Recovery method of rhodium
The method of adding a water-soluble halide and copper powder to an aqueous solution containing rhodium and copper ions simplifies and enhances the recovery of rhodium by precipitating cuprous halide, achieving high recovery rates.
Patent Information
- Application Number
- JP2023046272
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing methods for recovering rhodium from aqueous solutions containing copper ions are complex and inefficient.
A method involving the addition of a water-soluble halide to an aqueous solution to form cuprous halide, followed by the use of copper powder to precipitate it, allowing for the separation of rhodium ions from copper ions through solid-liquid separation.
Rhodium can be recovered at a high rate with reduced complexity and improved efficiency by this method.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering rhodium from an aqueous solution containing rhodium ions and copper ions. [Background technology]
[0002] Rhodium is more likely to exist in an ionic state in an aqueous solution than other platinum group metals, such as platinum, and therefore requires some ingenuity in separating the rhodium ions from the copper ions when other metal ions, such as copper ions, coexist in the aqueous solution. Conventional techniques relating to the recovery of rhodium from an aqueous solution containing rhodium and copper include those described in Patent Documents 1 to 3, for example. Patent Document 1 describes a method in which crude copper powder is added to a copper solution in which precious metals such as rhodium are dissolved to obtain a primary residue in which the precious metals are solidified, and this primary residue is subjected to a leaching treatment using a used copper electrolyte to obtain a secondary residue in which the precious metal concentration is higher than that of the primary residue, and the precious metals are recovered from the secondary residue.
[0003] Patent Document 2 describes a method of adding sulfate ions to an aqueous solution containing rhodium and copper, thereby separating the resulting crystal component made of copper sulfate from a liquid component containing the remaining rhodium.
[0004] Patent Document 3 describes a process in which a raw material containing copper and rhodium is leached with chlorine gas to obtain a chlorine leachate, and the chlorine leachate is subjected to solvent extraction to separate copper and rhodium. In this process, the following steps (1)-(3) are carried out between leaching and solvent extraction. The copper-depleted mother liquor separated in step (3) is then subjected to the solvent extraction. (1) An alkali is added to the chlorine leachate to obtain a hydroxide precipitate. (2) A sulfuric acid solution is added to the hydroxide to dissolve it, thereby preparing a hydroxide solution. (3) The hydroxide solution is heated and concentrated, then cooled to separate the precipitated copper sulfate crystals from the copper-free mother liquor. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-35800 A [Patent Document 2] JP 2010-163664 A [Patent Document 3] JP 2012-158778 A Summary of the Invention [Problem to be solved by the invention]
[0006] According to the methods described in Patent Documents 1 to 3, recovery of rhodium is possible to some extent, but the recovery process is complicated and the efficiency of rhodium recovery is not necessarily high. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a method for recovering rhodium which can overcome the various drawbacks of the prior art. [Means for solving the problem]
[0007] The present invention relates to a process for producing a rhodium-ion-containing copper ion-containing aqueous solution, the process comprising the steps of: adding a water-soluble halide to an aqueous solution containing rhodium ions and copper ions; adding copper powder to the aqueous solution to produce cuprous halide; and removing the cuprous halide from the aqueous solution. Effect of the Invention
[0008] According to the method of the present invention, recovery of rhodium from an aqueous solution containing rhodium ions and copper ions can be achieved at a high recovery rate without going through complicated steps. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention relates to a method for recovering rhodium from an aqueous solution containing rhodium ions and copper ions. The method of the present invention is roughly divided into the following steps: (1) A step of adding a water-soluble halide to an aqueous solution containing rhodium ions and copper ions (hereinafter also referred to as the "first step"). (2) A step of adding copper powder to the aqueous solution to produce cuprous halide (hereinafter also referred to as the "second step"). (3) A step of removing the cuprous halide from the aqueous solution (hereinafter also referred to as the "third step"). Steps 1 to 3 are carried out in this order. After completion of step 3, additional steps 1 and 2, which will be described later, are carried out as necessary. Each step will be described below.
[0010] <1st process> In this step, first, an aqueous solution from which rhodium is to be recovered (hereinafter also referred to as the "liquid to be recovered") is prepared. This aqueous solution contains rhodium (Rh) ions and copper (Cu) ions. In this specification, "rhodium ions" is a general term for rhodium aqua complexes and complexes having ligands other than H2O. Similarly, "copper ions" is a general term for copper aqua complexes and complexes having ligands other than H2O. There is no particular restriction on the valence of the rhodium ions and copper ions, and rhodium ions and copper ions of various valences may be contained in the liquid to be recovered. It is preferable that copper ions are contained in the liquid to be recovered mainly in the form of divalent ions. The liquid to be recovered may be, for example, a leachate of various ores, a leachate of scraps of various electronic components, or a leachate of an exhaust gas catalyst. During leaching, treatment with various mineral acids may be performed. As a result, the liquid to be recovered may be an aqueous solution containing anions of mineral acids, such as sulfate ions.
[0011] The liquid to be recovered generally contains rhodium ions in an amount of 100 mg / L to 2500 mg / L, and copper ions in an amount of 20,000 mg / L to 50,000 mg / L. When the liquid to be recovered contains sulfate ions, the liquid generally contains 150 g / L or more and 250 g / L or less of sulfate ions. When the liquid to be recovered contains sulfate ions, copper ions are generally known to exist as sulfate complexes. Meanwhile, rhodium ions are generally known to exist as aqua complexes or sulfato complexes.
[0012] The liquid to be recovered may contain ions of metals other than rhodium ions and copper ions, such as As, Ni, Pb, Sn, Zn, Fe, Sb, Bi, S, Te, Se, Au, Ag, Pt, and Pd.
[0013] In this step, a water-soluble halide is added to the liquid to be recovered. The purpose of adding the water-soluble halide is to convert the copper ions contained in the liquid to be recovered into poorly water-soluble cuprous halide and remove it from the liquid to be recovered in the second step described below. For this purpose, a water-soluble halide having a solubility in water of 20 g / 100 g or more at the liquid temperature where the second step is carried out is preferably used. Examples of such water-soluble halides include halides of Group 1 metals and halides of Group 2 metals. Hydrochloric acid can also be used as the water-soluble halide. Among these water-soluble halides, it is particularly preferable to use sodium chloride and potassium chloride, which are Group 1 metal halides, and magnesium chloride, which is a Group 2 metal halide, from the viewpoints of economy and ease of wastewater treatment in the subsequent steps.
[0014] The amount of water-soluble halide added to the liquid to be recovered is preferably 3 moles or more of halide ions per mole of copper in the liquid to be recovered, from the viewpoint of reliably generating poorly water-soluble cuprous halide in the second step. Furthermore, the amount of water-soluble halide added to the liquid to be recovered is preferably 5 moles or less of halide ions per mole of copper in the liquid to be recovered in order to prevent re-dissolution of the cuprous halide, more preferably 4 moles or less, and even more preferably 3.5 moles or less.
[0015] Prior to adding the water-soluble halide to the liquid to be recovered, the pH of the liquid to be recovered may be adjusted. This allows efficient precipitation of the cuprous halide in the next step, the second step. From this viewpoint, the pH of the liquid to be recovered is preferably adjusted to 0 or less, more preferably to -0.2 or less, and even more preferably to -0.4 or less.
[0016] <Second process> In this step, copper powder is added to the liquid to be recovered to which the water-soluble halide has been added. The copper powder is used as a reducing agent for the divalent copper ions contained in the liquid to be recovered. Various substances are known as reducing agents for metal ions, and in the present invention, by using copper powder as a reducing agent, it is possible to reduce only the copper ions among the rhodium ions and copper ions contained in the liquid to be recovered. The reason why only the copper ions are reduced and not the rhodium ions is that the reducing power of copper powder is very weak, so that the copper ions, which have a relatively base ionization tendency, are reduced, but the rhodium ions, which have a relatively noble ionization tendency, are not reduced.
[0017] In detail, the copper powder contains divalent copper ions (Cu 2+ ) to monovalent copper ions (Cu + ), and the copper powder itself is oxidized to monovalent copper ions by reducing the divalent copper ions. As a result, both the monovalent copper ions produced by the reduction of the divalent copper ions and the monovalent copper ions produced by the oxidation of the copper powder react with the halide ions contained in the liquid to be recovered to produce poorly soluble cuprous halide, and no residue is produced.
[0018] The copper powder used in this step preferably contains 70% by mass or more of metallic copper, more preferably 85% by mass or more, and even more preferably 95% by mass or more, from the viewpoint of ensuring the reduction of divalent copper ions. From the same viewpoint, the copper powder is measured using a volume cumulative particle size distribution measurement method using a laser diffraction scattering type particle size distribution measurement method. 50 It is preferable that the thickness is 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less.
[0019] The amount of copper powder added in this step is preferably such that the redox potential (vs. Ag / AgCl) of the liquid to be recovered at the temperature at which this step is carried out is 0 mV or more and 100 mV or less. When copper powder is added, the color of the liquid to be recovered becomes dark green. As the amount of copper powder added increases, the color of the liquid changes to green and finally becomes light warbler. When the color of the liquid becomes light warbler, it means that the reduction of the divalent copper ions in the liquid to monovalent copper ions has been completed. Therefore, it is preferable to add copper powder until the color of the liquid becomes this color.
[0020] <3rd process> In the second step, copper powder is added to the liquid to be recovered, generating copper halide, i.e., cuprous halide, in the liquid. This cuprous halide is poorly soluble in water and precipitates. Meanwhile, rhodium ions are present in the liquid to be recovered. Therefore, in the third step, a solid-liquid separation operation is performed, and the filtrate is recovered from the liquid to be recovered, while the solids are recovered. The solids contain cuprous halide and also small amounts of rhodium. On the other hand, the filtrate contains rhodium ions and a small amount of copper. The concentration of copper ions contained in the filtrate is preferably reduced by 80% or more, more preferably by 90% or more, and even more preferably by 95% or more, relative to the concentration of copper ions contained in the liquid to be recovered. The distribution rate of rhodium in the filtrate after solid-liquid separation is preferably 70 or more, more preferably 80% or more, and even more preferably 85% or more. On the other hand, the distribution rate of copper in the filtrate after solid-liquid separation is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less. The solid-liquid separation can be carried out by a known method, for example, a filtration method such as gravity filtration, vacuum filtration, pressure filtration, centrifugal filtration, a sedimentation method, a centrifugation method, a squeezing method, or the like.
[0021] <Additional process 1> In the third step, after copper ions have been removed and a filtrate containing rhodium ions has been obtained, an additional step 1 can be carried out to recover metallic rhodium from the filtrate. In order to recover metallic rhodium, it is preferable to add a reducing agent to the filtrate to reduce the rhodium ions to metallic rhodium. For this purpose, it is preferable to use, as the reducing agent, metal powders such as zinc powder and iron powder, and inorganic reducing agents such as sodium borohydride, and in particular, it is preferable to use zinc powder, since it provides a high recovery rate of rhodium and can increase the rhodium purity of the reduced product.
[0022] Prior to the addition of the reducing agent to the filtrate, it is preferable to adjust the pH of the filtrate from the viewpoint of gently proceeding with the reduction reaction and from the viewpoint of suppressing re-dissolution of the metallic rhodium produced by the reduction. For this purpose, the pH of the filtrate is preferably adjusted to -0.2 or more and 2 or less, more preferably adjusted to 0 or more and 1.5 or less, and even more preferably adjusted to 0.5 or more and 1 or less. Various pH adjusters, such as sodium hydroxide, can be used to adjust the pH.
[0023] In this way, a reduced product enriched in rhodium, i.e., a metal lump, is obtained. It is preferable to increase the purity of rhodium by subjecting this metal lump to a known refining method.
[0024] <Additional process 2> In the third step, when the solid content containing the cuprous halide is obtained from the liquid to be recovered, an additional step 2 can be carried out to regenerate copper powder from the solid content. From the viewpoint of economic efficiency, it is preferable that the copper powder obtained in this step is supplied to the second step and used for the reduction of the copper ions contained in the liquid to be recovered.
[0025] In this process, to produce copper powder from a solid content containing cuprous halide, the solid content is first mixed with water to obtain a dispersion liquid. From the viewpoints of economy and reactivity, the solid content concentration in this dispersion liquid is preferably 5% by mass or more and 30% by mass or less, more preferably 8% by mass or more and 25% by mass or less, and even more preferably 10% by mass or more and 15% by mass or less.
[0026] Once the dispersion is obtained, a basic substance is added to the dispersion. The basic substance may be a hydroxide of a Group 1 element or a hydroxide of a Group 2 element. Next, the pH of the dispersion is adjusted. Through this series of operations, cuprous hydroxide, which is a poorly water-soluble substance, is produced from the cuprous halide contained in the dispersion. The pH is preferably adjusted to 5 or more and 10 or less, more preferably 6 or more and 8 or less. Various pH adjusters, for example, acidic substances such as hydrochloric acid, may be used to adjust the pH.
[0027] The copper(I) hydroxide thus obtained is recovered from the dispersion by solid-liquid separation. The recovered copper(I) hydroxide contains a trace amount of rhodium. The distribution rate of copper in the cuprous hydroxide recovered by solid-liquid separation is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more. Furthermore, the distribution rate of rhodium in the cuprous hydroxide recovered by solid-liquid separation is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more.
[0028] The recovered cuprous hydroxide is mixed with water to form a dispersion, to which a reducing agent is added to reduce the cuprous hydroxide to obtain metallic copper. A known reducing agent can be used for the reduction of cuprous hydroxide. Examples of such reducing agents include inorganic reducing agents such as hydrazine and sodium borohydride, and metal powders such as zinc powder and iron powder. Of these reducing agents, it is preferable to use sodium borohydride stabilized with sodium hydroxide. This is because copper powder obtained by reduction using sodium borohydride stabilized with sodium hydroxide can be efficiently reduced when it is subjected to the second step and used to reduce copper ions. If copper powder produced by reduction using another reducing agent, such as hydrazine, is subjected to the second step and used to reduce copper ions, sufficient reducing power may not be exerted.
[0029] The sodium borohydride stabilized with sodium hydroxide can be, for example, an aqueous solution containing 40% by weight of sodium hydroxide and 12% by weight of sodium borohydride, such as that available under the trade name "VenSil".
[0030] In this way, the copper powder is regenerated. The obtained copper powder can be fed to the second step as it is or after adjusting the particle size. The copper powder obtained can be supplied in its entirety to the second step, for example. This makes it possible to maintain a balance between the supply and consumption of copper in the method of the present invention, which is very economical. However, it is not necessary to supply the entire amount of the recycled copper powder to the second step, and a portion of it may be used for another purpose. In addition, the copper powder supplied to the second step does not need to be 100% recycled copper powder, and may be a mixture of separately prepared copper powder and the recycled copper powder.
[0031] Although the present invention has been described based on the preferred embodiment, the present invention is not limited to the above embodiment. For example, in addition step 2, the reduction of cuprous hydroxide can be carried out using a combination of two or more reducing agents. EXAMPLES
[0032] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".
[0033] Example 1 (1) First step A liquid to be recovered containing 2130 mg / L of rhodium ions, 37200 mg / L of copper ions, and 221 g / L of sulfate ions was prepared. The pH of this liquid to be recovered was -0.2 (25°C). Sodium chloride was added to this liquid to be recovered. The amount of sodium chloride added was 15% (4.4 moles of halide ions per mole of copper ions) relative to the liquid to be recovered.
[0034] (2)Second process Copper powder (purity 95% or more) was added to the liquid to be recovered, which was kept at a temperature of 25°C. The amount of copper powder added was set so that the ORP of the liquid to be recovered was 230mV (vs. Ag / AgCl). 50 The particle size was 12 μm. The addition of copper powder caused the liquid to turn dark green, then green, and finally light green. Then, precipitation of cuprous chloride occurred in the liquid.
[0035] (3) Third step The liquid to be recovered was filtered to recover the filtrate and solids. The rhodium ion concentrations in the filtrate were 1695 mg / L and 3220 mg / L, respectively. The distribution ratio of rhodium in the filtrate and the solids was 86% and 14%, respectively, and the distribution ratio of copper in the filtrate and the solids was 10% and 90%, respectively.
[0036] (4) Additional process 1 A 24% aqueous sodium hydroxide solution was added to the filtrate recovered in the third step. The amount of the aqueous sodium hydroxide solution added was adjusted so that the pH of the liquid was 0.5 to 1. Next, zinc powder was added to the filtrate. The amount of zinc powder added was such that the ORP was -300 to -200 mV (vs. Ag / AgCl). This resulted in a reduced product in which rhodium was concentrated. The purity of rhodium in the reduced product was 40%. The copper content was 58%. The distribution rate of rhodium in the reduced product was 99.8%, and that of copper was 98.8%.
[0037] (5) Additional process 2 The solid matter recovered in the third step was mixed with water to prepare a dispersion with a solid matter concentration of 15%. A 48% aqueous solution of sodium hydroxide was added to this dispersion. The amount of the aqueous solution of sodium hydroxide added was 72% based on the solid matter. Furthermore, 36% hydrochloric acid was added to the dispersion to adjust the pH to 6 to 8. As a result, cuprous hydroxide was produced in the liquid. The resulting cuprous hydroxide was collected by filtration. The distribution ratio of copper in the collected cuprous hydroxide was 94%. The distribution ratio of rhodium was more than 99%. The recovered cuprous hydroxide was mixed with water to prepare a dispersion. The solid content of the dispersion was 15%. An aqueous solution containing 40% by mass of sodium hydroxide and 12% by mass of sodium borohydride was added to the dispersion to reduce the copper ions, thereby obtaining copper powder. The obtained copper powder was recovered by filtration, and the entire amount of the recovered copper powder was supplied to the second step, whereupon it was confirmed that reduction of copper ions had occurred.
[0038] Comparative Example 1 The same liquid as the liquid to be recovered used in Example 1 was prepared. Zinc powder was added to this liquid to be recovered. The zinc powder was added so that the ORP was -300 to -200 mV (vs. Ag / AgCl). By adding the zinc powder, a reduction product containing rhodium was obtained. The purity of rhodium in the reduction product was 5%. The copper content was 91%.
Claims
1. adding a water-soluble halide to an aqueous solution containing rhodium ions and copper ions; adding copper powder to the aqueous solution to produce cuprous halide; and removing the cuprous halide from said aqueous solution.
2. obtaining copper powder from the cuprous halide removed from the aqueous solution; The method according to claim 1 , further comprising the step of adding the obtained copper powder to the aqueous solution containing rhodium ions and copper ions.
3. generating cuprous hydroxide from the cuprous halide; The method according to claim 2, wherein the copper powder is obtained by reducing the obtained cuprous hydroxide.
4. 4. The method of claim 3, wherein the cuprous hydroxide is reduced with sodium borohydride stabilized with sodium hydroxide.
5. 2. The method according to claim 1, further comprising the step of adding zinc powder to the aqueous solution from which the cuprous halide has been removed to obtain a reduced product in which rhodium is concentrated.
Citation Information
Patent Citations
Method for recovering precious metal and method for producing copper
JP2009035800A
Method of separating rhodium and copper
JP2010163664A
Treating method for separating copper and rhodium from raw material containing copper and rhodium
JP2012158778A