Method for producing painted CFRP article
The vacuum degassing and thermal curing method addresses gas removal issues in CFRP manufacturing, ensuring high-quality painted CFRP articles by preventing defects like blisters and bulges.
Patent Information
- Application Number
- JP2024049158
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for manufacturing CFRP articles with powder in-mold coating face challenges in effectively removing gases trapped between the carbon fiber prepreg and the thermosetting powder coating layer, leading to defects such as blisters and bulges in the finished product.
A method involving vacuum degassing to remove gases between the carbon fiber prepreg and the thermosetting powder coating layer, followed by thermal curing while pressing the prepreg through the powder coating layer within a controlled mold environment.
This approach effectively prevents defects in the CFRP articles by ensuring complete removal of gases, resulting in high-quality, defect-free painted CFRP articles suitable for further processing.
Smart Images

Figure 2024144306000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates primarily to a method for producing painted CFRP (carbon fiber reinforced plastic) articles. [Background technology]
[0002] In one example, when a resin article is press-molded from a glass fiber-reinforced unsaturated polyester resin sheet, a primer coating is applied simultaneously with molding by in-mold coating using a powder paint, and then a finish coating is applied to the primer-coated resin article (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 58-110213 Summary of the Invention [Problem to be solved by the invention]
[0004] The main object of the present invention is to provide a powder in-mold coating technique for CFRP articles, which can be suitably used for the production of primer-coated CFRP articles. [Means for solving the problem]
[0005] According to one aspect of the present invention, there is provided a method for producing a CFRP article in which a layer of powder paint is applied to a surface of a carbon fiber prepreg, the method including degassing gas between the carbon fiber prepreg and the layer of powder paint by vacuum degassing, and thermally curing a thermosetting carbon fiber prepreg while pressing it against the layer of powder paint.
[0006] According to another aspect of the present invention, there is provided a method for producing a painted CFRP article, comprising: preparing a molding die consisting of an upper die and a lower die and having a mirror surface on its molding surface; maintaining the molding die at a molding temperature; forming a layer of thermosetting powder paint on at least a portion of the mirror surface; placing a thermosetting carbon fiber prepreg in a closed space formed by closing the molding die; degassing air between the layer of thermosetting powder paint and the thermosetting carbon fiber prepreg; and bringing the upper die and the lower die close to each other while degassing the closed space by vacuum, and pressing the carbon fiber prepreg placed therein together with the layer of powder paint. Effect of the Invention
[0007] A powder in-mold coating technique for CFRP articles is provided that may be suitably used for the production of primer-coated CFRP articles. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing a pressing device. [Diagram 2] FIG. 2 is a cross-sectional view of the mold. [Diagram 3] FIG. 3 is a cross-sectional view of the mold. [Figure 4] FIG. 4 is a cross-sectional view of the mold. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a manufacturing process of a painted CFRP article. [Figure 6] FIG. 6 is a cross-sectional view illustrating a manufacturing process of a painted CFRP article. [Figure 7] FIG. 7 is a cross-sectional view illustrating a manufacturing process of a painted CFRP article. [Figure 8] FIG. 8 is a cross-sectional view illustrating a manufacturing process of a painted CFRP article. [Figure 9] FIG. 9 is a cross-sectional view illustrating the manufacturing process of a painted CFRP article. [Figure 10]FIG. 10 is a cross-sectional view of the mold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, some embodiments of the present invention will be described with reference to the drawings. The dimensional ratios in the drawings are for the convenience of explanation and may differ from the actual ones. In addition, the same components in the drawings are indicated by the same reference numerals, and the description of overlapping components may be omitted.
[0010] 1. Press molding equipment The production of a painted CFRP article by the production method according to the embodiment can be preferably carried out using a press molding apparatus. 1 is a schematic diagram showing the configuration of a typical press molding apparatus. Referring to FIG 1, the press molding apparatus 1 has a press 10, a molding die 20, and a vacuum pump 30. The press 10 comprises a main frame 11, a bolster 12 fixed to the lower part of the main frame 11, a slide 13 that can be raised and lowered vertically, and a lifting mechanism 14 that raises and lowers the slide 13. The forming die 20 is composed of a lower die 20L fixed to the upper surface of the bolster 12 and an upper die 20U fixed to the lower surface of the slide 13.
[0011] As shown in Fig. 2, the lower mold 20L has a convex portion 21 having a vertical outer peripheral surface, and further has an annular convex portion 22 arranged along the outer periphery of the convex portion 21 and sharing the outer peripheral surface with the convex portion 21. The convex portion 21 is provided with a seal ring 23 that goes around its outer peripheral surface. The upper mold 20U has a recess 24 that can be fitted with the convex portion 21 of the lower mold 20L via the seal ring 23, and further has an annular recess 25 that is arranged along the outer periphery of the recess 24 and sharing the outer peripheral surface with the recess 24. The annular convex portion 22 of the lower mold 20L and the annular recess 25 of the upper mold 20U can be fitted with each other.
[0012] When the slide 13 is lowered to engage the convex portion 21 of the lower die 20L with the concave portion 24 of the upper die 20U, a closed space 26 is formed between the upper die 20U and the lower die 20L, as shown in FIG. Since the closed space 26 is made airtight by the action of the seal ring 23, it can be evacuated by operating a vacuum pump 30 connected to the closed space 26 through a hole provided in the upper mold 20U.
[0013] When the slide 13 is further lowered and the annular protrusion 22 and the annular recess 25 are mated, a molding cavity 27 is formed having a shear edge 31 formed between the inner wall surface of the annular protrusion 22 and the inner wall surface of the annular recess 25, as shown in Figure 4. Surfaces 28L, 28U of lower die 20L and upper die 20U exposed inside molding cavity 27 are molding surfaces.
[0014] Each of the upper mold 20U and the lower mold 20L has a built-in heater (not shown), which may be, for example, a steam heater, an oil heater, or an electric heater, making it possible to maintain the temperature of the molding mold 20 at any temperature within a temperature range suitable for curing the thermosetting carbon fiber prepreg (for example, 120 to 180°C).
[0015] 2. Manufacturing method of painted CFRP articles A method for producing a painted CFRP article according to a preferred embodiment comprises the following steps: The first step is to prepare a mold having an upper and lower part and a molding surface. A second step of holding the mold at a molding temperature. A third step of applying a layer of a thermosetting powder coating onto at least a portion of said molding surface. A fourth step of placing a thermosetting carbon fiber prepreg in the closed space formed by closing the mold. A fifth step of degassing the closed space by vacuum degassing the gas between the carbon fiber prepreg and the layer of thermosetting powder paint. A sixth step is to bring the upper and lower molds close to each other and press the carbon fiber prepreg placed therein together with the layer of powder paint.
[0016] The method according to the above-mentioned preferred embodiment will be described below by taking as an example a case in which the press molding apparatus shown in Figs. 1 to 4 is used. (1) First Step An example of the mold prepared in the first step is shown in Figure 4. The mold 20 is made up of an upper mold 20U and a lower mold 20L. The molding surfaces are 28U and 28L. The molding surface 28 may be specular or non-specular.
[0017] When the molding surface 28 has a non-mirror portion, the arithmetic mean roughness Ra of the non-mirror surface is preferably 2.5 μm or more, and more preferably 2.8 μm or more.
[0018] The arithmetic mean roughness Ra of the molding surface is a value measured using a contact type roughness measuring device under the following conditions. Calculation standard: ISO-97 standard, measurement type: roughness measurement, measurement length: 8.0 mm, cutoff wavelength: 0.8 mm, measurement range: ±64.0 μm, measurement speed: 0.6 mm / s, cutoff type: Gaussian, tilt correction: least squares linear correction, moving speed and return speed: 3.0 mm / s.
[0019] There is no limitation on the method for providing a non-mirror surface on the molding surface, and any of the techniques for matte finishing or embossing conventionally used in mold manufacturing can be used as appropriate. Specific examples of the method include, but are not limited to, etching, blasting, rough polishing, and hairline processing.
[0020] (2) Second step In a second step, the mold 20 is held at the molding temperature. The second step is usually started before the third step and subsequent steps, and is continued until the curing of the thermosetting carbon fiber prepreg is completed at least in the sixth step. In other words, before the third step and subsequent steps are performed, the mold 20 is heated to the molding temperature, and the mold 20 is maintained at the molding temperature at least until the sixth step is completed.
[0021] The molding temperature is set to a temperature at which the thermosetting prepreg can be cured within a desired time. The higher the molding temperature, the shorter the time required to sufficiently cure the thermosetting prepreg, and therefore the molding cycle in the case of continuous molding is shortened. However, in order to prevent the cured product (CFRP article) from deforming when demolded, it is preferable that the molding temperature is lower than the glass transition point of the matrix resin after the prepreg has cured. The molding temperature is usually set within the range of 120 to 180° C., taking the above-mentioned points into consideration.
[0022] (3) Third step In the third step, a layer 2 of thermosetting powder paint is formed on the molding surface 28U of the mold 20, as shown in FIG. The layer 2 of thermosetting powder paint may be formed on one or both sides of the molding surface 28. A preferred thermosetting powder coating is a powder coating for PIMC (powder in-mold coating). For powder coating for PIMC, for example, JP-A-59-91157 and JP-A-1-158080 can be referred to, and generally, epoxy resin, epoxy polyester resin, polyester resin, acrylic resin, polyurethane resin, etc. contain thickener, reactive diluent, shrinkage reducing agent, defoamer, particulate filler, colorant, pigment, etc. Density: 1.3 to 2.0 g / cm 3 The particle size is often in the range of 20 to 150 μm in the longitudinal direction. Commercially available powder coatings for PIMC are available, for example, from Tiger Coatings GmbH & Co. KG.
[0023] As shown in the example of Fig. 5, when forming a layer 2 of powder paint on the molding surface 28U of the upper mold, electrostatic powder coating is preferably used. This method is also preferable from the viewpoint of uniform coating, and therefore may also be preferably used when forming a layer of thermosetting powder paint on the molding surface of the lower mold in other examples. There are also cases where layers of powder paint are formed on both the molding surfaces of the upper and lower molds. The method of forming a layer of thermosetting powder paint on a molding surface is not limited to electrostatic powder coating. In another example, when forming this layer on the molding surface of the lower mold, a method of manually sprinkling the powder paint on the molding surface using a sieve may also be used. The thickness of the powder coating layer is made thicker towards the center, making it easier for gas to be pushed outwards when pressure is applied. After the powder coating is applied to the molding surface, it may be thickened by adding heat history for a certain period of time. Excessive flow can be suppressed by thickening. The time is preferably 30 to 600 seconds, more preferably 120 to 180 seconds. If the time is too short, the coating will not thicken, and if it is too long, the powder coating layer will crack due to thermal degradation, impairing the appearance.
[0024] (4) Fourth step In the fourth step, as shown in Figs. 6 and 7, the molding die 20 is closed to form a closed space 26, in which a thermosetting carbon fiber prepreg 3 is placed. As shown in FIG. 6, a layer 2 of thermosetting powder coating can be placed on the opposite mold surface. More specifically, with the molding die 20 open, the thermosetting carbon fiber prepreg 3 is placed on the molding surface 28L of the lower die 20L, and then the molding die 20 is closed to form a closed space 26. Alternatively, as shown in FIG. 7, a carbon fiber prepreg 3 may be laminated onto a layer 2 of thermosetting powder paint. The thermosetting carbon fiber prepreg 3 may be preformed in a net shape or a near net shape.
[0025] It is preferable that the charge rate of the carbon fiber prepreg 3 with respect to the molding surface is 80 to 90%. The charge rate is the ratio of the area of the carbon fiber prepreg 3 to the area of the molding surface. If the charge rate is 80% or more, the flow of the material is reduced, and defects such as cracking of the powder coating layer caused by the flow of the material can be suppressed. Generally, the charge rate in press molding is 30 to 50%. This is because it is easy to remove gas from the carbon fiber prepreg. If the charge rate is high, the gas tends to remain as voids in the CFRP article, which may deteriorate the appearance. In the present invention, the gas in the carbon fiber prepreg is removed by vacuum degassing and in-mold coating is performed, so that the deterioration of the appearance due to the voids can be eliminated.
[0026] The thermosetting carbon fiber prepreg 3 is an intermediate material used in the manufacture of CFRP (carbon fiber reinforced plastic) articles, and is made by impregnating a fiber reinforcement material made of carbon fiber with a thermosetting resin matrix.
[0027] Examples of thermosetting carbon fiber prepregs 3 include UD prepregs, woven prepregs, tow prepregs and sheet molding compounds (SMC). The fiber reinforcement of the UD prepreg is a UD sheet. Examples of the weave of the fiber reinforcement of the woven prepreg include plain weave, twill weave, and satin weave. The fiber reinforcement of the woven prepreg may be a non-crimp fabric. The fiber reinforcement of the SMC is a random mat formed by scattering chopped fiber bundles.
[0028] The thermosetting resin matrix contained in the thermosetting carbon fiber prepreg 3 is a composition containing a thermosetting resin and a curing agent, and various additives may be added in addition to the curing agent as necessary. Examples of such additives include, but are not limited to, thickeners, reactive diluents, low shrinkage agents, flame retardants, antifoaming agents, defoaming agents, mold release agents, particulate fillers, colorants, and silane coupling agents. Examples of thermosetting resins include, but are not limited to, epoxy resins, vinyl ester resins (also called epoxy (meth)acrylate resins), (meth)acrylate resins, unsaturated polyester resins, urea resins, polyurethane resins, and phenolic resins. Two or more types of thermosetting resins may be mixed together.
[0029] The thermosetting carbon fiber prepreg 3 may be a prepreg assembly including a plurality of carbon fiber prepregs. In this case, the prepreg assembly may include only the same type of carbon fiber prepreg, or may include two or more types of carbon prepregs. The thermosetting carbon fiber prepreg 3 may comprise a laminate of homogeneous or heterogeneous prepregs. When multiple UD prepregs are laminated, cross plies or angle plies may be employed as required. When the thermosetting carbon fibre prepreg 3 comprises a laminate of prepregs, it is preferred to degas it by vacuum bagging before placing it within the enclosed space 26 . The carbon fiber prepreg 3 or the prepreg laminate may be kept warm for a certain period of time in a temperature-controllable space such as an oven. In particular, if the carbon fiber prepreg 3 or the prepreg laminate is low in temperature before being placed in a mold, the behavior during molding becomes unstable, such as the resin flow becoming less, so the temperature can be adjusted to 20 to 60°C. In addition, if the carbon fiber prepreg 3 or the prepreg laminate contains a volatile component, it is also possible to remove the volatile component in advance by applying a heat history.
[0030] (5) Fifth step In a fifth step, the closed space is evacuated to remove any gas present between the carbon fiber prepreg and the layer of thermosetting powder paint. When the carbon fiber prepreg overlaps with the layer of thermosetting powder paint, gas may get between the carbon fiber prepreg and the layer of thermosetting powder paint. Also, gas may get into the layer of thermosetting powder paint. When the carbon fiber prepreg and the thermosetting powder paint are pressurized and cured in such a gas-containing state, the gas remains in the coated CFRP article in a compressed state. When the mold is subsequently opened and the pressure is removed, the compressed gas remaining in the coated CFRP article expands, causing holes or bulges in the coated CFRP article, deteriorating the appearance of the coated CFRP article. As the area of the carbon fiber prepreg increases, it becomes easier for gas to enter between the carbon fiber prepreg and the layer of thermosetting powder paint. Therefore, in the method for producing a coated CFRP article of the present invention, when the area of the carbon fiber prepreg is 1500 cm 2 The area of the carbon fiber prepreg is preferably 1600 cm 2 More preferably, 1800 cm 2 That's all.
[0031] The vacuum degassing method is as shown in FIG. When the volume reaches 0 L and the space becomes closed, vacuum degassing begins. To prevent the powder coating from entering the vacuum pump, a filter or the like may be installed between the mold and the vacuum pump.
[0032] 4, when the upper mold 20U and the lower mold 20L approach each other and the annular convex portion 22 of the lower mold 20L and the annular concave portion 25 of the upper mold 20U mate with each other, a molding cavity 27 having a shear edge is formed. Since a large pressure loss occurs at the shear edge, the degassing efficiency of the molding cavity 27 becomes low. However, while the degassing efficiency is reduced, the shear edge can suppress excessive outflow of the resin of the carbon fiber prepreg 3 or the prepreg laminate, which has a low viscosity during molding, and the molten powder paint, outside the molding surface, and is effective in stabilizing the thickness of the molded product and improving the surface quality.
[0033] Therefore, preferably, the descent speed of the upper mold 20U may be reduced so that the closed space 26 is sufficiently vacuum degassed before the shear edge is formed, or alternatively, or in addition, the descent of the upper mold 20U may be temporarily stopped before the shear edge is formed to vacuum degas the closed space 26. When using a mold in which no shear edge is formed, these considerations are not necessary. The vacuum pressure in the closed space 26 after vacuum degassing is preferably −0.1 MPa or less. The clamping speed of the upper mold 20U is preferably 2 mm / sec or less, more preferably 1 mm / sec or less, and even more preferably 0.7 mm / sec, because this allows a long vacuum degassing time.
[0034] The degree of vacuum achieved varies depending on the vacuum degassing device, but the vacuum time from when a closed space is created until pressure is started to be applied to the carbon fiber prepreg and the thermosetting powder paint is preferably 7 seconds or more, more preferably 15 seconds or more, and even more preferably 20 seconds or more. The time for vacuum degassing is preferably the time from when the specified vacuum level of the apparatus is reached until the shear edge state is reached.
[0035] (5) Sixth step In the sixth step, as shown in FIG. 8, the closed space containing the thermosetting carbon fiber prepreg is evacuated while the upper and lower dies are brought close to each other, and the carbon fiber prepreg is pressed together with the layer of powder paint. As shown in Figure 6, when the upper mold 20U and the lower mold 20L are separated, the pressure is 0 MPa. When the upper mold 20U starts to press the carbon fiber prepreg 3 through the powder paint layer 2 as shown in Figure 8, the pressure suddenly rises and reaches the molding pressure in an instant. It is preferable to perform vacuum degassing while applying pressure, since this makes it possible to remove gas generated by heating and compression, and gas pushed out from the carbon fiber prepreg and powder coating layers. The thermosetting carbon fiber prepreg is cured by applying pressure in a mold held at the mold temperature. The pressure time is set to be long enough to complete the cure. The temperature of the mold is maintained at the mold temperature while pressure is continued.
[0036] The molding pressure in the sixth step is preferably within the range of 3 to 10 MPa. The molding pressure is defined as a value obtained by dividing the pressing force of the press by the vertical projected area of the molding cavity.
[0037] After the sixth step is completed, the mold 20 is opened as shown in FIG. 9, and the in-mold coated CFRP article 4 is removed. The in-mold coated CFRP article 4 is composed of a CFRP part 3C formed by curing a thermosetting carbon fiber prepreg 3 and a coating film 2C adhered to its surface. The coating film 2C is formed by gelling and then curing a layer 2 of a thermosetting powder paint. There is no need to change the temperature of the mould 20 when removing the CFRP article 4. Typically, the temperature of the mould 20 is held at the moulding temperature until the next moulding cycle begins. Surface cracks can also be suppressed by gradually returning the removed CFRP article 4 to room temperature. For example, one possible step is to quickly place the removed CFRP article 4 in an oven whose temperature has been adjusted to 40 to 70°C, so that the temperature can be returned from the molding temperature to room temperature.
[0038] 3. Topcoat painting The thermosetting powder paint used in the manufacturing method according to the embodiment is preferably a primer paint, i.e., the painted CFRP article manufactured by the method according to the embodiment is preferably a primer-painted CFRP article. A primer-coated CFRP article is an intermediate product in the manufacture of a multi-coated CFRP article, which will be finished by applying a topcoat. When a primer-coated CFRP article is manufactured by the manufacturing method according to the embodiment, the primer coating is usually polished to flatten the surface before proceeding to the topcoat coating step, in which at least one coating film including a colored coating film is formed on the primer coating film.
[0039] The coating film formed in the topcoating step is preferably a baked coating film, and is formed by drying the applied paint at a temperature of 80°C or higher, typically 100°C or higher. The coating film formed in the overcoating step may include a colored coating film and a clear coating film formed thereon. The clear coating film may be formed as a top coat. The coating film formed in the overcoating step may include a colored coating film and an undercoat coating film formed thereunder. When a plurality of coating films are formed by overlaying in the overcoating step, the plurality of coating materials are preferably overlaid wet-on-wet and then baked simultaneously in one step.
[0040] 4. Experimental Results The results of the experiments carried out by the present inventors are given below.
[0041] (1) The materials used in Experiment 1-1 are as follows. Release agent: A water-based external release agent containing fluorine compounds and wax, commercially available for CFRP molding (Frelease 65, manufactured by NEOS Corporation). Powder primer: Tiger Drylac 261 / 10013 PIMC Epoxy Primer from Tiger Coatings GmbH & Co. KG. Sheet molding compound: Thermosetting 2.0 mm thick sheet molding compound (STR120 manufactured by Mitsubishi Chemical Corporation)
[0042] The following procedure will create a wall thickness of 0.84 to 6.00 mm with a projected area of 1810 mm. 2 A CFRP plate having a curved surface, one of which was painted with a primer, was molded. A press molding apparatus was prepared by mounting a molding die 40 having the structure shown in FIG. 10 on a hydraulic press. The molding die 40 has a lower die 40L and an upper die 40U which can be fitted together via a seal ring 43, and the lower die 40L is provided with a seal ring 43 which goes around its outer periphery. The lower die 40L is provided with an annular protrusion 42 along its outer periphery, and the upper die 40U is provided with an annular recess 45 which can be fitted together with the annular protrusion 42.
[0043] When the lower mold 40L and the upper mold 40U are mated, a closed space is formed, and a hole is provided in the annular recess 45 so that the inside can be evacuated and the hole is connected to a vacuum pump 50. When the annular protrusion 42 of the lower die 40L and the annular recess 45 of the upper die 40U were mated, a plate-shaped molding cavity having a shear edge was formed. The shear edge was formed between the inner wall surface of the annular protrusion 42 and the inner wall surface of the annular recess 45, with a gap of 0.05 to 0.1 mm. The molding cavity had a surface area of 1,810 mm2. 2 It had curved bottom and top surfaces, and its height was variable between 1 mm and 6 mm. The base material of the mold was carbon steel S55C, and the molding surface was a mirror finish that had been hard chrome plated.
[0044] The molding die was heated, and it was confirmed that the temperature had stabilized within the range of 140±4° C. Next, the parts of the inner wall surface of the annular convex portion 42 of the lower die 40L that contribute to the formation of the shear edge during molding were masked with heat-resistant tape, measures were taken to prevent powder from building up around the die, and a mold release agent was applied to the molding surface 48L of the lower die 40L and the molding surface 48U of the upper die 40U. Next, 258 g of the powder primer paint was quickly spread using a sieve on the mirror-finished molding surface 48L of the lower mold 40L. Immediately after the spread was completed, all the masking heat-resistant tape attached to the annular protrusion 42 of the lower mold 40L was peeled off.
[0045] The sheet molding compound laminate was placed on the molding surface 48L of the lower mold 40L on which the powder primer paint had been sprayed, and the mold 40 was closed to perform press molding. The sheet molding compound laminate was cut so as to be 20 mm away from the shear edge of the molding surface 48L all around, and three sheets were laminated together, with a thickness of 6 mm and a surface area of 1480 cm. 2 A laminate with a mass of 1540 g (charge rate of approximately 82%) was used. The press molding conditions were a predetermined molding pressure of 8 MPa and a pressing time of 600 seconds. The vacuum degassing of the closed space formed by closing the mold was started before the shear edge was formed. When the mold closing speed was set to 0.3 mm / s, the vacuum pressure in the closed space reached -0.1 MPa before the shear edge was formed. The operation of the vacuum pump was continued until the molding pressure reached 8 MPa. The evacuation time from when the closed space was formed until when evacuation was started and pressurization was started was 28.7 seconds.
[0046] A test piece measuring 150 mm x 70 mm was cut from the center of the molded CFRP plate, and a top coat was applied to the primer-coated surface using the following procedure. (i) The entire primer-coated surface of the test piece was hand-sanded with #600 sandpaper, and then the primer coating surface was rubbed with a cloth soaked in isopropyl alcohol to remove any abrasive residue. (ii) Following (i), polyurethane black paint and polyurethane clear paint were applied in that order to the primer-coated surface of the test specimen using a spray gun, and then dried in an oven at 100°C for 1 hour. As a result of observing the surface of the topcoat film formed by the above procedure, not a single blister was found that could be visually confirmed. In Table 1, samples with no visible blisters were marked with an ◯, and samples with one or more blisters were marked with an X.
[0047] (2) Experiments 1-2~8 The experiment was conducted in the same manner as in Experiment 1, except that the conditions were changed as shown in Table 1.
[0048] [Table 1]
[0049] (3) The materials used in Experiments 2-1 to 4 are as follows. Release agent: A water-based external release agent containing fluorine compounds and wax, commercially available for CFRP molding (Frelease 65, manufactured by NEOS Corporation). Powder primer: Tiger Drylac 261 / 10013 PIMC Epoxy Primer from Tiger Coatings GmbH & Co. KG. Sheet molding compound: Thermosetting 2.0 mm thick sheet molding compound (STR120 manufactured by Mitsubishi Chemical Corporation) Woven prepreg: Thermosetting twill prepreg with a thickness of 0.22 mm (Mitsubishi Chemical Corporation TR3524 362GMP), thermosetting twill prepreg with a thickness of 0.44 mm (Mitsubishi Chemical Corporation TRK501 362GMP)
[0050] (4) Experiment 2-1 The following procedure will create a wall thickness of 2.4 mm and a projected area of 900 cm 2 A CFRP plate was molded having a square surface with each side measuring 30 cm, one side of which was painted with a primer. A press molding apparatus was prepared by mounting a molding die 40 having the structure shown in FIG. 10 on a hydraulic press. The molding die 40 has a lower die 40L and an upper die 40U which can be fitted together via a seal ring 43, and the lower die 40L is provided with a seal ring 43 which goes around its outer periphery. The lower die 40L is provided with an annular protrusion 42 along its outer periphery, and the upper die 40U is provided with an annular recess 45 which can be fitted together with the annular protrusion 42.
[0051] When the lower mold 40L and the upper mold 40U are mated, a closed space is formed, and a hole is provided in the annular recess 45 so that the inside can be evacuated and the hole is connected to a vacuum pump 50. When the annular protrusion 42 of the lower die 40L and the annular recess 45 of the upper die 40U were mated, a plate-shaped molding cavity having a shear edge was formed. The shear edge was formed between the inner wall surface of the annular protrusion 42 and the inner wall surface of the annular recess 45, with a gap of 0.05 to 0.1 mm. The molding cavity had a surface area of 900 cm2. 2 It had curved bottom and top surfaces, and its height was variable between 1 mm and 3 mm. The base material of the mold was carbon steel S45C, and the molding surface was a mirror finish that had been hard chrome plated.
[0052] The molding die was heated, and it was confirmed that the temperature had stabilized within the range of 140±6° C. Next, the portions of the outer wall surface of annular convex portion 45 of upper die 40U that contribute to the formation of a shear edge during molding were masked with heat-resistant tape, measures were taken to prevent powder from building up around the die, and a mold release agent was applied to molding surface 48L of lower die 40L and molding surface 48U of upper die 40U. Next, 50 g of powder primer paint was applied to the mirror-finished molding surface 48U of the upper mold 40U using an electrostatic powder coating device so that the powder primer paint was uniformly applied to the entire molding surface. Immediately after application was completed, the powder prevention measures were removed, and all of the masking heat-resistant tape attached to the annular protrusion 45 of the upper mold 40U was peeled off. The preheat time for the applied powder coating was set to 120 seconds.
[0053] The sheet molding compound laminate was placed on the molding surface 48L of the lower die 40L, and the mold 40 was closed to perform press molding. The sheet molding compound laminate was cut so as to be 45 mm away from the shear edge of the molding surface 48L, and two sheets were laminated together. The thickness was 2 mm, the surface area was 440 cm2, and the thickness was 2 mm. 2 (Charge rate: approx. 49%) and a laminate with a mass of 270 g were used. The press molding conditions were a predetermined molding pressure of 20 MPa and a pressing time of 900 seconds. The vacuum degassing of the closed space formed by closing the mold was started before the shear edge was formed. When the mold closing speed was set to 1.0 mm / s, the vacuum pressure in the closed space reached -0.1 MPa before the shear edge was formed. The operation of the vacuum pump was continued until the molding pressure reached 20 MPa. The evacuation time from when the closed space was formed until when the evacuation was started and the pressurization was started was 25 seconds or more. As a result of observing the surface of the primer coating of the molded product using the above procedure, not a single blister was found that could be seen with the naked eye. In Table 2, samples with no visible blisters were marked with an ◯, and samples with one or more blisters were marked with an ×.
[0054] (2) Experiments 2-2 to 4 Except for changing the conditions as shown in Table 2, the experiment was conducted in the same manner as in Experiment 2-1.
[0055] [Table 2]
[0056] 5. Summary of the embodiment Preferred embodiments of the present invention include, but are not limited to, the following. (Embodiment 1) A method for manufacturing a CFRP article in which a layer of powder paint is applied to the surface of a carbon fiber prepreg, the method including degassing the gas between the carbon fiber prepreg and the layer of powder paint by vacuum degassing, and thermally curing the thermosetting carbon fiber prepreg while pressing it against a mold with the layer of powder paint between them. (Embodiment 2) The manufacturing method according to embodiment 1, wherein the vacuum degassing time is 7 seconds or longer. (Embodiment 3) The method according to embodiment 1 or 2, wherein the surface of the mold is a mirror surface. (Embodiment 4) The method according to any one of embodiments 1 to 3, wherein a thermosetting carbon fiber prepreg is thermally cured while being pressed against a layer of powder paint under vacuum degassing. (Embodiment 5) A method for manufacturing a CFRP article in which a layer of powder paint is applied to the surface of a carbon fiber prepreg, the method comprising: preparing a mold consisting of an upper mold and a lower mold and having a molding surface; maintaining the mold at a molding temperature; forming a layer of thermosetting powder paint on at least a portion of the molding surface; placing the thermosetting carbon fiber prepreg in a closed space formed by closing the mold; degassing any gas between the layer of thermosetting powder paint and the thermosetting carbon fiber prepreg; and bringing the upper mold and the lower mold close to each other while vacuum-degassing the closed space, and pressing the carbon fiber prepreg placed therein together with the layer of powder paint. (Embodiment 6) A manufacturing method according to embodiment 5, in which vacuum degassing is performed for 7 seconds or more before pressurization. (Embodiment 7) A manufacturing method according to embodiment 5 or 6, wherein the molding surface on which the powder coating layer is formed is a mirror surface. (Embodiment 8) The method according to any one of embodiments 1 to 7, wherein a thermosetting carbon fiber prepreg is placed over a layer of powder paint. (Embodiment 9) A manufacturing method described in any one of embodiments 1 to 8, in which the vacuum degassing is performed by using the upper and lower molds of a molding die to close the space in which the powder paint and the carbon fiber prepreg are placed, and then the side surfaces of the edge portions of the upper and lower molds are positioned to face each other. (Embodiment 10) A manufacturing method described in embodiment 9, in which vacuum degassing is continued even after the edge portion side of the upper mold and the edge portion side of the lower mold are positioned facing each other. (Embodiment 11) The method according to any one of embodiments 1 to 10, in which vacuum degassing is performed to prevent blistering after heat curing. (Embodiment 12) The method according to embodiment 2 or 6, wherein the vacuum degree of the vacuum degassing is -0.1 Pa or less. (Embodiment 13) The method according to any one of embodiments 1 to 12, wherein the time point at which the pressing or pressure starts is the time point at which molding pressure is applied. (Embodiment 14) The area of the carbon fiber prepreg is 1500 cm 2The above is the production method according to any one of the first to thirteenth embodiments. (Embodiment 15) The method according to any one of embodiments 1 to 14, wherein the charge rate of the carbon fiber prepreg relative to the molding surface is 80 to 90%. (Embodiment 16) The manufacturing method according to any one of embodiments 1 to 15, wherein the mold clamping speed for pressing the carbon fiber prepreg against the mirror surface via the powder paint layer is 2 mm / sec or less. (Embodiment 17) A manufacturing method described in any one of embodiments 1 to 16, in which a thermosetting carbon fiber prepreg is pressed onto a mirror surface through a layer of thermosetting powder paint when the thermosetting powder paint is in a semi-cured state. (Embodiment 18) A manufacturing method according to any one of embodiments 1 to 17, in which pressing is started within 200 seconds after forming the layer of powder coating on the mirror surface. (Embodiment 19) A manufacturing method according to any one of embodiments 1 to 18, in which the powder paint layer is arranged so that its thickness increases toward the center. (Embodiment 20) The manufacturing method according to any one of embodiments 1 to 19, wherein the coating is in-mold coating. (Embodiment 21) The manufacturing method described in any one of embodiments 1 to 20, wherein the powder paint is a primer paint. (Embodiment 22) A method for producing a multi-layer coated CFRP article, comprising: producing a primer-coated CFRP article using the manufacturing method described in embodiment 21; and applying a top coat to the primer-coated CFRP article. (Embodiment 23) The manufacturing method described in embodiment 22, wherein the topcoat coating includes a baked coating. (Embodiment 24) The manufacturing method described in embodiment 22, wherein the applied paint is dried at a temperature of 100°C or higher in the baking coating. (Embodiment 25) The manufacturing method according to any one of embodiments 22 to 24, wherein the primer coating film of the primer-coated CFRP article is polished to flatten its surface before the topcoat is applied.
[0057] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways within the scope of the effects of the invention, and can be combined with features described in other embodiments within the scope of feasibility. [Industrial Applicability]
[0058] Applying primer coating using the in-mold coating method is useful for efficiently producing top-coated CFRP articles. [Explanation of symbols]
[0059] 1 Press forming equipment 2 layers of powder paint 3 Carbon fiber prepreg 10 Press machine 11. Mainframe 12 Bolster 13 Slides 20 mold 20L lower mold 20U upper type 21 Convex 22 Annular protrusion 23 Seal ring 24 Recess 25 Annular recess 26 Closed space 27 Molding Cavity 28L, 28U molding surface 29 Non-specular area 30 Vacuum Pump 31 Share Edge 40 mold 40L lower mold 40U upper type 42 Annular protrusion 43 Seal ring 45 Annular recess 48L, 48U molding surface 50 Vacuum Pump
Claims
1. A method for producing a CFRP article in which a layer of powder paint is applied to a surface of a carbon fiber prepreg, comprising the steps of: a step of degassing the carbon fiber prepreg and the powder paint layer by vacuum degassing to remove any gas present between the carbon fiber prepreg and the powder paint layer, and then thermally curing the thermosetting carbon fiber prepreg while pressing the powder paint layer against a mold.
2. The method according to claim 1 , wherein the vacuum degassing is performed for 7 seconds or more.
3. The method according to claim 1 , wherein the surface of the mold is a mirror surface.
4. 2. The method according to claim 1, wherein the thermosetting carbon fiber prepreg is thermally cured while being pressed against the powder coating layer under vacuum degassing.
5. A method for producing a CFRP article in which a layer of powder paint is applied to a surface of a carbon fiber prepreg, comprising the steps of: Preparing a mold having a molding surface, the mold including an upper mold and a lower mold; maintaining the mold at a molding temperature; forming a layer of a thermosetting powder coating on at least a portion of the molding surface; placing a thermosetting carbon fiber prepreg in a closed space formed by closing the mold; Degassing the gas between the layer of thermosetting powder paint and the thermosetting carbon fiber prepreg; while evacuating the closed space to a vacuum, the upper mold and the lower mold are brought close to each other, and the carbon fiber prepreg placed therein is pressed together with the layer of powder paint; A method for producing a painted CFRP article, comprising:
6. The method according to claim 5, wherein the mixture is degassed under vacuum for 7 seconds or more before being pressed.
7. The method according to claim 5, wherein the molding surface on which the powder coating layer is formed is a mirror surface.
8. 6. The method of claim 1 or 5, wherein a thermosetting carbon fiber prepreg is placed over a layer of powder paint.
9. 7. The method according to claim 1 or 6, wherein the vacuum degassing is performed by forming a space in which the powder coating material and the carbon fiber prepreg are arranged into a closed space using an upper mold and a lower mold, and then positioning the side surfaces of the edge portions of the upper mold and the lower mold so that they face each other.
10. The method according to claim 9, wherein the vacuum degassing is continued even after the side surfaces of the edge portions of the upper mold and the lower mold are positioned to face each other.
11. The method according to claim 1 or 5, further comprising vacuum degassing to prevent blistering after heat curing.
12. The method according to claim 2 or 6, wherein the vacuum degassing is performed at a vacuum degree of -0.1 Pa or less.
13. The method according to claim 1 or 5, wherein the time when the pressing or pressure application starts is a time when molding pressure is applied.
14. The area of the carbon fiber prepreg is 1500 cm 2 The method for producing a composition according to claim 1 or 5,
15. The manufacturing method according to claim 1 or 5, wherein the charge rate of the carbon fiber prepreg with respect to the molding surface is 80 to 90%.
16. The method according to claim 1 or 5, wherein a mold clamping speed for pressing the carbon fiber prepreg against the mirror surface via the powder paint layer is 2 mm / sec or less.
17. 6. The method according to claim 1, wherein a thermosetting carbon fiber prepreg is pressed against the mirror surface via a layer of the thermosetting powder paint in a semi-cured state.
18. The method according to claim 1 or 5, wherein pressing is started within 200 seconds after the layer of powder paint is formed on the mirror surface.
19. 6. The method according to claim 1 or 5, wherein the powder coating layer is arranged so that its thickness increases toward the center.
20. The method according to claim 1 or 5, wherein the coating is in-mold coating.
21. The method according to claim 1 or 5, wherein the powder coating material is a primer coating material.
22. Producing a primer-coated CFRP article using the manufacturing method according to claim 21; applying a topcoat to the primer-coated CFRP article; A method for producing a multi-layer coated CFRP article, comprising:
23. The method of claim 22, wherein the top coat comprises a baked finish.
24. The method according to claim 22, wherein the applied coating is dried at a temperature of 100°C or higher in the baking coating.
25. The method of claim 22, further comprising sanding the primer coating of the primer-coated CFRP article to smooth its surface prior to the topcoat application.