Solution for forming polyamide-imide porous body
A solvent composition for PAI porous bodies with TMA, TODI, and MDI, and specific solvent ratios prevents gelation and enhances drying efficiency, producing uniform PAI films for diverse applications.
Patent Information
- Application Number
- JP2024051726
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for forming polyamideimide (PAI) porous bodies face issues with gelation and decreased drying efficiency when increasing the ratio of poor solvent to enhance porosity, leading to non-uniform coatings.
A specific solvent composition is used, comprising PAI with TMA and TODI/MDI at a molar ratio of 85/15 to 95/5, combined with a nitrogen-containing polar solvent and a poor solvent with a higher boiling point, within a 80/20 to 50/50 mass ratio, to prevent gelation and improve drying efficiency.
The solution results in an optically uniform PAI porous body with excellent surface condition and thickness, suitable for applications like speaker diaphragms and lithium battery components.
Smart Images

Figure 2024144348000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a solution capable of forming a polyamideimide (PAI) porous body having a high porosity. [Background technology]
[0002] As a porous PI film with excellent heat resistance, Patent Documents 1 and 2 disclose a porous PAI film made of PAI using trimellitic anhydride (TMA) as the acid component and o-tolidine diisocyanate (TODI) as the isocyanate component. This PAI has a high glass transition temperature of about 300°C and excellent heat resistance. Patent Document 3 discloses a porous PAI film made of polyamideimide (PAI) using trimellitic anhydride (TMA) as the acid component and o-tolidine diisocyanate (TODI) as the isocyanate component, and has a porosity of 75% by volume or more. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-152675 A [Patent Document 2] JP 2005-281668 A [Patent Document 3] Patent Publication No. 2022-031177 Summary of the Invention [Problem to be solved by the invention]
[0004] Each of the above-mentioned techniques uses a mixed solvent of a good solvent and a poor solvent for PAI, and a solution containing PAI and a solvent (PAI solution) is applied to a substrate to form a coating film, and then when the solvent in the coating film is volatilized and removed, phase separation occurs in the coating film to form a porous PAI coating on the substrate. As can be seen from a comparison of Examples 1, 4, and 5 of Patent Document 3, the porosity of the porous PAI increases as the ratio of the poor solvent to the PAI solution increases. However, in this method, if the ratio of the poor solvent is increased in an attempt to increase the porosity of the porous PAI coating, the solution gels, making it difficult to form a uniform coating film. In addition, if the ratio of a poor solvent with a higher boiling point than the amide-based solvent is increased, the drying time increases, resulting in a problem of reduced drying efficiency.
[0005] Therefore, the present invention is intended to solve the above-mentioned problems, and aims to provide a solution for forming a PAI porous body, which suppresses gelation even in a mixed solvent composition having a low ratio of a poor solvent with a higher boiling point than a good solvent for PAI, and has improved drying efficiency. [Means for solving the problem]
[0006] As a result of intensive research to solve the above problems, the present inventors discovered that in a PAI using TMA as an acid component and TODI and 4,4'-diphenylmethane diisocyanate (MDI) as isocyanate components, the above problems can be solved by setting the molar ratio of TODI to MDI in a specific range and combining it with a specific solvent composition, which led to the completion of the present invention.
[0007] The present invention has the following gist: A solution for forming a PAI porous body, comprising a PAI containing TMA as an acid component and TODI and MDI as isocyanate components in a molar ratio of TODI / MDI = 85 / 15 to 95 / 5, and a mixed solvent containing a nitrogen-containing polar solvent (A) and a poor solvent (B) having a boiling point 5°C or more higher than that of the nitrogen-containing polar solvent in a ratio of (A) / (B) = 80 / 20 to 50 / 50 (mass ratio). Effect of the Invention
[0008] The solution for forming a PAI porous body of the present invention has a higher proportion of a poor solvent with a high boiling point than the nitrogen-containing polar solvent, which is a good solvent, and therefore has excellent drying efficiency during the formation of a porous body. This solution is an optically uniform solution without gelation, and therefore a porous body with excellent surface condition and thickness uniformity can be obtained from this solution. The obtained PAI porous body can be suitably used as a speaker diaphragm, a low dielectric flexible substrate, an electrode binder, a separator for a lithium secondary battery, a protective film for a lithium secondary battery electrode, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below.
[0010] The PAI constituting the porous PAI film of the present invention must contain TMA as the acid component and TODI and MDI as the isocyanate components. The ratio of TODI to MDI must be TODI / MDI=85 / 15 to 95 / 5 (molar ratio). When the PAI porous body forming solution is prepared with TODI less than 85 mol %, a porous body cannot be obtained if the poor solvent ratio is reduced. Furthermore, when TODI exceeds 95 mol %, an optically uniform solution cannot be obtained within the range of the mixed solvent ratio of the present invention.
[0011] There is no limit to the size of the porous body, but the thickness is usually about 0.1 μm or more and 500 μm or less, and preferably 50 μm or more and 300 μm or less. There is no limit to the average pore size of the porous body, but it is usually about 0.01 μm or more and 15 μm or less, based on the number of pieces, and preferably more than 0.1 μm and less than 10 μm. Here, the thickness can be determined by measuring at 25 ° C. based on the JIS K7130 and the density can be determined by measuring based on the JIS Z8807. The average pore size can be confirmed by obtaining a SEM (scanning electron microscope) image of the cross section of the porous PI film at a magnification of 2000 to 100,000 times and analyzing it with image processing software such as Image-J.
[0012] The PAI porous body can be obtained, for example, by the following method: A solution containing PAI and a solvent (PAI solution) is applied onto a substrate to form a coating film, and when the solvent in the coating film is removed by volatilization, for example, at 80 to 200°C, phase separation occurs within the coating film to form a porous PAI film on the substrate, and then the porous PAI film is peeled off from the substrate.
[0013] The PAI solution for forming a porous body can be obtained, for example, by the following method: First, TODI, MDI, and an approximately equimolar amount of TMA relative to the total amount of TODI and MDI are polymerized in a nitrogen-containing polar solvent (a good solvent for PAI) to obtain a PAI solution, and then a poor solvent for PAI is added to the PAI solution to obtain an optically uniform solution for forming a PAI porous body.
[0014] Since the PAI solution contains a poor solvent for PAI, the poor solvent acts to induce phase separation in the coating film when the coating film is dried. The nitrogen-containing polar solvent (A) is preferably an amide-based solvent or a urea-based solvent. Examples of the amide-based solvent include N-methyl-2-pyrrolidone (NMP boiling point: 202°C), N,N-dimethylformamide, and N,N-dimethylacetamide (DMAc boiling point: 166°C). Examples of the urea-based solvent include tetramethylurea and dimethylethyleneurea. These may be used alone or in combination of two or more. Among these, NMP and DMAc are preferred. It is preferable that these solvents are dehydrated to a moisture content of 100 ppm or less.
[0015] The poor solvent (B) for PAI must have a boiling point 5° C. or more higher than that of the nitrogen-containing polar solvent. The type of solvent is preferably an ether-based solvent. As the ether-based solvent, triglyme (TRGM boiling point: 216° C.) and tetraglyme (TEGM boiling point: 275° C.) are preferable, and these may be used alone or in combination of two or more. The poor solvent for PAI refers to a solvent in which the solubility of PAI at 25° C. is less than 1% by mass.
[0016] The mixing ratio of the solvent (A) and the solvent (B) must be (A) / (B) = 80 / 20 to 50 / 50 (mass ratio). If the ratio of (B) exceeds 50 mass%, gelation of the solution occurs. If the ratio of (B) is less than 20 mass%, it becomes difficult to induce phase separation during drying, and sufficient porosity for a porous body cannot be obtained.
[0017] It is also possible to introduce a crosslinking structure into the PAI in order to improve the insolubility of the porous PAI or to improve the physical properties. The method of introducing the crosslinking structure is not particularly limited, and examples thereof include a thermal crosslinking method and a crosslinking agent addition method. As the crosslinking agent, a compound having a crosslinkable functional group of two or more in its structure is preferable, and diamine, triamine, diisocyanate, triisocyanate, multifunctional blocked isocyanate, polycarbodiimide, polymaleic anhydride copolymer, multifunctional epoxy resin, melamine resin, phenolic resin, etc. can be used. These may be used alone or in combination of two or more. Among them, multifunctional epoxy resin and multifunctional blocked isocyanate are preferable, and multifunctional blocked isocyanate is more preferable. The blending ratio of the crosslinking agent is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 5% by mass or less, based on the PAI resin component.
[0018] Examples of diamines include aliphatic diamines such as ethylenediamine, 1,3-propanediamine, 2-methyl-1,2-propanediamine, 2,2-dimethyl-1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexamethylenediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, methylbis(3-aminopropyl)amine, 1,5-diamino-2-methylpentane (MPMD), 2,5-dimethyl-1,6-hexamethylenediamine, 1,2-propanediamine, ... Examples of suitable diamines include panediamine, 2-methyl-1,2-propanediamine, 1,3-butanediamine, 1,3-diaminopentane (DAMP), 2,2,4-trimethylhexamethylenediamine (TMD), 1,5-diamino-2-butyl-2-ethylpentane, bis(2-aminoethyl)ether, 3,6-dioxaoctane-1,8-diamine, 4,7-dioxadecane-1,10-diamine, 4,7-dioxadecane-2,9-diamine, 4,9-dioxadecane-1,12-diamine, 5,8-dioxadecane-3,10-diamine, polyoxyalkylene diamines, polyoxyalkylene diols, and dimer diamines.Alicyclic diamines include 1,3- and 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, bis(4-amino-3-methylcyclohexyl)methane, bis(4-amino-3-ethylcyclohexyl)methane, bis(4-amino-3,5-dimethylcyclohexyl)methane, bis(4-amino-3-ethyl-5-methylcyclohexyl)methane (M-MECA), 2-methyl-1,3-diaminocyclohexane, 1,3- and 1,4-bis(aminomethyl)cyclohexane, 2,5(2,6)-bis(aminomethyl)cyclohexane, Examples of such compounds include 1,3- and 1,4-xylylenediamine, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane (i.e., isophoronediamine or IPDA), and 1,4-diamino-2,2,6-trimethylcyclohexane (TMCDA). The diamine compound may be a commercially available product, and examples thereof include Jeffamine (registered trademark) manufactured by Huntsman Chemicals under the trade names D-230, D-400, D-2000, D-4000, XTJ-511, ED-600, ED-900, ED-2003, XTJ-568, XTJ-569, XTJ-523, XTJ-536, XTJ-542, and XTJ-559; Polyetheramine (registered trademark) manufactured by BASF under the trade names D230, D400, and D2000; and PC Amine (registered trademark) manufactured by Nitroil under the trade names DA250, DA400, DA650, and DA2000.
[0019] Examples of triamines include aliphatic triamines such as 4-aminomethyl-1,8-octanediamine, 1,3,5-tris(aminomethyl)benzene, 1,3,5-tris(aminomethyl)cyclohexane, polyalkylene triamines, polyalkylene triols, etc. The triamine compounds may be commercially available, such as Jeffamine (registered trademark) manufactured by Huntsman Chemicals under the trade names T-403 and T-5000, Polyetheramine (registered trademark) manufactured by BASF under the trade names T403 and T5000, and PC Amine (registered trademark) manufactured by Nitroil under the trade names TA403 and TA5000.
[0020] Examples of diisocyanates include cyclohexane diisocyanate, methylcyclohexane diisocyanate, ethylcyclohexane diisocyanate, propylcyclohexane diisocyanate, methyl-diethyl-cyclohexane diisocyanate, phenylene diisocyanate, toluylene diisocyanate, bis(isocyanatophenyl)methane, propane diisocyanate, butane diisocyanate, pentane diisocyanate, and hexane diisocyanate. , hexamethylene diisocyanate (HDI), 1,5-diisocyanato-2-methylpentane (MPDI), heptane diisocyanate, octane diisocyanate, nonane diisocyanate, 1,6-diisocyanato-2,4,4-trimethylhexane, 1,6-diisocyanato-2,2,4-trimethylhexane (TMDI), decane diisocyanate, undecane diisocyanate, dodecane diisocyanate, isophorone diisocyanate (IPDI) ), bis(isocyanatomethylcyclohexyl)methane (H12MDI), isocyanatomethyl-methylcyclohexyl isocyanate, 2,5(2,6)-bis(isocyanatomethyl)bicyclo[2.2.1]heptane (NBDI), 1,3-bis(isocyanatomethyl)cyclohexane (1,3-H6-XDI), 1,4-bis(isocyanatomethyl)cyclohexane (1,4-H6-XDI), benzene diisocyanate, 4,4′-diphenylmethane diisocyanate diisocyanate (MDI), tolylene diisocyanate (TDI), o-tolidine isocyanate (TODI), 3,3'-dichloro-4,4'-diisocyanatobiphenyl, tris(4-isocyanatophenyl)methane, 1,5-diisocyanatonaphthalene, hydrogenated toluene diisocyanate, 1-isocyanatomethyl-5-isocyanato-1,3,3-trimethylcyclohexane, 1,3,5-tris(6t-isocyanatohexyl)biuret, and the like.
[0021] Examples of triisocyanates include nonane triisocyanate, decane triisocyanate, undecane triisocyanate, and dodecane triisocyanate.
[0022] Polyfunctional blocked isocyanates are reaction products of isocyanate compounds and isocyanate blocking agents. Usable isocyanate compounds include isocyanurate type, biuret type, adduct type, etc., and the structures of these compounds are aromatic isocyanate, aliphatic isocyanate, and alicyclic isocyanate. Examples of isocyanate blocking agents include phenol-based blocking agents such as phenol, cresol, xylenol, chlorophenol, and ethylphenol; lactam-based blocking agents such as ε-caprolactam (ε-CAP), δ-valerolactam, γ-butyrolactam, and β-propiolactam; active methylene-based blocking agents such as diethyl malonate, ethyl acetoacetate, and acetylacetone; and alcohol-based blocking agents such as methanol, ethanol, propanol, butanol, amyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, benzyl ether, methyl glycolate, butyl glycolate, diacetone alcohol, methyl lactate, and ethyl lactate. Examples of the blocking agents include coal-based blocking agents; oxime-based blocking agents such as formaldehyde oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, diacetyl monoxime, and cyclohexanone oxime; mercaptan-based blocking agents such as butyl mercaptan, hexyl mercaptan, t-butyl mercaptan, thiophenol, methylthiophenol, and ethylthiophenol; acid amide-based blocking agents such as acetate amide and benzamide; imide-based blocking agents such as succinimide and maleimide; amine-based blocking agents such as xylidine, aniline, butylamine, and dibutylamine; imidazole-based blocking agents such as imidazole and 2-ethylimidazole; imine-based blocking agents such as methyleneimine and propyleneimine; and pyrazole-based blocking agents such as methylpyrazole and ethylpyrazole.The polyfunctional blocked isocyanate compound may be a commercially available product, for example, blocked isocyanates manufactured by Baxenden under the trade names BI7683, BI7642, BI201, BI220, BI7950, BI7951, BI7960, BI7961, BI7963, BI7981, BI7982, BI7990, BI7991, and BI7992; blocked isocyanates manufactured by Sumitomo Bayer Urethane Co., Ltd. under the trade names Sumidur BL-3175, BL-4165, BL-1100, BL-1265, and Desmodur TPLS-2. 957, TPLS-2062, TPLS-2078, TPLS-2117, Desmotherm 2170, Desmotherm 2265, trade names Coronate 2512, Coronate 2513, and Coronate 2520 manufactured by Nippon Polyurethane Industry Co., Ltd., trade names B-830, B-815, B-846, B-870, B-874, and B-882 manufactured by Mitsui Takeda Chemicals Co., Ltd., and trade names TPA-B80E, 17B-60PX, E402-B80T, MF-B60B, MF-K60B, and SBN-70D manufactured by Asahi Kasei Chemicals Corporation.
[0023] Examples of polycarbodiimides include p-phenylene-bis(2,6-xylylcarbodiimide), tetramethylene-bis(t-butylcarbodiimide), cyclohexane-1,4-bis(methylene-t-butylcarbodiimide), etc. The polycarbodiimide may be a commercially available product, such as Carbodilite (registered trademark) manufactured by Nisshinbo Chemical Co., Ltd., under the trade names V-02, SV-02, V-02B, V-03, V-04, V-05, V-07, V-09, V-09GBV-10, E-02, E-03A, and E-05.
[0024] Examples of the polymaleic anhydride copolymer include styrene-maleic anhydride copolymer, olefin-maleic anhydride copolymer, etc. The polymaleic anhydride copolymer may be a commercially available product, such as Sekisui Plastics Co., Ltd.'s product name Dylark D332, and Polyscope's product name Xiran SZ08250.
[0025] As the multifunctional epoxy resin, commercially available products can be used, for example, jER828, jER834, jER1001, jER1004, jERYL903, jER152, and jER154 manufactured by Mitsubishi Chemical Corporation, Epicron 840, Epicron 850, Epicron 1050, Epicron 2055, Epicron 152, Epicron 165, Epicron N-730, Epicron N-770, Epicron N-865, and Epicron 830 manufactured by DIC Corporation, and Epicron N-770, Epicron N-865, and Epicron 830 manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. Epotohto YD-011, YD-013, YD-127, YD-128, Epotohto YDB-400, YDB-500, Epotohto YDCN-701, YDCN-704, Epotohto YDF-170, YDF-175, YDF-2004, Epotohto ST-2004, ST-2007, ST-3000, Dow Chemical Company DER317, DER331, DER661, DER664, DEN 431, DEN438, TEN, EPPN-501, EPPN-502, DER542, Sumitomo Chemical Co., Ltd. Sumi-Epoxy ESA-011, ESA-014, ELA-115, ELA-128, Sumi-Epoxy ESB-400, ESB-700, Sumi-Epoxy ESCN-195X, ESCN-220, Asahi Kasei Co., Ltd. AER330, AER331, AER661, AER664, AER711, A Examples of such compounds include ER714, AERECN-235, ECN-299, EPPN-201, EOCN-1025, EOCN-1020, EOCN-104S, and RE-306 manufactured by Nippon Kayaku Co., Ltd., CELLOXIDE 2021P manufactured by Daicel Corporation, YR-102 and YR-450 manufactured by Tohto Kasei Co., Ltd., TEPIC manufactured by Nissan Chemical Industries, Ltd., and Blenmar DGT, CP-50S, and CP-50M manufactured by Nippon Oil & Fats Co., Ltd.
[0026] Examples of the melamine resin include imino group type methylated melamine resin, methylol group type melamine resin, methylol group type methylated melamine resin, fully alkyl type methylated melamine resin, etc. The melamine resin may be a commercially available product, and examples thereof include Cymel 303, Cymel 254, Cymel 1170, Cymel 235, Cymel 238, Cymel 1123, and Mycoat 715 manufactured by Daicel-Allnex Co., Ltd., Sumimal M-40S manufactured by Sumitomo Chemical Co., Ltd., Super Beckamine J-820-60 and Super Beckamine L-121-60 manufactured by DIC Corporation, and Yuban 20SE-60 manufactured by Mitsui Chemicals, Inc.
[0027] As the phenolic resin, commercially available products can be used. For example, Tackirol 201 (alkylphenol formaldehyde resin), Tackirol 250-I (brominated alkylphenol formaldehyde resin with a bromination rate of 4%), Tackirol 250-III (brominated alkylphenol formaldehyde resin) manufactured by Taoka Chemical Co., Ltd., PR-4507 manufactured by Gun-ei Chemical Industry Co., Ltd., Vulkaresat 510E, Vulkaresat 532E, Vulkaresen E, Vulkaresen 105E, Vulkaresen 130E, Vulkaresol 315E, Amberol ST 137X manufactured by Hoechst, Sumilight Resin PR-22193 manufactured by Sumitomo Durez Co., Ltd., Symphorm-C-100 and Symphorm-C-1001 manufactured by Anchor Chem., Tamanol 531 manufactured by Arakawa Chemical Co., Ltd., and Schenectady manufactured by Schenectady Chem. SP1059, Schenectady SP1045, Schenectady SP-1055, Schenectady SP-1056, CRR-0803 manufactured by UCC, CRM-0803 manufactured by Showa Union Synthetic Co., Ltd., and Vulkadur A manufactured by Bayer.
[0028] The solids concentration of PAI in the PAI solution is preferably 5% by mass or more and 15% by mass or less, and more preferably 8% by mass or more and 13% by mass or less.
[0029] The polymerization of PAI can be carried out, for example, as follows. That is, TMA, TODI and MDI are polymerized in a nitrogen-containing polar solvent at a temperature of 100 to 200°C, preferably 120 to 180°C. In this reaction, the order of addition of the monomer and the solvent is not particularly limited and may be any order. In addition, it is preferable to use only trimellitic anhydride (TMA) as the acid component, but a part of TMA may be substituted with other acid components. Specifically, TMA may be substituted with pyromellitic anhydride, phthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, dimer acid, etc., so long as the substitution rate is 10 mol% or less. If this substitution rate exceeds 10 mol%, it may be difficult to obtain good mechanical properties when the porous PAI film is formed. Here, the dimer acid is a fatty acid mainly composed of a dibasic acid of C36 dicarboxylic acid produced by dimerization of C18 unsaturated fatty acid made from vegetable oils and fats, and can be obtained as a commercial product from Croda Japan, Tsuno Foods Industries, etc. The molar ratio of the acid component to the total of the isocyanate component is preferably 1 / 1.01 to 1.05. In this way, it is preferable to prepare a PAI solution using a small excess of the isocyanate component relative to TMA. In the polymerization reaction, it is preferable to mix a basic compound such as 1,8-diazabicyclo[5.4.0]undecene-7 (DBU) or triethylenediamine (DABCO) at 0.01 to 1 mol % relative to TMA. By setting such polymerization conditions, a PAI solution with high viscosity can be obtained. The solution viscosity of the PAI solution after polymerization (before mixing of the poor solvent) is preferably 50 Pa·s or more as the solution viscosity at 30°C when the PAI concentration is 20 mass%.
[0030] The PAI solution can be applied to the substrate using any coater. Examples of the coater include a die coater, a lip coater, a gravure coater, a bar coater, a doctor blade coater, a comma coater, a reverse roll coater, and a bar reverse roll coater. Multi-layer coating is also possible, in which case the composition of the PAI solution in each layer may be the same or different.
[0031] Examples of the substrate include metal foils (copper, aluminum, iron, silver, palladium, nickel, chromium, molybdenum, tungsten, or alloys thereof, etc.), polyester films (polyethylene terephthalate, polyethylene naphthalate, etc.), aromatic polyimide films, and fluororesin films (polytetrafluoroethylene, etc.). Among these, polyethylene terephthalate films or aluminum foils are preferred. It is preferable that these substrates have a smooth surface. In addition, release metal foils or plastic films having a heat-resistant release layer formed on the surface can also be preferably used. These release metal foils or plastic films can be commercially available products. EXAMPLES
[0032] The present invention will be described in detail below with reference to examples, but is not limited to these examples. The raw materials used in the examples are as follows. (monomer) TMA: Trimellitic anhydride TODI: o-Tolidine diisocyanate MDI: 4,4'-diphenylmethane diisocyanate (catalyst) DABCO: Triethylenediamine (Nitrogen-containing polar solvent (A)) NMP: N-methyl-2-pyrrolidone DMAc: N,N-dimethylacetamide (Poor Solvent (B)) TRGM: Triethylene glycol dimethyl ether TEGM: Tetraethylene glycol dimethyl ether
[0033] The coating drying process in the examples was carried out under the following conditions: Dryer: Inert oven (DN411I, manufactured by Yamato Scientific Co., Ltd.) Substrate: 100 μm PET film Wet film thickness: 200 μm Drying temperature: 160° C. The drying time was appropriately adjusted so that the residual volatile content of the coating film was 10% by weight or less. The residual volatile content was calculated by drying the obtained porous PAI film at 250° C. for 10 minutes, measuring the weight before and after drying, and using the following formula: Residual volatile content (wt%)=(AB) / A×100 In the formula, A indicates the weight before drying at 250° C., and B indicates the weight after drying at 250° C.
[0034] (Porosity) The porosity of the porous PAI film was calculated using the following formula: Porosity (volume %) = 100-100 × (W / D) / (S × T), where S is the area of the PAI porous film, T is its thickness, W is its mass, and D is the density of the corresponding non-porous PAI film.
[0035] <Example 1> In a glass reaction vessel, 1.00 mol of TMA, 0.92 mol of TODI, 0.10 mol of MDI, and 0.0005 mol of DABCO were charged together with NMP (water content 80 ppm) dehydrated so that the solid content concentration was 20% by mass under a nitrogen atmosphere, and the mixture was heated to 150 ° C while stirring and reacted for 5 hours to obtain a PAI solution with a solution viscosity of 210 Pa · s and a PAI solid content concentration of 20% by mass. TEGM was added to this PAI solution so that the ratio of the nitrogen-containing polar solvent (A) and the poor solvent (B) was the ratio in Table 1, and then diluted with a mixed solvent with the solvent ratio in Table 1 to obtain a PAI porous body forming solution with a solid content concentration of 10% by mass. This PAI solution was applied to a polyethylene terephthalate film with a thickness of 100 μm, and then dried at 160 ° C for 10 minutes to obtain a porous PAI film (A-1) with a thickness of 41 μm. The measurement results of the porosity of A-1 are shown in Table 1.
[0036] <Example 2> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the solvent ratio was changed as shown in Table 1. This PAI solution was applied onto a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a porous PAI film (A-2) having a thickness of 65 μm. The measurement results of the porosity of A-2 are shown in Table 1.
[0037] <Example 3> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the solvent ratio was changed as shown in Table 1. This PAI solution was applied onto a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 20 minutes to obtain a porous PAI film (A-3) having a thickness of 50 μm. The measurement results of the porosity of A-3 are shown in Table 1.
[0038] <Example 4> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the isocyanate molar ratio and the solvent ratio were changed as shown in Table 1. This PAI solution was applied onto a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a porous PAI film (A-4) having a thickness of 58 μm. The measurement results of the porosity of A-4 are shown in Table 1.
[0039] <Example 5> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the isocyanate molar ratio and the solvent ratio were changed as shown in Table 1. This PAI solution was applied onto a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a porous PAI film (A-5) having a thickness of 58 μm. The measurement results of the porosity of A-5 are shown in Table 1.
[0040] <Example 6> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the type of solvent and the solvent ratio were changed as shown in Table 1. This PAI solution was applied onto a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a porous PAI film (A-6) having a thickness of 65 μm. The measurement results of the porosity of A-6 are shown in Table 1.
[0041] <Example 7> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the type of solvent and the solvent ratio were changed as shown in Table 1. This PAI solution was applied to a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a porous PAI film (A-7) having a thickness of 35 μm. The measurement results of the porosity of A-7 are shown in Table 1.
[0042] <Comparative Example 1> An attempt was made to obtain a solution for forming a PAI porous body in the same manner as in Example 1, except that the isocyanate molar ratio and solvent ratio were changed as shown in Table 1. However, an optically uniform solution could not be obtained because the TODI component in the total isocyanate components exceeded 95 mol %.
[0043] <Comparative Example 2> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the isocyanate molar ratio and the solvent ratio were changed as shown in Table 1. This PAI solution was applied to a polyethylene terephthalate film having a thickness of 100 μm, and then dried at 160° C. for 15 minutes to obtain a PAI film (B-2) having a thickness of 20 μm. The measurement results of the porosity of B-2 are shown in Table 1. Since the TODI component in the total isocyanate component was less than 85 mol %, the poor solvent (B) ratio was lower than that of the nitrogen-containing polar solvent (A), and therefore the film did not become porous.
[0044] <Comparative Example 3> A solution for forming a PAI porous body was obtained in the same manner as in Example 1, except that the solvent ratio was changed as shown in Table 1. This PAI solution was applied to a polyethylene terephthalate film with a thickness of 100 μm, and then dried at 160° C. for 10 minutes to obtain a PAI film (B-3) with a thickness of 20 μm. The measurement results of the porosity of B-3 are shown in Table 1. Since the ratio of the poor solvent (B) was less than 20 mol %, the film was not made porous.
[0045] <Comparative Example 4> An attempt was made to obtain a solution for forming a PAI porous body in the same manner as in Example 1, except that the solvent ratio was changed as shown in Table 1. However, because the ratio of the poor solvent (B) exceeded 50%, the solution gelled and a homogeneous solution could not be obtained.
[0046] [Table 1] [Industrial Applicability]
[0047] The porous film obtained from the PAI solution for forming a porous body of the present invention can be suitably used as a speaker diaphragm, a low dielectric flexible substrate, an electrode binder, a separator for a lithium secondary battery, a protective film for an electrode of a lithium secondary battery, etc.
Claims
[Claim 1] A solution for forming a PAI porous body, comprising: PAI containing TMA as an acid component, and TODI and MDI as isocyanate components in a TODI / MDI ratio of 85 / 15 to 95 / 5 (molar ratio); and a mixed solvent containing a nitrogen-containing polar solvent (A) and a poor solvent (B) having a boiling point 5°C or more higher than that of the nitrogen-containing polar solvent in a ratio of (A) / (B) of 80 / 20 to 50 / 50 (mass ratio).
Citation Information
Patent Citations
Polyamide-imide resin for secondary battery separator, separator using the resin, and secondary battery using the separator
JP2004152675A
Porous membrane, method for producing the same and lithium ion secondary battery using the same
JP2005281668A
Porous polyamide imide film
JP2022031177A