Rhenium-containing zeolite and olefin metathesis catalyst including the same

A rhenium-containing zeolite with controlled active rhenium and acid content addresses inefficiencies in existing catalysts, providing high activity and economic efficiency for olefin metathesis reactions at low temperatures.

JP2024144841APending Publication Date: 2024-10-15TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023056984
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing olefin metathesis catalysts, particularly those containing rhenium on alumina, suffer from inactive rhenium species, economic inefficiency, rapid deactivation due to excessive Brønsted acid sites, and catalytic activity issues, especially at low temperatures.

Method used

A rhenium-containing zeolite with specific ranges of active rhenium content (0.5 to 10.0% by mass) and strong acid content (15 to 115 μmol/g) is developed, ensuring minimal inactive rhenium and optimal acid sites, enhancing catalytic activity and economic efficiency.

Benefits of technology

The catalyst exhibits high activity and economic efficiency, maintaining performance at low temperatures with reduced deactivation and side reactions, suitable for industrial olefin metathesis processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144841000001
    Figure 2024144841000001
Patent Text Reader

Abstract

To provide a rhenium-containing zeolite that serves as an olefin metathesis catalyst to exhibit superior economical efficiency and activity, and an olefin metathesis catalyst containing the rhenium-containing zeolite.SOLUTION: A rhenium-containing zeolite is a zeolite containing rhenium, fulfilling all of the following properties (i)-(iii). (i) In an analysis conducted with a thermogravimetry device, the active rhenium content, represented by the weight reduction within the range of 400-800°C, is 0.5 mass% to 10.0 mass% (excluding 10.0 mass%). (ii) The inert rhenium level is less than 1.0 mass%. (iii) The strong acid level is 15-115 μmol / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rhenium-containing zeolite and an olefin metathesis catalyst containing the same, and more specifically, to a rhenium-containing zeolite having an active rhenium amount and a strong acid amount each within a specific range, and an olefin metathesis catalyst that exhibits extremely high activity by containing the rhenium-containing zeolite. [Background technology]

[0002] Olefin metathesis is a reaction of rearrangement of the double bonds of two olefin molecules. For example, a method of producing ethylene and 2-butene by the olefin metathesis reaction of two propylene molecules, and a method of producing propylene from ethylene and 2-butene as raw materials, which is the reverse reaction, have been proposed (see, for example, Patent Documents 1 and 2).

[0003] The catalyst used in this case is generally a homogeneous or heterogeneous transition metal compound, particularly a compound of a transition metal of Groups 5 to 8. Representative examples of heterogeneous catalysts include tungsten-based catalysts, which are tungsten oxide on silica, molybdenum-based catalysts, which are molybdenum oxide on alumina, and rhenium-based catalysts, which are rhenium oxide on alumina.

[0004] Among them, rhenium-based catalysts are generally known to act as catalysts in the low temperature range from room temperature to about 100° C., and olefin metathesis catalysts that are active at low temperatures are expected to be industrially useful. However, it is known that rhenium species contained in olefin metathesis catalysts containing rhenium on alumina include inactive rhenium species that do not participate in the reaction (for example, see Non-Patent Document 1).

[0005] In addition, as catalysts that exhibit activity at low temperatures due to a cooperative action with Bronsted acid sites derived from the support, tungsten-based catalysts which are tungsten oxide on a support containing zeolite (see, for example, Patent Document 3 and Non-Patent Document 2), rhenium-based catalysts which are rhenium oxide on zeolite (see, for example, Non-Patent Document 3), and the like have been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-72612 A [Patent Document 2] Special Publication No. 2015-528500 [Patent Document 3] JP 2019-130527 A [Non-patent literature]

[0007] [Non-Patent Document 1] Catalysis Today Vol. 51, p. 289 (1999) [Non-Patent Document 2] Journal of the American Chemical Society, Vol. 140, p. 6661 (2018) [Non-Patent Document 3] ACS Catalysis Volume 11, Page 3530 (2021) Summary of the Invention [Problem to be solved by the invention]

[0008] However, the olefin metathesis catalyst containing an inactive rhenium species described in Non-Patent Document 1 has not been studied in relation to zeolite, and has problems not only in terms of economic efficiency but also in terms of performance such as catalytic activity. In addition, the catalysts described in Patent Document 3 and Non-Patent Documents 2 and 3 have problems in that they promote coking and oligomerization of the raw olefins and induce rapid deactivation of the catalyst due to the presence of excessive Bronsted acid sites.

[0009] Therefore, there has been a demand for an olefin metathesis catalyst that is economical, has excellent activity without rapid catalyst deactivation, and exhibits activity at low temperatures. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems and have found that a zeolite containing a specific amount of active rhenium and having a specific amount of strong acidity, when used as an olefin metathesis catalyst, is economical and has excellent activity, and also exhibits activity performance at low temperatures, thereby completing the present invention.

[0011] That is, the present invention relates to a rhenium-containing zeolite which is characterized by satisfying all of the following characteristics (i) to (iii): (i) In analysis using a thermogravimetric analyzer, the amount of active rhenium contained, which is the weight loss at 400 to 800°C, is less than 0.5 to 10.0% by mass. (ii) The amount of inert rhenium is less than 1.0 mass percent. (iii) The amount of strong acid is 15 to 115 μmol / g.

[0012] The present invention will be described in detail below.

[0013] The rhenium-containing zeolite of the present invention is a rhenium-containing zeolite that satisfies all of the above characteristics (i) to (iii), and in particular, by containing the rhenium-containing zeolite, the zeolite is useful as an olefin metathesis catalyst that is excellent in cost efficiency and activity and exhibits activity performance at low temperatures.

[0014] The rhenium (hereinafter sometimes referred to as Re)-containing zeolite of the present invention is one in which (i) the amount of active rhenium contained is less than 0.5 to 10.0 mass%. Here, if the amount of active rhenium contained is less than 0.5 mass%, sufficient catalytic activity cannot be exhibited when used as an olefin metathesis catalyst. On the other hand, if the amount is 10.0 mass% or more, coking and oligomerization of the raw olefins tends to progress when used as an olefin metathesis catalyst. The amount of active Re contained in the present invention is the amount of rhenium calculated as rhenium oxide (VII) from the weight loss at 400 to 800°C in an analysis using a thermogravimetric analyzer (sometimes referred to as TGA), and this is defined as the amount of active Re contained.

[0015] The Re-containing zeolite of the present invention, when used as an olefin metathesis catalyst, is particularly excellent in terms of economy and activity, and exhibits activity performance at low temperatures. Therefore, (ii) the amount of inactive Re, expressed as the difference between the total amount of Re contained and the amount of active Re contained, is less than 1.0 mass%, and is particularly preferably 0.01 mass% or more and less than 1.0 mass%, and more preferably does not contain inactive Re. Here, if the amount of inactive Re is 1.0 mass% or more, sufficient catalytic activity cannot be exhibited when used as an olefin metathesis catalyst. In addition, the total amount of Re contained is preferably 10 mass% or less. The total amount of Re contained can be measured, for example, by an ICP device.

[0016] In addition, the Re-containing zeolite of the present invention has (iii) a strong acid amount of 15 to 115 μmol / g. The strong acid amount can be measured by a method generally known as a method for measuring the amount of acid, for example, a method based on the ammonia-TPD method (see Measurement of solid acidity by ammonia temperature-programmed desorption method, Catalyst, vol. 42, p. 218 (2000)). Here, if the strong acid amount is less than 15 μmol / g, when used as an olefin metathesis catalyst, the synergistic action of the Brønsted acid and Re cannot be fully exerted, resulting in poor activity. On the other hand, if the strong acid amount is more than 115 μmol / g, when used as an olefin metathesis catalyst, the excess acid sites cause side reactions such as coking and oligomerization of the raw olefin, resulting in a significant decrease in catalytic activity.

[0017] The zeolite constituting the Re-containing zeolite of the present invention may be any zeolite, and examples of such zeolite include aluminosilicate compounds that belong to the structure codes FAU, AEL, FER, HEU, MEU, MEL, MFI, and NES defined by the International Zeolite Society. Among these, FAU-type faujasite is preferred because it is particularly suitable as an olefin metathesis catalyst, and examples of industrial products of the FAU-type zeolite include X-type zeolite with a high aluminum content and Y-type zeolite with a low aluminum content.

[0018] The Re-containing zeolite of the present invention can be produced by various methods, and one example thereof is a method including at least the following steps (1) and (2). (1) A step of adjusting the amount of strong acid in a zeolite having acid sites to 10 to 180 μmol / g. (2) A process for incorporating Re after the process (1).

[0019] Furthermore, if necessary, a step (3) of drying and / or calcining the solid containing Re may be added.

[0020] In the step (1), any method can be used to adjust the amount of strong acid in the zeolite to 10 to 180 μmol / g, for example, ion exchange with an alkali metal or dealumination by steam treatment of the zeolite can be used.

[0021] In the step (2), the method for incorporating Re can be any of impregnation, ion exchange, and physical mixing. Among these, impregnation or physical mixing is preferable because it is possible to incorporate Re efficiently. The rhenium compound used can be any compound, such as ammonium perrhenate.

[0022] As the step (3) which is added as necessary after the step (2), a step of drying and / or calcination may be carried out, and since this is a particularly efficient method for producing a Re-containing zeolite, it is preferable to carry out a step of drying at 60 to 120°C for 0.5 to 2 hours under a reduced pressure of 5 to 40 mmHg, followed by calcination at 300 to 600°C for 4 to 8 hours. Furthermore, since the volatilization of the contained Re is suppressed, the calcination temperature is preferably 350 to 450°C.

[0023] The Re-containing zeolite of the present invention can provide a novel olefin metathesis catalyst that is excellent in economy and activity and exhibits activity performance at low temperature, and the amount of the Re-containing zeolite contained in the olefin metathesis catalyst is not particularly limited, and since it results in a more active olefin metathesis catalyst, the content of the Re-containing zeolite is preferably 60 to 100 mass%. The form of the zeolite is not limited, and it can be used in any form, such as using the zeolite powder as it is as a catalyst, using it as a specific shape by compression molding, or mixing it with a binder or the like and molding it to use it as a specific shape.

[0024] Use of the olefin metathesis catalyst provides a catalyst that is excellent in efficiency, such as yield and productivity, when carrying out an olefin metathesis reaction, and enables olefins to be produced efficiently.

[0025] In the olefin metathesis reaction, the combination of the raw materials and the olefins produced may be any combination, and an example is the production of ethylene and butene from propylene.

[0026] In the olefin metathesis reaction, which is an embodiment of the reaction, the reaction temperature is not particularly limited, and may be, for example, about -40 to 300°C. In particular, a temperature range of 0 to 180°C is desirable, since it suppresses the production of by-products such as coke or oligomers and provides an efficient reaction that does not require excessive cooling or heating reaction equipment. There is also no restriction on the reaction pressure, and operation is possible within a pressure range of, for example, about 0.05 MPa to 6.0 MPa. The supply of the olefin, which is the reaction raw material, is not particularly limited as a ratio of the raw material mass to the catalyst mass, and may be, for example, 0.5 h. -1 ~10h -1 When the olefin is supplied as the raw material gas, it may be used as a single gas, a mixed gas, or a gas diluted with a single or mixed gas selected from inert gases such as nitrogen.

[0027] The reaction type is not limited, and for example, not only fixed bed, transport bed, fluidized bed, moving bed, and multi-tubular reactor, but also continuous flow type, intermittent flow type, and swing type reactors can be used. Effect of the Invention

[0028] The present invention relates to a Re-containing zeolite and an olefin metathesis catalyst containing the same. More specifically, the present invention relates to a rhenium-containing heterogeneous olefin metathesis catalyst, in which the strong acid amount and active Re amount are each within a specific range, thereby providing an olefin metathesis catalyst that exhibits high activity and is extremely useful industrially. EXAMPLES

[0029] Specific examples of the present invention will be described below as examples, but the present invention is not limited to these examples.

[0030] The olefin metathesis catalysts used in the examples were measured and defined by the following methods.

[0031] ~Measurement of Re content~ The Re content was measured using an ICP device (product name: Optima 8300, manufactured by PerkinElmer, Inc.). After accurately weighing the sample into a 100 ml polypropylene measuring flask, hydrofluoric acid, nitric acid and ultrapure water were added and left to dissolve overnight. After filling up the flask, an aliquot of the sample was measured by ICP-AES, and the metal content was calculated from the calibration curve, and the amount of Re was calculated.

[0032] ~Measurement of active Re amount~ A TG analyzer ((product name) STA 2500 Regulus, manufactured by NETZSCH) was used. The sample was granulated, then heated to 800°C at 10°C / min under a nitrogen / oxygen mixed gas flow, and held for 120 minutes. The weight loss at 400°C or higher was taken as Re(VII) oxide, and the amount of active Re was calculated. Active Re amount = Re atomic weight / oxidized Re(VII) formula weight x weight loss The amount of inactive Re was calculated as follows. Inactive Re amount = Re content - active Re amount ~Method for measuring strong acid content~ An NH3-TPD device (product name: BELCATII, manufactured by Microtrack-Bell Co., Ltd.) and a gas analyzer (product name: BELMass, manufactured by Microtrack-Bell Co., Ltd.) were used. The sample was granulated and then placed in a cell, and heated to 500°C at 10°C / min in a helium atmosphere and held there for 1 hour. The temperature was then lowered to 100°C, and 0.2% ammonia gas was introduced for 30 minutes. The temperature was then raised to 700°C at 10°C / min, and the desorbed ammonia was analyzed with the gas analyzer. The amount of strong acid in the sample was calculated from the amount of ammonia desorbed at sample temperatures of 400°C or higher.

[0033] Example 1 20.0 g of commercially available Y-type zeolite (manufactured by Tosoh Corporation, product name HSZ-330HUA) was immersed in an aqueous solution of 0.897 g of sodium carbonate and 50 ml of pure water, and stirred for 30 minutes. The resulting slurry was filtered, and the solid was washed three times with 50 ml of pure water and then dried to prepare a sodium ion-exchanged zeolite with a strong acidity of 32 μmol / g.

[0034] 10.0 g of the prepared sodium ion-exchanged zeolite was immersed in an aqueous solution of 0.670 g of ammonium perrhenate and 100 ml of pure water for 120 minutes. After that, it was dried at 80°C for 2 hours under reduced pressure (20 mmHg), and then calcined at 400°C for 5 hours in an air stream to prepare a rhenium-containing zeolite. The prepared rhenium-containing zeolite was compression-molded to a particle size of 2 to 4 mm to obtain an olefin metathesis catalyst A.

[0035] The rhenium content of the prepared rhenium-containing zeolite was 3.7 mass %, the active rhenium content was 3.6 mass %, the inactive rhenium content was 0.1 mass %, and the strong acid content was 40 μmol / g.

[0036] 3.0 g of olefin metathesis catalyst A was packed in the middle of a stainless steel reaction tube (inner diameter 16 mm, length 500 mm), and after heat pretreatment under dry air flow, a raw material gas (a mixed gas of propylene 52 Nml / min and nitrogen 4 Nml / min) was fed at 70°C and 101 kPa to carry out an olefin metathesis reaction. A ceramic tubular furnace was used for heating, and the temperature of the catalyst layer was controlled. The reaction outlet gas was analyzed using a gas chromatograph. The ethylene yield and butene yield were calculated by the following formulas.

[0037] Yield [%] = amount of olefin produced / (amount of raw propylene / 2) x 100 The ethylene yield in the reaction outlet gas was 23.4%, and the butene yield was 25.6%, indicating that the catalyst had high olefin metathesis activity. The results are shown in Table 1.

[0038] Example 2 Sodium ion exchange was carried out in the same manner as in Example 1 except that 1.79 g of sodium carbonate was used, to prepare a sodium ion-exchanged zeolite having a strong acidity of 10 μmol / g.

[0039] Rhenium was supported on the zeolite in the same manner as in Example 1, except that the prepared sodium ion-exchanged zeolite was used, to prepare a rhenium-containing zeolite and an olefin metathesis catalyst B.

[0040] The rhenium content of the prepared rhenium-containing zeolite was 3.9 mass %, the active rhenium content was 3.8 mass %, the inactive rhenium content was 0.1 mass %, and the strong acid content was 17 μmol / g.

[0041] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that the olefin metathesis catalyst B was used.

[0042] The ethylene yield in the reaction outlet gas was 20.7%, and the butene yield was 23.2%, indicating that the catalyst had high olefin metathesis activity. The results are shown in Table 1.

[0043] Example 3 50 g of commercially available Y-type zeolite (manufactured by Tosoh Corporation, product name HSZ-330HUA) was treated with steam at a water vapor pressure of 50.0 kPa at 600° C. for 5 hours to prepare a steam-treated zeolite with a strong acidity of 158 μmol / g.

[0044] Rhenium was supported on the zeolite in the same manner as in Example 1, except that the prepared steam-treated zeolite was used, to prepare a rhenium-containing zeolite and an olefin metathesis catalyst C.

[0045] The rhenium content of the prepared rhenium-containing zeolite was 3.9 mass %, the active rhenium content was 3.2 mass %, the inactive rhenium content was 0.7 mass %, and the strong acid content was 86 μmol / g.

[0046] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that the olefin metathesis catalyst C was used.

[0047] The ethylene yield in the reaction outlet gas was 18.6%, and the butene yield was 20.2%, indicating that the catalyst had high olefin metathesis activity. The results are shown in Table 1.

[0048] Example 4 Steam treatment was carried out in the same manner as in Example 3 except that the steam treatment temperature was 650° C., to prepare a steam-treated zeolite having a strong acidity of 100 μmol / g.

[0049] Rhenium was supported on the zeolite in the same manner as in Example 1, except that the prepared steam-treated zeolite was used, to prepare a rhenium-containing zeolite and an olefin metathesis catalyst D.

[0050] The rhenium content of the prepared rhenium-containing zeolite was 3.9 mass %, the active rhenium content was 3.7 mass %, the inactive rhenium content was 0.2 mass %, and the strong acid content was 77 μmol / g.

[0051] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that the olefin metathesis catalyst D was used.

[0052] The ethylene yield in the reaction outlet gas was 23.1%, and the butene yield was 23.4%, indicating that the catalyst had high olefin metathesis activity. The results are shown in Table 1.

[0053] Comparative Example 1 Rhenium was supported in the same manner as in Example 1, except that 10 g of a commercially available Y-type zeolite (manufactured by Tosoh Corporation, product name HSZ-330HUA) having a strong acidity of 227 μmol / g was used, to prepare a rhenium-containing zeolite and catalyst E.

[0054] The prepared rhenium-containing zeolite had a rhenium content of 3.2 mass%, an active rhenium content of 0.6 mass%, an inactive rhenium content of 2.6 mass%, and a strong acid content of 97 μmol / g, making it a rhenium-containing zeolite with a high inactive rhenium content.

[0055] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that Catalyst E was used.

[0056] The ethylene yield in the reaction outlet gas was 12.3%, and the butene yield was 13.8%, indicating that the catalyst had poor olefin metathesis activity. The results are shown in Table 1.

[0057] Comparative Example 2 A rhenium-containing zeolite and catalyst F were prepared by carrying rhenium in the same manner as in Example 1, except that 10 g of a commercially available Y-type zeolite (manufactured by Tosoh Corporation, product name HSZ-320NAA) having a strong acidity of less than 1 μmol / g was used and 1.34 g of ammonium perrhenate was used.

[0058] The prepared rhenium-containing zeolite contained 6.4 mass% rhenium, 6.3 mass% active rhenium, 0.1 mass% inactive rhenium, and less than 1 μmol / g strong acid, meaning that the rhenium-containing zeolite contained a low amount of strong acid.

[0059] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that catalyst F was used.

[0060] The ethylene yield in the reaction outlet gas was 0.0%, and the butene yield was 0.1%, indicating that the catalyst had poor olefin metathesis activity. The results are shown in Table 1.

[0061] Comparative Example 3 Steam treatment was carried out in the same manner as in Example 3 except that the water vapor pressure was 20 kPa and the steam treatment time was 5 hours, to prepare a steam-treated zeolite having a strong acidity of 190 μmol / g.

[0062] Rhenium was supported on the zeolite by the same procedure as in Example 1, except that the prepared steam-treated zeolite was used, to prepare a rhenium-containing zeolite and catalyst G.

[0063] The prepared rhenium-containing zeolite contained 4.2 mass % rhenium, 3.6 mass % active rhenium, 0.6 mass % inactive rhenium, and 125 μmol / g strong acid, making it a rhenium-containing zeolite with a high strong acid content.

[0064] An olefin metathesis reaction was carried out in the same manner as in Example 1, except that Catalyst G was used.

[0065] The ethylene yield in the reaction outlet gas was 10.8%, and the butene yield was 12.1%, indicating that the catalyst had poor olefin metathesis activity. The results are shown in Table 1.

[0066] [Table 1] [Industrial Applicability]

[0067] INDUSTRIAL APPLICABILITY The rhenium-containing zeolite of the present invention is particularly suitable as an olefin metathesis catalyst which can operate at low temperatures and has excellent activity and economy, and is therefore of extremely high industrial value.

Claims

1. A rhenium-containing zeolite characterized by satisfying any one of the following characteristics (i) to (iii): (i) In analysis using a thermogravimetric analyzer, the amount of active rhenium contained, which is the weight loss at 400 to 800° C., is 0.5 to less than 10.0 mass %. (ii) the amount of inert rhenium is less than 1.0% by weight; (iii) The amount of strong acid is 15 to 115 μmol / g.

2. 2. The rhenium-containing zeolite according to claim 1, characterized in that the zeolite is a FAU-type zeolite.

3. 3. The rhenium-containing zeolite according to claim 1, wherein the total amount of the active rhenium and the inactive rhenium is 10 mass% or less.

4. An olefin metathesis catalyst comprising the rhenium-containing zeolite of claim 1.

5. The olefin metathesis catalyst according to claim 4, comprising at least 60.0 mass% of a rhenium-containing zeolite.

Citation Information

Patent Citations

  • Production of 5c- and / or 6c-olefin

    JP2001072612A

  • Propylene fermentation via metathesis with little to no ethylene use

    JP2015528500A