Surface protective film with release film

The surface protection film with a release film, featuring a polyethylene terephthalate and (meth)acrylate copolymer adhesive layer, addresses zipping issues by using an amino-structured release layer with minimal silicone content and controlled peeling forces, enhancing peeling efficiency and reducing contamination.

JP2024144817APending Publication Date: 2024-10-15FUJIMORI KOGYO CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023056952
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Non-silicone release layers in surface protection films are prone to cause zipping when peeled off, leading to potential contamination of the adherend surface.

Method used

A surface protection film with a release film comprising a polyethylene terephthalate film and a (meth)acrylate copolymer adhesive layer, where the release layer contains an amino structure and has a Si content of 0.5 kcps or less, with a glass transition temperature (Tg) of +22°C or less, and a peeling force ratio A=B/C of 1.5 or less, using components that minimize chemical reactions and migration.

Benefits of technology

The solution effectively reduces zipping and surface contamination, ensuring easy peeling and maintaining the integrity of the adherend surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144817000001_ABST
    Figure 2024144817000001_ABST
Patent Text Reader

Abstract

To provide a surface protective film with a release film, in which a non-silicone-based release layer difficult to cause zipping is used.SOLUTION: A surface protective film 10 with a release film, in which the surface protective film 16 has a first substrate layer 14 made of a polyethylene terephthalate film and an adhesive layer 13 made by crosslinking a (meth) acrylate copolymer, the surface protective layer 16 is a surface protective film for optical use or electronic use, the release film 15 has a second substrate layer 11 and a release layer 12 formed on one surface of the second substrate layer 11 and contains an amino structure in the release layer 12 of the release film 15, and Si in the release layer 12 of the release film 15 is 0.5 kcps or less by fluorescent X-rays.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface protection film with a release film. [Background technology]

[0002] 2. Description of the Related Art Surface protective films are used to protect the surfaces of optical components, electronic components, and the like. For example, Patent Document 1 describes that in an optical surface protection film with a separator having a separator on the opposite side of the pressure-sensitive adhesive layer to the polyester film, the Si-Kα ray intensity of the surface of the pressure-sensitive adhesive layer after the separator is peeled off is 2.5 kcps or less in fluorescent X-rays. Patent Document 2 describes an optical surface protection film with a separator, in which the separator has a substrate and a non-silicone release layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-145341 A [Patent Document 2] JP 2017-31278 A Summary of the Invention [Problem to be solved by the invention]

[0004] When a non-silicone release layer is used, zipping is likely to occur when the release film is peeled off from the pressure-sensitive adhesive layer of the surface protection film.

[0005] An object of the present invention is to provide a surface protection film with a release film which is less susceptible to zipping. [Means for solving the problem]

[0006] A first aspect of the present invention is a surface protection film with a release film, the surface protection film having a first base layer made of a polyethylene terephthalate film and an adhesive layer made by crosslinking a (meth)acrylate copolymer, the surface protection film being an optical or electronic surface protection film, the release film having a second base layer and a release layer formed on one side of the second base layer, the release layer of the release film containing an amino structure, and Si in the release layer of the release film being 0.5 kcps or less by fluorescent X-ray.

[0007] The second aspect is a surface protection film with a release film, wherein, in the first aspect, the Tg of the surface protection film is +22°C or lower and the release layer of the release film contains a component that does not chemically react with the amino structure. A third aspect is a surface protection film with a release film according to the first or second aspect, wherein the Tg of the surface protection film is +11° C. or lower.

[0008] A fourth aspect is a surface protection film with a release film, in which, in any one of the first to third aspects, when the release film is peeled at a peel speed of 0.3 m / min and a peel angle of 180 degrees, the instantaneous maximum peel force is B and the average peel force when the release film is peeled at a peel speed of 0.3 m / min and a peel angle of 180 degrees is C, the value A calculated by the formula A=B / C is 1.5 or less. The fifth aspect is a surface protection film with a release film, in which, in any one of the first to fourth aspects, when the average peel force C is defined as when the release film is peeled at a peel speed of 0.3 m / min and a peel angle of 180 degrees, C is greater than 0.02 N / 25 mm.

[0009] A sixth aspect is a surface protection film with a release film according to any one of the first to fifth aspects, wherein the release layer of the release film contains a melamine structure. A seventh aspect is a surface protection film with a release film according to any one of the first to sixth aspects, wherein the release layer contains any one of acrylic, polyol, and polyether. Effect of the Invention

[0010] According to the present invention, it is possible to provide a surface protection film with a release film that uses a non-silicone release layer and is less susceptible to zipping. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a surface protection film with a release film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the present invention will be described based on preferred embodiments.

[0013] As shown in FIG. 1, a surface protective film 10 with a release film of the embodiment has a release film 15 and a surface protective film 16 .

[0014] The surface protection film 16 has a first base layer 14 made of a polyethylene terephthalate (PET) film and a pressure-sensitive adhesive layer 13 made by crosslinking a (meth)acrylate copolymer. The surface protection film 16 is a surface protection film for optical or electronic use.

[0015] Release film 15 has second base layer 11 and release layer 12 formed on one surface of second base layer 11. Release layer 12 of release film 15 contains an amino structure. Si in release layer 12 of release film 15 has a fluorescent X-ray intensity of 0.5 kcps or less.

[0016] In the surface protective film 10 with a release film of the embodiment, the Si in the release layer 12 of the release film 15 is 0.5 kcps or less by fluorescent X-rays. The amount of Si in the release layer 12 can be quantified by the intensity (kcps) of Si-Kα rays using fluorescent X-ray analysis. The amount of Si in the release layer 12 does not include the amount of Si in the second base layer 11. The amount of Si in the release layer 12 may be obtained by measuring the amount of Si in the release film 15 from the release layer 12 side, and then subtracting the amount of Si in the second base layer 11 not having the release layer 12.

[0017] The small amount of Si in the release layer 12 confirms that the content of silicone-based components such as organic silicone compounds in the release layer 12 is small. If the release layer contains a silicone-based component, when the release film and the surface protection film are bonded together, the silicone-based component may migrate in large quantities to the surface of the adhesive layer. In addition, the silicone-based component that has migrated to the surface of the adhesive layer may contaminate the surface of the adherend, such as an optical member or an electronic member. Therefore, by having the amount of Si in the release layer 12 within the above-mentioned range, surface contamination of the adhesive layer and the adherend can be suppressed.

[0018] In the surface protection film 10 with a release film of the embodiment, the release film 15 contains an amino structure in the release layer 12. The release layer 12 containing an amino structure may contain a component having an amino structure. Specific examples include a configuration consisting of one component having an amino structure, a configuration consisting of two or more components having amino structures, and a configuration consisting of at least one component having an amino structure and at least one component not having an amino structure.

[0019] The release layer 12 may be composed of one component or two or more components. When the release layer 12 is composed of a composition containing two or more components, chemical reactions, chemical bonds, etc. may occur between the components contained in the composition.

[0020] The component having an amino structure is not particularly limited, but the release agent component contained in the release layer 12 may be a component having an amino structure. The component having an amino structure is preferably a component not having Si, such as a silicone-based release agent. The component other than the silicone-based release agent may be a component other than a long-chain alkyl material. The release layer 12 may contain a component having an amino structure without a long-chain alkyl, and a component having a long-chain alkyl without an amino structure. The release agent component in the release layer 12 may be one type or two or more types.

[0021] Specific examples of components having an amino structure include amino resins such as melamine resins, amino alkyd resins, etc. The amino alkyd resin may include a mixture of an amino resin and an alkyd resin. The amino structure contained in the release layer 12 may be a melamine structure, or an amino structure other than a melamine structure.

[0022] Amino resins are resins produced by condensation of compounds having an amino group, such as melamine, urea, benzoguanamine, and aniline, with compounds having an aldehyde group, such as formaldehyde. Amino resins can be used as thermosetting resins, either alone or in combination with alkyd resins, acrylic resins, epoxy resins, etc.

[0023] The release film 15 preferably contains a melamine structure in the release layer 12. The release layer 12 containing a melamine structure may contain a component having a melamine structure. Specific examples include a configuration consisting of one component having a melamine structure, a configuration consisting of two or more components having a melamine structure, and a configuration consisting of at least one component having a melamine structure and at least one component not having a melamine structure.

[0024] The component having a melamine structure is not particularly limited, but may be a component having a melamine structure that is a release agent component contained in the release layer 12. A specific example of the component having a melamine structure is a melamine resin.

[0025] Examples of the melamine resin include alkylated melamine resins such as methylated melamine resin, ethylated melamine resin, and butylated melamine resin. More specifically, examples of the melamine resin include full ether type methylated melamine resin and methylol group type methylated melamine resin.

[0026] The thickness of the release layer 12, additives, etc. can be appropriately designed. The release layer 12 may contain, as a component other than the component having an amino structure, any one selected from a component that chemically reacts with the amino structure, a component that does not chemically react with the amino structure, and other components.

[0027] The component that does not chemically react with the amino structure may be a migratory component that can migrate from the release layer 12 to the pressure-sensitive adhesive layer 13. The migratory component may be added in a small amount compared to the release agent component. For example, the release agent component may be blended in an amount of 60 to 99 parts by weight and the migratory component may be blended in an amount of 1 to 40 parts by weight, assuming that the total amount of the release layer 12 is 100 parts by weight. The migratory component in the release layer 12 may be of one type or two or more types.

[0028] The amount of the migrating component is not particularly limited, but may be 39 parts by weight or less, assuming that the total amount of the release layer 12 is 100 parts by weight. The amount of the migrating component may be 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or less than this.

[0029] When the release layer 12 contains components other than the release agent component and the migrating component, the components other than the release agent component and the migrating component may be 39 parts by weight or less, assuming that the total amount of the release layer 12 is 100 parts by weight. The amount of the components other than the release agent component and the migrating component is not particularly limited, but may be 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or less than this.

[0030] The release layer 12 preferably contains any one of acrylic, polyol, and polyether. More specifically, the release layer 12 preferably contains any one of acrylic, polyol, and polyether as at least one of its components. Any one of acrylic, polyol, and polyether may be a component without an amino structure, may be the above-mentioned transition component, may be a component that chemically reacts with the amino structure, or may be a component that does not chemically react with the amino structure.

[0031] The release film 15 containing the migrating component in the release layer 12 is preferably of a slight migration type, in which only a small amount of the migrating component migrates to the adhesive layer. On the other hand, the release film 15 containing no migrating component in the release layer 12 is of a non-migration type, in which no migrating component migrates to the adhesive layer.

[0032] The occurrence of zipping can be suppressed in both the non-migration type and the slight migration type. The slight migration type release film 15 is more preferable than the non-migration type release film 15 because it can suppress the occurrence of zipping even when combined with the surface protection film 16 having the pressure-sensitive adhesive layer 13 that is relatively hard and has a high Tg.

[0033] The acrylic may be any component having an acrylic structure, and examples thereof include acrylic compounds, acrylic polymers, and acrylic resins. The polyol may be any component having a polyol structure, and examples thereof include polyol compounds. The polyether may be any component having a polyether structure, and examples thereof include polyether compounds. The release layer 12 may contain a polyol compound having a polyether structure, such as polyethylene glycol or polypropylene glycol.

[0034] If necessary, additives may be blended into the release layer 12. Examples of additives include stabilizers, antioxidants, UV absorbers, antistatic agents, thickeners, lubricants, foaming agents, defoamers, inorganic particles, and organic particles. The release layer 12 may be formed without containing these additives. Examples of lubricants include, but are not limited to, fatty acid esters.

[0035] A sulfonic acid such as paratoluenesulfonic acid may be used as an additive for the release layer 12. The sulfonic acid may be a catalyst for a curing reaction of a melamine resin. When the melamine resin is cured, the coating applied on the second base layer 11 may be treated under heating conditions, if necessary.

[0036] The amino resin (component having an amino structure) such as melamine resin contained in the release layer 12 is cured, thereby suppressing migration from the release layer 12 to the adhesive layer 13. In addition, components that chemically react with the amino structure are also bonded to the cured resin, thereby suppressing migration to the adhesive layer 13. For this reason, this is suitable for a release layer 12 of a low-migration or no-migration type.

[0037] The second base layer 11 of the release film 15 is not particularly limited, but a polyester resin film such as a polyethylene terephthalate (PET) film can be used. The thickness and additives of the second base layer 11 can be designed as appropriate. The second base layer 11 may contain silicon (Si) compounds such as silica (SiO2), silicates, clay minerals, and zeolites as an antiblocking agent, filler, etc.

[0038] The surface protection film 16 in the illustrated example has an adhesive layer 13 on one surface of a first base layer 14. The adhesive layer 13 is formed by crosslinking a (meth)acrylate copolymer. Examples of the (meth)acrylate copolymer include copolymers obtained by copolymerizing two or more monomers including a (meth)acrylic acid monomer or a (meth)acrylic acid derivative monomer such as (meth)acrylate or (meth)acrylamide. The thickness, additives, etc. of the adhesive layer 13 can be designed as appropriate.

[0039] In this specification, (meth)acrylate means acrylate and / or methacrylate. Similarly, (meth)acrylic acid, (meth)acrylate, (meth)acrylamide, etc. mean acrylic acid and / or methacrylic acid or derivatives thereof.

[0040] To crosslink the (meth)acrylate copolymer, ultraviolet curing, electron beam curing, a crosslinking agent, etc. may be used. The crosslinking agent may be a radical crosslinking agent such as a peroxide, or a reactive crosslinking agent such as an isocyanate compound or an epoxy compound.

[0041] The reactive crosslinking agent can react with polar functional groups, such as hydroxyl groups and carboxyl groups, contained in the (meth)acrylate copolymer to crosslink the copolymer. A (meth)acrylate copolymer having a polar functional group can be obtained by copolymerizing a (meth)acrylate monomer having a polar functional group with the (meth)acrylate copolymer.

[0042] The Tg of the surface protection film 16 is preferably equal to or lower than +22° C., and more preferably equal to or lower than +11° C. The Tg of the surface protection film 16 can be measured by attaching the surface protection film 16 having the first base layer 14 and the pressure-sensitive adhesive layer 13 to a viscoelasticity measuring device.

[0043] Tg generally means glass transition temperature. Glass transition temperature (Tg) is a type of transition temperature and can be measured using various methods such as differential scanning calorimetry (DSC), differential thermal analysis (DTA), and dynamic mechanical analysis (DMA).

[0044] When measuring the temperature dependence of the loss tangent tan δ using dynamic viscoelasticity measurement, the measurement is easy because the glass transition temperature (Tg) is detected from the peak temperature, not from the inflection point or baseline shift, etc. Therefore, even in the case of a laminate of different materials such as the surface protection film 16, the apparent Tg of the surface protection film 16 can be obtained by observing the apparent peak.

[0045] The Tg of the surface protection film 16 does not necessarily mean that the pressure-sensitive adhesive layer 13 and the first base material layer 14 undergo glass transition at the same temperature, as long as the Tg value can be measured by the above-mentioned method. The glass transition temperature (Tg) of the polyethylene terephthalate film constituting the first base material layer 14 and the glass transition temperature (Tg) of the crosslinked product of the (meth)acrylate copolymer constituting the pressure-sensitive adhesive layer 13 do not necessarily need to be the same.

[0046] In designing an acrylic pressure-sensitive adhesive, it is common to control the glass transition temperature (Tg) of the (meth)acrylate copolymer before crosslinking. The glass transition temperature (Tg) of the (meth)acrylate copolymer is not particularly limited, but in order to obtain a soft pressure-sensitive adhesive layer 13, it is preferably less than -30°C, and may be -70°C or more and -40°C or less.

[0047] According to the surface protection film 10 with a release film of the embodiment, the range of selectable Tg is wide, so that a relatively low Tg similar to that of conventional (meth)acrylate copolymers may be selected for the pressure-sensitive adhesive layer 13, or a higher Tg than that of conventional (meth)acrylate copolymers may be selected. The (meth)acrylate copolymer can be appropriately designed according to the application and performance of the surface protection film 16.

[0048] A polyethylene terephthalate (PET) film is used as the first base layer 14 of the surface protection film 16. The thickness, additives, and the like of the first base layer 14 can be designed as appropriate. The first base layer 14 may contain silicon (Si) compounds such as silica (SiO2), silicates, clay minerals, and zeolites as antiblocking agents, fillers, and the like.

[0049] In this specification, the instantaneous maximum peel force (instantaneous maximum peel force) when the release film 15 is peeled at a peel speed of 0.3 m / min and a peel angle of 180 degrees is designated as B, and the average peel force when the release film 15 is peeled at a peel speed of 0.3 m / min and a peel angle of 180 degrees is designated as C. These peel forces are measured by peeling the release film 15 from the pressure-sensitive adhesive layer 13 of the surface protection film 16.

[0050] When the ratio calculated by the formula A=B / C is A, the value of A is preferably 1.5 or less, and more preferably 1.2 or less. When the value of the ratio A of the instantaneous maximum peel force / average peel force is small, zipping is less likely to occur when the release film 15 is peeled from the surface protection film 16.

[0051] The value of the average peeling force C is preferably greater than 0.02 N / 25 mm, and more preferably greater than 0.04 N / 25 mm. When the value of the average peeling force C is small, the release film 15 can be easily peeled from the surface protection film 16.

[0052] In the surface protection film 10 with a release film, the release film 15 is superimposed on the surface protection film 16 with the release layer 12 facing the adhesive layer 13. The surface protection film 16 is used to protect the surface of an object to be protected in a state in which the release film 15 is peeled off from the surface protection film 10 with a release film. At this time, the adhesive layer 13 is used to attach the surface protection film 16 to the surface of the object to be protected.

[0053] The object to be protected by the surface protection film 16 is not particularly limited to optical members and electronic members, and examples thereof include optical films, optical glass, polarizing plates, retardation plates, display panels, touch panels, etc. Examples of optical films include polarizing films, retardation films, anti-reflection films, anti-glare films, ultraviolet absorbing films, infrared absorbing films, optical compensation films, brightness enhancing films, etc.

[0054] It is preferable that the surface protection film 16 is colorless and transparent, since the state of the object to be protected can be visually confirmed even after the surface protection film 16 is attached. The release film 15 may be colorless and transparent. It is possible to select colorless and transparent materials for the second base layer 11, the release layer 12, the adhesive layer 13, and the first base layer 14.

[0055] The surface protection film 16 may be used only in the manufacturing process of the object to be protected, or may remain attached to the object to be protected even after the object to be protected is shipped. In order for the surface protection film 16 to continue protecting the surface of the object to be protected, it is preferable that the surface protection film 16 has a suitable adhesive strength to the object to be protected. When the surface protection film 16 is to be peeled off from the object to be protected, it is preferable that the adhesive strength of the surface protection film 16 to the object to be protected is not too high.

[0056] The present invention has been described above based on a preferred embodiment, but the present invention is not limited to the above-mentioned embodiment, and various modifications are possible without departing from the gist of the present invention. EXAMPLES

[0057] The present invention will now be described in detail with reference to examples.

[0058] <How to prepare the release film> Four types of release films were produced by applying the following coating material for forming a release layer onto a 38 μm-thick PET film (Diafoil (registered trademark) T100, manufactured by Mitsubishi Chemical Corporation) and drying it. "Parts" refers to parts by weight.

[0059] For release film 1 (hereinafter referred to as "RF-1"), a paint was used in which 100 parts of the base agent "Aracoat (registered trademark) RL900" manufactured by Arakawa Chemical Industries, Ltd. was mixed with 3 parts of the hardener "Aracoat (registered trademark) RA2000" manufactured by Arakawa Chemical Industries, Ltd.

[0060] The paint used for RF-1 contains a component with an amino structure (melamine), a component that chemically reacts with the amino structure (polyol), and a component that does not chemically react with the amino structure (acrylic). Of these, the component that contributes to the peelability is acrylic.

[0061] For release film 2 (hereinafter referred to as "RF-2"), a paint was used that was prepared by adding 10 parts of polypropylene glycol (weight average molecular weight 1000) and 3 parts of paratoluenesulfonic acid to 90 parts of Allnex's full-ether type methylated melamine resin "Cymel (registered trademark) 303LF".

[0062] The paint used for RF-2 contains a component with an amino structure (melamine), a component that does not chemically react with the amino structure (polypropylene glycol), and other components (paratoluenesulfonic acid). Of these, the component that contributes to the peelability is polypropylene glycol.

[0063] For release film 3 (hereinafter referred to as "RF-3"), a paint was used that was prepared by adding 30 parts of an acrylic polymer (manufactured by Fujimori Kogyo Co., Ltd., hydroxyl value 59.8 mg KOH / g) and 3 parts of paratoluenesulfonic acid to 70 parts of a methylol group-type methylated melamine resin "Cymel (registered trademark) 370" manufactured by Allnex.

[0064] The paint used for RF-3 contains a component with an amino structure (melamine), a component that chemically reacts with the amino structure (acrylic polymer), and other components (paratoluenesulfonic acid). Of these, the component that contributes to the peelability is the acrylic polymer.

[0065] For release film 4 (hereinafter referred to as "RF-4"), a paint was used in which 3 parts of paratoluenesulfonic acid solution "Dryer 900" manufactured by Resonac Corporation was added to 100 parts of long-chain alkyl modified aminoalkyd resin "Tesfine (registered trademark) 303" manufactured by Resonac Corporation.

[0066] The paint used in RF-4 contains components with amino structures, components that chemically react with amino structures (alkyds), ​​and other components (paratoluenesulfonic acid). Of these, the component that contributes to peelability is the alkyd.

[0067] Furthermore, as release film 5 (hereinafter referred to as "RF-5"), a release film "Diafoil (registered trademark) MRF" (substrate thickness: 38 μm) manufactured by Mitsubishi Chemical Corporation was used.

[0068] Of RF-1 to RF-4, RF-1 and RF-2 are slight migration types, and their "ingredients that do not chemically react with amino structures" are migration ingredients. RF-3 and RF-4 are non-migration types that do not use migration ingredients. RF-5 is a type in which ingredients such as silicone migrate in large quantities from the release layer to the adhesive layer.

[0069] <Production of (meth)acrylate copolymer> Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 90 parts by weight of the monomers and solvent (ethyl acetate) shown in Table 1 (A) to (C) were added to the reactor. Then, 0.1 parts by weight of dimethyl azobisisobutyrate as a polymerization initiator was dropped over 2 hours, and the mixture was reacted at 65°C for 6 hours to obtain a (meth)acrylate copolymer.

[0070] The five (meth)acrylate copolymers thus obtained are hereinafter referred to as "AP-A", "AP-B", "AP-C", "AP-D" and "AP-E", respectively. Although no specific measurement results are shown, the weight average molecular weight of the (meth)acrylate copolymers thus obtained is within the range of 100,000 to 1,000,000.

[0071] The monomers used were 2-ethylhexyl acrylate (2EHA), dimethylacrylamide (DMAA), and 4-hydroxybutyl acrylate (4HBA). The values ​​in parentheses in (A) to (C) of Table 1 indicate the parts by weight of each monomer.

[0072] [Table 1]

[0073] <Calculation of Tg of (meth)acrylate copolymer> The Tg (°C) of the (meth)acrylate copolymer was calculated from the glass transition temperature Tgn (°C) of the homopolymer of each monomer and the weight fraction Wn of each monomer using the following formula. 1 / (Tg+273)=Σ[Wn / (Tgn+273)]

[0074] The Tgn of the homopolymers was determined from literature values ​​to be -70°C for 2EHA, +119°C for DMAA, and -32°C for 4HBA. Σ represents the sum of the values ​​of the term [Wn / (Tgn+273)] calculated for each monomer. The results are shown in Table 1 above.

[0075] <Production of Pressure-Sensitive Adhesive Composition and Surface Protective Film> A pressure-sensitive adhesive composition was obtained by adding a crosslinking agent TKA-100 (an isocyanurate of a hexamethylene diisocyanate compound, manufactured by Asahi Kasei Corporation) shown in (F) of Table 2 to a (meth)acrylate copolymer shown in (E) of Table 2 and mixing with stirring. The values ​​shown in parentheses in (E) to (F) of Table 2 are parts by weight of the (meth)acrylate copolymer and the crosslinking agent, respectively.

[0076] The obtained adhesive composition was applied onto a 38 μm thick PET film (Diafoil (registered trademark) T100, manufactured by Mitsubishi Chemical Corporation) and then dried at 120°C to remove the solvent, thereby obtaining a surface protection film with an adhesive layer thickness of 15 μm.

[0077] The ten types of surface protection films obtained are referred to below as "PF-A1," "PF-A2," "PF-B1," "PF-B2," "PF-C1," "PF-C2," "PF-D1," "PF-D2," "PF-E1," and "PF-E2," respectively.

[0078] [Table 2]

[0079] <Method for measuring Tg of surface protection film> The surface protection film was clamped and attached to a solid shear jig, which is an option for a viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.). The storage modulus and loss modulus were measured in shear mode under conditions of a strain of 1% and a frequency of 1 Hz while the set temperature of the device was raised from -50°C to +100°C at a heating rate of 2°C / min. From the results, the loss tangent tanδ of the surface protection film was calculated for each 1°C. The temperature at which this loss tangent value was maximized was defined as the Tg of the surface protection film. The results are shown in Table 2 above.

[0080] In practice, the Tg of the surface protection film was measured by producing a surface protection film with a release film using the production method described below, peeling off the release film, attaching the film to a viscoelasticity measuring device, and then measuring the Tg. However, since differences in release films do not result in differences in the Tg of the surface protection film, the results are shown for each surface protection film without distinguishing between different types of release films.

[0081] <Method for measuring the amount of Si contained in the peeling layer> The amount of Si present on the release layer surface of the release film was measured by X-ray fluorescence analysis, with F (kcps). The X-ray fluorescence analysis was performed using an XRF device manufactured by Rigaku Corporation, model number "ZSX (registered trademark) PrimsTVi", with a measurement range of a circle with a diameter of 30 mm, detected X-rays: Si-Kα, output: 30 kV, 100 mA, and a PETH analyzing crystal.

[0082] As a blank, the amount of Si present per area equivalent to a 30 mm circle of the base film used in the release film was designated as A (kcps), and was measured by fluorescent X-ray analysis under the same conditions as F (kcps). The value obtained by subtracting A (kcps) from F (kcps) was regarded as the amount of Si (kcps) contained in the release layer.

[0083] [Table 3]

[0084] <Method of manufacturing surface protection film with release film and method of measuring peel strength> Any one of the 10 types of surface protection films shown in Table 2 was laminated to any one of the 5 types of release films shown in Table 3. In this way, a total of 50 types of surface protection films with release films were produced.

[0085] The surface protection film with release film was cut to a width of 25 mm and a length of 150 mm to prepare a test specimen. The surface protection film side of the test specimen was fixed to a test device, and the release film was gripped and peeled off to measure the peel force (N / 25 mm). The peel speed was 0.3 m / min, and the peel angle was 180°.

[0086] A bench-top precision universal testing machine (Shimadzu Corporation, Autograph (registered trademark) AGS-X) was used as the testing machine, and peeling was performed over a length of 120 mm, measuring the peel force at a frequency of 60 times per second. From the measurement results, the peel force at the moment when the peel force showed the maximum value was designated as B, and the average peel force was designated as C. Furthermore, the value of A=B / C was calculated.

[0087] The results are shown in Table 4 for the measured values ​​of B (instantaneous maximum value), in Table 5 for the measured values ​​of C (average value), and in Table 6 for the value of A=B / C.

[0088] [Table 4]

[0089] [Table 5]

[0090] [Table 6]

[0091] For RF-1 to RF-4, the amount of Si contained in the peeling layer was 0.5 kcps or less as measured by fluorescent X-rays. For RF-1 and RF-2, the value of A=B / C was small for the eight types of PF-A1 to PF-D2, respectively, and zipping was suppressed. For RF-3 and RF-4, the A=B / C value was small for the six types of materials, PF-A1 to PF-C2, and zipping was suppressed. In RF-5, the value of A=B / C was small for all 10 types of surface protection films, and zipping was suppressed, but the release layer contained a large amount of Si.

[0092] In the combination of RF-1 or RF-2 with PF-A1 to PF-D2, the Tg of the surface protection film is +22°C or less, and the release layer of the release film contains a component with an amino structure and a component that does not chemically react with the amino structure.In addition, in the combination of RF-1 to RF-4 with PF-A1 to PF-C2, the Tg of the surface protection film is +11°C or less, and the release layer of the release film contains an amino structure. [Explanation of symbols]

[0093] 10... surface protection film with release film, 11... second base layer, 12... release layer, 13... adhesive layer, 14... first base layer, 15... release film, 16... surface protection film.

Claims

1. A surface protection film with a release film, The surface protection film has a first base layer made of a polyethylene terephthalate film and a pressure-sensitive adhesive layer made of a crosslinked (meth)acrylate copolymer, The surface protective film is an optical or electronic surface protective film, The release film has a second base layer and a release layer formed on one surface of the second base layer, The release layer of the release film contains an amino structure, A surface protection film with a release film, wherein the Si in the release layer of the release film is 0.5 kcps or less as measured by fluorescent X-rays.

2. 2. The surface protective film with a release film according to claim 1, wherein the Tg of the surface protective film is +22° C. or less, and the release layer of the release film contains a component that does not chemically react with the amino structure.

3. 2. The surface protective film with a release film according to claim 1, wherein the Tg of the surface protective film is +11° C. or less.

4. A surface protective film with a release film as described in claim 2 or 3, wherein when the instantaneous maximum peel force when the release film is peeled off at a peel speed of 0.3 m / min and a peel angle of 180 degrees is B and the average peel force when the release film is peeled off at a peel speed of 0.3 m / min and a peel angle of 180 degrees is C, the value A calculated by the formula: A = B / C is 1.5 or less.

5. 4. A surface protective film with a release film as described in claim 2 or claim 3, wherein C is an average peel force when the release film is peeled off at a peel speed of 0.3 m / min and a peel angle of 180 degrees, and C is greater than 0.02 N / 25 mm.

6. 4. The surface protective film with a release film according to claim 2, wherein the release layer of the release film contains a melamine structure.

7. 4. The surface protective film with a release film according to claim 2, wherein the release layer contains any one of acrylic, polyol, and polyether.

Citation Information

Patent Citations

  • Method for producing antistatic surface-protective film, and antistatic surface-protective film

    JP2021004271A

  • Release agent composition and release film

    JP2022010557A

  • Surface protective film and optical component

    JP2023013962A

  • Peeling agent composition, peeling sheet, and adhesive body

    WO2012020673A1

  • Surface protection film, optical member, and display device

    WO2019194069A1