Ultra-rapid hardening mortar material for grout, and mortar hardened product
A mortar material with controlled expansion rates using cement, calcium aluminate, and gypsum addresses excessive long-term expansion issues, ensuring structural integrity and adhesion.
Patent Information
- Application Number
- JP2023057482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Conventional mortar materials for grout exhibit excessive long-term expansion, leading to structural damage after application, despite having ultra-fast hardening properties.
A mortar material comprising cement, calcium aluminate, and gypsum, with controlled initial expansion coefficients ranging from 0.005% to 0.5% at 3 days, 0.01% to 0.75% at 7 days, and 0.015% to 1.0% at 28 days, ensuring a moderate long-term expansion rate.
The solution provides a mortar material with controlled expansion rates, preventing structural damage by maintaining stability and adhesion over an extended period.
Smart Images

Figure 2024145223000001 
Figure 2024145223000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an ultrafast hardening mortar material for grout and a hardened mortar product. [Background technology]
[0002] Grout is used for the construction of underground structures, the installation of bridge supports, the installation of various types of machinery, and for filling gaps in walls and columns in earthquake reinforcement. In recent years, there has been an increasing demand for streamlined construction, so there is a demand for mortar materials that have ultra-fast hardening properties and self-filling and self-leveling properties.
[0003] Mortar materials lose volume as the cement hydrates or dries, and so when used as grout, there is a risk that cracks may occur or that adhesion to existing structures may decrease. The occurrence of cracks not only mars the aesthetic appearance, but also poses the risk of adversely affecting the stability, waterproofing, and watertightness of the structure.
[0004] Therefore, in order to compensate for the shrinkage of cement, suppress the occurrence of cracks, and maintain the adhesion performance with the structure, for example, 3CaO·3Al 2 O 3 ·CaSO 4 (Auin), CaSO 4 In addition to calcium sulfoaluminate-based (aluminium-based expanding material) whose main component is CaO, lime-based (lime-based expanding material) whose main component is free lime, and expanding materials containing free lime, hydraulic material, and gypsum are also used.
[0005] Known examples of materials with excellent ultra-rapid hardening properties include ultra-rapid hardening cement compositions in which metal sulfates, fly ash, or the like are added to calcium aluminates or gypsum to ensure fluidity (Patent Documents 1 to 3). In addition, an ultra-fast hardening cement made by blending calcium aluminate, gypsum, and lithium carbonate (Patent Document 4), and a mortar made by blending Portland cement with calcium aluminate, anhydrous gypsum, lithium carbonate, and hydrated lime have also been proposed (Patent Document 5). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 03-12350 [Patent Document 2] Japanese Patent Application Publication No. 01-230455 [Patent Document 3] Japanese Patent Application Publication No. 11-139859 [Patent Document 4] Japanese Patent Application Publication No. 01-290543 [Patent Document 5] JP 2005-75712 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the above conventional materials do not take into consideration long-term expansion, and there is a problem that after application to a structure as grout, the expansion becomes excessive after a long period of time, which may cause damage to the structure, etc. Therefore, there is a demand for a mortar material for grout that takes into consideration the expansion performance from the initial stage to the long term.
[0008] In view of the above, an object of the present invention is to provide an ultra-fast hardening mortar material for grout that can maintain a suitable long-term expansion rate. [Means for solving the problem]
[0009] As a result of intensive research into solving the above-mentioned problems, the inventors have found that the above problems can be solved by an ultra-fast hardening mortar material for grout that contains cement, calcium aluminate, and gypsum and has an initial expansion rate adjusted to be within a predetermined range, and have arrived at the present invention. That is, the present invention is as follows.
[0010] [1] An ultra-fast hardening mortar material for grout containing cement, calcium aluminate, and gypsum, and having expansion rates of 0.005-0.5%, 0.01-0.75%, and 0.015-1.0% at ages of 3, 7, and 28 days, respectively. [2] The ultra-fast hardening mortar material for grout according to the above [1], in which the air content after mixing is 0 to 5%. [3] The ultra-fast hardening mortar material for grout according to [1] or [2] above, having a flow value after mixing of 170 to 320 mm. [4] J after mixing 14 The ultra-fast hardening mortar material for grout according to any one of the above [1] to [3], which has a funnel flow time of 6 to 10 seconds. [5] The ultra-fast hardening mortar material for grout according to any one of the above [1] to [4], further comprising a foaming agent. [6] The ultra-fast hardening mortar material for grout according to any one of the above [1] to [5], further comprising an antifoaming agent. [7] The ultra-rapid hardening mortar material for grout according to any one of [1] to [6] above, further comprising one or more water reducing agents selected from the group consisting of lignin-based water reducing agents, melamine-based water reducing agents, and naphthalenesulfone-based water reducing agents. [8] A hardened mortar body obtained by using the ultra-rapid hardening mortar material for grout according to any one of [1] to [7] above. Effect of the Invention
[0011] According to the present invention, it is possible to provide an ultra rapid hardening mortar material for grout that can maintain a suitable long-term expansion rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to this embodiment. In addition, "%" and "parts" in this specification are based on mass unless otherwise specified.
[0013] [Ultra-fast hardening mortar material for grout] The ultra-rapid hardening mortar material for grout of the present invention contains cement, calcium aluminate, and gypsum, and has expansion coefficients of 0.005-0.5%, 0.01-0.75%, and 0.015-1.0% at ages of 3 days, 7 days, and 28 days, respectively. The expansion coefficients are preferably 3 days≦age 7 days≦age 28 days. The ultra-fast hardening mortar material for grout can be used as a grout by mixing with water, and by adjusting the initial expansion rate to be within a specified range, the long-term expansion rate can be made moderate. This makes it possible to prevent damage to structures, etc. when used as a grout in such structures. Note that the term "long-term" refers to a material age of at least 60 days or more. The expansion rate in the present invention is measured according to the method specified in JIS A 6202:2017 "Expansive additives for concrete" Appendix A "Test method for the expansion properties of expansive additives using mortar".
[0014] The ultra-fast hardening mortar material for grout has an expansion rate of 0.005 to 0.5% at 3 days, preferably 0.01 to 0.4%, more preferably 0.05 to 0.3%, and further preferably 0.1 to 0.2%. If the expansion rate at 3 days is less than 0.005%, the long-term expansion rate may be insufficient, and if it exceeds 0.5%, the long-term expansion rate may be excessive.
[0015] The ultra-fast hardening mortar material for grout has an expansion rate of 0.01 to 0.75% at 7 days, preferably 0.02 to 0.5%, more preferably 0.08 to 0.4%, and further preferably 0.12 to 0.3%. If the expansion rate at 7 days is less than 0.01%, the long-term expansion rate may be insufficient, and if it exceeds 0.75%, the long-term expansion rate may be excessive.
[0016] The ultra-fast hardening mortar material for grout has an expansion rate of 0.015 to 1.0% at 28 days, preferably 0.03 to 0.6%, more preferably 0.1 to 0.5%, and further preferably 0.16 to 0.4%. If the expansion rate at 28 days is less than 0.015%, the long-term expansion rate may be insufficient, and if it exceeds 3.5%, the long-term expansion rate may be excessive.
[0017] The ultra-fast hardening mortar material for grout has an air content of 0 to 5% after mixing, more preferably 0 to 4%, and even more preferably 0 to 3%. When the air content after mixing is within the above range, strength development is improved. The air content in the present invention is measured in accordance with the method specified in JIS A 1116:2019 "Unit volume mass test method for fresh concrete and test method by mass of air content (mass method)".
[0018] The ultra-fast hardening mortar material for grout has a flow value after mixing of preferably 170 to 320 mm, more preferably 190 to 250 mm, and even more preferably 200 to 220 mm. When the flow value after mixing is within the above range, the filling property is improved. The flow value in the present invention is measured in the method specified in JIS R 5201:2015 "Physical test method for cement" without performing the 15 times drop motion.
[0019] The ultra-fast hardening mortar material for grout is J after mixing. 14 The funnel flow time is preferably 6 to 10 seconds, more preferably 7 to 9 seconds, and even more preferably 7.5 to 8.5 seconds. 14 When the funnel flow time is within the above range, the filling property is improved. 14 The funnel flow time was measured in accordance with the method specified in the Japan Society of Civil Engineers standard JSCE-F 541-2013 "Test method for fluidity of filling mortar."
[0020] The cement contained in the ultra-fast hardening mortar material for grout according to the present embodiment is not particularly limited, and examples thereof include various Portland cements such as normal, early strength, super early strength, low heat, and moderate heat, various mixed cements obtained by mixing these Portland cements with blast furnace slag, fly ash, silica fume, etc., environmentally friendly cements (eco-cements) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials, commercially available fine particle cements, white cements, etc., and various cements can be used in a fine powder form. Also, cements adjusted by increasing or decreasing the content of components used in normal cements can be used. Furthermore, a combination of two or more of these can also be used.
[0021] In order to obtain appropriate fluidity and early strength, the Blaine specific surface area value (hereinafter simply referred to as the "Blaine value") of the cement is set to 2,500 to 7,000 cm. 2 / g, and 2,750 to 6,000 cm 2 / g, and more preferably 3,000 to 4,500 cm 2 In the present invention, the Blaine specific surface area value is measured in accordance with JIS R 5201:2015 "Physical testing methods for cement."
[0022] The calcium aluminate contained in the ultra-fast hardening mortar material for grout according to this embodiment is CaO and Al 2 O 3 It is a general term for compounds that have hydration activity and are mainly composed of CaO and / or Al. 2 O 3 Compounds in which a part of the above has been replaced with alkali metal oxides, alkaline earth metal oxides, silicon oxide, titanium oxide, iron oxide, alkali metal halides, alkaline earth metal halides, alkali metal sulfates, and alkaline earth metal sulfates, etc., or CaO and Al 2 O 3 It is a substance mainly composed of these and a small amount of these in solid solution, and calcium aluminate may be either crystalline or amorphous.
[0023] As a specific example of a crystalline substance, CaO is C, Al 2 O 3 A, R 2 O(Na 2 OK 2 O, Li 2 O) is R, then C 3 A and C with alkali metals dissolved therein 14 RA 5 , C.A., C. 12 A 7 Or C 11 A 7 ·CaF 2 , C 4 A Fe 2 O 3 , and C 3 A 3 ·CaSO 4 Among them, amorphous calcium aluminate is preferred because of its good quick setting property. In the case of amorphous calcium aluminate, the vitrification rate is preferably 80% or more.
[0024] Calcium Aluminate CaO / Al 2 O 3 The molar ratio is not particularly limited, but from the viewpoint of achieving appropriate fluidity retention and initial strength, the molar ratio is preferably from 1.3 to 3.0, and more preferably from 1.5 to 2.0.
[0025] The method of obtaining calcium aluminate is to use CaO raw materials such as calcium carbonate and calcium hydroxide, and Al raw materials such as bauxite. 2 O 3 For example, the raw materials are mixed in a predetermined ratio, heated and melted in an electric furnace, and then quenched by contacting with compressed air or water. By adjusting the ratio of each raw material, the above CaO / Al 2 O 3 The molar ratio can be adjusted, and the vitrification rate can be adjusted by the temperature during heating and melting and the cooling method.
[0026] When calcium aluminate is obtained industrially, it may contain impurities. Specific examples of impurities include, for example, SiO 2 , Fe 2 O 3 , MgO, TiO 2 , MnO, Na 2 OK 2 O, Li 2 O, S, P 2 O 5 The presence of these impurities is not particularly problematic as long as it does not substantially impair the object of the present invention. Specifically, it is not particularly problematic when the total amount of these impurities is 10% or less.
[0027] It is preferable to use calcium aluminate with an ignition loss of 1% or more as specified in JIS R 5202:2015 "Methods for Chemical Analysis of Cement", and it is more preferable to use calcium aluminate with an ignition loss of 2% or more. When the ignition loss of calcium aluminate is 1% or more, it is easy to suppress the occurrence of "flakes". There is no particular limitation on the method of making the ignition loss 1% or more, but examples include a method of supplying moisture or humidity, a method of supplying carbon dioxide gas, etc.
[0028] The Blaine value of calcium aluminate is not particularly limited, but is usually 3,000 to 9,000 cm 2 / g is preferable, and 4,000 to 8,000 cm 2 / g is more preferred.
[0029] The content of calcium aluminate in the ultra-fast hardening mortar material for grout is preferably 2 to 30 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of cement in the mortar material, from the viewpoint of adjusting the expansion rate at ages of 3 days, 7 days, and 28 days.
[0030] The gypsum contained in the ultrafast-hardening mortar material for grout according to this embodiment is a general term for gypsum anhydrate, gypsum hemihydrate, or gypsum dihydrate, and is not particularly limited. From the viewpoint of strength development, however, the use of gypsum anhydrate or gypsum hemihydrate is preferable, and the use of gypsum anhydrate is more preferable.
[0031] The Blaine value of gypsum is not particularly limited, but is usually 3,000 to 9,000 cm 2 / g is preferable, and 4,000 to 8,000 cm 2 / g is more preferred.
[0032] The gypsum content in the ultra-fast hardening mortar material for grout is preferably 3 to 40 parts by mass, and more preferably 5 to 30 parts by mass, per 100 parts by mass of cement in the mortar material, from the viewpoint of adjusting the expansion rate at ages of 3 days, 7 days, and 28 days.
[0033] The grout ultra-fast hardening mortar material preferably further contains a foaming agent. The foaming agent may be an organic foaming agent, an inorganic foaming agent, or a composite foaming agent of these. Examples of organic foaming agents include oily substances such as vegetable oil and mineral oil, and nitrogen gas foaming substances that foam nitrogen gas under an alkaline atmosphere such as azo compounds, nitroso compounds, and hydrazine derivatives. Examples of inorganic foaming agents include percarbonates such as sodium percarbonate, potassium percarbonate, and ammonium percarbonate, permanganates such as potassium permanganate, peroxide substances such as hydrogen peroxide, and powder substances such as aluminum powder produced by the atomization method. Other foaming agents include flaky aluminum powder surface-treated with stearic acid.
[0034] The content of the foaming agent is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.45 parts by mass, and even more preferably 0.008 to 0.4 parts by mass, relative to 100 parts by mass of cement in the ultra rapid hardening mortar material for grout.
[0035] The ultra-fast hardening mortar material for grout preferably further contains an antifoaming agent. The type of antifoaming agent is not particularly limited as long as it does not significantly adversely affect the properties of the grout, and either liquid or powder form can be used. Examples of the antifoaming agent include polyether-based antifoaming agents, polyhydric alcohol-based antifoaming agents such as esters of polyhydric alcohols and alkyl ethers, alkyl phosphate-based antifoaming agents, and silicone-based antifoaming agents.
[0036] The content of the antifoaming agent is preferably 0.002 to 0.5 parts by mass, more preferably 0.005 to 0.45 parts by mass, and even more preferably 0.01 to 0.4 parts by mass, relative to 100 parts by mass of cement in the ultra rapid hardening mortar material for grout. By having the content of the antifoaming agent within the above range, strength development is improved.
[0037] The ultra-fast hardening mortar material for grout preferably further contains one or more water reducing agents selected from the group consisting of lignin-based water reducing agents, melamine-based water reducing agents, and naphthalenesulfone-based water reducing agents, and more preferably contains three types of water reducing agents, lignin-based water reducing agents, melamine-based water reducing agents, and naphthalenesulfone-based water reducing agents. Examples of lignin-based water reducing agents include "Mighty 150" manufactured by Kao Corporation and "Plastocrete NC" manufactured by Sika Japan. Examples of melamine-based water reducing agents include "Sikament FF24" manufactured by Sika Japan and "Master Rheobuild 4000" manufactured by BASF Pozzolith. Examples of naphthalenesulfone-based water reducing agents include "Mighty 100" manufactured by Kao Corporation, "Sanyo Revellon PHL" manufactured by Sanyo Chemical Industries, and "Cellflow" manufactured by Daiichi Kogyo Seiyaku.
[0038] The content of the water reducing agent is preferably 0.05 to 2.0 parts by mass, more preferably 0.1 to 1.8 parts by mass, and even more preferably 0.15 to 1.0 parts by mass, calculated as solid content, relative to 100 parts by mass of cement in the ultra rapid hardening mortar material for grout. By having the content of the water reducing agent within the above range, the filling property is improved.
[0039] The total content of cement, calcium aluminate, gypsum, foaming agent, defoamer, and water reducing agent, excluding aggregate, in the ultra-fast hardening mortar material for grout is preferably 90% or more, and more preferably 95% or more, which makes it easier to moderate the long-term expansion rate.
[0040] The aggregate used in the present invention may be the same fine aggregate or coarse aggregate as that used in ordinary cement mortar or concrete, i.e., river sand, river gravel, mountain sand, mountain gravel, crushed stone, crushed sand, limestone aggregate, lime sand, silica sand, colored sand, artificial aggregate, blast furnace slag aggregate, sea sand, sea gravel, artificial lightweight aggregate, heavy weight aggregate, etc., or a combination of these may be used.
[0041] The content of the aggregate is preferably 40 to 250 parts by mass, more preferably 50 to 230 parts by mass, and even more preferably 60 to 200 parts by mass, relative to 100 parts by mass of cement in the ultra rapid hardening mortar material for grout. By having the content of the aggregate within the above range, it is possible to improve the strength development and easily make the long-term expansion rate appropriate.
[0042] In the present invention, the use of an alkali metal carbonate can enhance the fluidity retention effect and further improve the strength development. Examples of the alkali metal carbonate include sodium carbonate, potassium carbonate, lithium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, and lithium hydrogen carbonate, and these can also be combined. In particular, the use of lithium carbonate is preferred from the viewpoint of strength development.
[0043] The content of the alkali metal carbonate is preferably 1 to 6 parts by mass, more preferably 2 to 5 parts by mass, in terms of solid content, per 100 parts by mass of cement in the ultra-fast hardening mortar material for grout. By having the content of the alkali metal carbonate within the above range, a certain handling time can be easily ensured, and strength development can be improved.
[0044] The ultra-fast hardening mortar material for grout of the present invention can contain a siliceous fine powder from the viewpoint of enhancing strength development. Examples of the siliceous fine powder include latent hydraulic substances such as ground granulated blast furnace slag, fly ash, and pozzolanic substances such as silica fume, among which silica fume is preferred. The type of silica fume is not limited, but from the viewpoint of fluidity, it is preferable to use ZrO as an impurity. 2 It is more preferable to use silica fume containing 10% or less of silica fume or acidic silica fume. Acidic silica fume is silica fume that has an acidic pH of 5.0 or less when 1 g of silica fume is added to 100 cc of pure water and stirred.
[0045] The fineness of the silica powder is not particularly limited, but usually, the fine powder of granulated blast furnace slag and fly ash has a Blaine value of 3,000 to 9,000 cm. 2 / g, and silica fume has a BET specific surface area of 20,000 to 300,000 cm 2 / g range.
[0046] The content of the siliceous fine powder is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 3 to 12 parts by mass, relative to 100 parts by mass of cement in the ultra rapid hardening mortar material for grout. By having the content of the siliceous fine powder within the above range, it is possible to enhance the strength development.
[0047] In the present invention, a setting retarder can also be used. As the setting retarder, a hydroxycarboxylic acid or a salt thereof is preferable, the hydroxycarboxylic acid is more preferably gluconic acid, and the salt is more preferably a sodium salt.
[0048] The content of the set retarder is preferably 0.3 to 6 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of cement in the ultra rapid hardening mortar material for grout.
[0049] In the present invention, one or more of the following may be used to the extent that they do not adversely affect performance: gas foaming substances, water reducing agents, setting regulators, air-entraining agents, rust inhibitors, water repellents, antibacterial agents, colorants, antifreeze agents, fine limestone powder, finely cooled blast furnace slag powder, sewage sludge incineration ash and its molten slag, urban waste incineration ash and its molten slag, and pulp sludge incineration ash; thickeners; shrinkage reducing agents; polymers; clay minerals such as bentonite and sepiolite; and anion exchangers such as hydrotalcite.
[0050] In the ultra-fast hardening mortar material for grout of the present invention, the method of mixing each material is not particularly limited, and each material may be mixed at the time of construction, or a part or all of the materials may be mixed in advance. As a mixer, any existing device such as a tilting mixer, an omni mixer, a Henschel mixer, a V-type mixer, a Plosser mixer, and a Nauta mixer can be used.
[0051] [Hardened mortar] The hardened mortar of the present invention contains the ultra rapid hardening mortar material for grout of the present invention described above and water, and is obtained by kneading the ultra rapid hardening mortar material for grout with water. The amount of mixing water in the present invention is not particularly limited because it varies depending on the purpose and application of use and the content ratio of each material, but is preferably 10 to 70 parts by mass, more preferably 14 to 65 parts by mass, and even more preferably 16 to 60 parts by mass, relative to 100 parts by mass of cement material. By keeping the amount of mixing water within the above range, filling properties and strength development are improved.
[0052] The application method using the ultra-fast hardening mortar material for grout of the present invention includes a method of adding a certain amount of water, mixing, and pouring into the application area, a method of filling the mixed grout using a pump, a method of mixing and then blowing compressed air into the grout, and a method of applying with a plastering trowel. The mixing method includes a method of putting the material into a container such as a pail can and mixing with a hand mixer, a method of mixing with a mixer, a method of mixing by hand, and the like, and is not particularly limited. The cement composition of the present invention becomes a hardened body by mixing and filling into the application area. That is, a hardened body is obtained using the ultra-fast hardening mortar material for grout of the present invention. EXAMPLES
[0053] The present invention will be further described below based on experimental examples, but the present invention is not limited to these.
[0054] <Experimental Example 1> The materials shown below were mixed with 100 parts by mass of cement in the ratios shown in Table 1 to prepare an ultra-fast hardening mortar material for grout. The aggregate and setting regulator were mixed in amounts of 100 parts by mass and 1.5 parts by mass, respectively, with respect to a total of 100 parts by mass of cement, calcium aluminate, and gypsum. 18 parts by mass of water was added to 100 parts by mass of the prepared ultra-fast hardening mortar material for grout, and the mixture was kneaded to prepare grout, and various measurements were performed. Furthermore, a hardened mortar was manufactured using the prepared grout, and its strength was measured.
[0055] (Materials used) Cement: A trial cement made to simulate ordinary Portland cement (a variety of commercially available pure chemicals were used to adjust the raw materials and chemical components used in the cement factory), with a Blaine value of 3,450 cm 2 / g. Calcium aluminate: Vitrification rate 97%, CaO / Al 2 O 3 Molar ratio 1.7, loss on ignition 1.0%, main component CaO·Al 2 O 3 and 12CaO 7Al 2 O 3 , Blaine value 5,000 cm2 / g. Gypsum: anhydrite, reagent. Aggregate: Fine aggregate, lime sand 0.6mm or less 50% and 0.6~1.2mm 50% were used. Density 2.52g / cm 3 . Defoamer: A mixture of special non-ionic surfactants and silica, a commercially available product. Foaming agent: Aluminum powder (surface treated), commercially available product. Water reducer 1: Naphthalenesulfonic acid-based water reducer, commercially available product. Set regulator: Sodium gluconate, reagent. Water: Tap water.
[0056] (Measurement items) Expansion rate: The expansion rate of the mixed grout was measured at 3, 7, 28, and 60 days using a method compliant with the method specified in JIS A 6202:2017 "Expansive additives for concrete" Appendix A "Test method for expansive additives using mortar". The results are shown in Table 1. Air content: The grout after mixing was measured in accordance with the method specified in JIS A 1116:2019 "Test method for unit volume mass of fresh concrete and test method by mass of air content (mass method)". The results are shown in Table 1. Flow value: The flow value of the mixed grout was measured without performing the 15 drop motions according to the method specified in JIS R 5201:2015 "Physical Testing Methods for Cement". The results are shown in Table 1. J 14 Funnel flow time: The mixed grout was measured according to the method specified in the Japan Society of Civil Engineers standard JSCE-F 541-2013 "Test method for fluidity of filling mortar." The results are shown in Table 1. Expansion and shrinkage rate: The expansion and shrinkage rate of the mixed grout was measured according to the method specified in JSCE-F 542-2013 "Test method for bleeding rate and expansion rate of filling mortar". The results are shown in Table 1. Compressive strength: The compressive strength of the hardened mortar was measured at 3 hours and 28 days according to the method specified in JSCE-G 505-2018 "Method of compressive strength test for mortar or cement paste using cylindrical specimens." The results are shown in Table 1.
[0057] [Table 1]
[0058] <Experimental Example 2> A grout was prepared and a hardened mortar was produced in the same manner as in Experimental Example 1, except that the water-reducing agent shown below was also used.
[0059] (Materials used) Water reducer 2: Lignin-based water reducer, commercially available product. Water reducer 3: Melamine-based water reducer, commercially available product. [Table 2] [Industrial Applicability]
[0060] The ultra-fast hardening mortar material for grout of the present invention contains cement, calcium aluminate, and gypsum, and has an initial expansion rate within a predetermined range, thereby making it possible to make the long-term expansion rate appropriate. Therefore, the material can be widely used in the fields of civil engineering and architecture, such as for fixing reinforcing steel bars to concrete structures used in water supply and sewage systems, agriculture and water supply, railways, electricity, roads, and architecture.
Claims
1. Contains cement, calcium aluminate, and gypsum; An ultra-fast hardening mortar material for grout, which has expansion rates of 0.005-0.5%, 0.01-0.75%, and 0.015-1.0% at ages of 3 days, 7 days, and 28 days, respectively.
2. The ultra-fast hardening mortar material for grout according to claim 1, wherein the air content after mixing is 0 to 5%.
3. The ultra-fast hardening mortar material for grout according to claim 1 or 2, wherein the flow value after mixing is 170 to 320 mm.
4. J after mixing 14 The ultra-fast hardening mortar material for grout according to claim 1 or 2, wherein the funnel flow time is 6 to 10 seconds.
5. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising a foaming agent.
6. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising an antifoaming agent.
7. The ultra-fast hardening mortar material for grout according to claim 1 or 2, further comprising one or more water reducing agents selected from the group consisting of lignin-based water reducing agents, melamine-based water reducing agents, and naphthalene sulfone-based water reducing agents.
8. A hardened mortar product obtained by using the ultra-fast hardening mortar material for grout according to claim 1 or 2.
Citation Information
Patent Citations
Nonshrinkage grout
JP1977150434A
Mortar material
JP1984213655A
Extremely quick-setting nonshrink grout material
JP1989230455A
Powdery or granular cement-based grout composition
JP2000247716A
Supper quick-hardening high-fluidity cement composition and mortar or concrete using the same