Polarizing plate set, and liquid crystal display device

The polarizing plate set addresses rainbow color unevenness and warpage issues in liquid crystal displays by using protective films with high retardation values and controlled rigidity ratios, ensuring balanced shrinkage and improved structural stability.

JP2024145055APending Publication Date: 2024-10-15SUMITOMO CHEM CO LTD

Patent Information

Application Number
JP2023057290
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing polarizing plate structures in liquid crystal display devices experience rainbow color unevenness and significant warpage when exposed to heat-resistant environments due to differences in the degree of shrinkage between polarizer layers, particularly when using protective films with varying retardation values.

Method used

A polarizing plate set is designed with specific rigidity ratios and orthogonal absorption axes for the viewing and backlight side polarizing plates, incorporating protective films with high in-plane retardation values and controlled rigidity ratios to balance shrinkage and reduce warpage.

Benefits of technology

The solution effectively suppresses rainbow unevenness and reduces warpage in liquid crystal display devices by balancing the shrinkage forces between polarizer layers, maintaining structural integrity under heat-resistant conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145055000001_ABST
    Figure 2024145055000001_ABST
Patent Text Reader

Abstract

To provide a polarizing plate set that suppresses rainbow unevenness, and can reduce, under a heat-resistant environment, warpage of a laminated structure obtained by sticking the polarizing plate set to a liquid crystal cell.SOLUTION: A pair of rectangular polarizing plate sets 3 is arranged in a liquid crystal cell 2, and each of a viewing side polarizing plate 3A and a backlight side polarizing plate 3B has: polarizer layers 6A and 6B; and protection films 5A and 5B. An in-plane phase difference value of the protection film 5A the viewing side polarizing plate 3A has is more than 6000nm, and an absorption axis of the polarizer layer 6A the viewing side polarizing plate 3A has directs at a long-side direction of the rectangular. The protection film 5A the viewing side polarizing plate 3A is more than 2.0 in a ratio of rigidity in a short-side direction to rigidity in the long-side direction. An absolute value of a difference between the rigidity in the long-side direction of the protection film 5A and rigidity in a long-side direction of the protection film 5B is equal to or less than 90 mm MPa.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate set and a liquid crystal display device. [Background technology]

[0002] Due to the display principle of a liquid crystal display device, polarizing plates are arranged on the viewing side and the backlight side of the liquid crystal cell in the center. Each polarizing plate is a laminate including at least a polarizer layer and a protective film for protecting the polarizer layer (see, for example, Patent Document 1). As the protective film, a biaxially oriented polyester resin film or the like having excellent mechanical properties (low moisture permeability and impact resistance) is used. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-123402 A Summary of the Invention [Problem to be solved by the invention]

[0004] When a protective film with a low retardation value, such as a biaxially stretched polyester resin film, is used as a component of the viewer-side polarizing plate, the low retardation causes strong rainbow color unevenness (hereinafter referred to as "rainbow unevenness"). Here, if a protective film with a high retardation value (for example, a uniaxially stretched polyester resin film) is used to suppress rainbow unevenness, it is possible to suppress rainbow unevenness. However, when a laminated structure produced by laminating a polarizing plate having such a protective film to both sides of glass is exposed to a heat-resistant environment of 80°C, the entire laminated structure warps significantly.

[0005] Therefore, an object of the present invention is to provide a polarizing plate set that can suppress rainbow unevenness and reduce warping of a laminated structure obtained by bonding the polarizing plate set to a liquid crystal cell in a heat-resistant environment, and to provide a liquid crystal display device including the polarizing plate set. [Means for solving the problem]

[0006] In a laminated structure having a laminated structure of "viewer-side polarizing plate / liquid crystal cell / backlight-side polarizing plate", the absorption axes of the polarizer layers of each polarizing plate are usually perpendicular to each other due to the principle of a liquid crystal display device. The polarizer layer has an absorption axis, so it is anisotropic, and due to this, the degree of shrinkage when exposed to a heat-resistant environment is also anisotropic. Therefore, the above-mentioned laminated structure is warped as a whole due to the difference in the degree of shrinkage between the polarizer layer of the viewer-side polarizing plate and the polarizer layer of the backlight-side polarizing plate. If the protective film of each polarizing plate has high rigidity, it is possible to suppress the shrinkage of the polarizer layer and to eliminate the warping of the entire laminated structure to some extent, but it is difficult to achieve a balance. The present inventors have found that the warping of the laminated structure in a heat-resistant environment can be reduced by making the rigidity of the protective film of each rectangular polarizing plate have a predetermined relationship, and have completed the present invention.

[0007] The present invention provides a pair of polarizing plate sets comprising a viewer-side polarizing plate to be placed on the viewer-side of a liquid crystal cell and a backlight-side polarizing plate to be placed on the backlight side of the liquid crystal cell, wherein the viewer-side polarizing plate and the backlight-side polarizing plate are both rectangular, the viewer-side polarizing plate and the backlight-side polarizing plate both have a polarizer layer and a protective film, the protective film of the viewer-side polarizing plate has an in-plane retardation value of 6000 nm or more, the absorption axis of the polarizer layer of the viewer-side polarizing plate is oriented in the long side direction of the rectangle, the viewer-side polarizing plate and the backlight-side polarizing plate are arranged such that the absorption axes of the polarizer layers thereof are perpendicular to each other, the protective film of the viewer-side polarizing plate has a ratio of the rigidity in the short side direction of the rectangle to the rigidity in the long side direction of the rectangle of 2.0 or more, and the absolute value of the difference between the rigidity in the long side direction of the protective film of the viewer-side polarizing plate and the rigidity in the long side direction of the protective film of the backlight-side polarizing plate is 90 mm·MPa or less.

[0008] The polarizing plate set of the present invention may have one or more of the features listed below.

[0009] The ratio of the contraction force in the long side direction of the polarizer layer of the backlight side polarizing plate to the contraction force in the long side direction of the polarizer layer of the viewer side polarizing plate may be 0.3 or more.

[0010] The ratio of the thickness of the polarizer layer of the backlight-side polarizing plate to the thickness of the polarizer layer of the viewer-side polarizing plate may be 0.6 or more.

[0011] The polarizer layer of the backlight side polarizing plate may have a thickness of 0.015 mm or more.

[0012] The contraction force in the long side direction of the polarizer layer of the backlight side polarizing plate may be 0.8 N / 2 mm or more.

[0013] The thickness of the protective film of the viewer-side polarizing plate may be 0.06 mm or more, and the thickness of the protective film of the backlight-side polarizing plate may be 0.06 mm or less.

[0014] The polarizer layers of the viewer-side polarizing plate and the backlight-side polarizing plate may each be a stretched polyvinyl alcohol film.

[0015] Each of the viewer-side polarizing plate and the backlight-side polarizing plate may have a (meth)acrylic resin film on the surface of the polarizer layer opposite to the protective film side.

[0016] The viewer-side polarizing plate and the backlight-side polarizing plate may both be disposed so that the protective film side is located farther from the liquid crystal cell.

[0017] Both the viewer-side polarizing plate and the backlight-side polarizing plate may have a pressure-sensitive adhesive layer on the surface of the (meth)acrylic resin film opposite to the polarizer layer.

[0018] The present invention also provides a liquid crystal display device comprising a liquid crystal cell and the above polarizing plate set. Effect of the Invention

[0019] According to the present invention, it is possible to provide a polarizing plate set that can suppress rainbow unevenness and reduce warping of a laminated structure obtained by bonding the polarizing plate set to a liquid crystal cell in a heat-resistant environment, and also to provide a liquid crystal display device including the polarizing plate set. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram showing a laminated structure according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing a main part of an embodiment of the present invention. [Diagram 3] FIG. 4 is a diagram showing measurement points of the amount of warpage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention is a component of a liquid crystal display device, and is a pair of polarizing plate sets, including a viewer-side polarizing plate arranged on the viewer side of a liquid crystal cell and a backlight-side polarizing plate arranged on the backlight side. The present invention is also a liquid crystal display device including a pair of polarizing plate sets. Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. Note that the same or corresponding parts in each drawing are given the same reference numerals, and duplicated explanations will be omitted.

[0022] <Laminated structure> As shown in FIG. 1, the liquid crystal display device 1 includes a liquid crystal cell 2 and a pair of polarizing plate sets 3 arranged so as to sandwich the liquid crystal cell 2 from both sides. The pair of polarizing plate sets 3 includes a viewer-side polarizing plate 3A arranged on one side of the liquid crystal cell 2 and a backlight-side polarizing plate 3B arranged on the other side. Here, the terms "viewer side" and "backlight side" are names derived from the configuration of the liquid crystal display device 1. Note that FIG. 1 shows the optical system portion of the liquid crystal display device 1 for explaining the polarizing plate set 3 of this embodiment, and shows only the portion of the structure having a laminated structure of "viewer-side polarizing plate 3A / liquid crystal cell 2 / backlight-side polarizing plate 3B". Hereinafter, the structure having this laminated structure will be referred to as a "laminated structure" (reference numeral 10).

[0023] The viewer-side polarizing plate 3A has a first protective film 5A, a first polarizer layer 6A, and a second protective film 7A laminated thereon, in that order from the side farthest from the liquid crystal cell 2. These layers are bonded to each other by an adhesive layer 8. The backlight-side polarizing plate 3B has a third protective film 5B, a second polarizer layer 6B, and a fourth protective film 7B laminated thereon, in that order from the side farthest from the liquid crystal cell 2. These layers are bonded to each other by an adhesive layer 8.

[0024] Both the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B further have an adhesive layer 9 described below, and are attached to the liquid crystal cell 2 via this adhesive layer. The liquid crystal cell 2, the viewer-side polarizing plate 3A, and the backlight-side polarizing plate 3B are all rectangular, and are attached so that their long sides coincide with each other. Hereinafter, in this specification, the terms "long side direction" and "short side direction" will be used based on this rectangle.

[0025] Regarding the aspect ratio of the rectangles of the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B, the length in the long side direction may be 1.2 to 3.0 times, 1.3 to 2.5 times, or 1.4 to 1.9 times the length in the short side direction.

[0026] 2 is a diagram in which the laminated structure 10 is disassembled to extract only the components related to the main part of this embodiment, and the left-right direction in the figure is the long side direction. As shown in Fig. 2, in the viewer-side polarizing plate 3A, the absorption axis P1 of the first polarizer layer 6A is oriented in the long side direction. On the other hand, in the backlight-side polarizing plate 3B, the absorption axis P2 of the second polarizer layer 6B is oriented in a direction perpendicular to the absorption axis P1 of the first polarizer layer 6A, i.e., in the short side direction of the backlight-side polarizing plate 3B.

[0027] <Protective film> In the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B, the first protective film 5A and the third protective film 5B are located farther from the liquid crystal cell 2 than the first polarizer layer 6A and the second polarizer layer 6B, respectively. On the other hand, the second protective film 7A and the fourth protective film 7B are located closer to the liquid crystal cell 2 than the first polarizer layer 6A and the second polarizer layer 6B, respectively. Of these, the first protective film 5A and the third protective film 5B in particular contribute to suppressing shrinkage of the first polarizer layer 6A and the second polarizer layer 6B.

[0028] (First protective film and third protective film) The first protective film 5A is made of an optically transparent thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as linear polyolefin resins (polyethylene resins, polypropylene resins, etc.) and cyclic polyolefin resins (norbornene resins, etc.); cellulose resins (cellulose ester resins, etc.); polyester resins (polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.); polycarbonate resins; (meth)acrylic resins; polystyrene resins; polyether ether ketone resins; polysulfone resins, or mixtures or copolymers thereof. Among these, polyester resins are preferred.

[0029] Specific examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polycyclohexane dimethyl terephthalate, and polycyclohexane dimethyl naphthalate.

[0030] The thickness of the first protective film 5A may be 10 μm to 200 μm, preferably 30 μm to 120 μm, more preferably 40 μm to 100 μm, further preferably 50 μm to 90 μm, and particularly preferably 60 μm to 85 μm. When the thickness of the first protective film 5A is 10 μm or more, the web handleability of the film tends to be high. On the other hand, when the thickness is 200 μm or less, it is preferable from the viewpoint of thinning of the polarizing plate.

[0031] The first protective film 5A preferably has an elastic modulus within a predetermined range. The elastic modulus in the long side direction (also a direction parallel to the absorption axis P1 of the first polarizer layer 6A) may be 1400 MPa to 2300 MPa, preferably 1500 MPa to 2200 MPa, and more preferably 1600 MPa to 1900 MPa. The elastic modulus in the short side direction (also a direction perpendicular to the absorption axis P1 of the first polarizer layer 6A) may be 3600 MPa to 4600 MPa, preferably 3800 MPa to 4400 MPa, and more preferably 3950 MPa to 4200 MPa. The elastic modulus here refers to the tensile elastic modulus at 80°C. A test piece cut into a rectangle of a predetermined length is pulled in the long side direction by a tensile tester, and the tensile elastic modulus can be calculated from the slope of the initial straight line in the obtained stress-strain curve.

[0032] The in-plane retardation value of the first protective film 5A is 6000 nm or more. This in-plane retardation value is preferably 7000 nm or more, more preferably 8000 nm or more, and even more preferably 10000 nm or more. When the in-plane retardation value is high, the number of peaks and valleys in the transmittance spectrum in the visible light wavelength region increases, so that light of almost all wavelengths in the wavelength region is transmitted. Therefore, the transmitted light becomes closer to white light, and rainbow unevenness is reduced.

[0033] The in-plane retardation value of the first protective film 5A can be controlled within a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high retardation value can be easily obtained by increasing the stretching ratio, decreasing the stretching temperature, and increasing the film thickness. The in-plane retardation value can be set by selecting the film formation conditions and thickness from the above conditions, taking into account the physical properties required for processing, etc.

[0034] The first protective film 5A may be a single layer or may be composed of multiple layers. A film composed of multiple layers can be produced by coextrusion. The first protective film 5A is preferably a uniaxially stretched film from the viewpoint of increasing the elastic modulus to the above-mentioned numerical range and increasing the retardation to the above-mentioned numerical range. As shown in FIG. 2, in the laminated structure 10, the stretching direction Q1 of the first protective film 5A is preferably the short side direction.

[0035] The first protective film 5A may have an antireflection layer on the surface opposite to the first polarizer layer 6A. The surface reflectance of the antireflection layer is preferably 5.7% or less. When the surface reflectance of the antireflection layer is 5.7% or less, rainbow unevenness tends to be less visible. Although the reason is not clear, it is presumed that the interface reflectance between the first protective film 5A including the antireflection layer and the air decreases. The surface reflectance of the antireflection layer is more preferably 5.0% or less, further preferably 3.5% or less, and particularly preferably 2.0% or less. The lower limit of the surface reflectance of the antireflection layer is not particularly limited, but may be, for example, 0.01%. The reflectance can be measured by any method. For example, the light reflectance at a wavelength of 550 nm can be measured from the surface on the antireflection layer side of the first protective film 5A, which is attached to a black acrylic plate via an adhesive on the side opposite to the antireflection layer side of the first protective film 5A alone, using a spectrophotometer (CM-2600d, manufactured by Konica Minolta Japan, Inc.).

[0036] The anti-reflection layer may be a single layer or a multi-layer. Examples of the anti-reflection layer include an anti-glare hard coat layer having a fine uneven surface to prevent reflection of external light. The anti-glare hard coat layer may be formed by dispersing a filler inside the hard coat layer to form an uneven surface, or may be formed by embossing the hard coat layer to form an uneven surface. For example, when forming an anti-glare hard coat layer using an ultraviolet curing resin, a resin composition obtained by dispersing a filler in an ultraviolet curing resin may be applied to the first protective film 5A and irradiated with ultraviolet light, or an ultraviolet curing resin may be applied to the first protective film 5A and the coating film may be adhered to the uneven surface of a mold and irradiated with ultraviolet light.

[0037] As another form of the antireflection layer, when the antireflection layer is a single layer, the antireflection effect can be obtained by forming a low refractive index layer made of a material with a lower refractive index than the first protective film 5A so that the thickness is 1 / 4 the wavelength of the light or an odd multiple of that. When the antireflection layer is a multi-layer, the antireflection effect can be obtained by alternately forming two or more low refractive index layers and high refractive index layers, and laminating them while appropriately controlling the thickness of each layer. If necessary, a hard coat layer can be laminated between the antireflection layer and the first protective film 5A.

[0038] The antireflection layer may be a known one, and is preferably a layer formed by coating an organic thin film having a lower refractive index than the first protective film 5A or a hard coat layer or the like laminated on the first protective film 5A.

[0039] The first protective film 5A has a ratio of the rigidity in the short side direction to the rigidity in the long side direction of 2.0 or more. The value of this ratio is preferably 2.1 or more, more preferably 2.2 or more, and even more preferably 2.3 or more. Examples of upper limits of this ratio include 5.0, 4.0, and 3.0. Here, rigidity is the product of the elastic modulus and the thickness of the film. For example, the rigidity of a film with an elastic modulus of 1705 MPa and a thickness of 0.08 mm (80 μm) is expressed as the product of these values, 136.4 (unit: mm MPa).

[0040] The first protective film 5A may have a rigidity in the long side direction of 60 mm·MPa to 200 mm·MPa, preferably 80 mm·MPa to 180 mm·MPa, and more preferably 100 mm·MPa to 160 mm·MPa, and a rigidity in the short side direction of 100 mm·MPa to 400 mm·MPa, preferably 130 mm·MPa to 360 mm·MPa, and more preferably 160 mm·MPa to 340 mm·MPa.

[0041] The third protective film 5B, together with the first protective film 5A, plays an important role in reducing warpage of the laminated structure 10. That is, the first protective film 5A and the third protective film 5B function to suppress the shrinkage of the first polarizer layer 6A and the second polarizer layer 6B, respectively. From the viewpoint of suppressing the shrinkage of each polarizer layer from both sides of the liquid crystal cell 2, the third protective film 5B has the following properties.

[0042] The material constituting the third protective film 5B may be the same as the thermoplastic resin constituting the first protective film 5A. The thermoplastic resin constituting the third protective film 5B may be the same as or different from the thermoplastic resin constituting the first protective film 5A.

[0043] Taking into consideration the balance with the rigidity of the first protective film 5A, the thickness of the third protective film 5B may be 10 μm to 100 μm, preferably 20 μm to 80 μm, more preferably 25 μm to 70 μm, even more preferably 30 μm to 65 μm, and particularly preferably 35 μm to 60 μm.

[0044] The third protective film 5B preferably has an elastic modulus within a predetermined range. The elastic modulus in the long side direction (which is also a direction perpendicular to the absorption axis P2 of the second polarizer layer 6B) may be 2000 MPa to 4500 MPa, preferably 2200 MPa to 4300 MPa, and more preferably 2400 MPa to 4100 MPa. The elastic modulus in the short side direction (which is also a direction parallel to the absorption axis P2 of the second polarizer layer 6B) may be 1800 MPa to 3200 MPa, preferably 2000 MPa to 3000 MPa, and more preferably 2200 MPa to 2800 MPa.

[0045] The in-plane retardation value of the third protective film 5B does not need to be as high as the in-plane retardation of the first protective film 5A. Even if the third protective film 5B has a property that causes rainbow unevenness, the rainbow unevenness caused by the third protective film 5B is difficult to visually recognize in the liquid crystal display device 1. This is presumably because the unpolarized light emitted by the backlight passes through the third protective film 5B, and therefore has little effect on the effect that the polarizing plate set 3 of this embodiment should achieve. The third protective film 5B may be a uniaxially stretched film or a biaxially stretched film.

[0046] The third protective film 5B may have a rigidity in the long side direction of 60 mm·MPa to 300 mm·MPa, preferably 80 mm·MPa to 250 mm·MPa, and more preferably 100 mm·MPa to 200 mm·MPa, and a rigidity in the short side direction of 60 mm·MPa to 200 mm·MPa, preferably 70 mm·MPa to 170 mm·MPa, and more preferably 80 mm·MPa to 135 mm·MPa.

[0047] The absolute value of the difference between the rigidity in the long side direction of first protective film 5A and the rigidity in the long side direction of third protective film 5B is 90 mm MPa or less. The absolute value of this difference is preferably 70 mm MPa or less, more preferably 50 mm MPa or less, and even more preferably 30 mm MPa or less.

[0048] (Second Protective Film and Fourth Protective Film) The second protective film 7A and the fourth protective film 7B may be made of the same thermoplastic resin as that constituting the first protective film 5A. Among them, (meth)acrylic resins or cellulose ester resins, which are excellent in mechanical properties, transparency, cost, etc., are preferred. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0049] The (meth)acrylic resin may be a polymer mainly composed of a structural unit derived from a methacrylic acid ester (e.g., containing 50% by mass or more of the structural unit), and is preferably a copolymer in which other copolymerization components are copolymerized with the structural unit derived from a methacrylic acid ester. The (meth)acrylic resin may contain two or more structural units derived from a methacrylic acid ester. Specifically, the (meth)acrylic acid ester may be an alkyl (meth)acrylate such as methyl (meth)acrylate, ethyl (meth)acrylate, or butyl (meth)acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. In addition, examples of polymerizable monomers that can be copolymerized with the (meth)acrylic acid ester include styrene-based monomers such as styrene and alkylstyrene; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile; and polyfunctional monomers such as alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dialkenyl esters of dibasic acids such as diallyl maleate; and unsaturated carboxylic acid diesters of glycols such as alkylene glycol di(meth)acrylate. The (meth)acrylic resin film may contain two or more kinds of (meth)acrylic resins. The (meth)acrylic resin may be a resin composition containing additives added as needed.

[0050] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure can be used. Examples of the (meth)acrylic resin having a ring structure include a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure. This is because the (meth)acrylic resin having a ring structure has high heat resistance, high moist heat resistance, high transparency, and high mechanical strength when biaxially stretched.

[0051] Examples of (meth)acrylic resins having a ring structure such as a lactone ring structure include those described in JP-A Nos. 2000-230016, 2001-151814, 2002-120326, 2002-254544, and 2005-146084.

[0052] Examples of (meth)acrylic resins having a glutaric anhydride structure or a glutarimide structure include those described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.

[0053] A film formed from a (meth)acrylic resin is unlikely to have a retardation in an unstretched state, but a retardation occurs when stretched, so that a retardation can be prevented from occurring even when stretched by blending a substance that functions as a retardation reducing agent into the (meth)acrylic resin. Examples of the retardation reducing agent include styrene-acrylonitrile copolymers. The retardation value can be controlled by the stretching ratio and the blending amount of the retardation reducing agent.

[0054] From the viewpoint of impact resistance and film formability of the film, it is preferable that the (meth)acrylic resin contains acrylic rubber particles. The amount of acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the total amount of the (meth)acrylic resin and the acrylic rubber particles. The upper limit of the amount of the acrylic rubber particles is not critical, but if the amount of the acrylic rubber particles is too large, the surface hardness of the film decreases, and when the film is subjected to a surface treatment, the solvent resistance to the organic solvent in the surface treatment agent decreases. Therefore, the amount of the acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 80% by mass or less, more preferably 60% by mass or less.

[0055] Specific examples of the cellulose ester resin include cellulose acetate, propionate, butyrate, and mixed esters thereof, of which triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, and cellulose acetate butyrate are preferred.

[0056] The thermoplastic resin constituting the second protective film 7A and the fourth protective film 7B may be the same as or different from the thermoplastic resin constituting the first protective film 5A.

[0057] The thickness of each of the second protective film 7A and the fourth protective film 7B may be 1 μm to 150 μm, preferably 5 μm to 100 μm, and more preferably 10 μm to 60 μm. The thickness is more preferably 50 μm or less, and particularly preferably 30 μm or less. Reducing the thickness of the second protective film 7A and the fourth protective film 7B is advantageous for reducing the thickness of the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B.

[0058] Both the second protective film 7A and the fourth protective film 7B may be a uniaxially stretched film or a biaxially stretched film.

[0059] <Polarizer layer> The first polarizer layer 6A and the second polarizer layer 6B each include a polarizer. The first polarizer layer 6A and the second polarizer layer 6B may each be a polarizer itself.

[0060] A polarizer is a film that has the property of absorbing linearly polarized light having a vibration plane parallel to its absorption axis and transmitting linearly polarized light having a vibration plane perpendicular to the absorption axis (parallel to the transmission axis). The polarizer may be, for example, a film in which a dichroic dye is adsorbed and aligned on a polyvinyl alcohol-based resin film, or a cured film in which a dichroic dye is aligned in a polymerizable liquid crystal compound and the polymerizable liquid crystal compound is polymerized.

[0061] The polarizer may be any of an absorptive polarizer (selectively transmitting linearly polarized light in one direction from natural light as described above and absorbing linearly polarized light in the other direction), a reflective polarizer (reflecting linearly polarized light in the other direction), and a scattering polarizer (scattering linearly polarized light in the other direction), but an absorptive polarizer is preferred from the viewpoint of excellent visibility when the polarizing plate is applied to a liquid crystal display device, etc. Among them, the polarizer is more preferably a polyvinyl alcohol-based polarizer made of a polyvinyl alcohol-based resin, further preferably a polyvinyl alcohol-based polarizer in which a dichroic pigment such as iodine or a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film, and particularly preferably a polyvinyl alcohol-based polarizer in which iodine is adsorbed and oriented in a polyvinyl alcohol-based resin film.

[0062] Polyvinyl alcohol resins can be obtained by saponifying polyvinyl acetate resins. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, as well as copolymers of vinyl acetate and monomers copolymerizable with vinyl acetate. Examples of monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having ammonium groups. Iodine and dichroic organic dyes are used as dichroic dyes.

[0063] A polarizer, which is a film in which a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film, can be produced, for example, through a dyeing step of dyeing a polyvinyl alcohol-based resin film with a dichroic dye, a crosslinking step of treating the film after the dyeing step in a crosslinking bath containing a crosslinking agent, and a stretching step of uniaxially stretching the film.

[0064] The method for producing a polarizer may further include other steps in addition to those described above, such as a swelling step for swelling the film before the dyeing step, a water washing step for washing the film surface after the crosslinking step, a drying step for subjecting the polyvinyl alcohol-based resin film after the crosslinking step to a drying treatment, an electromagnetic wave irradiation step for irradiating the film with electromagnetic waves after the crosslinking step, a complementary color step for adjusting the hue of the film after the crosslinking step, and a high-temperature, high-humidity step for subjecting the film after the crosslinking step to a high-temperature, high-humidity treatment.

[0065] The stretching step, i.e., the uniaxial stretching of the polyvinyl alcohol-based resin film, may be carried out simultaneously with any of the other process steps described above.

[0066] The various treatment steps included in the polarizer manufacturing method can be continuously carried out by continuously transporting the polyvinyl alcohol-based resin film, which is the raw film, along the film transport path of the polarizer manufacturing device. The film transport path is equipped with equipment (treatment baths, furnaces, etc.) for carrying out the various treatment steps described above in the order in which they are carried out. The treatment bath refers to a bath that contains a treatment liquid for treating the polyvinyl alcohol-based resin film, such as a swelling bath, dyeing bath, crosslinking bath, or washing bath.

[0067] The thickness of the first polarizer layer 6A may be 5 μm to 40 μm, preferably 10 μm to 35 μm, and more preferably 15 μm to 25 μm. The thickness of the second polarizer layer 6B may be 5 μm to 50 μm, preferably 10 μm to 40 μm, and more preferably 15 μm to 30 μm. The ratio of the thickness of the second polarizer layer 6B to the thickness of the first polarizer layer 6A (thickness of the second polarizer layer 6B / thickness of the first polarizer layer 6A) may be 0.6 or more, preferably 0.7 or more, and more preferably 0.9 or more.

[0068] The first polarizer layer 6A may have a contraction force in the long side direction (also a direction parallel to the absorption axis P1) of 2.0 N / 2 mm to 6.0 N / 2 mm, preferably 3.0 N / 2 mm to 5.0 N / 2 mm. The second polarizer layer 6B may have a contraction force in the long side direction (also a direction perpendicular to the absorption axis P2) of 0.8 N / 2 mm to 3.0 N / 2 mm, preferably 1.5 N / 2 mm to 2.5 N / 2 mm. The contraction force here refers to a contraction force in the long side direction that occurs when a rectangular test piece cut into a predetermined length is held in a machine and held at 80° C. for 4 hours so that the dimensions are maintained. The contraction force of the first polarizer layer 6A and the second polarizer layer 6B can be obtained as desired by adjusting the manufacturing conditions, such as the thickness of the unstretched raw film, the amount of boron contained in the crosslinking bath when manufacturing the polarizer, the immersion time in the crosslinking liquid, the temperature of the crosslinking bath, and the total stretch ratio based on the raw film.

[0069] The ratio of the contractile force of the second polarizer layer 6B in the long side direction to the contractile force of the first polarizer layer 6A in the long side direction (contractile force of the second polarizer layer 6B in the long side direction / contractile force of the first polarizer layer 6A in the long side direction) may be 0.3 or more, and preferably 0.4 or more. The upper limit of this ratio may be 1.0 or less, and preferably 0.8 or less, and more preferably 0.6.

[0070] <Adhesive layer> The adhesive layer 8 that bonds each polarizer layer and each protective film to each other can be a water-based adhesive or a curable adhesive that is cured by heating or by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, or X-rays.

[0071] Examples of the aqueous adhesive composition include a composition in which a polyvinyl alcohol resin or a urethane resin is dissolved in water as the main component, and a composition in which a polyvinyl alcohol resin or a urethane resin is dispersed in water as the main component. The aqueous adhesive composition may further contain a curing component or a crosslinking agent such as a polyaldehyde, a melamine compound, a zirconia compound, a zinc compound, a glyoxal compound, or a water-soluble epoxy resin. Examples of the aqueous adhesive composition include the adhesive composition described in JP 2010-191389 A, the adhesive composition described in JP 2011-107686 A, the composition described in JP 2020-172088 A, and the composition described in JP 2005-208456 A.

[0072] The curable adhesive composition is preferably an active energy ray curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray curable adhesive composition include a cationic polymerization type adhesive composition that contains a cationic polymerizable compound as a curable compound, a radical polymerization type adhesive composition that contains a radical polymerizable compound as a curable compound, and a hybrid type adhesive composition that contains both a cationic polymerizable compound and a radical polymerizable compound as a curable compound.

[0073] The cationic polymerizable compound is a compound or oligomer that undergoes cationic polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays or when heated. Specific examples of the epoxy compound include epoxy compounds, oxetane compounds, and vinyl compounds. Examples of the epoxy compound include alicyclic epoxy compounds (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule) such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate; aromatic epoxy compounds (compounds having an aromatic ring and an epoxy group in the molecule) such as diglycidyl ether of bisphenol A; and aliphatic epoxy compounds (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule) such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether. Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0074] Examples of cationic polymerization adhesive compositions include the cationic polymerizable compositions described in JP 2016-126345 A and JP 2021-113969 A.

[0075] The radical polymerizable compound is a compound or oligomer that undergoes a radical polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays or when heated, and specifically includes a compound having an ethylenically unsaturated bond. Examples of the compound having an ethylenically unsaturated bond include a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, and a vinyl compound having one or more vinyl groups in the molecule.

[0076] Examples of radical polymerization adhesive compositions include the radical polymerizable compositions described in JP 2016-126345 A, JP 2016-153474 A, and WO 2017 / 183335 A.

[0077] When the adhesive layer is formed from a water-based adhesive composition, the thickness may be, for example, 5 μm or less, preferably 1 μm or less, more preferably 0.5 μm or less, and may be 0.01 μm or more, preferably 0.05 μm or more. When the adhesive layer is formed from a curable adhesive composition (preferably an active energy ray curable adhesive composition), the thickness may be, for example, 15 μm or less, preferably 10 μm or less, more preferably 5 μm or less, and may be 0.1 μm or more, preferably 0.3 μm or more, more preferably 0.5 μm or more.

[0078] <Adhesive layer> The viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B are both attached to the liquid crystal cell 2 via an adhesive layer 9. The adhesive layer 9 can be obtained, for example, by dissolving or dispersing an adhesive component in a solvent to form an adhesive composition, applying this onto a release film, and drying it. This is attached to the second protective film 7A side of the viewer-side polarizing plate 3A and to the fourth protective film 7B side of the backlight-side polarizing plate 3B, respectively, and the release film is peeled off before being attached to the liquid crystal cell 2.

[0079] Examples of the adhesive composition constituting the adhesive layer 9 include adhesive compositions containing, as a base polymer, a (meth)acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, a polyether resin, etc. Among these, from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc., a (meth)acrylic adhesive composition containing a (meth)acrylic resin is preferred.

[0080] The thickness of the adhesive layer 9 is determined depending on the adhesive strength etc., and is, for example, from 1 μm to 50 μm, preferably from 2 μm to 40 μm, and more preferably from 3 μm to 30 μm.

[0081] <Liquid crystal cell> A conventionally known liquid crystal cell can be used as the liquid crystal cell 2. The thickness of the liquid crystal cell 2 may be 0.2 mm to 20 mm, preferably 0.4 mm to 10 mm, more preferably 0.6 to 5 mm, and further preferably 0.8 to 3 mm.

[0082] <Effects> In general, a laminated structure of "viewer-side polarizing plate / liquid crystal cell / backlight-side polarizing plate" formed as a part of a liquid crystal display device is usually rectangular, and the viewer-side polarizing plate and the backlight-side polarizing plate are also rectangular. The entire laminated structure is often designed so that the absorption axis of the polarizer layer of the viewer-side polarizing plate faces the long side direction. In this case, warping occurs in the laminated structure such that the viewer-side polarizing plate side is concave. Here, "warping" refers to warping that occurs as a change over time after the manufacture of the laminated structure, or in a heat-resistant environment as a test of the laminated structure.

[0083] The cause of the warping is believed to be the difference in the degree of shrinkage between the polarizer layer of the viewing side polarizer and the polarizer layer of the backlight side polarizer. In general, when a crosslinked structure is formed in the molecular structure of a polarizer, further crosslinking progresses as a change over time after production. In addition, when the polarizer is stretched, a force acts to return to the state before stretching. As a result, both polarizer layers shrink, and the difference in the degree of shrinkage leads to warping of the entire laminate structure.

[0084] In this embodiment, since the first protective film 5A and the third protective film 5B have the above-mentioned relationship in terms of rigidity, the degree of shrinkage of the first polarizer layer 6A and the second polarizer layer 6B is well balanced, and the shrinkage difference is small. Therefore, it is possible to reduce the warping of the entire laminated structure 10. In addition, since the in-plane retardation value of the first protective film 5A is 6000 nm or more, rainbow unevenness is suppressed.

[0085] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above embodiments. For example, in the above embodiments, both the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B have a polarizer layer and protective films attached to both sides of the polarizer layer with an adhesive, but the viewer-side polarizing plate 3A and the backlight-side polarizing plate 3B may further have other functional layers such as a retardation layer on the side closer to the liquid crystal cell 2. Alternatively, the second protective film 7A and the fourth protective film 7B may also function as a retardation layer. EXAMPLES

[0086] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the present invention is not limited to the following examples. Note that "%" and "parts" in the description are by mass% and parts by mass unless otherwise specified.

[0087] <Manufacturing of each component and physical property measurement> (Production Example 1: Production of Polarizer 1) A long polyvinyl alcohol film (average polymerization degree: about 2400, saponification degree: 99.9 mol% or more, thickness: 60 μm) was continuously conveyed and immersed in a swelling bath of pure water at 20 ° C. for a residence time of 31 seconds (swelling step). Thereafter, the film pulled out of the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / water at 2 / 100 (mass ratio) for a residence time of 122 seconds (dyeing step). Next, the film pulled out of the dyeing bath was immersed in a crosslinking bath at 56 ° C. with potassium iodide / boric acid / water at 12 / 4.1 / 100 (mass ratio) for a residence time of 70 seconds, and then in a crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at 9 / 2.9 / 100 (mass ratio) for a residence time of 13 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 5.5 times. Next, the film was pulled out of the crosslinking bath and immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step), and then introduced into a drying oven at 80°C for a residence time of 190 seconds and dried (drying step) to obtain a polarizer. The polarizer obtained in this manner (hereinafter referred to as "polarizer 1") had a thickness of 24 μm.

[0088] (Production Example 2: Production of Polarizer 2) Except for changing the thickness of the long polyvinyl alcohol film to 45 μm, a polarizer was produced in the same manner as in Production Example 1. The obtained polarizer (hereinafter referred to as "Polarizer 2") had a thickness of 18 μm.

[0089] (Production Example 3: Production of Polarizer 3) Except for changing the thickness of the long polyvinyl alcohol film to 30 μm, a polarizer was produced in the same manner as in Production Example 1. The obtained polarizer (hereinafter referred to as "Polarizer 3") had a thickness of 12 μm.

[0090] (Production Example 4: Production of polyethylene terephthalate resin (1)) While the esterification reactor was heated to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were charged into the esterification reactor to obtain a mixture. While stirring the mixture, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added as catalysts to the mixture. The gauge pressure in the esterification reactor was set to 0.34 MPa, and the pressurized esterification reaction was carried out at 240°C. Thereafter, the esterification reactor was returned to normal pressure, and 0.014 parts of phosphoric acid were added. Thereafter, the temperature was raised to 260°C over 15 minutes, and 0.012 parts of trimethyl phosphate were added to obtain a mixture. After 15 minutes, the mixture was dispersed using a high-pressure disperser, and after another 15 minutes, the esterification reaction product was transferred to a polycondensation reactor, and polycondensation reaction was carried out at 280°C under reduced pressure.

[0091] After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets to obtain polyethylene terephthalate resin (hereinafter referred to as "PET (1)").

[0092] (Production Example 5: Production of polyethylene terephthalate resin (2)) 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) and 90 parts of the PET (1) obtained in Production Example 4 were mixed and extruded in a kneading extruder to obtain a polyethylene terephthalate resin (2) containing an ultraviolet absorber (hereinafter referred to as "PET (2)").

[0093] (Production Example 6: Preparation of Coating Solution for Forming Adhesive Layer) A water-dispersible sulfonate metal salt group-containing copolymer polyester resin was prepared by carrying out an ester exchange reaction and a polycondensation reaction in a conventional manner between a dicarboxylic acid component consisting of 46 mol % terephthalic acid, 46 mol % isophthalic acid, and 8 mol % sodium 5-sulfonatoisophthalate, and a glycol component consisting of 50 mol % ethylene glycol and 50 mol % neopentyl glycol.

[0094] Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve, and 0.06 parts of nonionic surfactant were mixed to obtain a mixture. The mixture obtained was heated to 77°C and stirred, while adding 5 parts of the water-dispersible sulfonate metal salt group-containing copolymer polyester resin, and continued stirring until no resin lumps remained, to obtain a resin water dispersion. The obtained resin water dispersion was cooled to 25°C to obtain a uniform water-dispersible copolymer polyester resin solution with a solid content concentration of 5.0% by mass.

[0095] 3 parts of aggregated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of aggregated silica particles. 0.54 parts of the aqueous dispersion of aggregated silica particles was added to 99.46 parts of the water-dispersible copolymerized polyester resin liquid, and 20 parts of water was further added while stirring to obtain a coating liquid for forming an easy-adhesion layer.

[0096] (Production Example 7: Production of Protective Film 1) In order to prepare a film consisting of three layers, A layer, B layer, and C layer, using two extruders, PET (1) was dried and fed to extruder 1 (for outer layer A layer and outer layer C layer). In addition, PET (3) was prepared by mixing 90 parts of PET (1) produced in Production Example 4 and 10 parts of PET (2) produced in Production Example 5, and was dried under reduced pressure at 135 ° C for 6 hours, and then fed to extruder 2 (for intermediate layer B layer). PET (1) fed to extruder 1 and PET (3) fed to extruder 2 were melted at 285 ° C. The two types of polymers were filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10 μm, particle 95% cut) and laminated in a two-type three-layer merging block, extruded from a die in the form of a sheet, and then wrapped around a casting drum with a surface temperature of 30 ° C. using an electrostatic casting method, cooled and solidified, and an unstretched PET film was produced. At this time, the discharge rates of each extruder were adjusted so that the thickness ratio of layers A, B and C was 10:80:10.

[0097] Next, on both sides of the obtained unstretched PET film, a coating amount of 0.08 g / m2 after drying was applied by the reverse roll method. 2 The above-mentioned coating solution for forming an easy-adhesion layer was applied so that the film thickness was 100 mm, and then the film was dried at 80° C. for 20 seconds. The unstretched PET film on which the coating layer was formed was stretched 4.0 times in the width direction in a hot air zone at a temperature of 125° C. in a tenter stretching machine while holding the ends of the film with clips. Next, while maintaining the width stretched in the width direction, the film was treated at a temperature of 225° C. for 10 seconds, and further subjected to a relaxation treatment of 3.0% in the width direction to obtain a uniaxially stretched PET film (hereinafter referred to as "protective film 1") on which an easy-adhesion layer having a film thickness of about 80 μm was formed.

[0098] (Production Example 8: Production of Protective Film 2) A mixture of 90 parts of a (meth)acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extrusion molded to obtain a 40 μm thick acrylic resin film (hereinafter referred to as "protective film 2") that was stretched 2.0 times vertically and 2.4 times horizontally.

[0099] (Production Example 9: Production of Polarizing Plate 1 with Adhesive Layer) One side of the protective film 1 obtained in Production Example 7 and the protective film 2 obtained in Production Example 8 were each subjected to a corona treatment, and an epoxy-based ultraviolet-curable adhesive was applied to the corona-treated surface using an adhesive applicator. The 24 μm-thick polarizer 1 obtained in Production Example 1 was then placed on the coated layer surface, and then pressed and laminated using a lamination roll to obtain a polarizing plate precursor. This polarizing plate precursor was irradiated from the protective film 2 side with an ultraviolet irradiation device equipped with a belt conveyor (the lamp was a metal halide lamp manufactured by Eye Graphics Co., Ltd.) with an accumulated light amount of 200 mJ / cm. 2 The adhesive was cured by irradiating the film with ultraviolet light so that the wavelength was (UVB) to obtain a polarizing plate. From the above, a polarizing plate 1 having a protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) was obtained. The polarizing plate 1 has a configuration in which the uniaxial stretching direction of the protective film 1 and the absorption axis direction of the polarizer (stretching direction of the polarizer) are perpendicular to each other.

[0100] Next, a release film-attached adhesive layer having a (meth)acrylic adhesive layer (thickness 20 μm) on the release-treated surface of a release film was prepared. The release film-attached adhesive layer was laminated on the (meth)acrylic resin film side of the polarizing plate after the surface of the (meth)acrylic resin film was corona-treated, to obtain a polarizing plate 1 with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0101] (Production Example 10: Production of Polarizing Plate 2 with Adhesive Layer) A polarizing plate was obtained in the same manner as in Production Example 9, except that a biaxially stretched polyethylene terephthalate (PET) protective film made of a polyester resin having a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation) was used instead of the protective film 1 obtained in Production Example 7. From the above, a polarizing plate 2 having a protective film (biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) was obtained.

[0102] Then, a pressure-sensitive adhesive layer and a release film were laminated in the same manner as in Production Example 9 to obtain a polarizing plate 2 with a pressure-sensitive adhesive layer. The polarizing plate with a pressure-sensitive adhesive layer had a structure of protective film (a biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer / adhesive layer / protective film 2 ((meth)acrylic resin film) / pressure-sensitive adhesive layer / release film.

[0103] (Production Example 11: Production of Polarizing Plate 3 with Adhesive Layer) A polarizing plate 3 with an adhesive layer was obtained in the same manner as in Production Example 10, except that a protective film of biaxially stretched polyethylene terephthalate (PET) made of a polyester resin having a thickness of 38 μm (manufactured by Toray Industries, Inc., product name: Lumirror T60) was used instead of the protective film of biaxially stretched polyethylene terephthalate (PET) made of a polyester resin having a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation) for the polarizing plate 2 with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Toray Industries, Inc., product name: Lumirror T60) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0104] (Production Example 12: Production of Polarizing Plate 4 with Adhesive Layer) A polarizing plate 4 with an adhesive layer was obtained in the same manner as in Production Example 10, except that the 18 μm polarizing plate 2 prepared in Production Example 2 was used instead of the 24 μm polarizing plate 1 prepared in Production Example 1. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer 2 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0105] (Production Example 13: Production of Polarizing Plate 5 with Adhesive Layer) A polarizing plate 5 with an adhesive layer was obtained in the same manner as in Production Example 10, except that a protective film of biaxially stretched polyethylene terephthalate (PET) made of polyester resin having a thickness of 50 μm (manufactured by Toray Industries, Inc., product name: Lumirror T60) was used instead of the protective film of biaxially stretched polyethylene terephthalate (PET) made of polyester resin having a thickness of 38 μm (manufactured by Mitsubishi Chemical Corporation) for the polarizing plate 2 with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film having a thickness of 50 μm, manufactured by Toray Industries, Inc., product name: Lumirror T60) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0106] (Production Example 14: Production of Polarizing Plate 6 with Adhesive Layer) A polarizing plate 6 with an adhesive layer was obtained in the same manner as in Production Example 10, except that the 12 μm polarizer 3 prepared in Production Example 3 was used for the polarizing plate 2 with an adhesive layer instead of the 24 μm polarizer 1 prepared in Production Example 1. The polarizing plate with an adhesive layer has a structure of protective film (biaxially stretched polyester resin film having a thickness of 38 μm, manufactured by Mitsubishi Chemical Corporation) / adhesive layer / polarizer 3 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.

[0107] (Measurement of in-plane retardation value of polyester resin film) The in-plane retardation values ​​of the protective film 1 obtained in Manufacturing Example 7 and a 38 μm thick biaxially stretched polyethylene terephthalate (PET) protective film (manufactured by Mitsubishi Chemical Corporation) were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.).

[0108] (Measurement of elastic modulus of protective film at 80℃) The protective film obtained above was cut into a rectangle of 100 mm in length × 10 mm in width. Next, both ends of the test piece in the long side direction were clamped with the upper and lower grips of a tensile tester (Autograph AG-1S tester, manufactured by Shimadzu Corporation) so that the distance between the grips was 50 mm, and the test piece was pulled in the long side direction at a pulling speed of 50 mm / min in an environment of 80°C, and the tensile modulus of elasticity (MPa) of the resin film at 80°C was calculated from the slope of the initial straight line in the obtained stress-strain curve.

[0109] The test pieces prepared were one in which, when the protective film was attached to the polarizer, the long side direction was parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) and the width direction was perpendicular to the absorption axis of the polarizer (TD direction) (test piece 1), and one in which, when the protective film was attached to the polarizer, the long side direction was perpendicular to the absorption axis of the polarizer (TD direction) and the width direction was parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) (test piece 2). From test piece 1, the tensile modulus in the direction parallel to the absorption axis of the polarizer (stretching direction of the polarizer, MD direction) when the protective film is attached to the polarizer is obtained, and from test piece 2, the tensile modulus in the direction perpendicular to the absorption axis of the polarizer (TD direction) when the protective film is attached to the polarizer is obtained.

[0110] (polarizer contraction force) A rectangular test piece with a width of 2 mm and a length of 10 mm, with the long side in the stretching direction (MD, absorption axis direction), was cut out from the polarizer 1 obtained in Production Example 1 (specimen 3). A rectangular test piece with a width of 2 mm and a length of 10 mm, with the long side in the direction perpendicular to the stretching direction (TD, transmission axis direction), was cut out from the polarizer obtained in Production Examples 1 to 3 (specimen 4). This sample was set in a thermomechanical analyzer (TMA) "EXSTAR-6000" manufactured by SII Nano Technology Co., Ltd., and the shrinkage force in the long side direction generated when the sample was held at 80°C for 4 hours while keeping the dimensions constant was measured. The shrinkage force in the absorption axis direction of the polarizer was obtained from specimen 3, and the shrinkage amount in the direction perpendicular to the absorption axis direction of the polarizer was obtained from specimen 4.

[0111] <Example 1> A polarizing plate 1 with an adhesive layer was prepared as a polarizing plate on the viewing side, and a polarizing plate 2 with an adhesive layer was prepared as a polarizing plate on the backlight side. The polarizing plate 1 with an adhesive layer, which is a polarizing plate on the viewing side, was cut so that the long side direction was parallel to the absorption axis of the polarizing plate. The polarizing plate 2 with an adhesive layer, which is a polarizing plate on the backlight side, was cut so that the long side direction was perpendicular to the absorption axis of the polarizing plate. The size of the cut polarizing plate was 150 mm x 90 mm. After peeling the release film from the polarizing plate 1 with an adhesive layer, the adhesive layer was attached to one side of an alkali-free glass substrate (thickness 0.2 mm, Corning "Eagle XG", 160 mm x 102 mm). Furthermore, in order to reproduce the laminated state of an actual liquid crystal display device, the polarizing plate 2 with an adhesive layer was attached to a surface other than the polarizing plate-attached surface of the glass substrate so that the absorption axes of the two polarizing plates were perpendicular to each other, thereby obtaining a glass-attached optical laminate.

[0112] (Warpage evaluation) The glass-laminated optical laminate obtained by the above method was left to stand for 48 hours in an environment at a temperature of 80°C, and then taken out into an environment at a temperature of 23°C and a relative humidity of 55%, and the warpage state was evaluated 2 hours later. The polarizing plate 1 with the adhesive layer (the polarizing plate on the viewing side) was placed on the measurement table of a two-dimensional measuring device (Nikon Corporation, NEXIV (product name) MR-12072) so that it was on the upper side. Next, the surface of the measurement table was focused, and using that as a reference, 25 points on the sample surface were focused, and the height from the reference focus was measured. The difference between the maximum and minimum heights at the 25 measurement points was taken as the amount of warpage. Specifically, the points shown in FIG. 3 (reference numeral 30) were taken as the measurement points. The 25 points shown in FIG. 3 were points in an area 5 mm inward from the end of the polarizing plate, and were provided at intervals of about 20 mm in the short side direction and about 35 mm in the long side direction. The judgment criteria for the warpage evaluation are as follows. ◎: Very small (less than 0.4 mm) ○: Small (more than 0.4 mm and less than 0.7 mm) △: Large (more than 0.7 mm and less than 1.0 mm) ×: Very large (over 1.0 mm)

[0113] (Rainbow unevenness evaluation) The polarizing plate 1 with an adhesive layer, which is the viewing side polarizing plate, and the polarizing plate 2 with an adhesive layer, which is the backlight side polarizing plate, were cut so that the long side direction was parallel to the absorption axis of the polarizing plate. The size of the cut polarizing plate was 150 mm x 90 mm. After peeling off the release film from the polarizing plate 1 with an adhesive layer, the adhesive layer was attached to one side of an alkali-free glass substrate (thickness 0.2 mm, Corning "Eagle XG", 160 mm x 102 mm). Furthermore, in order to reproduce the display state of an actual liquid crystal display device, the polarizing plate 2 with an adhesive layer was attached to a surface other than the polarizing plate attachment surface of the glass substrate so that the absorption axes of the two polarizing plates were parallel (the transmission axes were parallel) with a glass substrate 20 (FIG. 3) sandwiched therebetween, to obtain a glass-attached optical laminate.

[0114] The above-mentioned glass-laminated optical laminate was placed on top of a backlight light source, with the polarizing plate 2 with an adhesive layer facing the light source, and the polarizing plate was visually observed in an oblique direction from the polyester resin film side of the polarizing plate 1 with an adhesive layer to confirm the visibility of rainbow unevenness, and an evaluation was performed based on the degree of coloring of the unevenness, etc., according to the following criteria. ○: Weak rainbow unevenness ×: Strong rainbow unevenness

[0115] <Examples 2 to 5, Comparative Examples 1 to 2> Polarizing plates with pressure-sensitive adhesive layers to be laminated on both sides of an alkali-free glass substrate were selected in combination as shown in Table 1, and glass-laminated optical laminates of Examples 2 to 5 and Comparative Examples 1 and 2 were obtained in the same manner as in Example 1. Each glass-laminated optical laminate was evaluated for warpage and rainbow unevenness.

[0116] <Result> The polarizing plate sets of Examples 1 to 5 satisfy both of the following: [1] The ratio (b / a) of the rigidity in the short side direction to the rigidity in the long side direction of the outer protective film (first protective film) of the viewer-side polarizing plate is 2.0 or more; and [2] The absolute value of the difference between the rigidity in the long side direction of the outer protective film (first protective film) of the viewer-side polarizing plate and the rigidity in the long side direction of the outer protective film (third protective film) of the backlight-side polarizing plate is 90 mm·MPa or less. In this case, both the warp evaluation and the rainbow unevenness evaluation are good. In contrast, the polarizing plate sets of Comparative Examples 1 and 2, which do not satisfy either [1] or [2] above, are poor in the warp evaluation or the rainbow unevenness evaluation.

[0117] [Table 1] [Industrial Applicability]

[0118] The present invention can be used as a component of a liquid crystal display device. [Explanation of symbols]

[0119] 1...liquid crystal display device, 2...liquid crystal cell, 3...polarizing plate set, 3A...viewer-side polarizing plate, 3B...backlight-side polarizing plate, 5A...first protective film, 5B...third protective film, 6A...first polarizer layer, 6B...second polarizer layer, 7A...second protective film, 7B...fourth protective film, 8...adhesive layer, 9...pressure-sensitive adhesive layer, 10...laminated structure, 20...glass substrate, 30...measurement point, P1...absorption axis of first polarizer layer, P2...absorption axis of second polarizer layer, Q1...stretching direction of first protective film, Q2...stretching direction of third protective film.

Claims

1. A pair of polarizing plates including a viewer-side polarizing plate arranged on the viewer side of a liquid crystal cell and a backlight-side polarizing plate arranged on the backlight side of the liquid crystal cell, The viewer-side polarizing plate and the backlight-side polarizing plate are both rectangular, each of the viewer-side polarizing plate and the backlight-side polarizing plate has a polarizer layer and a protective film; the in-plane retardation value of the protective film of the viewer-side polarizing plate is 6000 nm or more, an absorption axis of a polarizer layer of the viewer-side polarizing plate is oriented in a direction parallel to a long side of the rectangle; the viewer-side polarizing plate and the backlight-side polarizing plate are arranged such that the absorption axes of the polarizer layers of the viewer-side polarizing plate and the backlight-side polarizing plate are perpendicular to each other; the protective film of the viewer-side polarizing plate has a ratio of rigidity in a short side direction of the rectangle to rigidity in a long side direction of the rectangle of 2.0 or more; a polarizing plate set in which the absolute value of the difference between the rigidity of the protective film of the viewer-side polarizing plate in the long side direction and the rigidity of the protective film of the backlight-side polarizing plate in the long side direction is 90 mm·MPa or less.

2. The polarizing plate set according to claim 1 , wherein the ratio of the contractile force in the long side direction of the polarizer layer of the backlight side polarizing plate to the contractile force in the long side direction of the polarizer layer of the viewer side polarizing plate is 0.3 or more.

3. The polarizing plate set according to claim 1 , wherein a ratio of a thickness of the polarizer layer of the backlight side polarizing plate to a thickness of the polarizer layer of the viewer side polarizing plate is 0.6 or more.

4. The polarizing plate set according to claim 1 , wherein the polarizer layer of the backlight side polarizing plate has a thickness of 0.015 mm or more.

5. The polarizing plate set according to claim 1 , wherein the contractile force in the long side direction of the polarizer layer of the backlight side polarizing plate is 0.8 N / 2 mm or more.

6. The thickness of the protective film of the viewer-side polarizing plate is 0.06 mm or more, The polarizing plate set according to claim 1 , wherein the protective film of the backlight side polarizing plate has a thickness of 0.06 mm or less.

7. The polarizing plate set according to claim 1 , wherein the polarizer layers of the viewer-side polarizing plate and the backlight-side polarizing plate are both stretched polyvinyl alcohol films.

8. The polarizing plate set according to claim 1 , wherein each of the viewer-side polarizing plate and the backlight-side polarizing plate has a (meth)acrylic resin film on a surface of the polarizer layer opposite to the protective film.

9. The polarizing plate set according to claim 8 , wherein the viewer-side polarizing plate and the backlight-side polarizing plate are both arranged such that the protective film side is farther from the liquid crystal cell.

10. The polarizing plate set according to claim 8 , wherein each of the viewer-side polarizing plate and the backlight-side polarizing plate has a pressure-sensitive adhesive layer on a surface of the (meth)acrylic resin film opposite to the polarizer layer.

11. A liquid crystal display comprising a liquid crystal cell and the polarizing plate set according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Polarizing plate and image display device

    JP2014206702A

  • Liquid crystal display device

    JP2014219438A

  • Polarizing film, polarizing plate, and liquid crystal panel

    JP2015222368A

  • Liquid crystal display device

    JP2016504632A

  • Liquid crystal display device