Laminate and decorative sheet
A decorative sheet with a top coat layer having specific pKa values and a hindered amine light stabilizer addresses aggregation and breakdown issues, ensuring long-term weather resistance and adhesion.
Patent Information
- Application Number
- JP2024125765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2037-08-07
AI Technical Summary
Existing decorative sheets using UV absorbers and light stabilizers face issues with aggregation, chemical structure breakdown, and bleed-out, leading to decreased adhesion and stickiness, compromising weather resistance over time.
A decorative sheet with a top coat layer containing a photostabilizer with a pKa of 4.0 to 7.0 and an ultraviolet absorber with a pKa of -4.5 to -5.5, combined with a hindered amine light stabilizer of molecular weight 600 or more, is used to prevent decomposition and maintain weather resistance.
The solution provides a decorative sheet with stable weather resistance by preventing UV absorber and photostabilizer decomposition, enhancing adhesion and reducing stickiness, thus maintaining appearance and durability.
Smart Images

Figure 2024144666000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin laminate such as a resin film, and a decorative sheet using the same for use as a building interior material, a building exterior member such as an entrance door, the surface of fittings, the surface material of home appliances, etc. [Background technology]
[0002] In recent years, many decorative sheets using olefin resins have been proposed as alternatives to polyvinyl chloride decorative sheets. These decorative sheets are used to protect architectural interior materials for houses and public facilities, architectural exterior materials such as entrance doors, surfaces of fixtures, and surface materials of home appliances. For this reason, they are exposed to direct sunlight and wind and rain every day, and therefore require extremely high weather resistance (see Patent Document 1). The decorative sheet described in Patent Document 1 aims to improve weather resistance by blending light stabilizers, ultraviolet absorbers, etc. in the topcoat layer. However, it is known that with long-term use, the light stabilizers and ultraviolet absorbers are lost due to bleeding out of the topcoat layer, and the chemical structure of each material is destroyed by oxygen and light, causing a loss of function. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4032829 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when attempting to incorporate an ultraviolet absorber or light stabilizer in an amount sufficient to provide sufficient weather resistance to a target resin layer such as a top coat layer, aggregation of the ultraviolet absorber or light stabilizer blended in the resin composition constituting the resin layer may occur. Furthermore, the chemical structure of the ultraviolet absorber or light stabilizer in the resin composition is broken down and reduced in molecular weight, so that the decomposed components of the ultraviolet absorber or light stabilizer are likely to rise from the surface of the resin layer, i.e., so-called bleed-out occurs. This causes problems such as a decrease in adhesion to other resin layers. Furthermore, the components rise to the surface layer, causing problems such as stickiness.
[0005] The present invention has been made in view of the above-mentioned points, and has as its object to provide a decorative sheet having stable weather resistance. [Means for solving the problem]
[0006] The inventors have conducted various investigations into conditions that prevent the decomposition of the UV absorber and light stabilizer over time and enable use over a long period of time without deterioration in quality, and have found suitable conditions for the top coat layer. In order to solve the problems, a laminate according to a first aspect of the present invention is a laminate consisting of a plurality of resin layers, characterized in that the top coat layer located on the outermost surface side of the laminate contains a light stabilizer having a pKa of 4.0 to 7.0 and an ultraviolet absorber having a pKa of -4.5 to -5.5 when irradiated with light. A decorative sheet according to a first aspect of the present invention is characterized by comprising the above laminate. Effect of the Invention
[0007] According to one aspect of the present invention, by using a laminate having the above-mentioned configuration, it is possible to provide a decorative sheet having stable weather resistance over a long period of time. The light stabilizer is a hindered copolymer having an amino ether group and a molecular weight of 600 or more. By using a triazine or benzotriazole based ultraviolet absorbing agent or by using an ultraviolet absorbing agent having a triazine skeleton or a benzotriazole skeleton and a molecular weight of 400 or more, it is possible to provide a decorative sheet with further improved weather resistance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view illustrating a laminate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described with reference to the drawings. Here, the configuration shown in Fig. 1 is schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, etc. differ from the actual ones. Furthermore, the embodiments shown below are examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited to the materials, shapes, structures, etc. of the components described below. The technical idea of the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.
[0010] As shown in FIG. 1, the decorative sheet 1 of this embodiment is configured by arranging an ink layer 5, an adhesive layer 4, a transparent resin layer 3 as a surface protective layer, and a top coat layer 2 in this order on an original fabric layer 6 that constitutes a base material layer. An embossed pattern 3a that constitutes a concave-convex pattern is formed on the upper surface of the transparent resin layer 3. The concave-convex pattern may be formed by a method other than embossing. The transparent resin layer 3 is configured from an olefin resin layer. In the example of FIG. 1, an adhesive resin layer 7 is provided between the transparent resin layer 3 and the adhesive layer 4 to improve adhesion, but the adhesive resin layer 7 may not be provided.
[0011] This decorative sheet 1 is produced, for example, by forming an adhesive layer 4 on an original resin sheet having an ink layer 5 formed on one side of an original layer 6 to form a first laminate, and by forming a topcoat layer 2 containing an ultraviolet absorber and a light stabilizer on a resin sheet having a transparent resin layer 3 and an adhesive resin layer 7 co-extruded thereon to form a second laminate, and then bonding the first laminate and the second laminate together by dry lamination, extrusion lamination, or the like. The details of each layer are described below.
[0012] <Topcoat layer> A topcoat layer 2, which functions to protect the surface and adjust the gloss, is provided on the outermost layer of the decorative sheet 1. The topcoat layer 2 contains an ultraviolet absorbing agent and a light stabilizer. Here, in FIG. 1, the topcoat layer 2 is formed on the entire surface of the transparent resin layer 3 along the surface of the transparent resin layer 3, but is not limited thereto. The topcoat layer 2 may be embedded by wiping the recesses of the embossed pattern 3a formed on the transparent resin layer 3, by applying a resin composition to the recesses, and then scraping off the coating liquid with a squeegee or the like, so that the resin composition is embedded only in the recesses. The surface of the topcoat layer 2 may be flat, regardless of the recesses of the embossed pattern 3a. The topcoat layer 2 only needs to be embedded in at least the recesses of the embossed pattern 3a, and the embedded topcoat layer 2 can maintain high weather resistance even in the recesses where the layer thickness is thinned by forming the embossed pattern 3a. By providing the topcoat layer 2 so as to cover the entire surface of the transparent resin layer 3, a decorative sheet 1 with better weather resistance can be provided.
[0013] (Resin material) The resin material that is the main component of the topcoat layer 2 can be appropriately selected from polyurethane, acrylic silicone, fluorine, epoxy, vinyl, polyester, melamine, aminoalkyd, urea, and other resin materials. The type of the adhesive may be, but is not limited to, a one-liquid type, a two-liquid type, an ultraviolet curing method, or the like. Here, the term "main component" in this specification refers to a resin material that is contained in 70% by mass or more, and preferably 90% by mass or more, of the material that constitutes the target layer.
[0014] As the resin material used as the main component of the topcoat layer 2, a urethane-based resin using isocyanate is preferable from the viewpoints of workability, cost, cohesive strength of the resin itself, etc. As the isocyanate, a suitable curing agent such as an adduct, biuret, or isocyanurate, which is a derivative of tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), hexamethylene diisocyanate (HMDI), diphenylmethane diisocyanate (MDI), lysine diisocyanate (LDI), isophorone diisocyanate (IPDI), bis(isocyanatemethyl)cyclohexane (HXDI), trimethylhexamethylene diisocyanate (TMDI), etc., is suitable for use, but in consideration of weather resistance, a curing agent based on hexamethylene diisocyanate (HMDI) or isophorone diisocyanate (IPDI) having a linear molecular structure is preferable.
[0015] In addition, when improving the surface hardness, it is preferable to use a resin that is cured by active energy rays such as ultraviolet rays and electron beams. As the main material, known materials such as various monomers and commercially available oligomers can be used, but it is preferable to use polyfunctional monomers such as pentaerythritol triacrylate (PET3A), pentaerythritol tetraacrylate (PET4A), trimethylolpropane triacrylate (TMPTA), dipentaerythritol hexaacrylate (DPHA), polyfunctional oligomers such as Shikoh UV-1700B (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), or mixtures thereof.
[0016] These resins can be used in combination with one another. For example, a hybrid of a thermosetting resin and a photocurable resin can be used to improve surface hardness, suppress shrinkage upon curing, and improve adhesion. In this case, the topcoat layer 2 may be made up of multiple layers, for example, two layers: a thermosetting layer mainly made of a thermosetting resin, and a photocurable layer mainly made of a photocurable resin such as an ultraviolet curable resin. By making the topcoat layer up to two curable layers in this way, the surface hardness of the decorative sheet 1 can be improved. In this case, it is preferable that the photocurable layer is on the surface layer side.
[0017] (Light stabilizers and UV absorbers) In this embodiment, the top coat layer 2 contains a light stabilizer having a pKa of 4.0 to 7.0, and an ultraviolet absorbing agent having a pKa of −4.5 to −5.5 when irradiated with light. Here, when the topcoat layer 2 is composed of multiple layers, one or more of the multiple layers contain a light stabilizer having a pKa of 4.0 to 7.0 and an ultraviolet absorber having a pKa of -4.5 to -5.5 when irradiated with light. In this case, it is preferable that the other layers contain either a light stabilizer having a pKa of 4.0 to 7.0 or an ultraviolet absorber having a pKa of -4.5 to -5.5 when irradiated with light.
[0018] When the top coat layer 2 is constructed of two layers, a thermosetting layer and a photocurable layer, as described above, it is preferable to blend the above-mentioned ultraviolet absorber and light stabilizer on the thermosetting layer side. In this embodiment, the amount of ultraviolet absorber and light stabilizer in the layer in which they are blended is 1.0 to 15.0 parts by mass of ultraviolet absorber and 0.1 to 5.0 parts by mass of light stabilizer per 100 parts by mass of resin material. The light stabilizer is preferably a hindered amine light stabilizer having an amino ether group and a molecular weight of at least 600. The molecular weight of the light stabilizer may be measured, for example, in terms of number average molecular weight.
[0019] The method for measuring the number average molecular weight of the light stabilizer is not particularly limited, but may be, for example, gel permeation chromatography. It is preferable to use a GPC column packing material such as polystyrene gel and an eluent such as tetrahydrofuran (THF). It is also preferable to use a polystyrene polymer as a standard substance for GPC. However, when the light stabilizer is composed of a single substance, and the structure is known, the molecular weight of the light stabilizer may be calculated from the structural formula.
[0020] The ultraviolet absorber is preferably an ultraviolet absorber having a triazine skeleton or a benzotriazole skeleton and a molecular weight of at least 400. The molecular weight of the ultraviolet absorber may be calculated from its structural formula, or may be a number average molecular weight measured by a known method. For example, the ultraviolet absorber is a compound (1) having a hydroxyphenyltriazine skeleton or a compound (2) having a benzotriazole skeleton, which are preferably compounds having a maximum absorption at 270 nm to 400 nm. The ultraviolet absorbers are excited by absorbing light, and hydrogen atoms move within the molecule depending on the skeleton. They can return to the ground state by releasing heat. These can be shown by reaction formulas (3) and (4), respectively.
[0021] [ka]
[0022] [ka]
[0023] [ka]
[0024] [ka]
[0025] Examples of the compound having the hydroxyphenyltriazine skeleton include 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-dimethylphenyl)-s-triazine, 2-(2-hydroxy-4-hexyloxyphenyl)-4,6-diphenyl-s-triazine, 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-dimethylphenyl)-s-triazine, 2-[2-hydroxy-4-(3-dodecyloxy-2-hydroxypropyloxy)phenyl]-4,6-bis(2,4-dimethylphenyl)-s-triazine, 2-[2-hydroxy-4-(3-tridecyloxy-2-hydroxypropyloxy)phenyl]-4,6-bis(2,4-dimethylphenyl)-s-triazine, 2-[2-hydroxy-4-[3-(2-ethylhexyloxy)-2-hydroxypropyloxy]phenyl]-4,6-bis(2,4-dimethylphenyl)-s-triazine, 2-(2-hydroxy-4-hexyloxyphenyl)-4,6-dibiphenyl-s-triazine, 2-[2-hydroxy-4-[1-(i-octyloxycarbonyl)ethyloxy]phenyl]-4,6-dibiphenyl- Examples of such an s-triazine include 2,4-bis(2-hydroxy-4-octoxyphenyl)-6-(2,4-dimethylphenyl)-s-triazine, 2,4-bis(4-butoxy-2-hydroxyphenyl)-6-(2,4-dibutoxyphenyl)-s-triazine, 2,4,6-tris(2-hydroxy-4-octoxyphenyl)-s-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine (trade name CYASORB® UV-1164), and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine (trade name LA-F70).
[0026] Examples of the compound having the benzotriazole skeleton include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-(2-(octyloxycarbonyl)ethyl)phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-dodecyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-(2'-hydroxy 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-(dimethylbenzyl)phenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2,2'-methylene-bis(2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2-(2'-hydroxy-3'-(3,4,5,6-tetrahydrophthalimidylmethyl)-5'-methylbenzyl)phenyl)benzotriazole, 2-(5-chloro-2H-benzotriazol-2-yl)-6-tert-butyl-4-methylphenol (trade name LA-36), 2-(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol (trade name Tinuvin (registered trademark) 326), and the like.
[0027] Examples of benzotriazole-based ultraviolet absorbers include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, and 2,2'-methylenebis(4-tert-octyl-6-benzotriazolyl)phenol.
[0028] Examples of triazine-based ultraviolet absorbers include 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine. Examples include (2,4-dimethylphenyl)-1,3,5-triazine.
[0029] Benzophenone-based UV absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 2-hydroxy-4-octoxybenzophenone. benzophenone, 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone), and the like. Benzoate-based ultraviolet absorbers include phenyl salicylate, resorcinol monobenzoate, 2,4-di-tert-butylphenyl-3',5'-di-tert-butyl-4'-hydroxybenzoate, 2,4-di-tert-amylphenyl-3',5'-di-tert-butyl-4'-hydroxybenzoate, and hexadecyl-3,5-di-tert-butyl-4-hydroxybenzoate.
[0030] Examples of cyanoacrylate-based ultraviolet absorbents include ethyl-α-cyano-β,β-diphenylacrylate, and methyl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate. The light stabilizer is the following hindered amine compound (5), which can capture radicals through the reaction of reaction formula (6).
[0031] [ka]
[0032] [ka]
[0033] Hindered amine light stabilizers include bis(2,2,6,6-tetramethylpiperidin-4-yl)sebacate; bis(2,2,6,6-tetramethylpiperidin-4-yl)succinate; bis(1,2,2,6,6-pentamethylpiperidin-4-yl)sebacate; bis(1-octyloxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate; bis(1,2,2,6,6 -Pentamethylpiperidin-4-yl)n-butyl 3,5-di-tert-butyl 4-hydroxybenzyl malonate;1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidine and succinic acid condensate;2,2,6,6-Tetramethylpiperidin-4-yl stearate;2,2,6,6-Tetramethylpiperidin-4-yl dodecane;1,2,2,6,6- Pentamethylpiperidin-4-yl stearate;1,2,2,6,6-Pentamethylpiperidin-4-yl dodecane;Condensation product of N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-tert-octylamino-2,6-dichloro-1,3,5-triazine;Tris(2,2,6,6-tetramethylpiperidin-4-yl)nitrilotriacetate;Tetrakis(2,2,6,6-tetramethylpiperidin-4-yl) 4-Benzoyl-2,2,6,6-tetramethylpiperidine;4-Stearyloxy-2,2,6,6-tetramethylpiperidine;Bis(1,2,2,6,6-pentamethylpiperidyl)-2-n-butyl 2-(2-hydroxy-3,5-di-tert-butylbenzyl)malonate;3-n-octyl-7,7,9,9-tetramethyl-1,3,8-triaza;4-Benzoyl-2,2,6,6-tetramethylpiperidine;4-Stearyloxy-2,2,6,6-tetramethylpiperidine;Bis(1,2,2,6,6-pentamethylpiperidyl)-2-n-butyl 2-(2-hydroxy-3,5-di-tert-butylbenzyl)malonate;3-n-octyl-7,7,9,9-tetramethyl-1,3,8-triaza Spiro[4.5]decane-2,4-dione;Bis(1-octyloxy-2,2,6,6-tetramethylpiperidyl)sebacate;Bis(1-octyloxy-2,2,6,6-tetramethylpiperidyl)succinate;Condensation product of N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-morpholino 2,6-dichloro-1,3,5-triazine;2-Chloro-4,6-bis(4-n-butylamine) Condensation products of 2-chloro-4,6-bis(4-n-butylamino-1,2,2,6,6-pentamethylpiperidyl)-1,3,5-triazine and 1,2-bis-(3-aminopropylamino)ethane;Condensation products of 8-acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro[4.5]Decane-2,4-dione;3-Dodecyl-1-(2,2,6,6-tetramethylpiperidin-4-yl)pyrrolidine-2,5-dione;3-Dodecyl-1-(1-ethanoyl-2,2,6,6-tetramethylpiperidin-4-yl)pyrrolidine-2,5-dione;3-Dodecyl-1-(1,2,2,6,6-pentamethylpiperidin-4-yl)pyrrolidine-2,5-dione;Mixture of 4-Hexadecyloxy- and 4-Stearyloxy-2,2,6,6-tetramethylpiperidine;N,N'-Bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-Cyclohexyloxy- Condensation products of cyclohexylamino-2,6-dichloro-1,3,5-triazine; condensation products of 1,2-bis(3-aminopropylamino)ethane, 2,4,6-trichloro-1,3,5-triazine and 4-butylamino-2,2,6,6-tetramethylpiperidine; 2-undecyl-7,7,9,9-tetramethyl-1-oxa-3,8-diaza-4-oxospiro[4.5]decane; oxo-piperandinyl-triazine; reaction products of 7,7,9,9-tetramethyl-2-cycloundecyl-1-oxa-3,8-diaza-4-oxospiro[4.5]decane and epichlorohydrin.
[0034] In addition, N-alkoxy hindered amine light stabilizers include tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate; 1,2,3,4-butanetetracarboxylic acid tetrakis(1,2,2,6,6-pentamethyl-4-piperidinyl)ester; 1,2,3,4-butanetetracarboxylic acid 1,2,2,6,6-pentamethyl-4-piperidinyltridecylester; 1,2,3,4-butanetetracarboxylic acid 2,2,6,6-tetramethyl-4-piperidinyltridecylester; 1,2,3,4-butanetetracarboxylic acid 2,2,6,6-tetramethyl-4-piperidinyltridecylester; Examples of the polymer include 1,2,2,6,6-pentamethyl-4-piperidinyl ester of a polymer of tetracarboxylic acid and 2,2,6,6-tetramethyl-2,4,8,10-tetraoxaspiro[5.5]-undecane-3,9-diethanol; 2,2,6,6-tetramethyl-4-piperidinyl ester of a polymer of 1,2,3,4-butanetetracarboxylic acid and 2,2,6,6-tetramethyl-2,4,8,10-tetraoxaspiro[5.5]-undecane-3,9-diethanol; and bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate.
[0035] In addition, hydroxyl-substituted N-alkoxy HALS includes 1-(2-hydroxy-2- 1-(2-hydroxy-2-methylpropoxy)-2,2,6,6-tetramethyl-4-piperidinol; 1-(2-hydroxy-2-methylpropoxy)-4-octadecanoyloxy-2,2,6,6-tetramethylpiperidine; 1-(4-octadecanoyloxy-2,2,6,6-tetramethylpiperidin-1-yloxy)-2-octadecanoyloxy-2-methylpropane; 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol; a reaction product of 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol and dimethylsuccinate. Among these hindered amine-based light stabilizers, representative commercially available ones include, for example, Tinuvin 123, Tinuvin 152, Tinuvin NOR 371 FF, Tinuvin XT850 FF, Tinuvin XT855 FF, TINUVIN 5100, TINUVIN 622SF, Flamestat NOR 116 FF, and Adeka STAB LA-81, manufactured by ADEKA Corp. These may be used alone or in combination of two or more kinds.
[0036] When the UV absorber is blended in the topcoat layer 2, it is preferable to blend 1.0 parts by mass or more and 15.0 parts by mass or less with respect to 100 parts by mass of the resin that is the main component of the topcoat layer 2. More preferably, it is 2.5 parts by mass or more and 8.0 parts by mass or less. If the blending amount of the UV absorber is less than 1.0 part by mass, the effect of stabilizing the resin against UV rays may be low. On the other hand, if it is more than 15.0 parts by mass, there is a high possibility that bleeding out may occur. When a light stabilizer is blended in the topcoat layer 2, it is preferable to blend 0.1 parts by mass or more and 5.0 parts by mass or less with respect to 100 parts by mass of the resin that is the main component of the topcoat layer 2. More preferably, it is 0.3 parts by mass or more and 3.0 parts by mass or less. If the blending amount of the light stabilizer is less than 0.1 parts by mass, the effect of stabilizing the resin against the generated radicals may be low. On the other hand, if it is more than 5.0 parts by mass, there is a high possibility that bleeding out will occur.
[0037] (Other compounds) The top coat layer 2 preferably contains a gloss regulator made of inorganic particles. Examples of the inorganic particles include silica, clay, calcium carbonate, barium sulfate, alumina white, aluminum hydroxide, talc, bentonite, titanium oxide, etc., white carbon such as silicic anhydride, silicic acid hydrate, calcium silicate hydrate, and aluminum silicate hydrate, which are known as colloidal silica, and alumina sol. The particle size of the inorganic particles is preferably 1 μm or more and 20 μm or less. More preferably, it is 3 μm or more and 10 μm or less. If the particle size is smaller than 1 μm, the effect of adjusting the gloss may be low. On the other hand, if it is larger than 20 μm, the possibility of the filler being chipped increases. The inorganic particles contribute to the design (glossiness) of the decorative sheet, and therefore are blended in an amount appropriate for the design. The blending amount is generally 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the resin that is the main component of the top coat layer 2.
[0038] <Transparent resin layer> The transparent resin layer 3 constitutes the base material of the topcoat layer 2, and when the ink layer 5 is provided, it serves as a protective layer that protects the ink layer 5. The transparency of the transparent resin layer 3 needs to be sufficient to allow the ink layer 5 to be visible. Note that the laminate needs to include at least the transparent resin layer 3 and the topcoat layer 2. When the ink layer 5 is not provided, the transparent resin layer 3 does not need to be transparent. The transparent resin layer 3 is preferably a resin layer whose main component is an olefin resin and contains 0.3 parts by mass or more of a compound having a pKa of 7.0 or less per 100 parts by mass of the resin material. The compound having a pKa of 7.0 or less is preferably 15.0 parts by mass or less. The compound having a pKa of 7.0 or less is, for example, the same light stabilizer or ultraviolet absorber as that blended in the top coat layer 2 as described above.
[0039] In the transparent resin layer 3 of this embodiment, an embossed pattern is formed as shown in FIG. The embossed pattern 3a is formed to improve design. The embossed pattern 3a can be formed by a method of forming the embossed pattern 3a by applying heat and pressure using an embossing plate having a concave-convex pattern before forming the topcoat layer 2, or by a method of forming the embossed pattern 3a simultaneously with cooling the sheet using a cooling roll having a concave-convex pattern when forming a film using an extruder.
[0040] The resin material used as the main component of the transparent resin layer 3 is preferably made of an olefin-based resin, and in addition to polypropylene, polyethylene, polybutene, etc., α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pent ... Examples of the polyolefin include a homopolymer or a copolymer of two or more of α-olefins (such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, etc.) and a copolymer of ethylene or α-olefin with other monomers, such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, etc. Furthermore, when the surface strength of the decorative sheet 1 is to be improved, it is preferable to use a highly crystalline polypropylene.
[0041] In addition, various functional additives such as a heat stabilizer, a light stabilizer, an antiblocking agent, a catalyst capture agent, a colorant, a light scattering agent, and a gloss adjuster may be contained as necessary in the resin composition constituting the transparent resin layer 3. These various functional additives can be appropriately selected from well-known additives and used. When non-polar polypropylene is used for the transparent resin layer 3, if the adhesion between the transparent resin layer 3 and the resin layer disposed on the lower surface is low, it is preferable to provide an adhesive resin layer 7. The adhesive resin layer 7 is preferably an acid-modified resin such as polypropylene, polyethylene, or acrylic resin, and the layer thickness is preferably 2 μm or more and 20 μm or less from the viewpoint of adhesiveness and heat resistance. Moreover, the adhesive resin layer 7 is preferably formed by co-extrusion lamination with the transparent resin layer 3 from the viewpoint of improving adhesive strength.
[0042] <Ink layer and adhesive layer> As shown in FIG. 1, an adhesive layer 4 is provided on the lower surface side of the transparent resin layer 3 in order to improve adhesion between the ink layer 5 on the lower surface side and the transparent resin layer 3. The material of the adhesive layer 4 is not particularly limited, but may be appropriately selected from acrylic, polyester, polyurethane, epoxy, etc. The coating method may be appropriately selected depending on the viscosity of the adhesive, but generally, gravure coating is used, and the adhesive is applied by gravure coating to the side of the base fabric layer 6 on which the ink layer 5 is applied, and then laminated with the transparent resin layer 3 and the adhesive resin layer 7. The adhesive layer 4 may be omitted if sufficient adhesive strength is obtained between the transparent resin layer 3 and the ink layer 5.
[0043] An ink layer 5 is provided on the lower surface side of the adhesive layer 4. The ink layer 5 preferably contains at least a light stabilizer. As the light stabilizer, it is preferable to use a hindered amine-based material. By including a light stabilizer in the ink layer 5, it is possible to suppress fading of the pigment caused by radicals generated by deterioration of the binder resin itself that forms the ink layer 5 or the resins of other layers, which reduce the chemical components of the pigment in the ink, thereby maintaining a colorful image for a long period of time. It can be retained. The ink layer 5 of this embodiment includes a picture pattern layer 5a and a solid ink layer 5b. At least the picture pattern layer 5a contains a light stabilizer for the above-mentioned purpose. By providing the solid ink layer 5b on the lower surface side of the picture pattern layer 5a, it is possible to provide hiding power.
[0044] The ink of the picture pattern layer 5a may be used as a binder, such as nitrocellulose, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylic, polyester, etc., alone or modified from each of these. The binder is not particularly limited to water-based, solvent-based, emulsion-based, etc., and the curing method may be a one-liquid type or a two-liquid type using a curing agent. Furthermore, a method of curing the ink by irradiation with active energy rays such as ultraviolet rays or electron beams may be used. In particular, a common method is to use a urethane-based ink and cure it with isocyanate. In addition to these binders, the ink contains pigments, colorants such as dyes, extender pigments, solvents, various additives, etc., contained in ordinary inks. Examples of pigments with high versatility include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolone, cobalt, phthalocyanine, carbon, titanium oxide, iron oxide, and pearls such as mica.
[0045] In the solid ink layer 5b, the same material as the ink used in the picture pattern layer 5a can basically be used, but if the ink is a transparent material, opaque pigments, iron oxide, titanium oxide, etc. can be used. In addition, it is possible to impart hiding power by blending metals such as silver, copper, and aluminum. Generally, flake-shaped aluminum is used. The solid ink layer 5b does not have to be provided. These ink layers 5 can be formed directly on the base layer 6 by gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, inkjet printing, etc. When concealment is imparted by a metal, it is preferable to use a comma coater, a knife coater, a lip coater, metal vapor deposition, a sputtering method, or the like. In addition, for the interface where the resin material or ink is laminated, taking into consideration the adhesiveness, the surface to be laminated can be activated by performing a surface treatment such as corona treatment, ozone treatment, plasma treatment, electron beam treatment, ultraviolet treatment, or dichromate treatment before applying the resin material or ink, and then the lamination process can be performed, thereby improving the adhesiveness between the layers.
[0046] <Original layer> An original fabric layer 6 serving as a base layer is provided on the lower surface side of the ink layer 5. The original fabric layer 6 can be arbitrarily selected from paper such as tissue paper, titanium paper, and resin-impregnated paper, synthetic resins such as polyethylene, polypropylene, polystyrene, polybutylene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, and acrylic, or foams of these synthetic resins, rubbers such as ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene-styrene block copolymer rubber, and polyurethane, organic or inorganic nonwoven fabrics, synthetic paper, and metal foils such as aluminum, iron, gold, and silver. Furthermore, when an olefin-based resin is used as the raw fabric layer 6, the surface is often in an inactive state, so it is preferable to provide a primer layer (not shown) between the raw fabric layer 6 and the substrate (not shown) to which the decorative sheet 1 is attached. In addition, in order to improve the adhesion between the raw fabric layer 6 made of an olefin-based resin and the substrate, it is preferable that the back surface of the raw fabric layer 6 is subjected to corona treatment, plasma treatment, ozone treatment, electron beam treatment, ultraviolet treatment, dichromate treatment, or the like.
[0047] The primer layer may be made of the same material as the ink layer 5. Considering that the sheet 1 will be wound in the form of a web, it is preferable for the sheet 1 to contain an inorganic filler such as silica, alumina, magnesia, titanium oxide or barium sulfate in order to avoid blocking and to increase adhesion to the adhesive. In the decorative sheet 1 of this embodiment, taking into consideration printing workability, cost, etc., it is desirable that the base layer 6 be 20 μm to 150 μm, the adhesive layer 4 be 1 μm to 20 μm, the transparent resin layer 3 be 20 μm to 200 μm, and the top coat layer 2 be 3 μm to 20 μm, and it is preferable that the total thickness of the decorative sheet 1 be in the range of 45 μm to 400 μm.
[0048] <About action and other details> Since UV absorbers and light stabilizers require intermolecular interactions, it is preferable for them to be in close proximity. Here, we will look at the interaction when a UV absorber with a triazine or benzotriazole skeleton is used with a light stabilizer with a hindered amine skeleton. In general, the intermolecular interaction between a UV absorber and a light stabilizer occurs between the conjugated system of the UV absorber and the hindered amine skeleton of the light stabilizer. When a UV absorber absorbs light, there is a high probability that an intramolecular hydrogen bond is formed on the nitrogen of the triazine or benzotriazole skeleton. In other words, the hydrogen on the hydroxyl group is in a state that is easily dissociated.
[0049] And, by coexisting with a light stabilizer having a pKa of more than 7.0, the ultraviolet absorber in an excited state after absorbing light is likely to undergo a side reaction through an acid-base reaction with the light stabilizer. In other words, the ultraviolet absorber and light stabilizer cannot undergo the reactions of the above-mentioned reaction formulas (3), (4), and (6) that are originally generated, and the side reaction increases. In other words, it becomes easy to decompose by light, leading to a decrease in weather resistance. On the other hand, when a light stabilizer having a pKa of 7.0 or less is used, it is difficult to cause an acid-base reaction with the hydrogen on the hydroxyl group of the ultraviolet absorber in an excited state after absorbing light, so that the ultraviolet absorber and light stabilizer are likely to undergo the reactions of reaction formulas (3), (4), and (6). Therefore, weather resistance against light can be improved. In view of these circumstances, in this embodiment, a light stabilizer with a pKa of 4.0 to 7.0 and an ultraviolet absorber with a pKa of -4.5 to -5.5 when irradiated with light are contained in the resin composition constituting the topcoat layer 2, thereby providing a laminate having a topcoat layer 2 with high weather resistance, and a decorative sheet 1 with stable weather resistance can be provided using this laminate.
[0050] In addition, as in this embodiment, the transparent resin layer 3, which is the base material of the topcoat layer 2, is made of an olefin resin and contains 0.3 parts by mass or more of a light stabilizer having a pKa of 7.0 or less, thereby preventing a decrease in the weather resistance of the laminate. This is because, if the pKa of the light stabilizer is greater than 7.0, a side reaction is likely to occur due to an acid-base reaction near the interface between the topcoat layer 2 and the transparent resin layer 3, and the proportion of the light stabilizer in the topcoat layer 2 near the transparent resin layer 3 is likely to decrease. Therefore, it is preferable to use a light stabilizer having a pKa of 7.0 or less for the olefin resin. More preferably, the pKa is 6.0 or less. In addition, it is preferable that the pKa of the compound incorporated in the transparent resin layer 3 is 7.0 or less.
[0051] (Method for measuring the pKa of light stabilizers) A 1:1 solution of 0.1N perchloric acid / dioxane in acetonitrile:chloroform was dropped onto an organic reference substance with a known pKa value in an aqueous system, and the half-neutralization potential (HNP) in a non-aqueous system was titrated. A calibration curve of HNP versus pKa was then plotted. A light stabilizer was then titrated in the same manner, and the corresponding pKa was determined from the calibration curve plot.
[0052] (Method for measuring the pKa of ultraviolet absorbers when absorbing light) Here, the ultraviolet absorber was dissolved in acetonitrile so that the absorbance at the maximum absorption wavelength was 1, and nitrogen was bubbled for 15 minutes. After that, 70% perchloric acid was dropped into this solution to change the pH of the solution. At that time, the absorption spectrum of the solution was measured, and λma From the absorbance at x, the UV absorber and the UV absorber benzotriazole at each pH The pKa of the UV absorber at the time of light absorption was calculated from the point where the values were equal. The absorption spectrum was measured using a Hitachi High-Tech U-4000 spectrophotometer. EXAMPLES
[0053] Specific examples of the laminate and decorative sheet according to the present invention will be described below. For 100 parts by mass of highly crystalline homopolypropylene resin, 0.5 parts by mass of a hindered phenol-based antioxidant (Irganox 1010; manufactured by BASF), 0.5 parts by mass of a triazine-based ultraviolet absorber (CYASORB UV-1164; manufactured by SUNCHEM), and 0.5 parts by mass of a NOR-type light stabilizer (Tinuvin XT850 FF; manufactured by BASF) were used. The blended resin was melt-extruded using an extruder to form a 100 μm-thick transparent highly crystalline polypropylene sheet as a sheet-like transparent resin layer 3. Then, both sides of the obtained transparent resin layer 3 were subjected to a corona treatment to set the wetting tension of the sheet surface to 40 dyn / cm or more.
[0054] On the other hand, a pattern layer 5a was formed on one side of an 80 μm thick polyethylene sheet (raw material layer 6) with concealing properties by gravure printing using a two-component urethane ink (V180; manufactured by Toyo Ink Co., Ltd.), and a primer coat was applied to the other side of the raw material layer 6. Thereafter, a transparent resin layer 3 is applied onto the surface of the picture pattern layer 5a of the base fabric layer 6 using a dry lamination adhesive (Takelac A540, manufactured by Mitsui Chemicals, Inc., application amount 2 g / m 2 ) was interposed between the sheets and the sheet was laminated by dry lamination. An embossed pattern 3a was formed on the surface of the transparent resin layer 3 of the laminated sheets. A top coat layer 2 was formed on the transparent resin layer 3 having the embossed pattern 3a, to obtain a decorative sheet 1 having a total thickness of 190 μm to 200 μm. In each of the following Examples and Comparative Examples, the top coat layer 2 was formed using a composition selected from the following compositions for forming a top coat layer.
[0055] (Topcoat layer forming composition) The composition for forming the top coat layer is composed of a heat-curable composition, a photo-curable composition, or a heat-curable / photo-curable hybrid composition, as described below.
[0056] [Thermosetting composition] The thermosetting composition was prepared by blending the following polymer solution A with the following curing agent, gloss regulator, ultraviolet absorber, and light stabilizer. Polymer solution A In a four-neck flask equipped with a stirrer, a nitrogen inlet tube, and a reflux condenser, 80 g of methyl methacrylate and 20 g of 2-hydroxyethyl methacrylate were introduced, and 100 g of ethyl acetate was added to dissolve them, and the mixture was stirred in a nitrogen atmosphere on an oil bath. Polymerization was initiated by adding sucrose. The mixture was heated and stirred for 5 hours in an oil bath at 60° C. to obtain a colorless, viscous polymer solution A. Blend: 80 parts by mass Hardener Product name: Duranate 24A-100 Blend: 5 parts by mass · Gloss adjuster (inorganic particles) Product name: Sunsphere H122 (AGC Si-Tech Co., Ltd.) Properties: Spherical, average particle size 12μm, pore volume 2ml / g Blend: 10 parts by mass ·UV absorber Product name: Tinuvin 400 (manufactured by BASF) Blend: 5.0 parts by mass Light stabilizer Product name: Tinuvin 123 (manufactured by BASF) Blend: 2.0 parts by mass Dilution solvent Product name: Ethyl acetate Blend: 50 parts by mass
[0057] [Photocurable composition] The photocurable composition was prepared by mixing the following monomer with the following photoinitiator, gloss regulator, and light stabilizer. ·monomer Product name: Dipentaerythritol hexaacrylate Blend: 90 parts by mass Photoinitiators Product name: Irgacure 184 Blend: 8 parts by mass · Gloss adjuster (inorganic particles) Product name: Silica 430 (manufactured by Fuji Silysia Chemical Co., Ltd.) Properties: Amorphous, average particle size 4μm, pore volume 2.3ml / g Blend: 10 parts by mass ·UV absorber Product name: Tinuvin 400 (manufactured by BASF) Blend: 5.0 parts by mass Light stabilizer Product name: Tinuvin 123 (manufactured by BASF) Blend: 2.0 parts by mass Dilution solvent Product name: Ethyl acetate Blend: 60 parts by mass
[0058] [Thermo-curable / photo-curable hybrid composition] The heat-curable / photo-curable hybrid composition was prepared by blending the following polymer solution A and monomer with the following curing agent, photoinitiator, gloss regulator, UV absorber, and light stabilizer. Polymer solution A In a four-neck flask equipped with a stirrer, a nitrogen inlet tube, and a reflux condenser, 80 g of methyl methacrylate and 20 g of 2-hydroxyethyl methacrylate were introduced, and 100 g of ethyl acetate was added to dissolve them, and the mixture was stirred in a nitrogen atmosphere on an oil bath. Polymerization was initiated by adding sucrose. The mixture was heated and stirred for 5 hours in an oil bath at 60° C. to obtain a colorless, viscous polymer solution A. Blend: 40 parts by mass ·monomer Product name: Dipentaerythritol hexaacrylate Blend: 40 parts by mass Hardener Product name: Duranate 24A-100 Blend: 10 parts by mass Photoinitiators Product name: Irgacure 184 Blend: 10 parts by mass · Gloss adjuster (inorganic particles) Product name: Sunsphere H122 (AGC Si-Tech Co., Ltd.) Properties: Spherical, average particle size 12μm, pore volume 2ml / g Blend: 10 parts by mass ·UV absorber Product name: Tinuvin 400 (manufactured by BASF) Blend: 5.0 parts by mass Light stabilizer Product name: Tinuvin 123 (manufactured by BASF) Blend: 2.0 parts by mass Dilution solvent Product name: Ethyl acetate Blend: 50 parts by mass
[0059] <Example 1> As the top coat layer 2, a thermosetting composition (amount of coating after drying: 10 g / m 2 ) was applied to obtain a decorative sheet 1 of Example 1 having a layer thickness of 190 μm. <Example 2> A decorative sheet 1 of Example 2 was obtained in the same manner as in Example 1, except that the UV absorber in the thermosetting composition of Example 1 was replaced with Tinuvin 329 (manufactured by BASF).
[0060] <Example 3> A decorative sheet 1 of Example 3 was obtained in the same manner as in Example 1, except that the light stabilizer in the thermosetting composition of Example 1 was replaced with Tinuvin 152 (manufactured by BASF). <Example 4> As the top coat layer 2, a photocurable composition (amount of coating after drying: 10 g / m 2 ) was applied to obtain a decorative sheet 1 of Example 4 having a layer thickness of 190 μm.
[0061] <Example 5> As the top coat layer 2, a heat-curable / photo-curable hybrid composition (amount of coating after drying: 10 g / m2 ) was applied to obtain a decorative sheet 1 of Example 5 having a layer thickness of 190 μm. <Example 6> As the top coat layer 2, a thermosetting composition (amount of coating after drying: 10 g / m 2 ), photocurable composition (coating amount after drying: 5 g / m 2 ) were laminated in this order to form a topcoat layer 2 consisting of two layers, a thermosetting layer and a photocurable layer, thereby obtaining a decorative sheet 1 of Example 6 having a total thickness of 195 μm.
[0062] <Example 7> As the top coat layer 2, a thermosetting composition (amount of coating after drying: 10 g / m 2 ) and a thermosetting / photocurable hybrid composition (application amount 5 g / m2 after drying) were sequentially laminated to form a topcoat layer 2 consisting of two layers, a thermosetting layer and a thermosetting / photocurable hybrid layer, thereby obtaining a decorative sheet 1 of Example 7 having a total thickness of 195 μm. <Example 8> As the top coat layer 2, a thermosetting composition (amount of coating after drying: 10 g / m 2 ), heat-curable / photo-curable hybrid composition (coating amount after drying: 5 g / m 2 ), photocurable composition (coating amount after drying: 5 g / m 2 ) were laminated in this order to form a topcoat layer 2 consisting of three layers: a thermosetting layer, a thermosetting / photosetting hybrid layer, and a photosetting layer, thereby obtaining a decorative sheet 1 of Example 8 having a total thickness of 200 μm.
[0063] <Comparative Example 1> A decorative sheet of Comparative Example 1 was obtained in the same manner as in Example 1, except that the UV absorber in the thermosetting composition of Example 1 was replaced with Tinuvin 329 and the light stabilizer was replaced with Tinuvin 292 (manufactured by BASF). The ultraviolet absorbents and light stabilizers used are shown in Table 1. Table 1 also shows the evaluation results.
[0064] [Table 1]
[0065] <Evaluation> (Weather resistance (appearance)) The decorative sheets obtained in the examples and comparative examples were set in a metal weather device manufactured by Daipla Wintes Co., Ltd., and were then subjected to light conditions (illuminance: 60 mW / cm 2 , black panel temperature 63℃, internal humidity 50%RH) for 20 hours under condensation conditions (illuminance: 0mW / cm 2 A weather resistance test was conducted in which the panels were left for 4 hours at a temperature of 30°C (black panel temperature, 98% RH inside the layer) and for 500 or 1000 hours under water spray conditions (10 seconds before and after condensation). After the above test, the panels were kept for 2 days at a temperature of 25°C and 50% RH, and then the appearance of the panels, such as cracks and yellowing, was visually evaluated according to the following criteria.
[0066] (Coating appearance) ○: No change in appearance was observed. △: Fine cracks were found on the surface. ×: Numerous cracks were found on the surface. (Yellowing of substrate) ○: No change in appearance was observed. △: Some yellowing was observed. ×: Significant yellowing.
[0067] In the decorative sheets of each Example, as shown in Table 1, a light stabilizer with a pKa of 4.0 to 7.0 and an ultraviolet absorber with a pKa of -4.5 to -5.5 when irradiated with light were contained, which enabled the production of decorative sheets that could suppress changes in glossiness after weathering tests without producing haze, and were also less susceptible to changes in appearance. In addition, by setting the molecular weight of the light stabilizer to 600 or more, and the molecular weight of the ultraviolet absorber to 400 or more, the weather resistance could be further improved. From the above results, it is clear that the decorative sheet 1 of the embodiment based on the present invention is excellent in weather resistance and design. The decorative sheet of the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible without departing from the characteristics of the invention. [Explanation of symbols]
[0068] 1 Decorative sheet 2 Topcoat layer 3 Transparent resin layer (olefin resin layer) 3a Embossed pattern 4 Adhesive layer 5 Ink Layer 5a Pattern layer 5b Solid ink layer 6 Original fabric layer (base material layer) 7 Adhesive resin layer
Claims
1. A laminate consisting of a plurality of resin layers, A laminate characterized in that the top coat layer located on the outermost surface side of the laminate contains a light stabilizer having a pKa of 4.0 to 7.0 and an ultraviolet absorber having a pKa of -4.5 to -5.5 when irradiated with light.
2. 2. The laminate according to claim 1, wherein the light stabilizer is a hindered amine light stabilizer having an amino ether group and a molecular weight of 600 or more.
3. 3. The laminate according to claim 1, wherein the ultraviolet absorbing agent has a triazine skeleton or a benzotriazole skeleton and a molecular weight of 400 or more.
4. 4. The laminate according to claim 1, wherein the top coat layer contains a gloss adjuster made of inorganic particles.
5. 5. The laminate according to claim 1, wherein the top coat layer comprises a thermosetting layer and a photocurable layer formed on the thermosetting layer.
6. The main component of the resin is an olefin resin layer, and the olefin resin layer contains 0.3 parts by mass or more of a compound having a pKa of 7.0 or less per 100 parts by mass of the resin material, 6. The laminate according to claim 1, wherein the top coat layer is formed on the olefin resin layer.
7. A decorative sheet comprising the laminate according to any one of claims 1 to 6.
Citation Information
Patent Citations
Method of producing polarlized light diffraction device
JP2001133627A
Weather resistant hard coat film
JP2012076354A
Laminate
JP2014240200A
Method for manufacturing plastic film
JP2016516847A
Decorative sheet and decorative plate
JP2017007156A