resin is preferably 10 to 60 parts by mass, more preferably 15 to 50 parts by mass, and even more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the rubber component. The rubber-based adhesive may contain the above-mentioned fine particles, like the acrylic-based adhesive, and may also contain a sacrificial corrosion protection metal, a conductive material, a softener, an antioxidant, a filler, etc., as necessary.
[0048] <Urethane adhesive> The urethane-based adhesive is not particularly limited, and examples thereof include urethane resins obtained by reacting at least a polyol with a polyisocyanate compound. Examples of the polyol include polyether polyol, polyester polyol, polycarbonate polyol, polycaprolactone polyol, etc. Examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, hexamethylene diisocyanate, etc. These urethane adhesives may be used alone or in combination of two or more. In addition, as the urethane-based adhesive, a urethane resin obtained by reacting a polyurethane polyol with a polyfunctional isocyanate-based curing agent may be used. The polyurethane polyol may be a reaction product of the above-mentioned polyol with a polyisocyanate compound, or a reaction product of a polyol with a polyisocyanate compound and a chain extender such as a diamine. As the polyfunctional isocyanate-based curing agent, any compound having two or more isocyanate groups may be used, and the above-mentioned isocyanate compounds may be used. The urethane-based adhesive may contain the above-mentioned fine particles in addition to the urethane resin, and may also contain a tackifier resin, a sacrificial corrosion-protective metal, a conductive material, a softener, an antioxidant, a filler, etc., as necessary.
[0049] <Silicone-based adhesive> Examples of silicone-based adhesives include silicone-based adhesives of addition reaction type, peroxide curing type, or condensation reaction type. Among them, addition reaction type silicone-based adhesives are preferably used from the viewpoint of being curable at low temperature in a short time. The addition reaction type silicone-based adhesive is cured when the adhesive layer is formed. When an addition reaction type silicone-based adhesive is used as the silicone-based adhesive, the silicone-based adhesive may contain a catalyst such as a platinum catalyst. The silicone-based adhesive may contain fine particles, and may also contain a crosslinking agent and various additives for controlling adhesive strength.
[0050] <Thickness> The thickness of the adhesive layer is preferably 50 μm or more and 2500 μm or less, more preferably 100 μm or more and 2000 μm or less, and even more preferably 120 μm or more and 1500 μm or less. By making the thickness 50 μm or more, the self-repairing ability can be increased, and the anticorrosive properties of the anticorrosive tape can be improved, and the adhesive strength can also be easily increased. In addition, by making the thickness of the adhesive layer 2500 μm or less, the effect of improving the anticorrosive performance according to the thickness can be obtained.
[0051] <Storage modulus> The storage modulus of the pressure-sensitive adhesive layer at a temperature of 23° C. is preferably 50,000 to 1,000,000 Pa. When the storage modulus at a temperature of 23° C. is within the above range, when the pressure-sensitive adhesive layer is damaged by an external impact or the like, the force to restore the damaged part (hereinafter also referred to as self-repairing force) becomes strong. As a result, rust generation is suppressed and anticorrosive performance is improved. From the viewpoint of increasing the self-repairing force and improving the anticorrosive performance, the storage modulus of the pressure-sensitive adhesive layer at a temperature of 23° C. is more preferably 200,000 to 800,000 Pa, and further preferably 300,000 to 700,000 Pa. The storage modulus of the pressure-sensitive adhesive layer at a temperature of 23° C. can be measured by the method described in the Examples below. The storage modulus of the pressure-sensitive adhesive layer at a temperature of 23° C. can be adjusted by the composition of the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer.
[0052] <Base material> The substrate in the anticorrosive tape of the present invention is preferably one having excellent flexibility from the viewpoint of curved surface conformability. Examples of the substrate in the anticorrosive tape of the present invention include sheet-like materials such as resin films, woven fabrics, knitted fabrics, nonwoven fabrics, and metal foils. Examples of the resin film include polyethylene resin films, polypropylene resin films, acrylic resin films, fluorine resin films, polyvinyl chloride resin films, polycarbonate resin films, AES resin films, and ASA resin films. The woven fabric is, for example, a woven fabric made of natural fibers such as cotton, or synthetic resin fibers such as rayon, acetate, nylon, polyethylene terephthalate (PET), polyethylene, or polypropylene. The knitted fabric is made of, for example, natural fibers such as cotton, or synthetic resin fibers such as rayon, acetate, nylon, polyethylene terephthalate (PET), polyethylene, or polypropylene. The nonwoven fabric is made of synthetic resin fibers, such as polyamide, polyester, polyacrylic, polyolefin, or polyurethane. Examples of metal foils include metal foils of iron and its alloys, metal foils of metals having a lower electric potential than iron, such as chromium, zinc, titanium, aluminum, and magnesium, and metal foils of metals having a higher electric potential than iron, such as gold, silver, copper, tin, nickel, and cobalt. These sheet-like materials can be used alone or in combination of two or more. From the viewpoint of the corrosion resistance of the corrosion-resistant tape, the substrate is preferably a metal foil of a metal having a lower potential than iron, more preferably a zinc foil. When the substrate is a metal foil of a metal having a lower potential than iron, the substrate is preferably laminated directly on the pressure-sensitive adhesive layer. From the viewpoint of protecting the pressure-sensitive adhesive layer, the substrate is preferably a resin film, and more preferably at least one resin film selected from the group consisting of polyolefin-based resin films such as polyethylene-based resin films and polypropylene-based resin films, acrylic-based resin films, fluorine-based resin films, and polyvinyl chloride-based resin films. Among these, acrylic resin films are preferred from the viewpoints that the substrate is not deteriorated by ultraviolet irradiation and the substrate blocks ultraviolet light, making the pressure-sensitive adhesive layer less likely to deteriorate.
[0053] The thickness of the substrate is preferably 20 μm or more and 400 μm or less, more preferably 30 μm or more and 300 μm or less, and even more preferably 40 μm or more and 250 μm or less. When the substrate is 20 μm or more, it can function as a support. When the substrate is 400 μm or less, it is easy to increase the adhesion to the adherend.
[0054] <Surface protection film> The surface protective film in the anticorrosive tape of the present invention is not particularly limited as long as it is a resin film that can suppress the deformation of the substrate that causes wrinkles in the anticorrosive tape. Examples of the resin film used in the surface protective film in the anticorrosive tape of the present invention include polyester-based resin films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polypropylene-based resin films such as biaxially oriented polypropylene (OPP), polyamide-based resin films such as biaxially oriented nylon (ONy), polyimide-based resin films, polyacetal-based resin films, polycarbonate-based resin films, modified polyphenylene oxide-based resin films, polyphenylene sulfide-based resin films, polysulfone-based resin films, polyether ketone-based resin films, and biaxially oriented polypropylene. These resin films can be used alone or in combination of two or more. Among these resin films, at least one resin film selected from the group consisting of polyester-based resin films, polypropylene-based resin films, and polyamide-based resin films is preferred from the viewpoint of suppressing the occurrence of wrinkles in the anticorrosive tape during large-area application.
[0055] The thickness of the surface protection film is preferably 25 μm or more and 200 μm or less, more preferably 25 μm or more and 150 μm or less, even more preferably 38 μm or more and 100 μm or less, and even more preferably 38 μm or more and 75 μm or less. By making the surface protection film 25 μm or more, the occurrence of wrinkles in the anticorrosive tape during application over a large area can be further suppressed. In addition, by making the thickness 200 μm or less, the adhesion to the adherend can be easily increased.
[0056] The surface protection film may be directly laminated on the substrate, but is preferably laminated via an adhesive layer from the viewpoint of securing a certain adhesive force to the substrate. The adhesive layer may be composed of a known adhesive or pressure sensitive adhesive, or may be composed of a thermoplastic resin. In the case of a thermoplastic resin, it is also called a pseudo-adhesive layer, and the surface protection film may be attached to the substrate via the pseudo-adhesive layer by thermal lamination or the like. The substrate and the surface protective film may be laminated by a known laminating method such as thermal lamination, hot melt lamination, non-solvent lamination, wet lamination, dry lamination, extrusion coating lamination, or co-extrusion lamination.
[0057] <Composition of anti-corrosion tape> An example of the configuration of the anticorrosion tape of the present invention is shown in Figure 1. The anticorrosion tape 10 comprises a substrate 13, an adhesive layer 11 provided on one surface of the substrate 13, and a surface protection film 12 provided on the other surface of the substrate 13 for protecting the other surface of the substrate 13.
[0058] The anticorrosion tape 10 may have a release sheet (not shown) attached to the surface of the adhesive layer 11. The release sheet is preferably peeled off from the adhesive layer 11 before using the anticorrosion tape to expose the adhesive layer 11, and the anticorrosion tape is then attached to an adherend by the exposed adhesive layer 11. More specifically, the release sheet is preferably attached to the surface of the adhesive layer 11 opposite to the surface on which the base material 13 is provided, i.e., surface 11A. The release sheet may be a resin film, and it is preferable that the surface to be bonded to the pressure-sensitive adhesive layer is a release-treated surface that has been subjected to a release treatment using a silicone release agent or the like.
[0059] The anticorrosive tape of the present invention is used by being attached to various adherends, and the type of the adherend is not particularly limited. The anticorrosive tape of the present invention has excellent adhesive strength and anticorrosive properties, so it is preferable to use it by being attached to the surface of an adherend made of various metal materials. The metal material is preferably a metal material containing at least one selected from the group consisting of iron and alloys containing iron. Specific examples of the alloy containing iron include alloy steels such as nickel-chromium steel, nickel-chromium-molybdenum steel, chromium steel, chromium-molybdenum steel, and manganese steel, and various steel materials such as carbon steel. In addition to metal materials, concrete is also suitable as an adherend. For example, by attaching the anticorrosive tape of the present invention to a concrete structure that has deteriorated or been damaged, it is possible to prevent the concrete from peeling off due to further deterioration or damage. Of course, the adherend may be made of a material other than a metal material or concrete.
[0060] [Corrosion prevention method] The corrosion prevention method of the present invention includes a first step of preparing the corrosion prevention tape of the present invention, and a second step of peeling off the surface protective film from the corrosion prevention tape of the present invention and then attaching the corrosion prevention tape to an adherend, or peeling off the surface protective film from the corrosion prevention tape. This makes it possible to prevent wrinkles from occurring in the corrosion prevention tape when applied over a large area, and when applied to an adherend having a complex shape such as a curved portion, the corrosion prevention tape can be attached to the adherend while sufficiently conforming to the adherend. Each step of the corrosion prevention method of the present invention will be described below.
[0061] (First step) In the first step, the anticorrosive tape of the present invention is prepared. Since the anticorrosive tape of the present invention has been explained in the section on anticorrosive tape, the explanation of the anticorrosive tape will be omitted.
[0062] (Second step) In the second step, the surface protective film is peeled off from the anticorrosion tape and then the anticorrosion tape is attached to the adherend, or the anticorrosion tape is attached to the adherend and then the surface protective film is peeled off from the anticorrosion tape.
[0063] When the adherend has a complex shape, such as a curved shape, it is preferable to peel off the surface protective film from the anticorrosion tape before attaching the anticorrosion tape to the adherend, which allows the anticorrosion tape to be attached to the adherend while sufficiently conforming to the complex shape of the adherend.
[0064] Examples of adherends having a curved shape include weld lines on cylindrical pipes, flange connections at pipe joints, and 45° or 90° bent pipes, and the corrosion protection tape should be applied to areas that include these curved portions. Furthermore, examples of complex shapes other than curved shapes include parts having uneven shapes caused by fasteners such as bolts and nuts. Although such uneven shapes become complicated due to nuts and bolts, by peeling off the surface protective film and then attaching the anticorrosion tape, the anticorrosion tape can easily conform to the adherend even on an adherend having such uneven shapes. The complex shape may be a shape including a corner formed by connecting three faces, or may be a shape including a corner formed by simply connecting two faces.
[0065] When peeling off the surface protective film from the anticorrosion tape and then attaching the anticorrosion tape to the adherend, if the area to which the anticorrosion tape is attached is large, wrinkles may occur when the anticorrosion tape is attached to the adherend. For this reason, in this case, the area of application of the anticorrosion tape is set to 0.5 m 2 Preferably less than 0.1m 2 More preferably, 0.05 m or less. 2 The lower limit of the application area is, but is not particularly limited to, 0.0001 m 2 In this case, when the adherend has a curved shape, it is more preferable that the radius of curvature of the curved shape is equal to or less than a certain value as described above.
[0066] In the case of large-area construction, it is preferable to peel off the surface protection film from the anticorrosion tape after the anticorrosion tape has been attached to the adherend. This makes it possible to prevent wrinkles from forming when the anticorrosion tape is attached to the adherend. In particular, when the anticorrosion tape is attached to an area of 0.5 m or more, 2 More than 0.8m, preferably 0.8m 2 More than 1m, preferably 1m 2 When the thickness is more than 100 mm, the anti-corrosion tape of the present invention exhibits a more pronounced wrinkle-suppressing effect. 2 It is.
[0067] In the case of the above-mentioned large-area application, the shape of the adherend is not particularly limited, but may be flat or may have a corner such as an H-shaped steel beam. The adherend may also be attached to a part having a curved surface.
[0068] The adherends to which the corrosion prevention method of the present invention is applied are not particularly limited, and examples thereof include buildings, air conditioning equipment, building equipment, buried pipes, sanitary equipment, chemical plants, lifelines such as roads and bridges, automobiles, railway vehicles, ships, tanks, electrical equipment, electronic equipment, etc. As the material of the adherend, as described above, metal materials such as steel and concrete are preferred, and more specifically, concrete structures and steel structures are particularly preferred as the adherends. EXAMPLES
[0069] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0070] [Evaluation method]
[0071] In the examples and comparative examples, the substrate and the laminate of the substrate and the surface protective film were evaluated by the following evaluation methods. (Tensile load) The tensile load when the test piece was elongated by 0.5% and 2.5% was measured using a JIS K 7161-2:2014 1A test piece. Specifically, using a tensile tester (Tensilon Universal Material Tester manufactured by A&D Co., Ltd.), the tensile load when the test piece was elongated by 0.5% and 2.5% was read under the conditions of a chuck distance of 50 mm and a tensile speed of 300 mm / min.
[0072] (Thickness) The measurement was performed using a dial gauge.
[0073] (T-type peeling force) The surface protection film was attached to the anticorrosive tape and cut to a length of 150 mm x 30 mm to prepare a measurement sample. The attachment was performed by reciprocating twice in total at a speed of 10±0.5 mm / s, and the sample was left to cure at 23°C for 16 hours. The T-type peel strength of the surface protection film was measured by peeling the surface protection film from the anticorrosive tape at a tensile speed of 200 mm / min using a tensile tester (Tensilon Universal Material Tester, manufactured by A&D Co., Ltd.) according to the method described in JIS K 6854-3.
[0074] In the examples and comparative examples, the pressure-sensitive adhesive layer was evaluated by the following evaluation methods. (Storage modulus) The storage modulus was measured under the following conditions using a polymer dynamic viscoelasticity measuring device "DVA-200" (manufactured by IT Measurement and Control Co., Ltd.). Measurement mode: Shear Heating rate: 100℃ / min Measurement temperature: -100~200℃ Setting distortion: 0.1% Frequency: 10Hz
[0075] In the examples and comparative examples, the anticorrosive tapes were evaluated by the following evaluation methods. (Adhesive strength) The anticorrosive tape was cut to a length of 100 mm x 25 mm, and then attached to a SUS plate via an adhesive layer to prepare a measurement sample. The bonding to the SUS plate was performed by moving a 2 kg roller back and forth twice in total at a speed of 10 ± 0.5 mm / s. The test sample was fixed to the chuck of a tensile testing machine (Tensilon universal material testing machine manufactured by A&D Co., Ltd.). The anticorrosion sheet was then pulled 60 mm or more at a peel angle of 90° and a speed of 300 mm / min in an environment of 23°C and 50% RH, and the average value of the load (N) detected by the load cell was recorded and used as the adhesive strength (N / 25 mm). The adhesive strength of the anticorrosion tape was also measured on samples that had had the surface protective film peeled off and then had been subjected to an accelerated weather resistance test for 500 hours in accordance with cycle A of JIS K5600-7-7, for the purpose of evaluating weather resistance.
[0076] (Practical evaluation of convexity tracking ability) The convex portion followability was evaluated according to the following procedures 1. to 4. 2, an anticorrosive tape 10 (30 mm square) was attached to an adhesion surface 20A of an L-shaped SUS plate 20 so that the height h from the corner and the width t were 2 mm. Note that, for the anticorrosive tape 10 of the example, the surface protective film was peeled off before the anticorrosive tape 10 was attached to the SUS plate 20. 2. A squeegee was pressed against the portion of the anticorrosive tape 10 that was not attached to the L-shaped SUS plate 20 . 3. After the pressing in step 2 above, the height h was measured and visual inspection was performed to check for the occurrence of tears in the anticorrosive tape 10. If tears occurred in the anticorrosive tape 10 during the pressing, the height h was recorded as 2 mm. 4. Based on the measured value of the height h obtained in 3 above, the convex portion-following ability of the anticorrosive tape 10 was evaluated according to the following criteria. ◯: No lifting occurred (height h was 0 mm) and no tearing occurred in the anticorrosive tape 10. △·· Lifting occurred (height h is greater than 0 mm) or the anticorrosive tape 10 was torn × Lifting occurred (height h was greater than 0 mm) and the anticorrosive tape 10 was torn.
[0077] (Practical evaluation of large-area workability) As shown in Fig. 3, the anticorrosive tape 10 (width 100 mm, length 520 mm) of each of the examples and comparative examples was applied to the H-beam 30 in the following order: upper surface 31 of the upper flange, edge surface 32, lower surface 33 of the upper flange, and web 34 of the H-beam 30. Five evaluators performed the above application work within 30 seconds, and the large-area applicability of the anticorrosive tape was evaluated according to the following evaluation criteria. Note that, for the anticorrosive tape of the examples, the anticorrosive tape was applied to the H-beam 30 without peeling off the surface protective film, and after the anticorrosive tape was applied to the H-beam 30, the surface protective film was peeled off from the anticorrosive tape. <Wrinkles> ○: Four or more out of five evaluators found no wrinkles in the anticorrosive tape applied to the H-shaped steel beam. △: No wrinkles were found on the anticorrosive tape applied to the H-beam by 1 to 3 out of 5 evaluators. × Wrinkles were found in all of the anticorrosive tapes applied to the H-shaped steel beams by the five evaluators. <Floating and cracking> ○ No peeling or cracks were found in the anticorrosive tape applied to the H-beam steel by the five evaluators. × At least one of the five evaluators found defects, such as lifting or cracking, in the anti-corrosion tape applied to the H-beam steel by one or more evaluators.
[0078] (Practical evaluation of the peelability of surface protection films (1)) The anticorrosive tape was attached to a plate-shaped adherend. A masking tape (product name "#736", manufactured by Sekisui Chemical Co., Ltd.) was attached to the surface protection film of the anticorrosive tape attached to the adherend. Five seconds after application, the masking tape was pulled in a direction of 90° to the surface of the anticorrosive tape. This task was carried out by five evaluators, and the peelability of the surface protection film was evaluated according to the following criteria. ◎ Four or more of the five evaluators peeled the surface protection film off the substrate. ○: One to three of the five evaluators peeled the surface protection film off the substrate. △: None of the five evaluators were able to peel the surface protection film from the base material, and the masking tape peeled off from the surface protection film.
[0079] (Practical evaluation of peelability of surface protection film (2)) In the practical evaluation (1) of the releasability of the surface protection film described above, when the surface protection film could not be peeled off and was rated as ○ or △, a trigger was made at the edge of the surface protection film with the hand, the edge was held with the hand, and pulled in a direction of 90° to the surface of the anticorrosion tape. This task was carried out by five evaluators, and the releasability of the surface protection film was evaluated according to the following evaluation criteria. Good: Four or more of the five evaluators were able to peel the surface protection film from the substrate by hand. △: Two or more of the five evaluators were unable to peel the surface protection film from the substrate by hand.
[0080] (Total light transmittance) After peeling off the surface protective film, the anticorrosive tape was subjected to an accelerated weather resistance test for 500 hours in accordance with cycle A of JIS K5600-7-7. The anticorrosive tape after the test was attached to a glass plate with a thickness of 1 mm to prepare a measurement sample. The total light transmittance of the measurement sample was measured in accordance with JIS K 7361 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "Haze Meter NDH4000") under an atmosphere of 23°C and humidity of 50%.
[0081] (exterior) After peeling off the surface protective film, the anticorrosion tape was subjected to an accelerated weather resistance test for 500 hours in accordance with cycle A of JIS K5600-7-7. After the test, the anticorrosion tape was visually observed to examine the appearance of the substrate, and the appearance of the anticorrosion tape was evaluated according to the following evaluation criteria. ○: No yellowing or breakage of the substrate. △: The substrate was not broken, but yellowing was observed. ×: There is cracking or other damage to the base material.
[0082] [Examples 1 to 13, Comparative Examples 1 to 2] A pressure-sensitive adhesive composition was prepared according to the formulation shown in Tables 1 and 2. Nitrogen was purged into the pressure-sensitive adhesive composition to remove dissolved oxygen. The pressure-sensitive adhesive composition was then applied onto each substrate. A release sheet (PET film, manufactured by Nakamoto Packs Co., Ltd., product name: "NS-50-TA", thickness 50 μm) was then placed on the pressure-sensitive adhesive composition applied onto the substrate. In this state, the UV irradiation intensity is 5mW / cm 2 The intensity of the chemical lamp was adjusted so that the release sheet side was irradiated with ultraviolet light for 15 minutes, and an anticorrosive tape was obtained that was composed of a substrate and an adhesive layer, and had a release sheet attached to the surface of the adhesive layer. Then, a surface protective film with an adhesive layer was attached to the substrate, and an anticorrosive tape with a surface protective film on the surface of the substrate was produced. The release sheet was peeled off from the produced anticorrosive tape, and various evaluations were performed. The results are shown in Tables 1 and 2.
[0083] [Table 1]
[0084] [Table 2]
[0085] The components in Tables 1 and 2 are as follows. (Adhesive component) Olefin polymer: Product name "L-1253", manufactured by Kuraray Co., Ltd., hydrogenated polybutadiene having a (meth)acryloyl group at one end Tackifying resin 1: Product name "Alcon P140", manufactured by Arakawa Chemical Industries, Ltd., hydrogenated petroleum resin, softening point 140°C Tackifier resin 2: Product name "Alcon P100", manufactured by Arakawa Chemical Industries, Ltd., hydrogenated petroleum resin, softening point 100°C Fine particles: Product name: "Cellstar Z-27", manufactured by Tokai Kogyo Co., Ltd., glass balloon, average particle size 63 μm Zinc particles: Sakai Chemical Industry Co., Ltd., product name "Zinc powder #40", average particle size 50 μm Conductive material: Carbon nanotubes (CNT), manufactured by JEIO, product name "JENOTUBE8A", average diameter 6-9 nm, average length 100-200 μm Conductive material: Carbon black, manufactured by Oriental Sangyo Co., Ltd., product name "AT-NO.15S" Dispersant: Sekisui Chemical Co., Ltd., product name "S-LEC BX-L", polyvinyl butyral resin Crosslinking agent: Product name "TEAI-1000", manufactured by Nippon Soda Co., Ltd. Polymerization initiator: 2,2-dimethoxy-2-phenylacetophenone (base material) Soft acrylic sheet: Manufactured by Tatsuta Chemical Co., Ltd., product name "Soft acrylic sheet", 50NS: Fluorine resin, manufactured by AGC Inc., product name "50NS" LLDPE: Linear low-density polyethylene, manufactured by Sakai Chemical Industry Co., Ltd. 00C040M: Polyvinyl chloride resin, manufactured by Nippon Carbide Industries Co., Ltd., product name "00C040M" MF50T-MX: Urethane resin, manufactured by Nisshinbo Inc., product name "MF50T-MX" Lumirror S10: Polyethylene terephthalate, manufactured by Mitsubishi Chemical Corporation, product name "Lumirror Mirror S10" (Surface protection film) SRC-0503C: Polyethylene terephthalate, manufactured by Lintec Corporation, product name "SRC-0503C", PET75-H120(10) Blue: Polyethylene terephthalate colored blue, manufactured by Nichiei Shinka Co., Ltd., product name "PET75-H120(10) Blue" PET38-H120(10) Blue: Polyethylene terephthalate colored blue, manufactured by Nichiei Shinka Co., Ltd., product name "PET38-H120(10) Blue" PET100-H120(10) Blue: Polyethylene terephthalate colored blue, manufactured by Nichiei Shinka Co., Ltd., product name "PET100-H120(10) Blue" 115-60: Biaxially oriented polypropylene, manufactured by Kyodo Giken Chemical Co., Ltd., product name "115-60" 50BA: Polyethylene terephthalate, manufactured by Okamoto Corporation, product name "50BA", #672NZ-40: Polyethylene and polypropylene laminated film, manufactured by Sekisui Chemical Co., Ltd., product name "#672NZ-40" #6748C-40: Polyethylene and polypropylene laminated film, manufactured by Sekisui Chemical Co., Ltd., product name "#6748C-40" Fit Light Tape No. 738: A masking tape made of PET fiber, manufactured by Sekisui Chemical Co., Ltd., product name "Fit Light Tape No. 738"
[0086] The anticorrosion tapes of Examples 1 to 13 were provided with a substrate, a pressure-sensitive adhesive layer on one side of the substrate, and a surface protection film on the other side of the substrate for protecting the other side of the substrate, and therefore were evaluated as good in both convex conformability and large-area applicability. On the other hand, the anticorrosion tapes of Comparative Examples 1 and 2 were not provided with a surface protection film, and therefore were not evaluated as good in both convex conformability and large-area applicability. [Explanation of symbols]
[0087] 10 Anti-corrosion tape 11 Adhesive layer 12 Surface protection film 13 Base material 20 L-shaped SUS plate 20A Adhering surface 30H steel h Height t width
Claims
1. A first step of preparing an anticorrosive tape including a substrate, a pressure-sensitive adhesive layer provided on one surface of the substrate, and a surface protective film provided on the other surface of the substrate for protecting the other surface of the substrate; and a second step of peeling the surface protective film from the corrosion-preventive tape and then attaching the corrosion-preventive tape to an adherend, or attaching the corrosion-preventive tape to an adherend and then peeling the surface protective film from the corrosion-preventive tape.
2. the second step is a step of peeling off the surface protective film from the anticorrosive tape and then attaching the anticorrosive tape to the adherend, The corrosion prevention method according to claim 1 , wherein the adherend has a curved surface.
3. The area of the anticorrosive tape applied to the adherend is 0.5 m 2 The corrosion prevention method according to claim 2, wherein the corrosion prevention method is less than 100%.
4. the second step is a step of attaching the anticorrosion tape to the adherend and then peeling off the surface protective film from the anticorrosion tape; The area of the anticorrosive tape applied to the adherend is 0.5 m 2 The corrosion prevention method according to claim 1,
5. The corrosion prevention method according to claim 1, wherein the adherend is a concrete structure or a steel structure.
6. An anticorrosion tape comprising a substrate, an adhesive layer provided on one side of the substrate, and a surface protective film provided on the other side of the substrate for protecting the other side of the substrate.
7. a difference between a tensile load at 2.5% elongation and a tensile load at 0.5% elongation in a laminate including the substrate and the surface protective film is 2.5 N / mm or more and 6.0 N / mm or less; 7. The corrosion-preventive tape according to claim 6, wherein the difference between the tensile load at 2.5% elongation and the tensile load at 0.5% elongation in the substrate is 1.3 N / mm or less.
8. The anticorrosion tape according to claim 6, wherein a T-type peel force when peeling off the surface protective film is 0.1 N / 30 mm or more and 2.6 N / 30 mm or less.
9. 7. The anticorrosion tape according to claim 6, wherein the surface protective film is made of at least one resin selected from the group consisting of polyester-based resin films, polypropylene-based resin films, and polyamide-based resin films.
10. The corrosion-preventive tape according to claim 6, wherein the surface protective film has a thickness of 25 μm or more and 200 μm or less.
11. 7. The corrosion-protective tape according to claim 6, wherein the substrate is at least one resin selected from the group consisting of a polyethylene-based resin film, a polypropylene-based resin film, an acrylic-based resin film, a fluorine-based resin film, and a polyvinyl chloride-based resin film.
12. The corrosion-preventive tape according to claim 6, wherein the thickness of the substrate is from 20 μm to 400 μm.
13. After the surface protective film is peeled off, an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 is carried out for 500 hours, after which the total light transmittance of the anticorrosive tape is 50% or more; After the surface protective film is peeled off, an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 is carried out for 500 hours, after which the substrate is not broken, 7. The anticorrosion tape according to claim 6, wherein the adhesive strength of the anticorrosion tape after carrying out an accelerated weather resistance test in accordance with cycle A of JIS K5600-7-7 for 500 hours after peeling off the surface protective film is 20 N / 25 mm or more.
14. The anticorrosion tape according to claim 6, wherein the pressure-sensitive adhesive layer has a thickness of 50 to 2500 μm.
15. The corrosion protection tape according to claim 6 , wherein the pressure-sensitive adhesive layer contains a photocurable resin.
16. The anticorrosion tape according to claim 6, wherein the pressure-sensitive adhesive layer has a storage modulus of 50,000 to 1,000,000 Pa at a temperature of 23°C.
17. The corrosion-preventive tape according to claim 6, wherein the pressure-sensitive adhesive layer is formed from an acrylic pressure-sensitive adhesive.