Coating device, method, and electrode

The coating device and method enhance electrode manufacturing by applying bilayer powder layers solvent-free and uniformly, addressing incomplete coating issues, thereby improving conductivity and energy density while minimizing defects and material waste.

JP2024144391AActive Publication Date: 2024-10-11パワーコエスエー
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024055820
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-11
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing electrode manufacturing methods result in incomplete coating due to the need for solvents, leading to reduced electrical conductivity and energy density, and increased rejects.

Method used

A coating device and method that applies a bilayer powder layer directly onto a substrate using a crimping process with separate metering gaps and crimping rolls, ensuring solvent-free application and improved adhesion without mixing the powders until the boundary area, allowing for controlled layer thickness and composition.

Benefits of technology

The solution achieves high electrical conductivity and energy density in electrodes by ensuring uniform deposition and adhesion of bilayer powder layers, reducing defects and material waste, and optimizing material usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144391000001_ABST
    Figure 2024144391000001_ABST
Patent Text Reader

Abstract

To provide a coating device and a method for manufacturing an electrode.SOLUTION: In relation to a coating device 10 to manufacture an electrode 11 having a two-layer structured powder layer 12 on a substrate 15, the coating device includes: a feed unit 17 configured to feed the substrate 15 into a pressing gap 18; a first metering unit 19 to accommodate a first powder 20 and a second powder 21 for parallel filling of a first metering gap 22 with the first powder and the second powder; and a roller device 23. The roller device includes a first application roller 24, a first pressing roller unit 25, and a second pressing roller unit 26. The first metering gap is provided between the first application roller and the first pressing roller unit. The pressing gap is provided between the first pressing roller unit and the second pressing roller unit. The first metering gap is provided to apply the first powder and the second powder as a two-layer structured layer 27 to the first pressing roller unit with a first application force. The pressing gap is provided to transfer the two-layer structured layer from the first pressing roller unit to a first side 28 of the substrate with a pressing force.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to a coating device for producing an electrode with at least one bilayer powder layer on a substrate having the features of independent claim 1, to a method for producing an electrode with at least one bilayer powder layer having the features of independent claim 6 as well as to an electrode with a bilayer powder layer having the features of independent claim 13.

[0002] In an attempt to fabricate solvent-free or dry electrodes, electrodes have traditionally been fabricated with a single layer coating. To improve battery cell performance, traditional electrode fabrication has pursued the approach of fabricating electrodes with multiple layer coatings (different compositions of individual layers) because such electrodes have enhanced energy density and electrical conductivity.

[0003] Currently, electrodes with multilayer coatings produced without the use of solvents are often produced as free-standing films, where two powders are pressed against a current collector in a calendar gap.

[0004] However, it is still typical for electrodes to be wet processed and therefore contain solvents.

[0005] Another way is the sequential application of the individual layers to the side of the substrate provided for this purpose, for example in two successively arranged calender gaps, in which the application and pressing of the individual layers as free-standing films can take place in each case.

[0006] However, in this case, a certain amount of moisture in the adhesion promoter or powder is often necessary, since otherwise the adhesion of the layers cannot be guaranteed. This can result in a substrate or current collector that is not completely covered. This, in turn, can result in an increase in rejects or a decrease in power of the electrodes thus produced.

[0007] It is therefore an object of the present invention to at least partially overcome at least one of the above-mentioned disadvantages. In particular, it is an object of the present invention to provide a coating device which allows for dry electrode production, whereby the electrical conductivity or energy density of the electrode is increased. Furthermore, it is an object of the present invention to provide a method for dry electrode production and the electrodes thus produced.

[0008] The above-mentioned problem is solved by a coating device having the features of independent claim 1, a method having the features of independent claim 6 and an electrode having the features of independent claim 13. Further features and details of the invention emerge from the dependent claims, the description and the drawings. In this specification, the disclosures to the individual aspects of the invention are always or can be linked to one another, since features and details explained in connection with the coating device according to the invention are naturally also valid in connection with the method according to the invention and / or in connection with the electrode according to the invention and respectively vice versa.

[0009] According to the invention, in a first aspect of the invention, a coating device for producing an electrode having at least one double-layered powder layer, in particular a double-layered cathode layer and / or a double-layered anode layer, on a substrate, in particular a current collector, is envisaged. The coating device comprises a feed unit for feeding the substrate into a crimping gap, a first metering unit for receiving a first powder and a second powder and for filling the first metering gap with the first powder and the second powder in parallel, and a roll arrangement, the roll arrangement comprising a first application roll, a first crimping roll unit and a second crimping roll unit, wherein the first metering gap is arranged between the first application roll and the first crimping roll unit, and the crimping gap is arranged between the first crimping roll unit and the second crimping roll unit. The first metering gap is provided for applying the first powder and the second powder as a first at least two-layer layer to the first pressure roll unit with a first application force. The pressure gap is provided for transferring the first at least two-layer layer from the first pressure roll unit to a first side of the supplied substrate with a pressure force.

[0010] The coating device is based on roll-transported coating, where the at least two-layer structure is first applied to a roll and then transferred or pressed from the roll onto the substrate, which is particularly advantageous for coating the substrate with solvent-free, dry, powdery materials, and therefore the coating device is highly suitable for dry electrode production.

[0011] The first and second pressing roll units may each have one pressing roll. To apply a pressing force for transferring the layers of the at least two-layer structure, the pressing rolls of the first and second pressing roll units, which form a pressing gap, rotate opposite each other at the same rotation speed, which can provide an optimal coating result. The first application roll may have a lower rotation speed than the pressing roll of the first application roll unit, which forms a metering gap with the first application roll, which ensures that the first powder and the second powder remain attached to the first pressing unit as a first layer and are carried by the first pressing unit.

[0012] The first dosing unit simultaneously doses both the first and second powders, so that the desired two-layer structure can be applied during the crimping process, i.e., through the crimping gap. It should be noted that the first and second powders are filled side by side and only mix in the boundary area. In order to reduce the mixing of the first and second powders, it is conceivable that the first dosing unit has a first chamber for the first powder and a second chamber for the second powder.

[0013] The ratio of the amounts of the first and second powders in the first layer may be variable in order to produce different layer thicknesses, for which it is conceivable that a control unit is provided for open-loop and / or closed-loop control of the ratio of the amounts of each powder.

[0014] Furthermore, parallel, simultaneous metering or filling of the metering gap increases the efficiency of the coating equipment, since only one roll fixture is required to apply the two-layer powder layer onto the substrate. By applying the two-layer powder layer simultaneously, the formation of a boundary layer between the two powder layers is reduced or prevented, which improves adhesion and electrical connection.

[0015] Within the scope of the invention of the coating device, it may be advantageous if a second metering unit is provided which receives the third and fourth powders and fills the second metering gap with the third and fourth powders in parallel, the roll arrangement has at least one second application roll, and the second metering gap is provided between the second application roll and the second pressure roll unit, where the second metering gap is provided for applying the third and fourth powders as a second at least two-layer layer to the second pressure roll unit with a second application force, and the pressure gap between the first and second pressure roll units is provided for transferring the second at least two-layer layer from the second pressure roll unit to the second side of the supplied substrate with a pressure force.

[0016] The second application roll may have a lower rotational speed than the pressure roll of the second pressure roll unit, which forms a metering gap with the second application roll, thereby ensuring that the third powder and the fourth powder continue to adhere to the second pressure unit as a second layer and are carried by the second pressure unit.

[0017] The second metering unit simultaneously meters both the third and fourth powders, so that the desired two-layer structure can be applied during the crimping process, i.e., through the crimping gap. It should be noted that the third and fourth powders are filled side by side and only mix in the boundary area. In order to reduce the mixing of the third and fourth powders, it is conceivable that the second metering unit has a third chamber for the third powder and a fourth chamber for the fourth powder.

[0018] The ratio of the amounts of the third and fourth powders in the second layer may be variable to produce different layer thicknesses, for which it is conceivable that the control unit provides open-loop and / or closed-loop control of the ratio of the amounts of each powder.

[0019] It is further contemplated that the first powder and the third powder have the same composition and / or that the second powder and the fourth powder have the same composition.

[0020] It is conceivable within the scope of the present invention that the first pressure roll unit has at least one first pressure roll and at least one second pressure roll, and at least one first press gap is provided between the at least one first pressure roll and the at least one second pressure roll. Additionally or alternatively, the second pressure roll unit has at least one third pressure roll and at least one fourth pressure roll, and at least one second press gap is provided between the at least one third pressure roll and the at least one fourth pressure roll.

[0021] The first and / or second press gaps press the first or second layer before it is transferred to the substrate. This can produce a tighter packing of the first and second layers, which can further improve the electrical conductivity. Furthermore, the press gap has the additional effect of reducing the shear forces acting in both the metering gap and the crimping gap, since less force is required for the application or transfer in these gaps. This results in a uniform application and transfer, and reduces the number of defects during application or transfer.

[0022] It is also conceivable here for the first pressure roll unit and / or the second pressure roll unit to have further pressure rolls and therefore further press gaps.

[0023] It may be envisaged within the scope of the invention that the first metering unit has a first separating plate in the area of ​​the first metering gap for separating the first powder from the second powder, and additionally or alternatively, the second metering unit has a second separating plate in the area of ​​the second metering gap for separating the third powder from the fourth powder.

[0024] In this case, the first or second separating plate extends only into the area of ​​the first or second metering gap without closing the respective metering gap. The separating plate is used to separate the individual powders until just before the application of the powder as the first or second layer. The separating plate reduces mixing in the boundary area of ​​the first or second layer, which is particularly advantageous for the energy density of the first or second layer.

[0025] Here, it is conceivable that the first and / or the second separating plate have a structure that can comb through the powders in order to break up any possible agglomerations and / or to provide a better transport to the metering gap. It is also conceivable that the separating plate is vibrated by electrical and / or pneumatic excitation, which can further improve the transport.

[0026] It is further conceivable that in the region of the first metering gap a first shielding thin plate is provided in the region of the first applied roll and / or a second shielding thin plate is provided in the region of the first pressure roll unit, and / or that in the region of the second metering gap a third shielding thin plate is provided in the region of the second applied roll and / or a fourth shielding thin plate is provided in the region of the second pressure roll unit.

[0027] The shielding lamellae are used to prevent the powder from coming into contact with the first and / or second pressure roll unit before the metering gap or from adhering to the first and / or second application roll. At the same time, such shielding lamellae can easily control the drawing of the powder into the first and / or second metering gap. At the same time, it is conceivable that the first and / or second application roll and / or the first and / or second pressure roll unit have structures for cleaning them or for removing adhering material. This allows the cleanest possible application of a new first or second layer or a clean transfer of the first and / or second layer onto the substrate.

[0028] Furthermore, in the case of a coating apparatus it is conceivable that the first coating roll and / or the second coating roll and / or the first pressure roll unit and / or the second pressure roll unit are temperature adjustable.

[0029] The above-mentioned object is furthermore achieved in a second aspect of the invention by a method according to the invention for producing an electrode having at least one bilayer powder layer, in particular a bilayer cathode layer and / or a bilayer anode layer, on a substrate, in particular a current collector, in a coating apparatus as described above, which method comprises the steps of: - feeding the substrate into the crimping gap by a feeding unit; - filling the first metering gap with the first powder and the second powder in parallel by means of a first metering unit, - applying the first powder and the second powder as a first at least two-layer layer to a first pressure roll unit in a first metering gap with a first application force; - transferring the first at least bilayer layer to a first side of the substrate in a first crimping gap by a crimping force; It has.

[0030] By simultaneously depositing the first and second powders as a first layer onto the substrate, the forces applied to each individual powder in the layer can be reduced or evenly distributed.

[0031] It is also conceivable that the second metering unit fills the second metering gap with a third powder and a fourth powder in parallel, the third powder and the fourth powder being applied as a second at least two-layer layer in the second metering gap by a second application force to the second pressing roll unit, and the second at least two-layer layer being transferred to a second side of the substrate in the pressing gap by a pressing force.

[0032] By means of the second metering unit and the second metering gap, at least a two-layer powder layer can also be applied to the second side of the substrate, whereby in the case of electrode production, both the anode layer and the cathode layer are applied to the substrate or current collector in one step.

[0033] Within the scope of the present invention, it is optionally possible for the first metering unit to continuously fill the first metering gap and / or for the second metering unit to continuously fill the second metering gap.

[0034] This provides particularly uniform results when producing at least two layers on each side of the substrate.

[0035] It may further be envisaged within the scope of the present invention that the first metering unit meters the first and second powders in the crimping gap in the case of the first at least two-layer layer such that a first layer thickness of 40-150 μm is set, where the first layer of the first powder has a layer thickness of 10-70 μm. Additionally or alternatively, the second metering unit meters the third and fourth powders in the case of the second at least two-layer layer in the crimping gap in the case of the second at least two-layer layer such that a second layer thickness of 40-150 μm is set, where the first layer of the third powder has a layer thickness of 10-70 μm.

[0036] This layer thickness or the required amount of material is set by the first or second metering unit and is generated by the first application force in the first metering gap or the second application force in the second metering gap and by the pressing force in the pressing gap, which can be controlled in an open-loop and / or closed-loop manner by the control unit.

[0037] In the context of the present invention, it is conceivable to press a first at least two-layered layer in at least one first press gap of a first pressure roll unit and / or to press a second at least two-layered layer in at least one second press gap of a second pressure roll unit.

[0038] Pressing in each press gap causes compression of the first and / or second layers, which produces a closer packing of the respective at least bi-layered powder layers on the first and / or second sides of the substrate, which allows a reduction in the first and / or second adhesion and / or compression forces.

[0039] Furthermore, it is conceivable to adjust the temperature of the first covering roll and / or the second covering roll and / or the first pressing roll unit and / or the second pressing roll unit to a temperature of 80°C to 150°C, particularly 100°C to 120°C.

[0040] This allows for improved deposition of the first and second powders as a first layer onto the first compression roll unit and / or improved deposition of the third and fourth powders as a second layer onto the second compression roll unit. Furthermore, temperature adjustment of the individual rolls can improve delivery of the first layer to the first side of the substrate and / or delivery of the second layer to the second side of the substrate, since bonding of the individual powders of each layer is enhanced by heat.

[0041] In this case, it is also conceivable to temperature-regulate the supply unit in order to pre-warm the substrate for delivery, i.e. for pressing a first layer onto a first side of the substrate and / or for pressing a second layer onto a second side of the substrate.

[0042] Within the scope of the present invention, it is advantageous that the first pressure roll unit and the second pressure roll unit rotate facing each other at the same first rotation speed, and the ratio of the first rotation speed of the first pressure roll unit to the second rotation speed of the first covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3, and / or the ratio of the first rotation speed of the second pressure roll unit to the third rotation speed of the second covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3.

[0043] When the first pressure roll unit has a first pressure roll and a second pressure roll and / or the second pressure roll unit has a third pressure roll and a fourth pressure roll, the first rotation speed is effective as the rotation speed of the first pressure roll of the first pressure roll unit and the third pressure roll of the second pressure roll unit, since they form a pressure gap. In this case, the second pressure roll and the fourth pressure roll, respectively, may have a rotation speed different from the first rotation speed.

[0044] Here, it has been found to be advantageous that the ratio of rotation speeds results in an increased stability of the first layer or the first at least bilayered powder layer on the current collector of the electrode and / or the second layer or the second at least bilayered powder layer on the current collector of the electrode.

[0045] The above mentioned object is further solved in a third aspect of the present invention by an electrode according to the invention having a bilayer powder layer produced by the above mentioned coating device and / or by the above mentioned method, wherein the substrate is a current collector having a first side and a second side, and the first at least bilayer layer consists of a first powder and a second powder.

[0046] Within the scope of the present invention it is conceivable that the second at least bilayer layer consists of a third powder and a fourth powder.

[0047] Here, the electrode can be used as both an anode and a cathode, in which case the cathode bilayer powder layer can be different from the anode bilayer powder layer, and the anode current collector and the cathode current collector can be different.

[0048] Such electrodes have an optimally compressed first at least bilayer layer and / or a second at least bilayer layer, the first at least bilayer layer and / or the second at least bilayer layer being solvent-free, while the electrodes thus produced have high electrical conductivity and energy density.

[0049] A particularly good ratio of the material usage of the first, second, third and fourth powders for the first at least bilayer layer and / or the second at least bilayer layer of the electrode, or anode or cathode, to the existing electrical conductivity is obtained when the first at least bilayer layer and the second at least bilayer layer have a layer thickness of 40 to 150 μm, where the first powder of the first layer and the third powder of the third layer have a layer thickness of 10 to 70 μm. This also allows for a cost-effective use of materials.

[0050] The advantages discussed with respect to the coating apparatus of the first aspect of the invention also apply to the method of the second aspect of the invention as well as to the electrode of the third aspect of the invention.

[0051] Further advantages, features and details of the invention will become apparent from the following description, in which several embodiments of the invention are described in detail with reference to the drawings. In this application, the features described in the claims and in the specification may each individually or in any combination form the essence of the invention. The invention is illustrated in the following drawings. [Brief description of the drawings]

[0052] [Figure 1] FIG. 2 shows a schematic diagram of a coating apparatus for application and delivery of a first layer. [Diagram 2] FIG. 2 shows a schematic diagram of a coating apparatus for application and delivery of a first layer and a second layer. [Diagram 3] FIG. 2 is a diagram showing a portion of the first metering gap of FIG. 1; [Figure 4] FIG. 2 is a schematic diagram showing a method using the coating apparatus shown in FIG. 1. [Diagram 5] FIG. 3 is a schematic diagram showing a method using the coating apparatus shown in FIG. 2. [Figure 6] FIG. 2 is a schematic diagram of an electrode.

[0053] 1 and 2 each show a coating device 10 for producing an electrode 11 having at least one bilayer powder layer 12, in particular a bilayer cathode layer 13 and / or a bilayer anode layer 14, on a substrate 15, in particular a current collector 16. Here, FIG. 1 shows a coating device 10 for coating on one side of a substrate 15 by deposition 130 and delivery 140 of at least one first bilayer powder layer 12, and FIG. 2 shows a coating device 10 for coating on both sides of a substrate 15 by deposition 130 and delivery 140 of at least one first bilayer powder layer 12, i.e. first bilayer layer 27, and at least one second bilayer powder layer 12, i.e. second bilayer layer 34.

[0054] Both the coating apparatus 10 of FIG. 1 and the coating apparatus 10 of FIG. 2 have a supply unit 17 for supplying 110 the substrate 15 into the compression gap 18, a first metering unit 19 for containing a first powder 20 and a second powder 21 and filling the first metering gap 22 in parallel with the first powder 20 and the second powder 21, and a roll arrangement 23, which has a first coating roll 24, a first compression roll unit 25 and a second compression roll unit 26.

[0055] Here, the first metering gap 22 is provided between the first applied roll 24 and the first pressure roll unit 25, and the pressure gap 18 is provided between the first pressure roll unit 25 and the second pressure roll unit 26.

[0056] The first metering gap 22 is provided for depositing 130 the first powder 20 and the second powder 21 as a first at least two-layer layer 27 onto the first compression roll unit 25 with a first deposition force FA1. The compression gap 18 is provided for transferring 140 the first at least two-layer layer 27 from the first compression roll unit 25 to a first side 28 of the supplied substrate 15 with a compression force FP.

[0057] In order to be able to apply 130 the two-layer powder layer 12 to the substrate 15 on both sides, the coating device 10 of FIG. 2 has a second metering unit 29 which receives a third powder 31 and a fourth powder 32 and fills 120 the second metering gap 30 in parallel with the third powder 31 and the fourth powder 32. The roll arrangement 23 additionally has at least one second application roll 33. The second metering gap 30 is provided between the second application roll 33 and the second pressure roll unit 26, and the second metering gap 30 is provided for applying 130 the third powder 31 and the fourth powder 32 as a second at least two-layer layer 34 to the second pressure roll unit 26 with a second application force FA2. In this case, the pressing gap 18 is also provided for transferring 140 the second at least two-layer layer 34 from the second pressing roll unit 26 to the second side 35 of the supplied substrate 15 by a pressing force FP.

[0058] 2, the first pressure roll unit 25 includes at least one first pressure roll 36 and at least one second pressure roll 37, with at least one first press gap 38 between the at least one first pressure roll 36 and the at least one second pressure roll 37. Additionally, the second pressure roll unit 26 includes at least one third pressure roll 39 and at least one fourth pressure roll 40, with at least one second press gap 41 between the at least one third pressure roll 39 and the at least one fourth pressure roll 40.

[0059] 3 shows an enlarged portion of the first metering gap 22 with the first metering unit 19. Here, the first metering unit 19 has a first separating plate 42 for separating the first powder 20 from the second powder 21 in the region of the first metering gap 22. Further separating plates can likewise be provided in the case of the second metering unit 29 and the second metering gap 30.

[0060] 3 further shows that in the region of the first metering gap 22 a first shielding lamella 44 is provided in the region of the first putter roll 24 and / or a second shielding lamella 45 is provided in the region of the first pressure roll unit 25. Similarly, in the region of the second metering unit 29 or the second metering gap 30 a third shielding lamella 46 can be provided in the region of the second putter roll 33 and / or a fourth shielding lamella 47 can be provided in the region of the second pressure roll unit 26.

[0061] 4 and 5 respectively show a schematic representation of a method 100 for producing an electrode 11 having at least one bilayer powder layer 12, in particular a bilayer cathode layer 13 and / or a bilayer anode layer 14, on a substrate 15, in particular a current collector 16, in a coating apparatus 10 as shown in FIG. 1 or 2: · feeding 110 the substrate 15 into the crimping gap 18 by a feeding unit 17; filling 120 the first metering gap 22 with a first powder 20 and a second powder 21 in parallel by a first metering unit 19; applying 130 the first powder 20 and the second powder 21 as a first at least two-layer layer 27 to a first pressure roll unit 25 in a first metering gap 22 with a first application force FA1; · Transferring 140 the first at least bilayer layer 27 in the first crimping gap 18 to the first side 28 of the substrate 15 with a crimping force FP.

[0062] In the method 100 shown in Fig. 5, which is implemented in the coating apparatus 10 shown in Fig. 2, the second metering unit 29 fills 120 the second metering gap 30 with a third powder 31 and a fourth powder 32 in parallel. Here, the third powder 31 and the fourth powder 32 are applied 130 to the second pressing roll unit 26 in the second metering gap 30 as a second at least two-layered layer 34 by a second application force FA2, and then the second at least two-layered layer 34 is transferred 140 to the second side 35 of the substrate 15 in the pressing gap 18 by a pressing force FP.

[0063] Here, for both embodiments of the coating apparatus 10 or method 100, the first metering unit 19 of Figures 1 and 2 or Figures 4 and 5 continuously fills the first metering gap 22 120, and the second metering unit 29 of Figures 2 or 5 continuously fills the second metering gap 30 120.

[0064] Here, the first metering unit 19 meters the first powder 20 and the second powder 21 in the crimping gap 18 in the case of the first at least two-layer layer 27 such that a first layer thickness SD1 of 40-150 μm is adjusted, whereby the first layer 48 of the first powder 20 has a layer thickness SP1 of 10-70 μm. The same applies for the second metering unit 29, which also meters the third powder 31 and the fourth powder 32 in the case of the second at least two-layer layer 34 in the crimping gap 18 in the case of the third powder 31 such that a second layer thickness SD2 of 40-150 μm is adjusted, whereby the third layer 49 of the third powder 31 has a layer thickness SP3 of 10-70 μm.

[0065] As already described above, the coating apparatus 10 shown in FIG. 2 has a first pressure roll 36 and a second pressure roll 37 in the first pressure roll unit 25, and a third pressure roll 39 and a fourth pressure roll 40 in the second pressure roll unit 26.

[0066] Thus, here the first at least two-layered layer 27 is pressed 150 in at least one first press gap 38 of the first pressure roll unit 25, and the second at least two-layered layer 34 is pressed 150 in at least one second press gap 41 of the second pressure roll unit 26.

[0067] For optimal application and delivery, in the coating apparatus 10 shown in Figure 2, in the method 100 shown in Figure 5, the first application roll 24 and the second application roll 33 and the first pressure roll unit 25 and the second pressure roll unit 26 are thermostated 160 to a temperature between 80°C and 150°C. In this case, each roll can be thermostated 160 to its own temperature.

[0068] In the method 100 shown in Figures 4 and 5, the first pressure roll unit 25 and the second pressure roll unit 26 rotate facing each other at the same first rotation speed v1. In this case, the ratio of the first rotation speed v1 of the first pressure roll unit 25 to the second rotation speed v2 of the first covering roll 24 is 10:1 to 10:4. In the method 100 shown in Figure 5, a second covering roll 33 is provided, in which the ratio of the first rotation speed v1 of the second pressure roll unit 26 to the third rotation speed v3 of the second covering roll 33 is 10:1 to 10:4.

[0069] However, in the method 100 shown in Fig. 5, the second rotation speed v2 of the first applicator roll 24 does not have to correspond to the third rotation speed v3 of the second applicator roll 33. In the method 100 shown in Fig. 5 with the applicator 10 shown in Fig. 2, the first rotation speed v1 is the rotation speed of the first applicator roll 36 of the first applicator roll unit 25 and the third applicator roll 39 of the second applicator roll unit 26, since they form the applicator gap 18. In this case, the second applicator roll 37 and the fourth applicator roll 40 may have a rotation speed different from the first rotation speed v1.

[0070] 6 shows an electrode 11 as produced in the coating apparatus 10 shown in FIG. 2 and the method 100 shown in FIG. 5, the electrode 11 having a first bilayer powder layer 12 and a second bilayer powder layer 12 on a substrate 15. Here, the substrate 15 is a current collector 16 having a first side 28 and a second side 35, and the first at least bilayer layer 27, i.e., the first bilayer powder layer 12, is comprised of a first powder 20 and a second powder 21. Further, the second at least bilayer layer 34, i.e., the second bilayer powder layer 12, is comprised of a third powder 31 and a fourth powder 32. Here, the anode layer 14 has a first layer thickness SD1 and the cathode layer 13 has a second layer thickness SD2 of 40-150 μm, the first powder 20 of the first layer 48 has a first layer thickness SP1 of 10-70 μm and the third powder 31 of the third layer 49 has a third layer thickness SP3 of 10-70 μm, which allows for a cost-efficient use of materials. [Explanation of symbols]

[0071] 10 Coating device 11 electrodes 12 Two-layered powder layer 13 Cathode layer 14 Anode layer 15 Base material 16 Current collector 17 Supply Unit 18 Crimp Gap 19 First metering unit 20 First Powder 21 Second Powder 22 First metering gap 23 Roll equipment 24 First application roll 25 First bonding roll unit 26 Second pressure roll unit 27 First bilayer layer 28 First Side 29 Second metering unit 30 Second metering gap 31 The Third Powder 32 Fourth Powder 33 Second application roll 34 Second bilayer layer 35 Second Side 36 First crimping roll 37 Second bonding roll 38 First press gap 39 Third bonding roll 40 Fourth crimping roll 41 Second press gap 42 First Separation Thin Plate 43 Second Separation Thin Plate 44 First shielding sheet 45 Second shielding sheet 46 Third shielding sheet 47 Fourth Shielding Sheet 48 First Layer 49 Third Layer 100 ways 110 supply 120 Parallel filling 130 Adherence 140 Delivery 150 Press 160 Temperature adjustment FA1 First adhesion FP Crimping Force FA2 Second Adhesion SD1 1st layer thickness SD2 Second layer thickness SP1 Thickness of the first layer SP3 Third layer thickness v1 First rotation speed v2 Second rotation speed v3 Third rotation speed

Claims

1. A coating device (10) for producing an electrode (11) having at least one bilayer powder layer (12), in particular a bilayer cathode layer (13) and / or a bilayer anode layer (14), on a substrate (15), in particular a current collector (16), comprising: The coating device (10) comprises: a supply unit (17) for supplying (110) a substrate (15) into the crimping gap (18); a first dosing unit (19) that contains a first powder (20) and a second powder (21) and fills (120) a first dosing gap (22) with said first powder (20) and said second powder (21) in parallel; A roll facility (23); It has The roll facility (23) comprises a first application roll (24), a first pressure roll unit (25) and a second pressure roll unit (26), the first metering gap (22) is provided between the first applied roll (24) and the first pressure roll unit (25), and the pressure gap (18) is provided between the first pressure roll unit (25) and the second pressure roll unit (26); the first metering gap (22) is provided for applying (130) the first powder (20) and the second powder (21) as a first at least two-layer layer (27) to the first pressure roll unit (25) with a first application force (FA1); the pressing gap (18) is provided for transferring (140) the first at least two-layered layer (27) from the first pressing roll unit (25) to a first side (28) of the supplied substrate (15) by a pressing force (FP); A coating device (10).

2. a second metering unit (29) is provided which contains a third powder (31) and a fourth powder (32) and which fills (120) the second metering gap (30) with said third powder (31) and said fourth powder (32) in parallel, The roll facility (23) comprises at least one second coating roll (33), a second metering gap (30) is provided between the second application roll (33) and the second pressure roll unit (26); the second metering gap (30) is provided for depositing (130) the third powder (31) and the fourth powder (32) as a second at least two-layered layer (34) onto the second pressing roll unit (26) with a second deposition force (FA2); the pressing gap (18) is provided for transferring (140) the second at least two-layered layer (34) from the second pressing roll unit (26) to a second side (35) of the supplied substrate (15) by a pressing force (FP); The coating device (10) of claim 1.

3. the first pressure roll unit (25) comprises at least one first pressure roll (36) and at least one second pressure roll (37), with at least one first press gap (38) between the at least one first pressure roll (36) and the at least one second pressure roll (37); and / or the second pressure roll unit (26) has at least one third pressure roll (39) and at least one fourth pressure roll (40), and at least one second press gap (41) is provided between the at least one third pressure roll (39) and the at least one fourth pressure roll (40); The coating device (10) according to claim 1 or 2.

4. the first metering unit (19) has a first separating plate (42) for separating the first powder (20) and the second powder (21) in the region of the first metering gap (22); and / or the second metering unit (29) has a second separating plate (43) for separating the third powder (31) and the fourth powder (32) in the region of the second metering gap (30). The coating device (10) according to any one of claims 1 to 3.

5. in the region of the first metering gap (22), a first shielding lamella (44) is provided in the region of the first application roll (24) and / or a second shielding lamella (45) is provided in the region of the first pressure roll unit (25), and / or in the region of the second metering gap (30), a third shielding lamella (46) is provided in the region of the second application roll (33) and / or a fourth shielding lamella (47) is provided in the region of the second pressure roll unit (26), The coating device (10) according to any one of claims 1 to 4.

6. A method (100) for producing an electrode (11) having at least one bilayer powder layer (12), in particular a bilayer cathode layer (13) and / or a bilayer anode layer (14), on a substrate (15), in particular a current collector (16), in a coating device (10) according to any one of claims 1 to 5, comprising the steps of: Feeding (110) a substrate (15) into the crimping gap (18) by a feeding unit (17); - filling (120) the first metering gap (22) with a first powder (20) and a second powder (21) in parallel by a first metering unit (19); A step (130) of depositing the first powder (20) and the second powder (21) as a first at least two-layer layer (27) on a first pressure roll unit (25) in the first metering gap (22) with a first deposition force (FA1); transferring (140) the first at least bi-layer layer (27) to a first side (28) of the substrate (15) in a first of the crimp gaps (18) by a crimping force (FP); The method (100),

7. The second metering unit (29) fills (120) the second metering gap (30) with a third powder (31) and a fourth powder (32) in parallel, and the third powder (31) and the fourth powder (32) are applied (130) in the second metering gap (30) as a second at least two-layer layer (34) to the second pressure roll unit (26) with a second application force (FA2); The second at least bi-layer layer (34) is delivered (140) to a second side (35) of the substrate (15) by the pressing force (FP) in the pressing gap (18); The method of claim 6.

8. The method (100) according to claim 6 or 7, wherein the first metering unit (19) continuously fills (120) the first metering gap (22) and / or the second metering unit (29) continuously fills (120) the second metering gap (30).

9. the first metering unit (19) meters the first powder (20) and the second powder (21) in the crimping gap (18) in the case of the first at least two-layer layer (27) in such a way that a first layer thickness (SD1) of 40 to 150 μm is adjusted, and the first layer (48) made of the first powder (20) has a layer thickness (SP1) of 10 to 70 μm; and / or the second metering unit (29) meters the third powder (31) and the fourth powder (32) in such a way that in the case of the second at least two-layer layer (34) a second layer thickness (SD2) of 40 to 150 μm is adjusted in the compression gap (18), and the first layer (49) made of the third powder (31) has a layer thickness (SP3) of 10 to 70 μm. The method (100) of any one of claims 6 to 8.

10. pressing (150) said first at least bi-layer layer (27) in at least one first pressing nip (38) of said first pressing roll unit (25); and / or pressing (150) the second at least bi-layered layer (34) in at least one second pressing nip (41) of the second pressure roll unit (26); The method (100) of any one of claims 6 to 9.

11. The method (100) according to any one of claims 6 to 10, wherein the first applying roll (24) and / or the second applying roll (33) and / or the first pressure roll unit (25) and / or the second pressure roll unit (26) are thermostated (160) to a temperature of 80°C to 150°C.

12. 12. The method (100) according to any one of claims 6 to 11, wherein the first pressure roll unit (25) and the second pressure roll unit (26) rotate opposite each other at the same first rotational speed (v1), and wherein a ratio between the first rotational speed (v1) of the first pressure roll unit (25) and the second rotational speed (v2) of the first apply roll (24) is between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:3, and / or a ratio between the first rotational speed (v1) of the second pressure roll unit (26) and the third rotational speed (v3) of the second apply roll (33) is between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:

3.

13. Electrode (11) having a two-layer powder layer (12) produced by the coating device (10) according to any one of claims 1 to 5 and / or the method (100) according to any one of claims 6 to 12, The substrate (15) is a current collector (16) having a first side (28) and a second side (35); The first at least bilayer layer (27) comprises a first powder (20) and a second powder (21); Electrode (11).

14. 14. The electrode (11) of claim 13, wherein the second at least bi-layer (34) comprises a third powder (31) and a fourth powder (32).

Citation Information

Patent Citations

  • Manufacturing apparatus for electrode for lithium ion secondary battery

    JP2016119207A

  • Manufacturing method of electrode plate

    JP2018101518A

  • Method for manufacturing electrode

    JP2018125201A

  • Method for manufacturing electrode for secondary battery

    JP2018147807A

  • Dry film manufacturing method, rolling device, dry film, and substrate coated with dry film

    JP2020522090A