Rubber composition incorporating preformed natural rubber-carbon black composite material
A rubber composition combining a carbon black composite with a conjugated diene elastomer and sulfur-based curative addresses the balance of rolling resistance, tear, and tread wear challenges, enhancing tire performance.
Patent Information
- Application Number
- JP2024051513
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
Existing rubber compositions for tires face a challenge in maintaining a balance between rolling resistance, tear characteristics, and tread wear without significant trade-offs.
A rubber composition incorporating at least 20 phr of a composite material with reinforcing carbon black dispersed in natural rubber, combined with a conjugated diene elastomer, a cure activator, and a sulfur-based curative, which together provide at least 90 phr of vulcanizable elastomer, optionally including reinforcing fillers like silica, to enhance performance.
The composition achieves improved rolling resistance and tear characteristics while minimizing adverse effects on tread wear, expanding the 'performance triangle' of tire properties.
Smart Images

Figure 2024144343000001 
Figure 2024144343000002 
Figure 2024144343000003
Abstract
Description
[Technical field]
[0001] Aspects of the exemplary embodiments relate to compositions suitable for use in various tire components, such as tire treads, substrates, and wire coatings, and in particular compositions incorporating preformed natural rubber-carbon black composites in addition to conventional forms of natural rubber. [Background technology]
[0002]
[0002] Tire treads are typically formed from natural rubber or other elastomers blended with various additives, such as fillers and curing aids, prior to the addition of a sulfur-based curative, such as elemental sulfur. Such blend ingredients are often selected to improve performance indicators related to tread wear and tire mileage. There is often a trade-off between improved tread wear and mileage and other parameters, such as tear and rolling resistance.
[0003]
[0003] US Patent No. 8,536,262 B2 describes an inner tread rubber layer of a tire formed from a rubber containing a minor amount of syndiotactic-1,2-polybutadiene and a major amount of at least one of a polymer or copolymer of isoprene and / or 1,3-butadiene, and a copolymer of styrene and isoprene and / or 1,3-butadiene. The composition further includes a blend of rubber reinforcing carbon black fillers having iodine absorption values (ASTM D2515) of about 20 to about 50 g / kg and 100 to about 300 g / kg, respectively. The inner tread rubber layer is disposed between the tire cap and the carcass and is designed to substantially maintain the hysteresis properties of the rubber and promote tire handling while reducing the tendency for internal heat to build up during tire use. The addition of an extra tread layer, although beneficial, may increase the cost or time to build the tire.
[0004]
[0004] More recently, elastomeric composites containing natural rubber latex and carbon black have been developed for use in tire compositions, such as those described in U.S. Patent Nos. 9,156,955 B2 and 10,767,028 B2. The composites can be mixed with curatives and other additives to produce compositions suitable for forming, for example, tire treads. However, such composites tend to offer a limited range of properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Patent No. 8,536,262B2 [Patent Document 2] U.S. Patent No. 9,156,955B2 [Patent Document 3] U.S. Patent No. 10,767,028B2 [Patent Document 4] US Publication No. 20100071817A1 [Patent Document 5] US Publication No. 20150105491A1 [Patent Document 6] U.S. Patent No. 5,587,416A [Patent Document 7] U.S. Patent No. 5,800,608A [Patent Document 8] U.S. Patent No. 5,882,617A [Patent Document 9] U.S. Patent No. 9,359,215B2 [Patent Document 10] US Publication No. 20020081247A1 [Patent Document 11] US Publication No. 20050032965A1 [Patent Document 12] U.S. Patent No. 5,708,069 [Patent Document 13] U.S. Patent No. 7,550,610 [Patent Document 14] U.S. Patent No. 5,789,514 [Patent Document 15] U.S. Patent No. 6,322,811 [Patent Document 16] U.S. Patent No. 4,082,703 [Non-patent literature]
[0006] [Non-Patent Document 1] Gruber et al., "Raman Studies of Heat-Treated Carbon Blacks," Carbon, Vol. 32 (No. 7), pp. 1377-1382 (1994) [Non-Patent Document 2] The Vanderbilt Rubber Handbook (1978), pp. 344-347 [Non-Patent Document 3] The Vanderbilt Rubber Handbook (1978), pp. 346 and 347 Summary of the Invention [Problem to be solved by the invention]
[0007]
[0005] A need remains for rubber compositions formed from composites that can maintain the rolling resistance and tear characteristics of tires formed from the cured compositions without unduly affecting tread wear. [Means for solving the problem]
[0008] According to one aspect of the exemplary embodiment, the rubber composition includes at least 20 phr of a composite material, at least 3 phr of a conjugated diene elastomer, a cure activator, and a sulfur-based curative. The composite material includes reinforcing carbon black dispersed in natural rubber. The composite material and the conjugated diene elastomer together provide at least 90 phr of vulcanizable elastomer in the rubber composition.
[0009]
[0007] The rubber composition may further comprise a reinforcing filler other than carbon black. The reinforcing filler may comprise silica. The rubber composition may comprise at least 5 phr, or at least 8 phr, of silica, or up to 30 phr, or up to 18 phr of silica.
[0010] The composite may provide a rubber composition having at least 20 phr of reinforcing carbon black, or at least 30 phr, or up to 80 phr, or up to 55 phr of reinforcing carbon black. The composite may provide a rubber composition having at least 50 phr of natural rubber, or at least 70 phr, or up to 95 phr, or up to 90 phr of natural rubber. The composite may be solid at 21° C. and atmospheric pressure.
[0011] The conjugated diene elastomer may comprise at least one of natural rubber and synthetic polyisoprene. The rubber composition may comprise at least 5 phr of the conjugated diene elastomer, or at least 10 phr, or up to 50 phr, or up to 30 phr of the conjugated diene elastomer.
[0012] The cure activator may be selected from the group consisting of fatty acids, zinc oxide, and mixtures thereof. The rubber composition may further comprise at least 0.1 phr of at least one processing aid selected from the group consisting of resins, oils, and mixtures thereof.
[0013] The rubber composition may further comprise at least 1 phr of at least one of an antioxidant and an antiozonant, and / or at least 0.5 phr of a cure accelerator, and / or at least 0.05 phr of a cure inhibitor.
[0014] The composite material and the conjugated diene elastomer together can provide at least 98 phr of vulcanizable elastomer in the rubber composition. In another aspect of the exemplary embodiment, an article is formed from the rubber composition of any of the aspects described above. The article can include a tire tread.
[0015] In another aspect of the exemplary embodiment, a method of forming a rubber composition includes blending a composite material with a conjugated diene elastomer at a temperature of at least 115° C. to form a mixture. The composite material includes reinforcing carbon black dispersed in natural rubber. The composite material and the conjugated diene elastomer together provide at least 90 phr of a total of 100 phr of vulcanizable elastomer. The mixture is blended with a sulfur-based curative to form the rubber composition.
[0016] In the method, the mixture may further include silica.
[0017] The method may further include curing the rubber composition to form a shaped article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017]
[0018] An aspect of the exemplary embodiment relates to a rubber composition adapted for use in forming molded or extruded articles, and articles formed from the composition, such as tire treads, etc. The composition includes a preformed composite material, a conjugated diene-based elastomer, a reinforcing filler, such as silica, a sulfur-based curative, and optionally one or more of processing aids, such as oils and waxes, coupling agents, antioxidants, antiozonants, other components of a sulfur-based cure package, such as cure activators, cure accelerators, and cure inhibitors, and other additives known in the art.
[0018]
[0019] An exemplary composite material includes natural rubber and carbon black as major components. Combination of the composite material with a separate conjugated diene-based rubber results in a cured rubber composition having a multiphase morphology in which the carbon black is non-uniformly dispersed throughout the rubber composition, which provides good rolling resistance and tear characteristics for the tire without unduly affecting treadwear.
[0019]
[0020] In the description of the invention, the term "phr" refers to parts by weight of a respective material per 100 parts by weight of rubber or elastomer. The term "phf" refers to parts by weight per 100 parts by weight of filler. By convention, the uncured rubber utilized in a sealant composition totals 100 phr.
[0020]
[0021] The terms "rubber" and "elastomer" can be used interchangeably unless otherwise noted. The terms "cure" and "vulcanize" can be used interchangeably unless otherwise noted.
[0021]
[0022] As used herein, Mooney viscosity (ML1+4) is measured in MU at 100° C. according to ASTM D1646-19a, “Standard Test Methods for Rubber-Viscosity, Stress Relaxation, and Pre-Vulcanization Characteristics (Mooney Viscometer).”
[0022]
[0023] The glass transition temperature (Tg) of an elastomer or elastomeric composition referred to herein refers to the glass transition temperature of the respective elastomer or elastomeric composition in its uncured state, or, in the case of an elastomeric composition, possibly in its cured state. The Tg values referred to herein are those determined as the peak midpoint by differential scanning calorimetry (DSC) at a temperature rate of increase of 10° C. per minute, in accordance with ASTM D3418-21, "Standard Test Method for Transition Temperatures and Enthalpies of Fusion and Crystallization of Polymers by Differential Scanning Calorimetry."
[0023] composite material
[0024] The composite material includes natural rubber and reinforcing carbon black, the reinforcing carbon black being dispersed in the natural rubber, hi one embodiment, the natural rubber and carbon black together comprise at least 90% by weight, or at least 95% by weight, or at least 98% by weight, or up to 100% by weight of the composite material.
[0024]
[0025] In one embodiment, the composite material has a Mooney viscosity of 100 M.U. or less, or 85 M.U. or less, or at least 60 M.U. The composite material may be a solid or a flowable liquid at room temperature (21° C.) and atmospheric pressure. In another embodiment, the composite material may be in the form of a solid, e.g., strip or crumb, at room temperature.
[0025]
[0026] The composite is non-vulcanized and free of sulfur-based and organic peroxide curatives. The composite may also be free of reinforcing fillers other than carbon black, and free of cure accelerators, cure activators, and cure inhibitors, examples of which are described below.
[0026]
[0027] The composite material can be used in an amount of at least 20 phr, or at least 30 phr, or at least 50 phr, or at least 80 phr, or at least 100 phr, or up to 160 phr, or up to 150 phr, or up to 140 phr in the rubber composition. The elastomer content (mainly natural rubber) in the composite material contributes a total of 100 phr of elastomer in the rubber composition. Thus, the maximum phr of the composite material in the rubber composition depends, at least in part, on its rubber content. For example, the composite material can provide at least 10 phr, or at least 20 phr, or at least 50 phr, or at least 60 phr, or at least 70 phr, or at least 80 phr, or up to 95 phr, or up to 90 phr of total elastomer in the rubber composition.
[0027]
[0028] The composite may contribute at least 10 phr, or at least 15 phr, or at least 20 phr, or at least 30 phr, or at least 40 phr, or up to 80 phr, or up to 60 phr, or up to 50 phr of carbon black to the rubber composition.
[0028]
[0029] The weight ratio of carbon black to natural rubber in the composite may be at least 20:80, or at least 30:70, or up to 50:50, or up to 40:60, for example, about 35:65.
[0029]
[0030] The carbon black in the composite may be a single reinforcing carbon black or may include two or more different types of carbon black.
[0030]
[0031] Carbon blacks useful in composites have a molecular weight of 15 mm or less as determined in accordance with ASTM D6556-21, "Standard Test Method for Carbon Black-Total and External Surface Area by Nitrogen Adsorption." 2 / g~300m 2 / g, or at least 40m 2 Exemplary carbon blacks include the ASTM designations N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990, and N991, as identified by ASTM D1765-21, "Standard Classification System for Carbon Blacks Used in Rubber Products."
[0031]
[0032] A mixture of two or more forms of carbon black can be utilized. One example of a composite suitable for use herein includes two types of carbon black and is described in U.S. Patent No. 10,767,028 B2. Other composites with different carbon blacks are described in U.S. Publication No. 20100071817 A1.
[0032]
[0033] In one embodiment, the carbon black is pretreated, for example with silicon, prior to forming the composite. One exemplary silicon-treated carbon black is available from Cabot Corporation as CRX™ 2000 ECOBLACK®.
[0033]
[0034] Exemplary composite materials including carbon black and natural rubber are available from Cabot Corporation as Engineered Elastomer Composites (E2C™), e.g., E2C™ DX9620 and E2C™ DX9640. E2C™ DX9620 has a Mooney viscosity ML(1+4) of about 69 M.U. at 100° C., a modulus of elasticity at 300% of about 17.0 MPa, a tensile strength of about 29.8 MPa, an elongation at break of about 528%, and a tan δ of about 0.130 at 60° C. E2C™ DX9640 has a Mooney viscosity of about 84 M.U., a modulus of elasticity at 300% of about 18.5 MPa, a tensile strength of about 30.1 MPa, an elongation at break of about 473%, and a tan δ of about 0.15 at 60° C.
[0034]
[0035] When two or more forms of carbon are used, the first carbon black in the composite can acquire a more crystalline structure than the second carbon black by heat treating at a temperature between 1100° C. and 1800° C. The partially crystallized first carbon black has an oil absorption number of 120 cm−1 or less as determined in accordance with ASTM D2414-22, “Standard Test Method for Carbon Black-Oil Absorption Number (OAN).” 3 / 100g~200cm 3 / 100 g OAN structure and a Raman crystallite plane size (La) of 25 Å to 50 Å, as determined using the method of Gruber et al., "Raman Studies of Heat-Treated Carbon Blacks," Carbon, Vol. 32(No. 7), pp. 1377-1382 (1994).
[0035]
[0036] In one particular embodiment, the carbon black has an average molecular weight of at least 95 mm as measured by STSA. 2 / g and a dibutyl phthalate adsorption of greater than 80 mL / 100 g, and the composite material comprises at least 65 phr of carbon black. In another particular embodiment, the carbon black has an external surface area of at least 75 m as measured by STSA. 2 / g surface area and dibutyl phthalate adsorption of greater than 60 mL / 100 g, and the composite material comprises at least 70 phr of carbon black. * S+94, where L is the amount of carbon black in the composite in phr and S is the surface area of the carbon black as measured by STSA in m 2 / g) These and other suitable composite materials are described, for example, in U.S. Publication No. 20150105491A1.
[0036]
[0037] While the composite material can consist essentially of carbon black and natural rubber (e.g., the two materials together are at least 95% or at least 98% or up to 100% by weight of the composite material), it is also contemplated that the composite material can include other constituent materials. For example, in one embodiment, 2-25%, or up to 15%, or up to 8% by weight of the composite can be composed of other rubber-forming elastomers. These other elastomers can include other conjugated diene elastomers, such as synthetic cis-1,4-polyisoprene, polybutadiene, butadiene copolymers, isoprene copolymers, and mixtures of these elastomers. Suitable copolymers are selected from the group consisting of butadiene / styrene copolymers, isoprene / butadiene copolymers, isoprene / styrene copolymers, and isoprene / butadiene / styrene copolymers.
[0037]
[0038] The composite material can be formed by mixing the carbon black with the natural rubber at an appropriate temperature (e.g., at least 100°C, or at least 120°C) for a sufficient time to achieve a highly dispersed mixture. In one embodiment, the carbon black is added to the natural rubber as a slurry and a coagulant, e.g., an acid, is used to coagulate the mixture. Such a method is described in U.S. Pat. No. 9,156,955 B2. A slurry can be formed by mixing the carbon black with water, which can be milled to improve dispersion, for example, as described in U.S. Publication No. 20150105491 A1.
[0038] Conjugated Diene-Based Elastomers
[0039] The conjugated diene based elastomer (not forming part of the composite) may be present in the rubber composition in an amount of at least 3 phr, or at least 5 phr, or at least 6 phr, or at least 8 phr, or at least 10 phr, or at least 12 phr, and / or up to 90 phr, or up to 80 phr, or up to 60 phr, or up to 40 phr, or up to 30 phr, or up to 20 phr, or up to 16 phr, for example, in the range of 10 to 30 phr.
[0039]
[0040] In one embodiment, the weight ratio of conjugated diene-based elastomer to natural rubber present in the composite is at least 5:95, or at least 6:94, or at least 10:90, or at least 12:88, or up to 30:70, or up to 25:75, or up to 20:80.
[0040]
[0041] Conjugated diene-based elastomers consist of one or more elastomers derived solely or predominantly (e.g., at least 60% by weight, or at least 90% by weight, or at least 95% by weight) from conjugated dienes. For example, conjugated diene-based elastomers can be selected from natural rubber, synthetic polyisoprene, polybutadiene, and mixtures and copolymers thereof. All of these elastomers contain double bonds in each monomer unit.
[0041]
[0042] Natural rubber is derived primarily from isoprene (2-methyl-1,3-butadiene) and is therefore primarily (e.g., at least 99% by weight) polyisoprene. As used herein, the term "natural rubber" means that rubber of natural origin can be collected from sources such as the Hevea rubber tree, as well as from non-Hevea sources (e.g., guayule shrub and dandelion, e.g., TKS). In other words, the term "natural rubber" should be interpreted to exclude synthetic polyisoprene. Natural rubber produced from field grade coagulum (cup lumps) obtained from Hevea brasiliensis trees is a common form of natural rubber. For example, technically specified rubber or block rubber (TSR) is natural rubber available from Indonesia, where it may also be called standard Indonesian rubber (SIR), Malaysian (SMR), and Thai (STR). This natural rubber can be obtained in several grades, including TSR10 and TSR20, with the TSR10 grade having a higher purity.
[0042]
[0043] In one embodiment, the conjugated diene based elastomer is at least 60% by weight natural rubber, or at least 80% by weight, or at least 90% by weight, or at least 95% by weight, or up to 100% by weight natural rubber.
[0043]
[0044] In some embodiments, synthetic polyisoprene, particularly cis-1,4-polyisoprene having a cis content of at least 94% by weight, or at least 96% by weight, can be used for the conjugated diene based elastomer. The Tg of the synthetic polyisoprene can range from -60°C to -70°C. In one embodiment, a mixture of synthetic polyisoprene and natural rubber is used as the conjugated diene based elastomer.
[0044]
[0045] Other conjugated diene-based elastomers which may optionally be present in minor amounts (e.g., up to a total of 10 phr, or up to 5 phr, or up to 2 phr) can include one or more of butadiene rubber (BR), isoprene-isobutylene copolymers, and halobutyl rubbers, such as bromobutyl rubber and chlorobutyl rubber.
[0045] Other vulcanizable elastomers
[0046] Apart from the natural rubber present in the composite and the conjugated diene based elastomers, other vulcanizable elastomers may be present in the rubber composition in minor amounts (e.g., up to a total of 10 phr, or up to 5 phr, or up to 2 phr), and these include nitrile rubber, liquid rubber, polynorbornene copolymer, ethylene-propylene-diene rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrated acrylonitrile butadiene rubber, isoprene- Butadiene copolymers, butyl rubber, hydrogenated styrene-butadiene rubber, butadiene acrylonitrile rubber, terpolymers formed from ethylene monomer, propylene monomer, and / or ethylene propylene diene monomer (EPDM), isoprene-based block copolymers, butadiene-based block copolymers, styrenic block copolymers, styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-[ethylene-(ethylene / propylene [styrene]-styrene block copolymers (SEEPS), styrene-isoprene-styrene block copolymers (SIS), random styrene copolymers, hydrogenated styrenic block copolymers, styrene butadiene copolymers, polyisobutylene, ethylene vinyl acetate (EVA) polymers, polyolefins, amorphous polyolefins, semi-crystalline polyolefins, alpha-polyolefins, reactor-ready polyolefins, acrylates, metallocene-catalyzed polyolefin polymers and elastomers, reactor-made thermoplastic polyolefin elastomers, olefin block copolymers, copolyester block copolymers, polyurethane block copolymers, polyamide block copolymers, thermoplastic polyolefins, thermoplastic vulcanizates, ethylene vinyl acetate copolymers, ethylene n-butyl acrylate copolymers, ethylene methyl acrylate copolymers, neoprene, acrylic acid, urethanes, poly(acrylates), ethylene acrylic acid copolymers, polyether ether ketones, polyamides, atactic polypropylene, polyethylene including atactic polypropylene,Ethylene-propylene polymers, propylene-hexene polymers, ethylene-butene polymers, ethylene-octene polymers, propylene-butene polymers, propylene-octene polymers, metallocene-catalyzed polypropylene polymers, metallocene-catalyzed polyethylene polymers, ethylene-propylene-butylene terpolymers, copolymers made from propylene, ethylene, C4-C, 10 The polymer may be selected from alpha-olefin monomers, polypropylene polymers, maleated polyolefins, polyester copolymers, copolyester polymers, ethylene acrylic acid copolymers, and / or polyvinyl acetate, and mixtures thereof, and / or the polymer optionally includes modifications and / or functionalizations selected from one or more of hydroxyl-, ethoxy-, epoxy-, siloxane-, amine-, amine siloxane-, carboxy-, phthalocyanine-, and silane-sulfide-groups at the polymer chain ends or pendant positions within the polymer.
[0046]
[0047] In one embodiment, the rubber composition is free of such other vulcanizable elastomers. Reinforcing Fillers
[0048] One or more reinforcing fillers other than the carbon black found in the composite may be present in the rubber composition. Examples of such reinforcing fillers include silica, calcium carbonate (CaCO3), titanium dioxide, hydrated aluminum silicate clays, 2:1 layered silicate clays and organophilic clays formed therefrom, calcium silicate, graphite, graphene, carbon nanotubes, wollastonite, talc, diatomaceous earth, starch, lignin, alumina, another carbon black, e.g., different from the carbon black present in the composite, and mixtures thereof.
[0047]
[0049] The reinforcing fillers may be present in the rubber composition from 0 to 150 phr, for example, at least 2 phr, or at least 4 phr, or at least 6 phr, or at least 8 phr, or up to 100 phr, or up to 80 phr, or up to 50 phr, or up to 20 phr, or up to 15 phr, up to 10 phr, for example, from 5 to 15 phr.
[0048]
[0050] In one embodiment, the reinforcing filler comprises or consists of silica particles, such as amorphous (e.g., precipitated) silica and / or crystalline silica. The term "silica" is used herein to refer to silicon dioxide, SiO2 (which may contain minor impurities, generally less than 1% by weight, generated from the process in which silica is formed). The term "precipitated silica" is used to refer to synthetic amorphous silica, which is usually obtained by a process of precipitation of silicates using an acidifying agent.
[0049]
[0051] Silica may be present in the rubber composition in an amount of at least 2 phr, or at least 4 phr, or at least 6 phr, or at least 8 phr, or up to 100 phr, or up to 80 phr, or up to 50 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, up to 10 phr, for example, from 5 to 15 phr.
[0050]
[0052] Silica can be prepared in a variety of ways. Precipitated silica can be prepared, for example, by digesting amorphous silica found in rice husk or other biological waste with sodium hydroxide to form sodium silicate, and then precipitating silica from the sodium silicate by reaction with an acidifying agent, for example, sulfuric acid or carbon dioxide. The resulting silica precipitate is washed and filtered. Methods for the preparation of precipitated silica are disclosed, for example, in U.S. Pat. No. 5,587,416A, U.S. Pat. No. 5,800,608A, U.S. Pat. No. 5,882,617A, and U.S. Pat. No. 9,359,215B2, as well as U.S. Publication No. 20020081247A1, and U.S. Publication No. 20050032965A1. Precipitated silica can also be formed from silica gel, as described, for example, in U.S. Pat. No. 5,708,069, U.S. Pat. No. 7,550,610, and U.S. Pat. No. 5,789,514. Silica gel can be derived, for example, by hydrophobizing silica hydrogel with, for example, organomercaptosilanes and alkylsilanes, and drying the product.
[0051]
[0053] Various methods are available for determining the surface area of silica. In the ASTM D6845-20 "Standard Test Method for Silica, Precipitated, Hydrated-CTAB(Cetyltrimethylammonium Bromide) Surface Area" test method, the measurement of the specific surface area of silica excludes the area contained by micropores too small to accommodate the CTAB molecules. This test method is suitable for characterizing all types of rubber grade silica.
[0052]
[0054] Silica used in reinforcing fillers must be at least 120m in accordance with ASTM D6845-20. 2 / g, or at least 140m 2 / g, or at least 220m 2 / g, or at least 240m2 The silica can have a CTAB specific surface area of 500 m 2 / g or 400m 2 / g or 300m 2 / g.
[0053]
[0055] Exemplary precipitated silicas suitable for use herein include Hi-Sil™ 532, Hi-Sil™ 532EP, and Hi-Sil™ EZ 160G, manufactured by PPG Industries; Hubersil™ 4155, manufactured by JMHuber Company; Zeosil™, with designations 115GR, 125GR, 165GR, 175GR, 185GR, 195GR, 1085GR, 1165MP, 1115MP, HRS1200MP, Premium MP, Premium 200MP, Premium SW, and 195HR, manufactured by Solvay; Ultrasil™, with the designations VN2, VN3, VN3GR, 5000GR, 6000GR, 7000GR, and 9000GR, manufactured by Evonik; Zeopol™, with the designations 8755LS and 8745, manufactured by Evonik; Newsil™, with the designations 115GR and 2000MP, manufactured by Wuxi Quechen Silicon Chemical Co., Ltd; and Tokusil™ 315, manufactured by Maruo Calcium Co., Ltd, and mixtures thereof.
[0054]
[0056] In one embodiment, silica is present in the rubber composition at 1 phr or more, for example, at least 2 phr, or at least 5 phr, or at least 6 phr, or at least 7 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, or up to 14 phr, or up to 12 phr, or up to 10 phr. Silica may be a reinforcing filler in at least 2 phf, or at least 4 phf, or at least 8 phf, or at least 12 phf, or up to 25 phf, or up to 20 phf, or up to 18 phf.
[0055]
[0057] In one embodiment, the weight ratio of silica to total elastomer (eg, natural rubber) in the rubber composition is at least 4:100, or at least 6:100, and may be up to 20:100, or up to 15:100.
[0056]
[0058] In one embodiment, the weight ratio of silica to carbon black in the rubber composition is at least 4:100, or at least 7:100, or at least 12:100, or at least 15:100, and may be up to 3:10, or up to 2:10.
[0057]
[0059] In one embodiment, the silica may also be surface treated, for example with a coupling agent and / or a polyalkylene oxide, such as polyethylene glycol, prior to incorporation of the pretreated silica into the rubber composition. The pretreatment may function to enhance the dispersion and / or adhesion of the silica to the elastomer. In another embodiment, the silica may be treated in situ in the rubber composition with a coupling agent and / or a polyalkylene oxide, typically prior to addition of the curative.
[0058]
[0060] Polyalkylene glycols that can be used for silica pretreatment or in situ in the rubber composition include polyethylene glycol, polypropylene glycol, and mixtures thereof. In one embodiment, the polyalkylene oxide is polyethylene glycol. The polyalkylene oxide can have a weight average molecular weight Mw of at least 500, for example, at least 2,000, or at least 4,000, or up to 15,000, or up to 12,000, or up to 10,000, or up to 8,500. The polyalkylene oxide may be absent from the rubber composition. When a polyalkylene oxide, such as polyethylene glycol, is utilized, it may be included in an amount of at least 0.1 phr, for example, at least 0.2 phr, or at least 0.3 phr, or up to 5 phr, or up to 3 phr, or up to 2 phr, or up to 1 phr, or up to 0.6 phr.
[0059]
[0061] Examples of commercially available polyethylene glycols include Carbowax™ PEG 3350 and Carbowax™ PEG 8000, manufactured by Dow Chemical Company, where the numbers indicate the approximate weight average molecular weight. Other polyalkylene oxide polymers, such as those described in U.S. Patent No. 6,322,811 and U.S. Patent No. 4,082,703, can also be used.
[0060]
[0062] Suitable coupling agents generally include a first portion, which is reactive with the hydroxyl groups (e.g., silanol groups) present on the surface of the precipitated silica, and a second portion capable of reacting with a diene-based elastomer, for example, natural rubber. The two portions are linked by a linking group, for example, a hydrocarbyl or sulfide-based bridge, so that the precipitated silica is chemically bonded to the elastomer. Examples of silica coupling agents include those containing groups such as alkyl, alkoxy, mercapto, blocked mercapto, sulfide-containing groups (e.g., monosulfide-based alkoxy-containing groups, disulfide-based alkoxy-containing groups, tetrasulfide-based alkoxy-containing groups), amino, vinyl, epoxy, and combinations thereof. The silica coupling agent can be present in an amount sufficient to obtain a weight ratio of the total amount of coupling agent to the silica filler of at least 0.1:100 or up to 1:5, for example, at least 1:100, or at least 1:50, or up to 1:20, or up to 1:10.
[0061]
[0063] Additional reinforcing fillers other than silica and carbon black may be utilized in a total amount of, for example, up to 30 phr, or up to 20 phr, or up to 10 phr, or up to 1 phr, or may be absent. Examples of such additional reinforcing fillers include alumina, aluminum hydroxide, clay (reinforcing grades), magnesium hydroxide, boron nitride, aluminum nitride, titanium dioxide, reinforcing zinc oxide, and combinations thereof.
[0062]
[0064] In one embodiment, the components of the rubber composition other than natural rubber, carbon black, and silica are present in the rubber composition in a total amount of 40 phr or less, or 30 phr or less, or 20 phr or less, or 15 phr or less.
[0063] Processing Aids
[0065] Processing aids can be used in a total amount of 1 to 20.0 phr, or up to 10 phr, or up to 5 phr in the rubber composition and can include one or more of resins and liquid plasticizers, such as oils.
[0064]
[0066] Exemplary resins that can be used in the rubber composition include tackifying resins, such as non-reactive phenol formaldehyde, and stiffening resins, such as reactive phenol formaldehyde resins and resorcinol or resorcinol and hexamethylenetetramine, benzoxazine resins, hydrocarbon resins, such as aromatic, aliphatic, and cycloaliphatic resins.
[0065]
[0067] Exemplary hydrocarbon resins may have a Tg of at least 30° C., or up to 50° C. The hydrocarbon resin Tg may be determined by DSC following the procedure discussed above for measuring elastomer Tg. The hydrocarbon resin may have a softening point of at least 70° C., or up to 100° C. The softening point of a hydrocarbon resin is generally related to its Tg. The Tg is generally lower than its softening point, and the lower the Tg, the lower the softening point.
[0066]
[0068] Examples of aliphatic resins include C5 fraction homopolymer and copolymer resins. Examples of cycloaliphatic resins include cyclopentadiene ("CPD") homopolymer or copolymer resins, dicyclopentadiene ("DCPD") homopolymer or copolymer resins, and combinations thereof.
[0067]
[0069] Examples of aromatic resins include aromatic homopolymer resins and aromatic copolymer resins, which refers to a hydrocarbon resin that includes a combination of one or more aromatic monomers in combination with one or more other (non-aromatic) monomers, with the majority by weight of all monomers generally being aromatic.
[0068]
[0070] Specific examples of aromatic resins include coumarone-indene resins, alkyl-phenol resins, and vinyl aromatic homopolymer or copolymer resins. Examples of alkyl-phenol resins include alkylphenol-acetylene resins, such as p-tert-butylphenol-acetylene resins, alkylphenol-formaldehyde resins (e.g., those with low degrees of polymerization). Vinyl aromatic resins can include one or more of the following monomers: alpha-methylstyrene, styrene, ortho-methylstyrene, meta-methylstyrene, para-methylstyrene, vinyltoluene, para(tert-butyl)styrene, methoxystyrene, chlorostyrene, hydroxystyrene, vinylmesitylene, divinylbenzene, vinylnaphthalene, and the like. Examples of vinyl aromatic copolymer resins include vinyl aromatic / terpene copolymer resins (e.g., limonene / styrene copolymer resins), vinyl aromatic / C5 fraction resins (e.g., C5 fraction / styrene copolymer resins), vinyl aromatic / aliphatic copolymer resins (e.g., CPD / styrene copolymer resins, and DCPD / styrene copolymer resins).
[0069]
[0071] In the case of aromatic resins based on one or more of the vinyl aromatic monomers mentioned above (e.g., styrene, alpha-methylstyrene), at least 80% by weight, or at least 85% by weight, or at least 90% by weight, or at least 95% by weight, or up to 100% by weight of the monomers in the aromatic resin may be aromatic monomers.
[0070]
[0072] Other aromatic resins include terpene resins such as alpha-pinene resins, beta-pinene resins, limonene resins (e.g., L-limonene, D-limonene, dipentene, which is a racemic mixture of L and D isomers), beta-phellandrene, delta-3-carene, delta-2-carene, and combinations thereof.
[0071]
[0073] In one embodiment, the hydrocarbon resin includes a combination of aromatic and aliphatic / cycloaliphatic hydrocarbons. In such cases, the total amount of any aliphatic and / or cycloaliphatic resins used in combination with the aromatic resin may be 5 phr or less, or less than 4 phr, or less than 3 phr, or more than 20 wt. %, or less than 15 wt. %, or less than 10 wt. % of the total amount of hydrocarbon resin.
[0072]
[0074] The aromatic resin can have a Mw of at least 1000 g / mole and / or up to 4000 g / mole.
[0075] The total amount of resin in the rubber composition may be at least 1 phr, or at least 2 phr, or up to 20 phr, or up to 10 phr, or up to 5 phr, or may be absent.
[0073]
[0076] The term liquid plasticizer is used to refer to plasticizer components that are liquid at room temperature (i.e., liquid at 25°C and above), including oils and non-oily. Hydrocarbon resins, in contrast to liquid plasticizers, are generally solid at room temperature. Liquid plasticizers generally have a Tg below 0°C, generally well below 0°C, for example, below -30°C, or below -40°C, or below -50°C, for example, a Tg between 0°C and -100°C.
[0074]
[0077] Suitable liquid plasticizers include oils (e.g., oils of petroleum and vegetable origin) and non-oily liquid plasticizers, such as ether plasticizers, ester plasticizers, phosphate plasticizers, and sulfonate plasticizers. Liquid plasticizers can be added during or after the mixing process as extender oils (used to extend the rubber). Petroleum-based oils can include aromatic, naphthenic, lower polycyclic aromatic (PCA) oils, and mixtures thereof. Vegetable oils can include oils collected from plants, nuts, seeds, and mixtures thereof, such as triglycerides. The Tg of the oils used can be from -40°C to -100°C.
[0075]
[0078] If present, the rubber composition may contain at least 1 phr of liquid plasticizer, or up to 20 phr, or up to 10 phr, or up to 5 phr of liquid plasticizer. In one embodiment, no liquid plasticizer is utilized.
[0076]
[0079] In addition to one or more of the above processing aids, the rubber composition may include a peptizer, such as pentachlorothiophenol, dibenzamidodiphenyl disulfide, or mixtures thereof. If used, typical amounts of peptizers may range from 0.1 phr to 1 phr. Degradation inhibitors (antioxidants, antiozonants)
[0080] The rubber composition may include one or more anti-aging agents, such as antiozonants and / or antioxidants. These compounds help protect tires from oxidation and ozone oxidation. Representative anti-aging agents include amine-based antioxidants, such as monophenols, bisphenols, thiobisphenols, polyphenols, polymeric hindered phenols, hydroquinone derivatives, phosphites, phosphate blends, thioesters, naphthylamines, diphenolamines and other diarylamine derivatives, para-phenylenediamines (PPDs), quinolines, and blended amines. Exemplary amine-based antioxidants include diphenyl-p-phenylenediamines, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamines (6PPDs), oligomerized 2,2,4-trimethyl-quinolines (TMQs), and others, such as those disclosed in The Vanderbilt Rubber Handbook (1978), pages 344-347. The antioxidant may comprise at least 0.1 phr, or at least 0.3 phr, or at least 1 phr, or at least 2 phr, or up to 10 phr, or up to 5 phr of the rubber composition.
[0077]
[0081] Exemplary antiozonants include physical protectants, such as waxes. Suitable waxes include paraffin waxes and microcrystalline waxes, which may be of the type described in The Vanderbilt Rubber Handbook (1978), pages 346 and 347. Waxes may be present at 0.1 phr or more, such as at least 0.3 phr, or at least 0.5 phr, or up to 5 phr, or up to 2 phr.
[0078] Hardening Package Vulcanizing Agent
[0082] Exemplary cure packages include a vulcanizing (curing) agent and one or more of a cure accelerator, a cure activator, and a cure inhibitor. The cure package can be used at 0.5 to 20 phr, or at least 5 phr, or up to 10 phr in the rubber composition.
[0079]
[0083] The vulcanization of the rubber composition can be carried out in the presence of a sulfur-based vulcanizing agent. Examples of suitable sulfur-based vulcanizing agents include elemental sulfur (free sulfur), insoluble polymeric sulfur, soluble sulfur, and sulfur-donating vulcanizing agents such as amine disulfides, polymeric polysulfides, or sulfur olefin adducts, and mixtures thereof.
[0080]
[0084] Sulfur vulcanizing agents can be used in the rubber composition in an amount of from 0.1 to 10 phr, for example, at least 0.3 phr, or at least 0.4 phr, or at least 0.5 phr, or at least 0.7 phr, or up to 5 phr, or up to 3 phr.
[0081] Curing accelerators, curing activators, curing inhibitors
[0085] The cure accelerator acts as a catalyst for the vulcanizing agent. Suitable cure accelerators include amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates, and xanthates. Examples of thiazole cure accelerators include 2-mercaptobenzothiazole and 2,2'-dithiobis(benzothiazole) (MBTS). Examples of sulfenamide cure accelerators include benzothiazole sulfenamides, such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS), and N-tert-butyl-2-benzothiazole-sulfenamide (TBBS). Guanidine cure accelerators include diphenylguanidine (DPG).
[0082]
[0086] Cure accelerators that have a fast vulcanization onset time, referred to as a "t0," of less than 3 minutes are called ultraaccelerators. Exemplary ultraaccelerators that can be used include 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane (BDBZTH), tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram monosulfide (TMTM), tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetraisobutylthiuram disulfide (TiBTD), dipentamethylenethiuram tetrasulfide (DPTT), zinc dibutyldithiocarbamate (ZDBC), zinc diethyldithiocarbamate, zinc dimethyldithiocarbamate, copper dimethyldithiocarbamate, tellurium diethyldithiocarbamate (TDEC), dibenzyldithiocarbamate, zinc dimethyl ... Zinc carbamate (ZBED), zinc diisononyldithiocarbamate, zinc pentamethylenedithiocarbamate, zinc dibenzyldithiocarbamate (ZBEC), zinc isopropylxanthate (ZIX), zinc butylxanthate (ZBX), sodium ethylxanthate (SEX), sodium isobutylxanthate (SIBX), sodium isopropylxanthate (SIPX), sodium n-butylxanthate (SNBX), sodium amylxanthate (SAX), potassium ethylxanthate (PEX), potassium amylxanthate (PAX), zinc 2-ethylhexylphosphorodithioate (ZDT / S), and mixtures thereof.
[0083]
[0087] In some cases, a combination of enhancers is used, one acting faster than the other.
[0088] The accelerator may be incorporated in the rubber composition at 0.1 to 10 phr, or at least 0.5 phr, or at least 1 phr, or at least 2 phr, or up to 8 phr, or up to 5 phr. The amount of accelerator may be selected to obtain an acceptable cure time, for example, up to 90 minutes.
[0084]
[0089] Cure activators are additives used to support vulcanization. Cure activators include both inorganic and organic cure activators. Zinc oxide is a widely used inorganic cure activator, and when used, may be present at 1 phr to 10 phr, for example, at least 2 phr, or up to 5 phr.
[0085]
[0090] Organic cure activators include stearic acid, palmitic acid, lauric acid, mixtures thereof, the zinc salts of each of the foregoing, and thiourea compounds such as thiourea, and dihydrocarbylthioureas, such as dialkylthioureas and diarylthioureas, and mixtures thereof. Specific thiourea compounds include N,N'-diphenylthiourea, trimethylthiourea, N,N'-diethylthiourea (DEU), N,N'-dimethylthiourea, N,N'-dibutylthiourea, ethylenethiourea, N,N'-diisopropylthiourea, N,N'-dicyclohexylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1,1-diphenyl-2-thiourea, 2,5-dithiobiurea, guanylthiourea, 1-(1-naphthyl)-2-thiourea, 1-phenyl-2-thiourea, p-tolylthiourea, and o-tolylthiourea. One commonly used organic cure activator is a blend of stearic acid, palmitic acid, and oleic acid, with stearic acid being the major component of the blend.
[0086]
[0091] If used, the total amount of organic cure activators may be from 0.1 to 6 phr, such as at least 0.5 phr, or at least 1 phr, or up to 4 phr.
[0092] Cure inhibitors control the vulcanization process and are generally used to slow or inhibit vulcanization until a desired time and / or temperature has been reached. Exemplary cure inhibitors include cyclohexylthiophthalimide.
[0087]
[0093] If used, the amount of set inhibitor may be at least 0.1 phr, or up to 3 phr, or up to 2 phr. Exemplary Compositions
[0100] Table 1 illustrates exemplary rubber compositions according to aspects of the exemplary embodiment.
[0088] [Table 1]
[0089] Preparation of Rubber Composition
[0101] The rubber composition can be prepared by mixing the composite, natural rubber, and / or other vulcanizable elastomers, if used, silica, and other rubber mixing ingredients (without curatives) with at least one mechanical mixer under high shear rubber mixing conditions up to an elevated temperature in at least one successive mixing step, commonly referred to as a "non-productive" mixing step, followed by a final "productive" mixing step in which a sulfur-based cure package, e.g., sulfur-based curatives and cure accelerators, are added to the mixture and mixed at a lower mix temperature to avoid unnecessarily pre-curing the rubber mixture during the mixing steps.
[0090]
[0102] The components can be mixed in a non-productive mix step to a temperature of 115°C to 150°C, e.g., about 124°C, for several minutes. Once the curing package has been added, the subsequent productive mix step can be carried out at a temperature below the vulcanization (cure) temperature, e.g., below 180°C, or up to 160°C, or up to 120°C, e.g., at least 40°C, or at least 60°C, e.g., at a temperature of 100-115°C for 2 minutes to avoid undesirable pre-curing of the rubber composition. Mixing can be carried out, for example, by kneading the components together in a Banbury mixer or on a mill roll. The rubber composition can be cooled to a temperature below 40°C between each of the mixing steps. For example, the rubber composition can be removed from the mixer after each mixing step, sheeted off an open mill, and allowed to cool to below 40°C after each mixing step.
[0091]
[0103] Once the curing package is thoroughly mixed, the rubber composition can be extruded, molded, or otherwise shaped to form an article, such as a tire tread. The temperature of the mixture can be raised to effect the curing. Curing of the pneumatic tire or parts thereof can be carried out at 120°C to 200°C, such as at least 140°C, or up to 180°C, or about 150°C. Any of the conventional vulcanization processes can be used, such as heating in a press or mold, or heating with superheated steam or hot air. Such tires can be built, molded, shaped, and cured by a variety of methods that are known and readily apparent to those skilled in the art.
[0092]
[0104] In one embodiment, a tire is provided having a tread formed at least in part from the exemplary rubber composition. Other portions of the tire, such as the tire sidewall, or wire coating, may additionally or alternatively be formed at least in part from the rubber composition described herein. The tire may be for an on-road vehicle, such as a pneumatic tire for an automobile or truck, or for an off-road vehicle, such as an airplane. The tire tread may have a tread depth of at least 20 mm, such as 22 to 28 mm, suitable for use on trucks.
[0093]
[0105] The rubber compositions are not limited to use in tires, but may also find use in rubber gloves, surgical equipment, and the like. Item characteristics
[0106] Use of the rubber composition in tires, such as tire treads, can result in tires having improved or desirable tread properties. These improved or desirable properties can include tear resistance and elongation at break. The rubber composition can also produce improvements in the properties of wire coatings and substrate compounds.
[0094]
[0107] These improvements have been partially demonstrated through laboratory experiments, plant-scale testing and field evaluations using a commercial composite material, E2C™ DX9640 from Cabot Corporation. Replacing a portion of the natural rubber in a rubber composition with a composite natural rubber and carbon black material can significantly enhance compound properties beneficial for improving mileage, especially stiffness and abrasion resistance.
[0095]
[0108] Without intending to limit the scope of the exemplary embodiments, the following examples illustrate the preparation of exemplary rubber compositions utilizing composite materials and their properties. EXAMPLES
[0096]
[0109] Table 1. Tire tread cap formulations are prepared with the goal of achieving equal or better tread wear (as shown by Grosch test for medium radial truck (MRT) tires), improved rolling resistance (as shown using rebound at 100°C) and equal or better tear resistance (as shown by original and aged strebler adhesion at 100°C) when composites are utilized. Tire substrate and wire coating formulations are also prepared with the goal of achieving rolling resistance and tear resistance. EXAMPLES
[0097]
[0110] The formulation shown in Table 2 is used to prepare a rubber composition adapted for use in truck tire tread caps.
[0111] Examples A, B, and C are prepared using carbon black ASTM grade N121 and natural rubber without any compounding materials. Example A is formulated as a baseline tread composition adapted for use in medium truck radial tires. Example B adds silica to the baseline composition, and Example C uses a modified cure package.
[0098]
[0112] For these three examples, in the first mixing step, the natural rubber is mixed with a portion of the carbon black (30 phr) until the mixture reaches 160°C. It is then dripped out of the mixer and allowed to cool. In the second mixing step, the remainder of the carbon black (18 phr), silica, wax, and antioxidants, if used, are added. In the productive mixing step, sulfur, accelerators, and cure inhibitors are added and the mixture is dripped out of the mixer at a temperature below the cure temperature.
[0099]
[0113] Examples D, E, and F are prepared using both natural rubber and a composite material (a material containing approximately 64.5% natural rubber and 35.5% carbon black by weight). The amounts of carbon black and natural rubber in these three compositions are approximately the same as in the baseline formulations A, B, and C. Each of these examples uses silica. Example E uses a modified cure package, and Example F uses a higher surface area silica than the silica for Examples D and E.
[0100]
[0114] To prepare Examples D, E, and F, in a single non-productive run, the composition is mixed until the temperature reaches 124°C and dripped from the mixer. In the productive run, sulfur, accelerators, and cure inhibitors are added and the mixture composition is mixed in the mixer until it reaches 104°C and dripped from the mixer. During this run, the rotor speed is kept constant at 50 rpm. Mixing at lower temperatures in the non-productive and productive runs helps preserve the polymer filler network in the composite, thus maintaining the performance index. In the cure run, the rubber composition is heated to a temperature of 150°C for 32 minutes.
[0101] [Table 2]
[0102]
[0115] Performance tests were performed on the cured samples as follows:
[0116] Specific Gravity: Determined in accordance with ASTM D297-21, "Standard Test Methods for Rubber Products-Chemical Analysis."
[0103]
[0117] Stiffness in the cured state: Storage modulus G' is determined with a Rubber Process Analyzer (RPA500). Storage modulus values are measured at 10% strain for uncured samples and at 10% and 50% strain after curing (units: MPa) at a temperature of 40°C. Measurements on cured samples indicate the ride and handling of tires using the rubber composition in the tread. The tan delta value (ratio of G'' to G') at 10% strain is also obtained.
[0104]
[0118] Tensile Properties: The tensile modulus (MPa), tensile strength, MPa, and elongation at break (%) of the ring at 300% strain for the samples before and after aging are measured with an Instron Corporation instrument.
[0105]
[0119] Predicted Rolling Resistance: As an indication of a tire's wet braking performance, the rebound percentage is measured on cured samples at a given temperature using a ZwickRoell 5109 Rebound Resilience Tester according to ASTM D7121-05(2018) "Standard Test Method for Rubber Property-Resilience Using Schob Type Rebound Pendulum". The higher the value, the better. Rebound is a measure of the compound's hysteresis when subjected to load, and generally the higher the measured rebound, the lower the rolling resistance.
[0106]
[0120] The Strebler Adhesion Steady State Average Load to itself is determined at 100°C (N / mm) on cured samples before and after aging. This is a peel test that determines interfacial adhesion by pulling one rubber composition from another at right angles to the untorn test sample, where the two ends of the rubber composition are torn apart at an angle of 180° to each other.
[0107]
[0121] Crack Growth: DeMattia cut growth (mm / min) is determined in accordance with ASTM D813-07(2019), "Standard Test Method for Rubber Deterioration-Crack Growth" on aged specimens at 95°C. In Table 3, the higher the cut growth rate, the greater the resistance of the tread groove to surface crack growth.
[0108]
[0122] Abrasion resistance: Abrasion resistance, which indicates tread wear, is determined as the Grosch abrasion rate of the worn rubber (units: mg / km). The test rubber specimen is placed at a slip angle and subjected to a constant load (Newtons) while it traverses a given distance on a rotating abrasive disc. Medium and high severity abrasion tests are carried out. The main difference between these two tests concerns the load and the slip angle. The high severity Grosch is the average of two specimens tested at an angle of 12 degrees and a load of 70N, and the medium severity is the average of two tests at loads of 70N and 40N and angles of 12 degrees and 6 degrees, respectively.
[0109]
[0123] The results are shown in Table 3. The results are normalized by setting the results for Example A as 100. In general, for all parameters, higher values are better.
[0110] [Table 3]
[0111]
[0124] The results in Table 3 show that Examples D and E had higher aged Strebler adhesion values and better abrasion resistance at high severity, lower and medium severity abrasion resistance. This improved balance to performance metrics is achieved by using composite materials to replace a portion of the natural rubber in the compound. Example F showed a similar improvement in Strebler values to Examples D and E, with a tradeoff between abrasion resistance at low and high severity.
[0112]
[0125] Example E is identical to Example D except that it contains slightly less sulfur, accelerators, and cure inhibitors. Compared to Example A, Example E provides a 10% improvement in the rolling resistance index while also improving the compound's tear resistance index and Grosch abrasion resistance at high severity, while maintaining stiffness and elongation at break values within typical guidelines for trunk line drive applications.
[0113]
[0126] An increase in percent dispersion based on a higher 300% to 100% tensile elastic ratio (i.e., better filler-polymer interaction) was observed in the samples containing the composites. In this case, an additional non-productive mixing step can further improve the dispersion and processing indices. EXAMPLES
[0114]
[0127] The formulation shown in Table 4 is used to prepare a rubber composition adapted for use as a truck tire tread base material.
[0128] Examples G, H, and I are prepared using carbon black ASTM grade N347 and natural rubber without any composites. Example G is formulated as a baseline tread base material composition suitable for use in medium truck radial tires. Example H has carbon black partially replaced with silica compared to the baseline composition, and Example I uses a modified curing package.
[0115]
[0129] For these three examples, in the first mixing step, the natural rubber is mixed with a portion of the carbon black (up to 17.1 phr), silica (up to 9.7 phr), oil and cure activator until the mixture reaches 155°C. It is then dripped from the mixer and allowed to cool. In the second mixing step, the silica (up to 5.5 phr) and silane are mixed to a temperature of 145°C. After cooling, the remainder of the carbon black (up to 5 phr), silica (up to 1.8 phr), wax and antioxidant are mixed in the third mixing step. In the productive mixing step, the sulfur, accelerators and cure inhibitors are added and the mixture is dripped from the mixer at a temperature below the cure temperature.
[0116]
[0130] Examples J and K are prepared using both natural rubber and a composite material (a material containing approximately 64.5% by weight natural rubber and 35.5% by weight carbon black). The amounts of carbon black and natural rubber in these three compositions are approximately the same as in the baseline formulations G, H, and I. Each of these examples uses silica. Example K uses the same cure package as Example I.
[0117]
[0131] To prepare Examples J and K, the first non-productive step is similar to the first non-productive step for Examples H and I. The difference is that the amount of natural rubber in the first non-productive step for Examples J and K is lower. The second non-productive step for Examples J and K corresponds to the second non-productive step for Examples H and I. In the third non-productive step, in Examples J and K, the composite material is added with the remaining amount of silica (1.8 phr) and weathering agent and mixed until the temperature reaches 124°C. In the productive step, sulfur, accelerators, and cure inhibitors are added and the mixture composition is mixed in the mixer until it reaches 104°C and dripped from the mixer. During this step, the rotor speed is kept constant at 50 rpm. In the curing step, the rubber composition is heated to a temperature of 150°C for 32 minutes.
[0118] [Table 4]
[0119]
[0132] The results for these formulations are shown in Table 5.
[0120] [Table 5]
[0121]
[0133] Example K provided improvements in Bose fatigue and RPA500 tan(δ) values while maintaining results for Strebler, DeMattia, and elongation at break above the minimum acceptable values defined in the general guidelines for MTR tread base material compounds. Improvements to as-cured stiffness (G') and tensile properties were also observed.
[0122]
[0134] The results of Examples 1 and 2, and other evaluations not reported here, demonstrate that improvements in tread wear and tire mileage can be achieved with the exemplary compositions without significant trade-offs with other parameters, such as tear and rolling resistance / hysteresis, that typically occur when modifying rubber compounds. This shows that the exemplary compositions can expand the "performance triangle" of rolling resistance, tear, and tread wear, thus overcoming challenges typically faced during the formulation of new compounds for tire programs.
[0123]
[0135] Each of the documents referenced above is incorporated herein by reference. Except in the examples or where otherwise expressly indicated, all numerical amounts herein specifying amounts of materials, reaction conditions, molecular weights, number of carbon atoms, and the like, shall be understood to be modified by the word "about." Unless otherwise indicated, each chemical or composition referenced herein should be construed as being a commercial grade material that may contain isomers, by-products, derivatives, and other materials as would normally be expected to be present in a commercial grade. However, unless otherwise indicated, the amount of each chemical component is presented exclusive of any solvents or diluent oils that may normally be present in the commercial material. It is to be understood that the upper and lower limits of the amounts, ranges, and ratios set forth herein may be independently combined. Similarly, the ranges and amounts for each element of the invention may be used together with the ranges or amounts for any of the other elements.
[0124]
[0136] It will be appreciated that the above-disclosed and other features and functions, or alternatives thereof, can be combined to create many other different systems or applications. Various presently unforeseen or unanticipated alternatives, modifications, or improvements thereon may be made by those skilled in the art, which are also intended to be encompassed by the following claims. [Embodiment of the invention] 1. A composite material containing at least 20 phr of reinforcing carbon black dispersed in natural rubber; at least 3 phr of conjugated diene elastomer, a cure activator, and Sulfur-based hardener wherein the composite material and the conjugated diene elastomer together provide at least 90 phr of vulcanizable elastomer in the rubber composition. 2. The rubber composition according to 1, further comprising a reinforcing filler other than carbon black. 3. The rubber composition according to claim 2, wherein the reinforcing filler comprises silica. 4. The rubber composition according to 3, containing at least 5 phr of silica. 5. The rubber composition according to 1, wherein the composite material provides a rubber composition having at least 20 phr of reinforcing carbon black. 6. The rubber composition according to claim 1, wherein the composite material provides a rubber composition having at least 50 phr of natural rubber. 7. The rubber composition according to 1, wherein the composite material is a solid. 8. The rubber composition according to 1, wherein the conjugated diene elastomer comprises at least one of natural rubber and synthetic polyisoprene. 9. The rubber composition according to 1, comprising at least 5 phr of a conjugated diene elastomer. 10. The rubber composition according to 1, wherein the cure activator is selected from the group consisting of fatty acids, zinc oxide, and mixtures thereof. 11. The rubber composition of 1, further comprising at least 0.1 phr of a processing aid selected from the group consisting of resins, oils, and mixtures thereof. 12. The rubber composition according to 1, further comprising at least 1 phr of at least one of an antioxidant and an antiozonant. 13. The rubber composition according to 1, further comprising at least 0.5 phr of a cure accelerator. 14. The rubber composition according to 1, further comprising at least 0.05 phr of a cure inhibitor. 15. The rubber composition according to 1, wherein the composite material and the conjugated diene elastomer together provide at least 98 phr of vulcanizable elastomer in the rubber composition. 16. An article formed from the composition described in 1. 17. The article according to 16, comprising a tire tread. 18. A method for forming a rubber composition, comprising: blending a composite material comprising reinforcing carbon black dispersed in natural rubber with a conjugated diene elastomer at a temperature of at least 115° C. to form a mixture, the composite material and the conjugated diene elastomer together providing at least 90 phr of the total 100 phr of vulcanizable elastomer; Thereafter, blending the mixture with a sulfur-based curative to form a rubber composition. A method comprising: 19. The method of claim 18, wherein the mixture further comprises silica. 20. The method of claim 18, further comprising the step of curing the rubber composition to form a shaped article.
Claims
1. a composite material comprising at least 20 phr of reinforcing carbon black dispersed in natural rubber; at least 3 phr of a conjugated diene elastomer; a cure activator, and Sulfur-based hardener wherein said composite material and said conjugated diene elastomer together provide at least 90 phr of vulcanizable elastomer in said rubber composition.
2. 4. The rubber composition of claim 3, comprising at least 5 phr of silica.
3. 10. The rubber composition of claim 1, wherein said composite material provides a rubber composition having at least 20 phr of said reinforcing carbon black.
4. The rubber composition of claim 1 , wherein said composite material provides a rubber composition having at least 50 phr of said natural rubber.
5. The rubber composition of claim 1 , wherein the composite material is a solid.
6. The rubber composition of claim 1 , wherein the conjugated diene elastomer comprises at least one of natural rubber and synthetic polyisoprene.
7. 2. The rubber composition of claim 1 comprising at least 5 phr of said conjugated diene elastomer.
8. 10. The rubber composition of claim 1, further characterized by at least 1 phr of at least one of an antioxidant and an antiozonant.
9. 13. An article formed from the composition of claim 1.
10. 10. The article of claim 9, characterized as a tire tread.
Citation Information
Patent Citations
US10,767,028B2
Apparatus and method for producing amorphous silica ash
US20020081247A1
Method of preparing silicas, silicas with specific pore-size and / or particle-size distribution, and the uses thereof, in particular for reinforcing polymers
US20050032965A1
Tire with a thin outer sidewall rubber layer
US20100071817A1
Formation of Latex Coagulum Composite for Tire Composition
US20150105491A1