Active energy ray-curable adhesive composition, cured product and adhesive sheet
A specific formulation of active energy ray-curable adhesive composition with linear aliphatic hydrocarbon group-containing polyether polyol and polyisocyanate improves adhesive strength, step followability, and resistance to heat and moisture, addressing the limitations of existing compositions in display devices and optical members.
Patent Information
- Application Number
- JP2024049877
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing active energy ray-curable adhesive compositions used in display devices and optical members lack sufficient adhesive strength, step followability, heat and humidity resistance, and light resistance.
A predetermined active energy ray-curable adhesive composition containing specific components such as linear aliphatic hydrocarbon group-containing polyether polyol, polyisocyanate, and hydroxyl group-containing mono(meth)acrylate, with a balanced ratio of these components to achieve a cured product with improved adhesive strength, step followability, and resistance to heat, moisture, and light.
The adhesive composition exhibits excellent adhesive strength, step followability, and resistance to heat and moisture, while maintaining light stability, enhancing the performance of bonded materials in display devices and optical members.
Smart Images

Figure 2024144313000001 
Figure 2024144313000002 
Figure 2024144313000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an active energy ray-curable pressure-sensitive adhesive composition, a cured product, and a pressure-sensitive adhesive sheet. [Background technology]
[0002] In recent years, display devices such as touch panels have been used in digital information devices such as mobile phones, portable game consoles, car navigation systems, etc. Furthermore, such display devices often use optical members such as liquid crystal elements, light-emitting diode elements, and organic electroluminescence elements.
[0003] When manufacturing a display device, a transparent double-sided pressure-sensitive adhesive sheet is used for the purpose of bonding the display device to the optical member or bonding optical members to each other. Such double-sided pressure-sensitive adhesive sheets are required to have properties such as adhesive strength and transparency. As such a pressure-sensitive adhesive sheet, an active energy ray-curable pressure-sensitive adhesive composition containing polyurethane obtained by reacting a hydroxyl group-containing (meth)acrylate and a hydroxyl group-containing photopolymerization initiator with a prepolymer of polyol and polyisocyanate, and various monomers has been proposed (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-037689 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] The active energy ray-curable pressure-sensitive adhesive composition of Patent Document 1 has room for improvement in terms of the property of not discoloring when exposed to sunlight, light from optical members, or the like (in the present disclosure, this is also referred to as "light resistance"), but such improvement poses a problem in terms of improving adhesive strength, step-following ability, moist heat resistance, and the like.
[0006] An object of the present disclosure is to provide an active energy ray-curable pressure-sensitive adhesive composition, a cured product, and a pressure-sensitive adhesive sheet that are excellent in adhesive strength, step-following ability, moist heat resistance, and light resistance. [Means for solving the problem]
[0007] The present inventors conducted intensive research to solve the above-mentioned problems and found that the above-mentioned problems can be solved by using a specific active energy ray-curable pressure-sensitive adhesive composition, a cured product thereof, and a pressure-sensitive adhesive sheet having the cured product, thereby completing the present invention.
[0008] That is, the present invention relates to the following items 1 to 3. (Item 1) (A) (a1) a polyurethane which is a reaction product of a linear aliphatic hydrocarbon group-containing polyether polyol, (a2) a polyisocyanate, and (a3) a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate; (B) a primary hydroxyl group-containing mono(meth)acrylate; (C) a mono(meth)acrylate having no hydroxyl group, The component (C) contains (c1) a (meth)acrylate having a glass transition temperature of less than -5°C when made into a homopolymer and / or (c2) a (meth)acrylate having a glass transition temperature of -5°C or higher when made into a homopolymer, the amount of the component (a1) is 35 to 70 mol %, the amount of the component (a2) is 25 to 60 mol %, and the amount of the component (a3) is 1 to 20 mol %, relative to 100 mol % in total of the components (a1), (a2), and (a3); An active energy ray-curable pressure-sensitive adhesive composition, in which the amount of the component (A) is 10 to 40 mass%, the amount of the component (B) is 20 to 35 mass%, the amount of the component (c1) is 20 to 40 mass%, and the amount of the component (c2) is 10 to 25 mass%, relative to 100 mass% (solid content) of the total amount of the components (A), (B), and (C). (Item 2) Item 2. A cured product of the active energy ray-curable pressure-sensitive adhesive composition according to item 1. (Item 3) Item 3. A pressure-sensitive adhesive sheet having the cured product according to item 2 on at least one surface of a substrate. Effect of the Invention
[0009] The adhesive layer of the active energy ray-curable adhesive composition of the present disclosure (also referred to as the "cured product" in the present disclosure) has excellent adhesive strength, conformability to unevenness, moist heat resistance, and light resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Throughout the present disclosure, the range of the values of each physical property, content, etc. may be set appropriately (for example, by selecting from the upper and lower limit values described in each item below). Specifically, for the value α, when A1, A2, A3, etc. are exemplified as the lower limit of the value α and B1, B2, B3, etc. are exemplified as the upper limit of the value α, the range of the value α is exemplified as A1 or more, A2 or more, A3 or more, B1 or less, B2 or less, B3 or less, A1 to B1, A1 to B2, A1 to B3, A2 to B1, A2 to B2, A2 to B3, A3 to B1, A3 to B2, A3 to B3, etc. In addition, in the present disclosure, "to" is used to mean that the values described before and after it are included as the lower limit and upper limit. Hereinafter, each component of the active energy ray-curable pressure-sensitive adhesive composition provided in the present disclosure, the cured product, the pressure-sensitive adhesive sheet, etc. will be described in detail.
[0011] <Component (A)> The component (A) is a polyurethane which is a reaction product of (a1) a linear aliphatic hydrocarbon group-containing polyether polyol, (a2) a polyisocyanate, and (a3) a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate.
[0012] <Component (a1)> The component (a1) is a polyether polyol containing a linear aliphatic hydrocarbon group. It is not preferable to use a polyether polyol (such as polypropylene glycol or dipropylene glycol) containing a branched aliphatic hydrocarbon group as an alternative to the component (a1) because it will deteriorate the light resistance. The term "polyether polyol containing a linear aliphatic hydrocarbon group" refers to a polyether polyol in which the aliphatic hydrocarbon portion has only a linear chain and does not contain any branching, alicyclic rings, or aromatic rings in that portion.
[0013] Examples of the component (a1) include one or more selected from polyethylene glycol and polytetramethylene ether glycol.
[0014] The component (a1) may be a commercially available product, such as polyethylene glycol under the product name "Polyethylene Glycol #1,540" (manufactured by Nacalai Tesque, Inc.) or polytetramethylene ether glycol under the product names "PTMG650", "PTMG1000", "PTMG2000", and "PTMG3000" (all manufactured by Mitsubishi Chemical Corporation).
[0015] The component (a1) is preferably polytetramethylene ether glycol, since this tends to make the adhesive layer flexible and tends to provide excellent durability after a light resistance test.
[0016] The upper limit of the number average molecular weight of the (a1) component is 10,000, 9,000, 8,000, 7,000, 6,000, 5,000, 4,000, 3,000, 2,000, 1,000, etc., and the lower limit is 9,000, 8,000, 7,000, 6,000, 5,000, 4,000, 3,000, 2,000, 1,000, 700, etc. In one embodiment, the number average molecular weight of the (a1) component is preferably 700 or more and 10,000 or less. The lower the number average molecular weight of the (a1) component, the harder the adhesive layer tends to be, and the higher the number average molecular weight of the (a1) component, the softer the adhesive layer tends to be. Therefore, within the above preferred range, both adhesive strength and step followability are easily achieved. In the present disclosure, the number average molecular weight can be determined by the method described in JIS K7252-1:2016. In addition, the term "step-following ability" in this disclosure is used in the same meaning as described in JP-A-2020-037689.
[0017] The (a1) component may contain a repeating unit containing a hydrocarbon group having an ether bond, such as polytetramethylene ether glycol represented by the general formula (1). The upper limit of the number of carbon atoms in the hydrocarbon group in the repeating unit of the (a1) component may be 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, etc., and the lower limit may be 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, etc. In one embodiment, the number of carbon atoms in the hydrocarbon group in the repeating unit of the (a1) component is preferably 1 to 30, more preferably 3 to 6, and particularly preferably 4 to 6, since compatibility with other components is easily improved and the effects of the present disclosure are easily achieved.
[0018] General formula (1): [ka]
[0019] (In the formula, n is an integer of 1 to 30.)
[0020] The upper limit of n in the general formula (1) is 30, 25, 20, 15, 10, 5, 4, 3, 2, etc., and the lower limit is 25, 20, 15, 10, 5, 4, 3, 2, 1, etc. In one embodiment, n in the general formula (1) is preferably about 1 to 30.
[0021] The upper limit of the number of hydroxyl groups of the (a1) component is 3.0, 2.8, 2.5, 2.3, 2.0, 1.8, etc., and the lower limit is 2.8, 2.5, 2.3, 2.0, 1.8, 1.5, etc. In one embodiment, the number of hydroxyl groups of the (a1) component is preferably 1.5 or more and 3.0 or less, more preferably 1.8 or more and 2.5 or less. It is preferable that the number of hydroxyl groups of the (a1) component is within the above range because the adhesive layer has better step followability and cutting ability. In the present disclosure, the number of hydroxyl groups can be determined by the method described in JIS K1557-1:2007. Specifically, the number of hydroxyl groups can be determined by an acetylation method.
[0022] The upper limit of the content (solid content) of the (a1) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is 99, 95, 90, 85, 80, 75, 70, 65, 60, 55% by mass, and the lower limit is 95, 90, 85, 80, 75, 70, 65, 60, 55, 50% by mass, etc. In one embodiment, the content (solid content) of the (a1) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is preferably 50 to 99% by mass, since the effects of the present disclosure are satisfactorily exhibited.
[0023] The upper limit of the content (solid content) of the (a1) component in 100 mol% of the total amount of the (a1), (a2), and (a3) components of the present disclosure is 70, 65, 60, 55, 50, 45, 40 mol%, etc., and the lower limit is 65, 60, 55, 50, 45, 40, 35 mol%, etc. In one embodiment, the content (solid content) of the (a1) component in 100 mol% of the total amount of the (a1), (a2), and (a3) components of the present disclosure is 35 to 70 mol%, since the effects of the present disclosure are satisfactorily exhibited.
[0024] <(a2) component> The (a2) component is a polyisocyanate. Examples of the (a2) component include at least one selected from aliphatic polyisocyanates and aromatic polyisocyanates. Examples of the aliphatic polyisocyanate include at least one selected from linear aliphatic polyisocyanates, branched aliphatic polyisocyanates, and alicyclic aliphatic polyisocyanates. Examples of the polyisocyanate include di-, tri-, and tetra-.
[0025] Examples of linear aliphatic diisocyanates include one or more selected from trimethylene diisocyanate, tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, and decamethylene diisocyanate.
[0026] Examples of the branched aliphatic diisocyanate include one or more selected from methyl 2,6-diisocyanatohexanoate and trimethylhexamethylene diisocyanate.
[0027] Examples of the alicyclic aliphatic diisocyanate include one or more selected from dicyclohexylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, cyclohexane-1,4-diylbis(methylene)diisocyanate, 1-methylcyclohexane-2,4-diyldiisocyanate, 1,4-cyclohexane diisocyanate, hydrogenated xylene diisocyanate, hydrogenated tolylene diisocyanate, and norbornene diisocyanate.
[0028] An example of the linear aliphatic triisocyanate is lysine triisocyanate.
[0029] Other polyisocyanates include the above-mentioned polyisocyanates, various known polyisocyanate adducts, and polymers of these isocyanates. Examples of such polyisocyanates include biurets, nurates, adducts, and allophanates. Examples of polyisocyanate biurets include product names: "Duranate 24A-100", "Duranate 22A-75P", and "Duranate 21S-75E" (all manufactured by Asahi Kasei Corporation). Examples of polyisocyanate nurates include product names: "Coronate HK" and "Coronate HXR" (both manufactured by Tosoh Corporation). Examples of polyisocyanate adducts include product names: "Duranate P301-75E" (manufactured by Asahi Kasei Corporation). An example of an allophanate of polyisocyanate is the product name "Coronate 2770" (manufactured by Tosoh Corporation).
[0030] The (a2) component is preferably an aliphatic diisocyanate, more preferably a linear aliphatic diisocyanate and / or an alicyclic aliphatic diisocyanate, since the adhesive layer is likely to have excellent durability after a moist heat resistance test and a light resistance test and is likely to exhibit good conformability to unevenness.
[0031] The average number of isocyanate groups in component (a2) may be approximately 2 or more and 10 or less. The average number of isocyanate groups can be calculated by the following formula: Average number of isocyanate groups = (number average molecular weight (Mn) x isocyanate group concentration (%)) / (42.02 x 100). The isocyanate group concentration (%) in the formula is a value measured by the method described in JIS K 1603-1:2007.
[0032] The upper limit of the molecular weight of the (a2) component is 1,000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, etc., and the lower limit is 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, 25, etc. In one embodiment, the molecular weight of the (a2) component is preferably about 25 to 1,000. In the present disclosure, when simply described as "molecular weight", it refers to a value calculated based on atomic weight.
[0033] The upper limit of the content (solid content) of the (a2) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.5% by mass, and the lower limit is 45, 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.5, 0.1% by mass, etc. In one embodiment, the content (solid content) of the (a2) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is preferably 0.1 to 50% by mass, since the effects of the present disclosure are satisfactorily exhibited.
[0034] The upper limit of the content (solid content) of the (a2) component in 100 mol% of the total amount of the (a1), (a2), and (a3) components of the present disclosure is 60, 55, 50, 45, 40, 35, 30 mol%, etc., and the lower limit is 55, 50, 45, 40, 35, 30, 25 mol%, etc. In one embodiment, the content (solid content) of the (a2) component in 100 mol% of the total amount of the (a1), (a2), and (a3) components of the present disclosure is 25 to 60 mol%, as the effects of the present disclosure are favorably exhibited.
[0035] Examples of the upper limit of the content ratio (mass basis, solid content equivalent) of the (a1) component to the (a2) component [(a1) component) / (a2) component)] are 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc., and examples of the lower limit are 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, etc. In one embodiment, the content ratio (mass basis, solid content equivalent) of the (a1) component to the (a2) component [(a1) component) / (a2) component)] is preferably about 50 / 50 to 99 / 1, more preferably about 65 / 35 to 95 / 5.
[0036] Examples of upper limits of the molar ratio of the (a1) component to the (a2) component [((a1) component) / ((a2) component)] include 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85, while examples of lower limits include 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, and 10 / 90. In one embodiment, the molar ratio of the component (a1) to the component (a2) [(component (a1)) / (component (a2))] is preferably about 10 / 90 to 90 / 10.
[0037] The upper limit of the ratio (NCO(a2) / OH(a1)) of the number of moles of isocyanate groups in component (a2) (NCO(a2)) to the number of moles of hydroxyl groups in component (a1) (OH(a1)) is 2.00, 1.95, 1.90, 1.85, 1.80, 1.75, 1.70, 1.65, 1.60, 1.55, 1.50, 1.45, 1.40, 1.35, 1.30, 1.25, 1.20, 1.15, 1.10, 1.05, 1.00, 0.95, 0.90, and 0.85. , 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, etc. are examples, and as the lower limit, 1.95, 1.90, 1.85, 1.80, 1.75, 1.70, 1.65, 1.60, 1.55, 1.50, 1.45, 1.40, 1.35, 1.30, 1.25, 1.20, 1.15, 1.10, 1.05, 1.00, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.5, etc. are examples. The ratio (NCO(a2) / OH(a1)) of the number of moles of isocyanate groups in the (a2) component (NCO(a2)) to the number of moles of hydroxyl groups in the (a1) component (OH(a1)) is usually about 0.5 to 2.00.
[0038] <(a3) component> The (a3) component is a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate. By using the (a3) component, the active energy ray curable adhesive composition has excellent curability, and the adhesive layer has excellent cuttability. When the active energy ray curable adhesive composition is produced without the (a3) component, curing failure occurs, and the adhesive layer becomes too soft at room temperature. When cutting a substrate or the like containing such an adhesive layer, the adhesive layer tends to adhere to the surface of the blade of the cutting device, so an active energy ray curable adhesive composition not containing the (a3) component is not preferred. When a hydroxyl group-containing poly(meth)acrylate having multiple (meth)acryloyl groups is used as an alternative to the (a3) component, the adhesive layer becomes too hard and the adhesive force is not easily exerted, which is not preferred. When a hydroxyl group-containing alcohol is used as a (partial) alternative to the (a3) component, curing failure occurs in the active energy ray curable adhesive composition, and the obtained adhesive layer also has poor cuttability, which is not preferred.
[0039] Examples of hydroxyl group-containing mono(meth)acrylates include one or more selected from 2-hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxybutyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethylphthalate, glycerol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl(meth)acrylate.
[0040] Examples of the isocyanate group-containing mono(meth)acrylate include one or more selected from 2-((meth)acryloyloxy)ethyl isocyanate and 2-(2-(meth)acryloyloxyethyloxy)ethyl isocyanate.
[0041] The (a3) component is preferably an isocyanate group-containing mono(meth)acrylate having 5 to 10 carbon atoms, more preferably 2-((meth)acryloyloxy)ethyl isocyanate, because the active energy ray-curable pressure-sensitive adhesive composition has excellent curability and the pressure-sensitive adhesive layer also has excellent cuttability.
[0042] Examples of upper limits of the molecular weight of the (a3) component include 1,000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, and 50, and examples of lower limits include 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, and 25. In one embodiment, the molecular weight of the (a3) component is preferably about 25 to 1,000.
[0043] The upper limit of the carbon number of the (a3) component is, for example, 30, 25, 20, 15, 10, 5, etc., and the lower limit is, for example, 25, 20, 15, 10, 5, 1, etc. In one embodiment, the carbon number of the (a3) component is preferably about 1 to 30.
[0044] The upper limit of the content (solid content) of the (a3) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is 40, 35, 30, 25, 20, 15, 10, 5, 1, 0.5, and 0.1% by mass, and the lower limit is 35, 30, 25, 20, 15, 10, 5, 1, 0.5, 0.1, and 0.05% by mass. In one embodiment, the content (solid content) of the (a3) component in 100% by mass of the total of the (a1), (a2), and (a3) components of the present disclosure is preferably 0.05 to 40% by mass, since the effects of the present disclosure are satisfactorily exhibited.
[0045] The upper limit of the content (solid content) of the (a3) component in 100 mol% of the total of the (a1), (a2), and (a3) components of the present disclosure is 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2 mol%, etc., and the lower limit is 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1 mol%, etc. In one embodiment, the content (solid content) of the (a3) component in 100 mol% of the total of the (a1), (a2), and (a3) components of the present disclosure is 1 to 20 mol%, since the effects of the present disclosure are favorably exhibited.
[0046] Examples of upper limits of the content ratio of the component (a1) to the component (a3) (based on mass, converted into solid content) [(component (a1)) / (component (a3))] include 99.9 / 0.1, 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, and 60 / 40, while examples of lower limits include 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, and 55 / 45. In one embodiment, the content ratio of the (a1) component to the (a3) component (by mass, converted into solid content) [((a1) component) / ((a3) component)] is preferably about 55 / 45 to 99.9 / 0.1, and more preferably about 80 / 20 to 95 / 5.
[0047] Examples of the upper limit of the content ratio (mass basis, solid content equivalent) of the (a2) component to the (a3) component [(a2) component) / (a3) component)] are 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, etc., and examples of the lower limit are 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc. In one embodiment, the content ratio (mass basis, solid content equivalent) of the (a2) component to the (a3) component [(a2) component) / (a3) component)] is preferably about 55 / 45 to 99 / 1, and more preferably about 70 / 30 to 90 / 10.
[0048] Examples of the upper limit of the molar ratio of the (a1) component to the (a3) component [((a1) component) / ((a3) component)] are 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, etc., and examples of the lower limit are 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, etc. In one embodiment, the molar ratio of the (a1) component to the (a3) component [((a1) component) / ((a3) component)] is preferably about 40 / 60 to 99 / 1.
[0049] Examples of the upper limit of the molar ratio of the (a2) component to the (a3) component [((a2) component) / ((a3) component)] are 99 / 1, 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, etc., and examples of the lower limit are 95 / 5, 90 / 10, 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, etc. In one embodiment, the molar ratio of the (a2) component to the (a3) component [((a2) component) / ((a3) component)] is preferably about 50 / 50 to 99 / 1.
[0050] <Other additives that can be added to component (A)> Component (A) may contain various additives as necessary, such as a catalyst, a crystal nucleating agent, a crystallization promoter, and a chain transfer agent.
[0051] The (A) component can be produced by various known polyurethane production methods. The (A) component can be obtained by reacting the (a1) component with the (a2) component to produce a urethane prepolymer (also referred to as the "(A') component" in this disclosure) having one or more isocyanate groups or hydroxyl groups at its terminal, and then reacting the (A') component with the (a3) component. The reaction temperature and reaction time are usually 70°C or higher and 85°C or lower, and 1 hour or higher and 5 hours or lower. If necessary, one or more selected from the (c1) component and the (c2) component of the present disclosure can be used as a diluent during the production of the polyurethane resin.
[0052] Examples of the upper limit of the weight average molecular weight of the (A) component include 100,000, 90,000, 80,000, 70,000, 60,000, 50,000, 40,000, 30,000, 20,000, 15,000, and 10,000, and examples of the lower limit include 90,000, 80,000, 70,000, 60,000, 50,000, 40,000, 30,000, 20,000, 15,000, 10,000, and 5,000. In one embodiment, the weight average molecular weight of the (A) component is preferably 5,000 or more and 100,000 or less, and more preferably 15,000 or more and 90,000 or less. If the weight average molecular weight of the (A) component is less than the lower limit, the adhesive strength of the adhesive layer tends to be weak, and if it is more than the upper limit, the viscosity of the active energy ray-curable adhesive composition tends to be high, making production difficult. In the present disclosure, the weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography.
[0053] The upper limit of the (meth)acrylic equivalent of component (A) is 1,000, 900, 800, 700, 600, 500, 400, 390, 380, 370, 360, 350, 340, 330, 320, 310, 300, 290, 280, 270, 260, 250, 240, 230, 220, 210, 200, 190, 180, 170, 160 g / g eq, etc. are exemplified, and as the lower limit, 900, 800, 700, 600, 500, 400, 390, 380, 370, 360, 350, 340, 330, 320, 310, 300, 290, 280, 270, 260, 250, 240, 230, 220, 210, 200, 190, 180, 170, 160, 150 g / eq, etc. are exemplified. In one embodiment, the (meth)acrylic equivalent of the (A) component is preferably about 150 to 1,000 g / eq. If the (meth)acrylic equivalent of the (A) component is too high, the adhesive strength tends to be low, so it is preferably about the upper limit or less. In the present disclosure, the (meth)acrylic equivalent is represented by the solid mass g of the (A) component per (meth)acrylic group.
[0054] The upper limit of the content (solid content) of the component (A) in 100% by mass of the total of the components (A), (B), and (C) of the present disclosure is 40, 35, 30, 25, 20, 15% by mass, etc., and the lower limit is 35, 30, 25, 20, 15, 10% by mass, etc. In one embodiment, the content (solid content) of the component (A) in 100% by mass of the total of the components (A), (B), and (C) of the present disclosure is 10 to 40% by mass, preferably 15% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 30% by mass or less, since the active energy ray-curable pressure-sensitive adhesive composition has excellent curability and the pressure-sensitive adhesive layer has excellent adhesive strength and step-following ability.
[0055] <(B) component> The (B) component is a primary hydroxyl group-containing mono(meth)acrylate. By using the (B) component, the active energy ray-curable pressure-sensitive adhesive composition has excellent curability, and the pressure-sensitive adhesive layer has excellent durability after a moist heat resistance test. When a mono(meth)acrylate having no hydroxyl group or a mono(meth)acrylate containing a secondary hydroxyl group is used as a substitute for the (B) component, the durability of the pressure-sensitive adhesive layer after a moist heat resistance test tends to be poor.
[0056] Examples of the component (B) include one or more selected from 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate.
[0057] The (B) component is preferably 2-hydroxyethyl (meth)acrylate and / or 4-hydroxybutyl (meth)acrylate, since the active energy ray-curable pressure-sensitive adhesive composition has excellent curability and the pressure-sensitive adhesive layer has excellent durability after a moist heat resistance test.
[0058] Examples of upper limits of the content ratio of component (A) to component (B) (based on mass, converted into solid content) [(component (A)) / (component (B))] include 85 / 15, 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, and 20 / 80, while examples of lower limits include 80 / 20, 75 / 25, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85. In one embodiment, the content ratio of the (A) component to the (B) component (based on mass, converted into solid content) [((A)) / ((B))] is preferably about 15 / 85 to 85 / 15, since the adhesive layer is likely to exhibit excellent step conformability and durability after a moist heat resistance test.
[0059] Examples of upper limits for the content (in terms of solid content) of the (B) component relative to 100% by mass of the total amount of the (A) component, the (B) component, and the (C) component of the present disclosure are 35, 34, 33, 32, 31, 30, 29, 28, 27, 26, 25, 24, 23, 22, and 21% by mass, and examples of lower limits are 34, 33, 32, 31, 30, 29, 28, 27, 26, 25, 24, 23, 22, 21, and 20% by mass. In one embodiment, the content of the (B) component (converted into solid content) in the total amount of the (A) component, the (B) component, and the (C) component of the present disclosure (100% by mass) is 20% by mass or more and 35% by mass or less, preferably 25% by mass or more and 35% by mass or less, and more preferably 30% by mass or more and 35% by mass or less, because the adhesive layer is likely to exhibit excellent step-following ability and durability after a moist heat resistance test.
[0060] <(C) component> The component (C) is a mono(meth)acrylate that does not have a hydroxyl group. Examples of the component (C) include one or more selected from (c1) (meth)acrylates having a glass transition temperature (also referred to as "Tg" in the present disclosure) of less than -5°C when made into a homopolymer and (c2) (meth)acrylates having a glass transition temperature of -5°C or higher when made into a homopolymer. The "glass transition temperature when made into a homopolymer" is the value described in Wiley-Interscience's "Polymer Handbook."
[0061] <(c1) component> The component (c1) is a (meth)acrylate that, when made into a homopolymer, has a glass transition temperature of less than −5° C. By using the component (c1), the adhesive layer becomes flexible and has good step-following ability.
[0062] As component (c1), tetradecyl methacrylate (Tg: -72°C), 2-ethylhexyl acrylate (Tg: -70°C), ethoxydiethylene glycol acrylate (Tg: -70°C), isooctyl acrylate (Tg: -70°C), ethyl carbitol acrylate (Tg: -67°C), n-octyl acrylate (Tg: -65°C), lauryl methacrylate (Tg: -65°C), isononyl acrylate (Tg: -58°C), n-butyl acrylate (Tg: -56°C), 2-methoxyethyl acrylate (Tg: -50°C), isopropyl acrylate (Tg: -58 ... Examples include one or more selected from decyl methacrylate (Tg: -41°C), nonyl acrylate (Tg: -37°C), 2-ethoxyethyl methacrylate (Tg: -31°C), isobutyl acrylate (Tg: -26°C), n-lauryl acrylate (Tg: -23°C), phenoxyethyl acrylate (Tg: -22°C), isostearyl acrylate (Tg: -18°C), 2-ethylhexyl methacrylate (Tg: -10°C), and (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate (Tg: -7°C).
[0063] The component (c1) is preferably 2-ethylhexyl acrylate, since it imparts flexibility to the adhesive layer and provides excellent conformability to uneven surfaces.
[0064] Examples of upper limits for the number of carbon atoms in the alkyl group of component (c1) are 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, and 5, and examples of lower limits are 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, and 4. In one embodiment, the number of carbon atoms in the alkyl group of component (c1) is preferably 4 or more and 18 or less.
[0065] The upper limit of the content (solid content) of the (c1) component in 100% by mass of the total of the (A) component, the (B) component, and the (C) component of the present disclosure is 40, 35, 30, 25% by mass, etc., and the lower limit is 35, 30, 25, 20% by mass, etc. In one embodiment, the content (solid content) of the (c1) component in 100% by mass of the total of the (A) component, the (B) component, and the (C) component of the present disclosure is 20% by mass or more and 40% by mass or less, preferably 25% by mass or more and 40% by mass or less, and more preferably 30% by mass or more and 40% by mass or less, because the adhesive layer becomes flexible and is likely to have excellent step conformability.
[0066] <(c2) component> The component (c2) is a (meth)acrylate having a glass transition temperature of −5° C. or higher when made into a homopolymer. By using the component (c2), the storage modulus of the adhesive layer is increased, and the cuttability is excellent.
[0067] (c2) Component: 2-methoxyethyl methacrylate (Tg: -2°C), (3-ethyloxetan-3-yl)methyl methacrylate (Tg: 2°C), benzyl acrylate (Tg: 6°C), methyl acrylate (Tg: 8°C), cyclohexyl acrylate (Tg: 15°C), diethylaminoethyl methacrylate (Tg: 16-24°C), dimethylaminoethyl methacrylate (Tg: 18°C), n-butyl methacrylate (Tg: 20°C), cyclic trimethylolpropane formal acrylate (Tg: 27°C), n-stearyl acrylate (Tg: 30°C), n-stearyl methacrylate (Tg: 38°C), t-butyl acrylate (Tg: 41°C), glycidyl methacrylate (Tg: 46°C) , isobutyl methacrylate (Tg: 48°C), 3,3,5-trimethylcyclohexyl acrylate (Tg: 52°C), benzyl methacrylate (Tg: 54°C), tetrahydrofurfuryl methacrylate (Tg: 60°C), glycidyl acrylate (Tg: 60°C), ethyl methacrylate (Tg: 65°C), cyclohexyl methacrylate (Tg: 66°C), isobornyl acrylate (Tg: 97°C), methyl methacrylate (Tg: 105°C), t-butyl methacrylate (Tg: 107°C), dicyclopentanyl acrylate (Tg: 120°C), 1-adamantyl acrylate (Tg: 153°C), and one or more selected from 1-adamantyl methacrylate (Tg: 250°C).
[0068] The component (c2) is preferably isobornyl acrylate, since this increases the storage modulus of the adhesive layer and facilitates excellent cuttability.
[0069] Examples of upper limits for the number of carbon atoms in the alkyl group of component (c2) are 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, and 5, and examples of lower limits are 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, and 4. In one embodiment, the number of carbon atoms in the alkyl group of component (c2) is preferably 4 or more and 18 or less.
[0070] The upper limit of the content (solid content) of the (c2) component in 100% by mass of the total of the (A), (B) and (C) components of the present disclosure is 25, 20, 15% by mass, etc., and the lower limit is 20, 15, 10% by mass, etc. In one embodiment, the content (solid content) of the (c2) component in 100% by mass of the total of the (A), (B) and (C) components of the present disclosure is 10% by mass or more and 25% by mass or less, preferably 10% by mass or more and 20% by mass or less, and more preferably 10% by mass or more and 15% by mass or less, since the storage modulus of the adhesive layer is increased and the cuttability is easily excellent.
[0071] Examples of upper limits of the molecular weight of the (C) component include 1,000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, and 50, and examples of lower limits include 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 50, and 25. In one embodiment, the molecular weight of the (C) component is preferably about 25 to 1,000.
[0072] Examples of the upper limit of the content ratio of the (c1) component to the (c2) component (mass basis, solid content equivalent) [((c1) component / ((c2) component)] are 90 / 10, 85 / 15, 80 / 20, 75 / 15, 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85. Examples of the lower limit are 85 / 15, 80 / 20, 75 / 15, 70 / 30, 65 / 35, 60 / 40, Examples include 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, 10 / 90, etc. In one embodiment, the content ratio (by mass, converted into solid content) of the (c1) component to the (c2) component [((c1) component / ((c2) component)]] is preferably about 10 / 90 to 90 / 10, since the adhesive layer becomes flexible, the adhesive layer is easily excellent in conformity to unevenness, and the storage modulus is also increased, making the adhesive layer easily excellent in cuttability.
[0073] Examples of upper limits of the content ratio of component (A) to component (C) (based on mass, converted into solid content) [(component (A)) / (component (C))] include 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85, while examples of lower limits include 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, and 10 / 90. In one embodiment, the content ratio of the (A) component to the (C) component (based on mass, converted into solid content) [((A) component) / ((C) component)] is preferably about 10 / 90 to 70 / 30, since this makes the adhesive layer flexible and tends to have excellent step-following properties, and also increases the storage modulus, tending to provide excellent cuttability.
[0074] Examples of upper limits of the content ratio of the component (B) to the component (C) (based on mass, converted into solid content) [(component (B)) / (component (C))] include 70 / 30, 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, and 15 / 85, while examples of lower limits include 65 / 35, 60 / 40, 55 / 45, 50 / 50, 45 / 55, 40 / 60, 35 / 65, 30 / 70, 25 / 75, 20 / 80, 15 / 85, and 10 / 90. In one embodiment, the content ratio of the (B) component to the (C) component (based on mass, converted into solid content) [((B) component) / ((C) component)] is preferably about 10 / 90 to 70 / 30, since the adhesive layer becomes flexible, which leads to excellent step-following ability, and the storage modulus is also increased, which leads to excellent cuttability, and further to excellent durability after a moist heat resistance test.
[0075] The upper limit of the content (solid content) of the (C) component in 100% by mass of the total of the (A) component, the (B) component, and the (C) component of the present disclosure is 65, 60, 55, 50, 45, 40, 35% by mass, etc., and the lower limit is 60, 55, 50, 45, 40, 35, 30% by mass, etc. In one embodiment, the content (solid content) of the (C) component in 100% by mass of the total of the (A) component, the (B) component, and the (C) component of the present disclosure is 30% by mass or more and 65% by mass or less, preferably 40 to 60% by mass, and more preferably 50 to 55% by mass, since the adhesive layer becomes flexible, the step-following property is easily excellent, and the storage modulus is also increased, and the cuttability is easily excellent.
[0076] <(D) component> The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure preferably contains a radical photopolymerization initiator (also referred to as "component (D)" in the present disclosure) because the pressure-sensitive adhesive layer has excellent curability.
[0077] Examples of the component (D) include one or more types selected from alkylphenone type photopolymerization initiators, acylphosphine oxide type photopolymerization initiators, hydrogen abstraction type photopolymerization initiators, and oxime ester type photopolymerization initiators.
[0078] Examples of alkylphenone type photopolymerization initiators include benzyl dimethyl ketals such as 2,2-dimethoxy-1,2-diphenylethan-1-one, α-hydroxyalkylphenones such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and α-aminoalkylphenones such as 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one.
[0079] Examples of the acylphosphine oxide type photopolymerization initiator include one or more selected from 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.
[0080] An example of the hydrogen abstraction type photopolymerization initiator is phenylglyoxylic acid methyl ester.
[0081] Examples of the oxime ester type photopolymerization initiator include one or more selected from 1,2-octanedione, 1-[4-(phenylthio)phenyl-2-(O-benzoyloxime)], and ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime).
[0082] The component (D) is preferably an α-hydroxyalkylphenone type photopolymerization initiator and / or an acylphosphine oxide type photopolymerization initiator, since the active energy ray-curable pressure-sensitive adhesive composition has excellent curability.
[0083] Component (D) may be a commercially available product. The products in question are 2,2-dimethoxy-1,2-diphenylethan-1-one (product name: "OMNIRAD 651", manufactured by IGM Resins), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (product name: "H0991", manufactured by Tokyo Chemical Industry Co., Ltd.) (product name: "OMNIRAD1173", manufactured by IGM Resins) (product name: "Lunacure 100", manufactured by DKSH Japan Co., Ltd.), 1-hydroxycyclohexyl phenyl ketone (product name: "OMNIRAD184", manufactured by IGM Resins) (product name: "Lunacure 200", manufactured by DKSH Japan Co., Ltd.), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (product name: "OMNIRAD 2959", manufactured by IGM Resins) Resins), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (product name: "OMNIRAD 907", IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (product name: "OMNIRAD TPO", IGM Resins), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (product name: "OMNIRAD 819", IGM Resins), phenylglyoxylic acid methyl ester (product name: "OMNIRAD MBF", IGM Resins), 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (product name: "OMNIRAD OXE 01", IGM Examples include ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) (product name: "OMNIRAD OXE 02", manufactured by IGM Resins).
[0084] The upper limit of the content (solid content) of the (D) component relative to 100% by mass of the total amount of the (A), (B) and (C) components of the present disclosure is 5, 4, 3, 2, 1.5, 1, 0.5, 0.2% by mass, and the lower limit is 4, 3, 2, 1.5, 1, 0.5, 0.2, 0.1% by mass, etc. In one embodiment, the content (solid content) of the (D) component relative to 100% by mass of the total amount of the (A), (B) and (C) components of the present disclosure is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 2% by mass or less, and even more preferably 0.2% by mass or more and 1.5% by mass or less.
[0085] <Other additives that can be added> The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure may contain various additives as necessary.
[0086] Examples of additives include surface conditioners, surfactants, ultraviolet absorbers, antioxidants, light stabilizers, tackifiers, inorganic fillers, silane coupling agents, colloidal silica, defoamers, wetting agents, rust inhibitors, plasticizers, chain transfer agents, and photosensitizers.
[0087] The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure may contain a solvent. Examples of the solvent include ketone solvents, aromatic solvents, alcohol solvents, glycol solvents, glycol ether solvents, ester solvents, petroleum-based solvents, haloalkane solvents, and amide solvents.
[0088] Examples of the ketone solvent include methyl ethyl ketone, acetylacetone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone.
[0089] Examples of aromatic solvents include toluene and xylene.
[0090] Examples of the alcohol solvent include methanol, ethanol, n-propanol, isopropanol, butanol, and the like.
[0091] Examples of glycol solvents include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, and polypropylene glycol.
[0092] Examples of glycol ether solvents include ethylene glycol dimethyl ether, ethylene glycol diethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monoisobutyl ether, and ethylene glycol mono-t-butyl ether.
[0093] Examples of the ester solvent include ethyl acetate, butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, and propylene glycol monomethyl ether acetate.
[0094] Examples of petroleum-based solvents include product names "T-SOL 100" and "T-SOL 150" (both manufactured by ENEOS Corporation).
[0095] An example of the haloalkane solvent is chloroform.
[0096] An example of the amide solvent is dimethylformamide.
[0097] The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure can be used without containing a solvent. Therefore, the active energy ray-curable pressure-sensitive adhesive composition of the present disclosure preferably does not contain a solvent, because this can reduce costs and environmental impacts.
[0098] The viscosity (mPa·s / 25° C.) of the active energy ray-curable pressure-sensitive adhesive composition of the present disclosure is preferably from 100 to 10,000, more preferably from 300 to 8,000, and even more preferably from 500 to 7,000. In the present disclosure, the viscosity is a value measured (5 minutes) using an E-type viscometer (product name: "TVE-10", manufactured by Toki Sangyo Co., Ltd.).
[0099] The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure can be obtained by mixing the components (A), (B), and (C), and optionally the component (D) and other additives that can be added. The order of mixing may be sequential, or all may be mixed at once.
[0100] <Cured product> The present invention also includes a product obtained by irradiating an active energy ray-curable pressure-sensitive adhesive composition with active energy rays such as ultraviolet rays and curing the composition.
[0101] When the active energy ray-curable pressure-sensitive adhesive composition contains a solvent, it is considered to carry out a drying treatment before the ultraviolet ray irradiation.
[0102] Examples of ultraviolet light sources include ultraviolet irradiation devices having a xenon lamp, a high-pressure mercury lamp, and a metal halide lamp. In the device, the conditions of the ultraviolet irradiation intensity, the integrated light amount, and the transport speed are usually as follows: irradiation intensity is 80 mW / cm 2 More than 160mW / cm 2 The conveying speed is 3 m / min to 50 m / min, and the cumulative light intensity is 100 mJ / cm 2 More than 3,000mJ / cm 2 The following is the result.
[0103] The active energy ray-curable pressure-sensitive adhesive composition may be applied to various plastic film substrates to form a layer of the active energy ray-curable pressure-sensitive adhesive composition, and then the layer may be irradiated with ultraviolet light to obtain a cured product.
[0104] Examples of methods for coating the active energy ray-curable pressure-sensitive adhesive composition include bar coater coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, offset printing, flexographic printing, and screen printing.
[0105] The coating amount is usually 1g / m2 after drying. 2 More than 1,000g / m 2 Less than 3 g / m 2 More than 500g / m 2 The range is as follows.
[0106] The thickness of the cured product of the present disclosure is preferably from 10 μm to 1,000 μm, more preferably from 25 μm to 700 μm, after drying, since the adhesive layer is more likely to exhibit step-following ability and is less likely to produce bubbles.
[0107] The upper limit of the storage modulus G' (also referred to as "G'" in the present disclosure) at 20 ° C. and 1 Hz of the cured product of the present disclosure is 100 × 10 5 , 90×10 5 , 80×10 5 , 70×10 5 , 60×10 5 , 50×10 5 , 40×10 5 , 30×10 5 , 20×10 5 , 10×10 5 , 5×10 5 , 4×10 5 , 3×10 5 , 2×10 5 , 1.5×10 5 Pa, etc., are given as examples, with a lower limit of 90 x 10 5 , 80×10 5 , 70×10 5 , 60×10 5 , 50×10 5 , 40×10 5 , 30×10 5 , 20×10 5 , 10×10 5 , 5×10 5 , 4×10 5 , 3×105 , 2×10 5 , 1.5×10 5 , 1×10 5 In one embodiment, the lower limit of the storage modulus G' at 20°C and 1 Hz of the cured product of the present disclosure is preferably 1 x 10 Pa because the cuttability of the cured product is likely to be excellent. 5 Pa, more preferably 1.5×10 5 In one embodiment, the upper limit of the storage modulus G′ at 20° C. and 1 Hz of the cured product of the present disclosure is preferably 100×10 Pa or more, since the cured product is likely to have excellent step conformability. 5 Pa or less, and more preferably 90×10 5 In the present disclosure, the storage modulus of the cured product can be determined by the method described in JIS K7244-1:1998.
[0108] Specifically, the storage modulus is measured by measuring the dynamic viscoelasticity under the following conditions using a commercially available measuring device (product name: "MCR302", manufactured by Anton Paar). Then, the storage modulus G' at 20°C is calculated from the measurement results.
[0109] Deformation mode: Torsion Measurement frequency: 1Hz Distortion: 0.01~1%AUTO setting Heating rate: 3℃ / min Measurement temperature: 0~100℃ Shape: Parallel plate 8.0mmφ
[0110] In the present disclosure, the storage modulus (G') is a value proportional to the maximum energy accumulated through a load cycle, and represents the rigidity of the adhesive layer. The rigidity refers to the resistance to deformation due to external forces such as bending and twisting. The larger the storage modulus value at 20°C and 1 Hz, the higher the rigidity of the adhesive layer at 20°C, and the smaller the value, the lower the rigidity of the adhesive layer at 20°C. The preferred storage modulus G' at 20°C and 1 Hz of the cured product of the present disclosure is 1×10 5 Since the compressive strength exceeds 100 Pa, the cured product of the present disclosure tends to have excellent cuttability at room temperature.
[0111] <Molded object> An example of the application of the active energy ray-curable pressure-sensitive adhesive composition is coating between substrates of various known articles. The articles are not particularly limited and may be various known articles.
[0112] Examples of such articles include the main bodies and remote controls of home appliances such as refrigerators, televisions, and air conditioners, the housings and displays of information terminals such as mobile phones, smartphones, tablets, and personal computers, and plastic molded products such as automobile parts and automobile interior materials.
[0113] The active energy ray curable adhesive composition of the present disclosure is suitable for optical applications. For example, it can be applied to a display panel with a multi-layer structure in a digital display device. In addition, the adhesive layer is strong at room temperature, and the problem of the cut part adhering to the punching blade during punching processing and being unable to be separated, or the problem of the adhesive layer adhering to the punching blade, is unlikely to occur, and it can be cut into various shapes. The adhesive layer of the present disclosure is also suitable for use in displays such as televisions, smartphones, and tablets because of its excellent transparency.
[0114] <Applicable substrates> The active energy ray-curable pressure-sensitive adhesive composition of the present disclosure can be applied to various substrates.
[0115] Examples of the substrate include metal, plastic, glass, and other resins. Examples of metals include iron, aluminum, aluminum-plated steel sheets, tin-free steel sheets (TFS), stainless steel sheets, zinc phosphate-treated steel sheets, zinc / zinc alloy-plated steel sheets (bonded steel sheets), and other treated steel sheets. Examples of plastics include thermoplastic plastic substrates and thermosetting plastic substrates. Examples of thermoplastic plastic substrates include general-purpose plastic substrates and engineering plastic substrates. Examples of general-purpose plastic substrates include olefin-based, polyester-based, acrylic-based, vinyl-based, and polystyrene-based substrates. Examples of olefins include polyethylene, polypropylene, and norbornene. Examples of polyesters include polyethylene terephthalate (PET) and polyethylene naphthalate (PEN). An example of the acrylic resin is polymethyl methacrylate (PMMA). Examples of vinyl-based materials include polyvinyl chloride, polyvinylidene chloride, and polyvinyl alcohol. Examples of polystyrene-based resins include polystyrene (PS) resin, styrene-acrylonitrile (AS) resin, and styrene-butadiene-acrylonitrile (ABS) resin. Examples of engineering plastic substrates include general-purpose engineering plastics and super engineering plastics. Examples of general-purpose engineering plastics include polycarbonate and polyamide (nylon). An example of a super engineering plastic is polyether ether ketone (PEEK). Examples of the thermosetting plastic substrate include polyimide, epoxy resin, and melamine resin. Other examples of the plastic substrate include triacetyl cellulose resin. The substrate of the present disclosure is preferably a thermoplastic substrate, more preferably one or more selected from polyesters, acrylics, and general-purpose engineering plastics, and even more preferably a polyester or acrylic and a general-purpose engineering plastic.
[0116] The adhesive layer of the present disclosure is particularly preferably used for optical applications because of its excellent transparency. That is, the adhesive layer of the present disclosure is particularly suitable for bonding optical substrates. The adhesive layer of the present disclosure is suitable for use as an optical transparent adhesive (also referred to as "OCA" in the present disclosure).
[0117] The substrate for optics of the present disclosure is not particularly limited and may be any of various known substrates. The substrate for optics may be used alone or in combination of two or more kinds.
[0118] Examples of optical substrates include polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate (PEN), polyethylene films, polypropylene films, cellophane, diacetyl cellulose films, triacetyl cellulose films, acetyl cellulose butyrate films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene-vinyl acetate copolymer films, polystyrene films, polycarbonate films, polymethylpentene films, polysulfone films, polyether ether ketone films, polyether sulfone films, polyether imide films, polyimide films, fluororesin films, polyamide films, acrylic resin films, norbornene-based resin films, and cycloolefin resin films; glass, tin-doped indium oxide films, ITO films, and transparent conductive films.
[0119] Specifically, the combination of the pressure-sensitive adhesive layer and the optical substrate of the present disclosure is (1) Glass, an adhesive layer of the present disclosure, and a transparent conductive film (also referred to as "ITO" in this disclosure). (2) Support film, adhesive layer of the present disclosure, ITO (3) Support film, adhesive layer of the present disclosure, and liquid crystal display (4) Glass, adhesive layer of the present disclosure, and liquid crystal display etc. EXAMPLES
[0120] The present disclosure will be described in more detail below with reference to Production Examples, Comparative Production Examples, Examples, Comparative Examples, Evaluation Examples, and Comparative Evaluation Examples, but the present disclosure is not limited to these Examples. In the following description, parts and % are based on mass.
[0121] In the present examples, the weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) under the following conditions. (GPC measurement conditions) Model: Product name: "HLC-8420GPC", manufactured by Tosoh Corporation Column: Product name: "TSKgel G1000H", "TSKgel G2000H", manufactured by Tosoh Corporation Developing solvent: Tetrahydrofuran Flow rate: 0.6mL / min Measurement temperature: 40℃ Detector: Refractive Index Detector (RI) Standard: Monodisperse polystyrene Sample: Prepare a 1% solids solution from the resin in tetrahydrofuran, filter the solution through a microfilter, and then collect 20 μL of the solution.
[0122] In each production example, the NCO content of the urethane prepolymer was measured as follows: Measuring device: Automatic potentiometric titrator (product name: "AT-700", manufactured by Kyoto Electronics Manufacturing Co., Ltd.) Measurement steps: 1: Weigh out approximately 0.500g to 1.000g of sample into a weighing bottle. 2: Inject 10 mL of 0.15 mol / L dibutylamine solution in toluene. 3: Place the weighing bottle containing the sample in an ultrasonic cleaner to completely dissolve the sample. 4: Make sure the sample is completely dissolved and leave it for 15 minutes (away from direct sunlight and heat). 5: After 15 minutes, add 100 mL of isopropyl alcohol to the weighing bottle. Place the stirrer piece in the weighing bottle. 6: Titrate using 0.1 mol / L hydrochloric acid solution (f=1.00) to determine the NCO value. Input the amount of sample to be measured into the automatic titrator and then measure. If the measurement difference is within 0.30, it is acceptable. If it is 0.30 or more, measure one sample again to confirm that it is within 0.30.
[0123] <Production Example 1: Production of component (A)-1> A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and an air inlet was charged with 77.2 parts of polytetramethylene ether glycol having a number average molecular weight of 2,000 (product name: "PTMG2000", manufactured by Mitsubishi Chemical Corporation) (also referred to as "PTMG2000" in this disclosure) as the component (a1), 7.9 parts of isophorone diisocyanate (product name: "Isophorone Diisocyanate", manufactured by Tokyo Chemical Industry Co., Ltd.) (also referred to as "IPDI" in this disclosure) as the component (a2), 14 parts of 2-ethylhexyl acrylate (product name: "2-ethylhexyl acrylate", manufactured by Mitsubishi Chemical Corporation) (also referred to as "2-EHA" in this disclosure), and 0.1 parts of tin octylate, and the mixture was reacted at 70°C for 2 hours to obtain a 2-EHA solution of a hydroxyl group-terminated urethane prepolymer, which is an intermediate. The resulting reaction product was mixed with 0.9 parts of 2-isocyanatoethyl methacrylate (product name: "Karenz MOI", manufactured by Resonac Corporation) (also referred to as "MOI" in this disclosure) as component (a3), and the mixture was allowed to react at 70°C for 2 hours. Completion of the reaction was confirmed by NCO measurement, thereby obtaining a 2-EHA solution of the reaction product (also referred to as "component (A)-1" in this disclosure).
[0124] <Production Examples 2 to 5 and Comparative Production Examples 1 to 2: Production of Components (A)-2 to (A)-5 and Components (A)-C1 to (A)-C2> The same procedure as in Production Example 1 was carried out except that the content of each component was changed as shown in Table 1. Table 2 shows the molar amount of each component.
[0125] [Table 1]
[0126] The numbers in Table 1 indicate the parts by mass of the components (a1), (a1)', (a2) and (a3) in the component (A). The meanings of the terms in Table 1 are as follows: ': A symbol representing a comparison component. PTMG2000: Polytetramethylene ether glycol (product name: "PTMG2000", manufactured by Mitsubishi Chemical Corporation) PPG2000: Polypropylene glycol (product name: "Adeca Polyether P-2000, diol type, 2,000", Fujifilm Wako Pure Chemical Industries, Ltd.) IPDI: Isophorone diisocyanate (product name: "Isophorone Diisocyanate", manufactured by Tokyo Chemical Industry Co., Ltd.) HDI: Hexamethylene diisocyanate (product name: "HDI", manufactured by Tosoh Corporation) MOI: 2-isocyanatoethyl methacrylate (product name: Karenz MOI, manufactured by Resonac Co., Ltd.) 4HBA: 4-Hydroxybutyl acrylate (product name: "4-Hydroxybutyl acrylate 4HBA", manufactured by Mitsubishi Chemical Corporation) HEA: 2-hydroxyethyl acrylate (product name: "HEA", manufactured by Osaka Organic Chemical Industry Co., Ltd.)
[0127] [Table 2]
[0128] The numbers in Table 2 indicate the molar amounts of the components (a1), (a1)', (a2) and (a3) in the component (A).
[0129] <Examples 1 to 14 and Comparative Examples 1 to 12: Preparation of active energy ray-curable pressure-sensitive adhesive compositions (1) to (14) and (C1) to (C12)> The components were mixed in the mass % amounts shown in Tables 3 and 4 to obtain active energy ray-curable pressure-sensitive adhesive compositions (1) to (14) and (C1) to (C12).
[0130] <Evaluation Example 1-1: Preparation of Adhesive Sheet (1)> The active energy ray curable pressure-sensitive adhesive composition (1) was applied onto a 75 μm thick heavy release treated polyester film (product name: "SP-PET-03-75BU", manufactured by Mitsui Chemicals Tohcello Co., Ltd.) so that the thickness of the adhesive layer after curing was 600 μm, and the release treated surface of a 38 μm thick light release treated polyester film (product name: "SP-PET-01-75BU", manufactured by Mitsui Chemicals Tohcello Co., Ltd.) was attached to the coating layer of the active energy ray curable pressure-sensitive adhesive composition. Next, the obtained coated film was heated in the atmosphere under a high pressure mercury lamp (100 mW / cm 2 , 900mJ / cm 2 ) was irradiated with ultraviolet light to produce a laminated film (1) (light release treated polyester film / adhesive layer / heavy release treated polyester film) including an adhesive layer. Next, the light release treated polyester film and the heavy release treated polyester film were peeled off to obtain a sheet (adhesive sheet (1)) consisting of only the adhesive layer (also referred to as the "cured product" in this disclosure).
[0131] <Evaluation Examples 1-2 to 1-14 and Comparative Evaluation Examples 1-1 to 1-12: Adhesive Sheets (2) to (14) and Adhesive Sheets (C1) to (C12)> The same procedure as in Evaluation Example 1-1 was repeated except that the active energy ray-curable adhesive composition (1) was replaced with the active energy ray-curable adhesive compositions (2) to (14) and the active energy ray-curable adhesive compositions (C1) to (C12), respectively. Note that the active energy ray-curable adhesive composition (C7) of Comparative Example 7 was not subjected to the following evaluation because it was not sufficiently cured.
[0132] <Evaluation Example 2-1: Preparation of Laminate (1)> The same laminated film as in Evaluation Example 1-1 (1) was prepared, the light release treated polyester film was peeled off from the laminated film, and instead, a 50 μm thick polyester film (product name: "Cosmoshine A-4300", manufactured by Toyobo Co., Ltd.) was attached with a 2 kg roller and left to stand for 2 hours. Next, a test piece of 8 cm x 8 cm was cut from this, and the heavy release treated polyester film was peeled off to prepare a single-sided adhesive sheet (Cosmoshine A-4300 / adhesive layer). A single-sided adhesive sheet (adhesive layer / Cosmoshine A-4300) (5 cm x 5 cm x 650 μm) was placed on a glass plate (10 cm x 10 cm x 2 mm), and the two were brought into close contact with a 2 kg roller to prepare a laminate (Cosmoshine A-4300 (50 μm thick) / adhesive layer (600 μm thick) / glass plate (2 mm thick)).
[0133] <Evaluation Examples 2-2 to 2-14 and Comparative Evaluation Examples 2-1 to 2-12: Laminates (2) to (14) and Laminates (C1) to (C12)> The same procedure as in Evaluation Example 2-1 was repeated, except that the laminate film (1) in Evaluation Example 1-1 was replaced with the laminate films (2) to (14) in Evaluation Examples 1-2 to 1-14 and the laminate films (C1) to (C12) in Comparative Evaluation Examples 1-1 to 1-12, respectively.
[0134] <Performance evaluation (1): Adhesive strength> The laminates (1) to (14) and (C1) to (C12) were left to stand for 24 hours under conditions of 25°C and 50% humidity. The single-sided adhesive sheet (adhesive layer / Cosmoshine A-4300) was peeled off from the glass plate in a 180° direction at a speed of 300 mm / min to measure the adhesive strength (N / 25 mm). A commercially available machine (product name: Tensilon Universal Material Tester, manufactured by A&D Co., Ltd.) was used for the measurement. A value of 5 N / 25 mm or more indicates good adhesive strength, and the higher the value, the better the adhesive strength.
[0135] <Performance evaluation (2): Storage modulus (G')> The pressure-sensitive adhesive sheets (1) to (14) and (C1) to (C12) were subjected to a commercially available measuring device (product name: "MCR302", manufactured by Anton Paar) to measure their dynamic viscoelasticity under the following conditions. From the measurement results, the storage modulus G' at 20°C and 1 Hz was calculated. 5 A storage modulus of more than Pa indicates a high storage modulus. The cured product obtained from the active energy ray-curable pressure-sensitive adhesive composition of Comparative Example 2 had poor step conformability (described below) due to an excessively high storage modulus, while the cured product obtained from the active energy ray-curable pressure-sensitive adhesive composition of Comparative Example 11 had poor cuttability due to a low storage modulus. (Measurement conditions) Deformation mode: Torsion Measurement frequency: 1Hz Distortion: 0.01~1% AUTO setting Heating rate: 3℃ / min Measurement temperature: 0~100℃ Shape: Parallel plate 8.0mmφ
[0136] <Performance evaluation (3): Step-following ability> The same laminate film as in Evaluation Example 1-1 (1) was produced, and the light release treated polyester film was peeled off, and instead, a 50 μm thick polyester film (product name: "Cosmoshine A-4300", manufactured by Toyobo Co., Ltd.) was attached with a 2 kg roller and left to stand for 2 hours. Next, a test piece of 8 cm x 8 cm was cut from this, and the heavy release treated polyester film was peeled off to produce a single-sided adhesive sheet (Cosmoshine A-4300 / adhesive layer). A polyester film piece (5 cm x 5 cm x 50 μm) was placed on a glass plate (10 cm x 10 cm x 2 mm), and a single-sided adhesive sheet (adhesive layer / Cosmoshine A-4300) (5 cm x 5 cm x 150 μm) was placed on top of that, and the laminate (Cosmoshine A-4300 (50 μm thick) / adhesive layer (600 μm thick) / polyester film piece (50 μm thick) / glass plate (2 mm thick)) was produced by adhering it with a 2 kg roller, and evaluated under a condition of 20°C. The step-following ability of the adhesive layer in this state was visually evaluated according to the following criteria. The laminate films (2) to (14) of Evaluation Examples 1-2 to 1-14 and the laminate films (C1) to (C12) of Comparative Evaluation Examples 1-1 to 1-12 were also evaluated in the same manner. AA: No lifting was observed along any side of the polyester film piece, and no air bubbles were observed. A: No lifting is observed along each side of the polyester film piece, but up to 5 tiny air bubbles can be seen. B: Wide floating areas are observed along each side of the polyester film piece, and multiple large bubbles as well as fine bubbles can be seen.
[0137] <Performance rating (4): Color (b*)> The pressure-sensitive adhesive sheets (1) to (14) and (C1) to (C12) are measured in accordance with JIS Z 8781-4:2013 using a commercially available measuring device (product name: "Spectrophotometer SE6000", manufactured by Nippon Denshoku Industries Co., Ltd.), and the color difference is measured according to the basic coordinate method. * was calculated.
[0138] <Performance evaluation (5): Durability (after humidity and heat resistance test)> The laminates (1) to (14) and (C1) to (C12) were left to stand in a thermohygrostat at a temperature of 85° C. and a humidity of 85% for 500 hours, and then the durability of the adhesive layer was evaluated according to the following criteria. A: No peeling of the base material, no deviation of the adhesive layer position, no whitening in the adhesive layer, no air bubbles, and no damage to the adhesive layer. B: At least one of the following defects occurs: peeling of the base material, misalignment of the adhesive layer, whitening in the adhesive layer, air bubbles, or damage to the adhesive layer.
[0139] <Performance evaluation (6): Durability (after light resistance test)> The laminates (1) to (14) and (C1) to (C12) were subjected to 50 mW / cm 2 After leaving the sample in the SUV (product name: "Super Accelerated Light Fastness Tester Metal Weather" manufactured by Daipla Wintes Co., Ltd.) for 100 hours, the sample was measured in accordance with JIS Z 8781-4:2013 using a commercially available measuring device (product name: "Spectrophotometric Color Difference Meter SE6000" manufactured by Nippon Denshoku Industries Co., Ltd.) to determine the b before the test. * The change from the value (Δb*) was calculated.
[0140] [Table 3]
[0141] [Table 4]
[0142] The terms in Tables 3 and 4 have the following meanings: *1: The amounts used (mass %) listed in the table are the ratios when the total mass of components (A), (B), and (C) (components (c1) and (c2)) is taken as 100 mass %. Additionally, the mass % of component (A) does not include the 2-EHA solution. The 2-EHA solution of component (A) is included in the mass % of 2-EHA of component (c1). *2: The amount (mass%) of component (D) used is the ratio when the total mass of components (A), (B), and (C) is 100 mass%. *3: Measurement was not possible because the adhesive sheet portion of the laminate was destroyed after being left stationary for 100 hours during the light resistance test. 4HBA: 4-hydroxybutyl acrylate (product name: "4-HBA", manufactured by Osaka Organic Chemical Industry Co., Ltd.) HEA: 2-hydroxyethyl acrylate (product name: "HEA", manufactured by Osaka Organic Chemical Industry Co., Ltd.) 2EHA: 2-Ethylhexyl acrylate (product name: "2-Ethylhexyl acrylate", manufactured by Mitsubishi Chemical Corporation, Tg: -70°C) NOAA: n-octyl acrylate (product name: "NOAA", manufactured by Osaka Organic Chemical Industry Co., Ltd., Tg: -65°C) IBXA: Isobornyl acrylate (product name: "IBXA", manufactured by Osaka Organic Chemical Industry Co., Ltd., Tg: 97°C) FA-513AS: Dicyclopentanyl acrylate (product name: "FA-513AS", manufactured by Resonac Holdings, Inc., Tg: 120°C) L200: 1-Hydroxycyclohexyl phenyl ketone (product name: "Lunacure 200", manufactured by DKSH Japan Co., Ltd.)
Claims
1. (A) (a1) a linear aliphatic hydrocarbon group-containing polyether polyol, (a2) a polyisocyanate, and (a3) a polyurethane which is a reaction product of a hydroxyl group-containing mono(meth)acrylate and / or an isocyanate group-containing mono(meth)acrylate, (B) a primary hydroxyl group-containing mono(meth)acrylate; (C) a mono(meth)acrylate having no hydroxyl group, The component (C) contains (c1) a (meth)acrylate having a glass transition temperature of less than −5° C. when made into a homopolymer and / or (c2) a (meth)acrylate having a glass transition temperature of −5° C. or higher when made into a homopolymer, the amount of the component (a1) is 35 to 70 mol %, the amount of the component (a2) is 25 to 60 mol %, and the amount of the component (a3) is 1 to 20 mol %, relative to 100 mol % in total of the components (a1), (a2), and (a3); The active energy ray-curable pressure-sensitive adhesive composition contains 10 to 40 mass% of the component (A), 20 to 35 mass% of the component (B), 20 to 40 mass% of the component (c1), and 10 to 25 mass% of the component (c2) relative to 100 mass% (solid content) of the total amount of the components (A), (B), and (C).
2. A cured product of the active energy ray-curable pressure-sensitive adhesive composition according to claim 1.
3. A pressure-sensitive adhesive sheet having the cured product according to claim 2 on at least one surface of a substrate.
Citation Information
Patent Citations
Ultraviolet-curable adhesive composition
JP2016186007A
Ultraviolet-curable adhesive, cured product, and adhesive sheet
JP2018100403A
Active energy ray-curable adhesive composition, cured product and adhesive sheet
JP2020037689A
UV-curing adhesive composition and adhesive
JP6132140B2