Laminate, structure, and semiconductor device

By improving the crystallinity of the gallium nitride layer within a laminate structure, a mirror-finished gallium nitride film is achieved, addressing the challenge of surface finish in CVD deposition for semiconductor devices.

JP2024145344APending Publication Date: 2024-10-15TOSOH CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023057653
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing laminates using gallium nitride thin films are not suitable for forming a mirror-finished surface when a gallium nitride film is deposited on a gallium nitride-based film by the CVD method, which is necessary for alignment and microfabrication in semiconductor devices.

Method used

A laminate structure comprising a silicon substrate, an aluminum nitride layer, and a gallium nitride layer is formed, where the crystallinity of the gallium nitride layer is improved by controlling the degree of tilt and twist of the crystal axis, allowing the CVD gallium nitride film to achieve a mirror-finished surface.

Benefits of technology

The laminate structure enables the formation of a gallium nitride film with a mirror surface, facilitating easy alignment and microfabrication in semiconductor devices, enhancing manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145344000001_ABST
    Figure 2024145344000001_ABST
Patent Text Reader

Abstract

To provide at least one of the laminate, structure, and semiconductor device that can make the surface thereof become a mirror surface when a gallium nitride film is formed on a gallium nitride layer with a CVD method.SOLUTION: A laminate includes a silicon substrate, an aluminum nitride layer, and a gallium nitride layer in this order. A half-value width at diffraction peak in an X-ray rocking curve measurement on a (10-12) surface of the gallium nitride layer is less than 14°.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate, a structure, and a semiconductor device. [Background technology]

[0002] Gallium nitride thin films have high energy efficiency and are being used as energy-saving devices in LEDs, AC adapters, etc. Gallium nitride thin films are also expected to be applied to HEMT (High Electron Mobility Transistor) devices as next-generation power devices. A known example of such a laminate using a gallium nitride thin film is described in Patent Document 1. Patent Document 1 proposes providing a crack-free laminate film that includes a buffer layer and a gallium nitride film in this order, and has a compressive stress of -2.0 GPa or more and 5.0 GPa or less throughout the laminate film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2021 / 200836 Summary of the Invention [Problem to be solved by the invention]

[0004] By the way, when a semiconductor device is manufactured using the above-mentioned laminate, a gallium nitride film (hereinafter also referred to as "CVD gallium nitride film") may be formed on the gallium nitride film of the laminate by CVD during the process. In this case, marking may be performed on the surface of the CVD gallium nitride film for the purpose of aligning the mask used in photolithography, and in this case, it is desirable that the surface of the CVD gallium nitride film is a mirror surface to facilitate marking. In addition, CVD gallium nitride films may require microfabrication to manufacture devices, and for this reason it is desirable for the surface of the CVD gallium nitride film to be uneven enough to prevent diffuse reflection of light, i.e. a mirror surface.

[0005] However, the laminated film described in Patent Document 1 above still has room for improvement in terms of making the surface mirror-finished when a gallium nitride film is formed on a gallium nitride-based film by a CVD method.

[0006] An object of the present disclosure is to provide at least one of a laminate, a structure and a semiconductor device that can provide a mirror-finished surface when a gallium nitride film is formed on a gallium nitride layer by a CVD method. [Means for solving the problem]

[0007] The inventors of the present disclosure have studied how to make the surface of a CVD gallium nitride film mirror-finished when a gallium nitride film (CVD gallium nitride film) is formed on a gallium nitride layer by a CVD method in a laminate having a silicon substrate, an aluminum nitride layer, and a gallium nitride layer in this order. As a result, the inventors thought that if the crystallinity of the gallium nitride layer that becomes the underlayer of the CVD gallium nitride film in the laminate is increased, the crystallinity of the CVD gallium nitride film can be improved and its surface can be made mirror-finished. The crystallinity of the gallium nitride layer that becomes the underlayer can be evaluated by the degree of tilt of the crystal axis growth direction and the degree of twist of the crystal around the crystal growth direction. When the (000-1) plane of the crystal of the gallium nitride layer is used as the growth plane, the degree of tilt can be evaluated by measuring the half-width of the diffraction peak of the (0002) plane, for example, by X-ray rocking curve measurement (hereinafter also referred to as "XRC measurement"), and the degree of twist can be evaluated by measuring the half-width of the diffraction peak of the (10-12) plane by XRC measurement. In both the tilt and twist cases, the narrower the half-width of the diffraction peak, the higher the crystallinity. Therefore, first, the degree of tilt of the gallium nitride layer of the laminate was evaluated by measuring the half-width of the diffraction peak of the (0002) plane by XRC measurement for the cases where the surface of the CVD gallium nitride film was mirror-finished and the case where it was not mirror-finished. However, in that case, no significant difference was observed in the half-width value of the diffraction peak whether the surface of the CVD gallium nitride film was mirror-finished or not mirror-finished. In contrast, when the degree of twist of the gallium nitride layer of the laminate was evaluated by measuring the half-width value of the diffraction peak of the (10-12) plane by XRC measurement for the cases where the surface of the CVD gallium nitride film was mirror-finished and the case where it was not mirror-finished, it was found that a significant difference was observed in the value of the half-width value. Thus, the inventors of the present disclosure have arrived at the present disclosure.

[0008] The present invention is as described in the claims, and the gist of the present disclosure is as follows. (1) A laminate comprising a silicon substrate, an aluminum nitride layer, and a gallium nitride layer in this order, wherein the half-width of a diffraction peak of the (10-12) plane of the gallium nitride layer in an X-ray rocking curve measurement is less than 14°. (2) The laminate according to (1), wherein the gallium nitride layer is a layer made of a sputtered film formed by a sputtering method. (3) The laminate according to (1) or (2), wherein the crystal plane of the surface of the silicon substrate is a (111) plane. (4) A structure comprising the laminate according to any one of (1) to (3) above, and a gallium nitride film formed by a CVD method on the gallium nitride layer of the laminate. (5) A semiconductor device comprising the structure described in (4). Effect of the Invention

[0009] According to the present disclosure, there is provided at least one of a laminate, a structure and a semiconductor device that can provide a mirror-finished surface when a gallium nitride film is formed on a gallium nitride layer by a CVD method. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing one embodiment of a laminate of the present disclosure. [Diagram 2] FIG. 1 is a cross-sectional view illustrating one embodiment of a structure of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The embodiments of the present disclosure will now be described in detail.

[0012] <Laminate> First, an embodiment of the laminate of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing one embodiment of the laminate of the present disclosure. 1 includes, in this order, a silicon substrate 1, an aluminum nitride layer 2, and a gallium nitride layer 3. In the laminate 10, the half-width W1 of a diffraction peak in an X-ray rocking curve measurement (XRC measurement) of the (10-12) plane of the gallium nitride layer 3 is less than 14°.

[0013] According to this laminate 10, when a gallium nitride layer is formed on the gallium nitride layer 3 by a CVD method, the surface can be made mirror-finished. The reason why such an effect is obtained is considered to be as follows. The half-width W1 of the diffraction peak in the XRC measurement of the (10-12) plane of the gallium nitride layer 3 indicates the degree of twist of the crystal around the growth direction of the gallium nitride crystal contained in the gallium nitride layer 3. Therefore, by making the half-width W1 of the diffraction peak less than 14°, the twist of the gallium nitride crystal constituting the gallium nitride layer 3 is suppressed, and when a gallium nitride film is formed on the gallium nitride layer 3 by the CVD method, the lateral growth of the gallium nitride crystal is promoted, and a gallium nitride film with a flat surface is formed. As a result, it is considered that the surface of the obtained gallium nitride film is a mirror surface. In this specification, the surface of the gallium nitride film is a mirror surface means that the surface roughness of the surface of the gallium nitride film is 0.5 μm or less, and preferably 0.2 μm or less.

[0014] The silicon substrate 1, the aluminum nitride layer 2 and the gallium nitride layer 3 will now be described in detail.

[0015] (Silicon substrate) The silicon substrate 1 includes cubic silicon crystals. The crystal plane of the surface of the silicon substrate 1 is not particularly limited, and examples of such crystal planes include a (111) plane, a (100) plane, and a (110) plane. Among them, the crystal plane of the surface of the silicon substrate 1 is preferably a (111) plane. In this case, in the crystals contained in the aluminum nitride layer 2 and the gallium nitride layer 3, twisting of the crystal axes along their thickness direction is suppressed, and when a gallium nitride film is formed on the gallium nitride layer 3 by a CVD method, the flatness of the surface of the gallium nitride film is further improved. As a result, the surface of the CVD gallium nitride film is easily made mirror-finished.

[0016] The thickness of the silicon substrate 1 is not particularly limited, but is preferably 0.3 mm or more, more preferably 0.5 mm or more, and particularly preferably 0.7 mm or more. The thickness of the silicon substrate 1 can be, for example, 2.0 mm or less, 1.5 mm or less, or 1.0 mm or less.

[0017] (Aluminum nitride layer) The aluminum nitride layer 2 is a layer that relieves stress from the silicon substrate 1 to the gallium nitride layer 3, and can also function as a layer that suppresses reaction between the silicon substrate 1 and the gallium nitride layer 3. The aluminum nitride layer 2 contains hexagonal aluminum nitride crystals.

[0018] The crystal plane of the surface of the aluminum nitride layer 2 is not particularly limited, and examples of the crystal plane of the surface of the aluminum nitride layer 2 include the (0001) plane, the (10-10) plane, and the (10-12) plane. Among them, the crystal plane of the surface of the aluminum nitride layer 2 is preferably the (0001) plane. In this case, the twisting of the crystal axis along the thickness direction of the crystal contained in the gallium nitride layer 3 is suppressed, and when a gallium nitride film is formed on the gallium nitride layer 3 by a CVD method, the flatness of the surface of the gallium nitride film is further improved. As a result, it is easier to make the surface of the CVD gallium nitride film a mirror surface.

[0019] The aluminum nitride layer 2 may be a layer formed by a sputtering method or another method, but is preferably a layer formed by a sputtering method. In this case, compared with the case where the aluminum nitride layer 2 is formed by a CVD method such as MOCVD, the stress from the silicon substrate 1 is more easily alleviated, and when a CVD gallium nitride film is formed on the gallium nitride layer 3, cracks are less likely to occur in the CVD gallium nitride film.

[0020] The thickness of the aluminum nitride layer 2 is not particularly limited, but is preferably 30 nm or more, more preferably 50 nm or more, and particularly preferably 100 nm or more. By making the thickness of the aluminum nitride layer 2 30 nm or more, it is possible to obtain a thin film with good crystallinity. The thickness of the aluminum nitride layer 2 may be 500 nm or less, 300 nm or less, or 200 nm or less.

[0021] (Gallium nitride layer) In the gallium nitride layer 3, the half-width W1 of the diffraction peak in X-ray rocking curve measurement of the (10-12) plane is not particularly limited as long as it is less than 14°, but is preferably 10° or less, more preferably 5° or less, and particularly preferably 3° or less. The half width of the diffraction peak may be 0.00001° or more, or 0.0001° or more.

[0022] The gallium nitride layer 3 may be a layer made of a sputtering film formed by a sputtering method or a layer made by another method, but is preferably a layer made of a sputtering film formed by a sputtering method. In this case, compared with the case where the gallium nitride layer 3 is formed by a CVD method such as an MOCVD method, the stress from the silicon substrate 1 is more easily alleviated, and when a CVD gallium nitride film is formed on the gallium nitride layer 3, cracks are less likely to occur in the CVD gallium nitride film.

[0023] The thickness of the gallium nitride layer 3 is not particularly limited, but is preferably 10 nm or more, more preferably 50 nm or more, and particularly preferably 100 nm or more. By making the thickness of the gallium nitride layer 3 10 nm or more, it is possible to obtain a thin film with good crystallinity. The thickness of the gallium nitride layer 3 may be 600 nm or less, 500 nm or less, or 400 nm or less.

[0024] <Method of manufacturing laminate> The laminate of this embodiment can be manufactured by any method as long as it satisfies the above-mentioned characteristics. For example, the laminate 10 of this embodiment can be obtained by a manufacturing method including a step of forming an aluminum nitride layer 2 by introducing a nitrogen-containing gas while sputtering an aluminum metal sputtering target onto a silicon substrate 1, and a step of forming a gallium nitride layer 3 on the aluminum nitride layer 2 by sputtering a gallium nitride sputtering target.

[0025] (Metal Aluminum Sputtering Target) The metal aluminum sputtering target includes aluminum. The aluminum is a bulk whose main component is aluminum, and furthermore, the main component is at least one of single crystal and polycrystal of aluminum, and furthermore, the main component is polycrystal of aluminum. The aluminum in the metal aluminum sputtering target may contain at least one of indium and gallium as a dopant, or silicon or the like to exhibit electrical conductivity or semiconductor properties. In this specification, the term "main component" refers to a component whose content is 50 mass% or more.

[0026] The aluminum metal sputtering target may further include a backing plate bonded to the bulk of the target.

[0027] The target may further include a bonding material between the bulk and the backing plate. Various materials can be used as the bonding material, but indium is preferred from the viewpoint of suppressing thermal diffusion and thermal expansion during sputtering.

[0028] (Gallium nitride sputtering target) The gallium nitride sputtering target includes gallium nitride. The gallium nitride is a bulk whose main component is gallium nitride, and may be at least one of a single crystal and a polycrystal whose main component is gallium nitride, or a polycrystal whose main component is gallium nitride. The gallium nitride in the gallium nitride sputtering target may contain indium or aluminum as a dopant, or silicon to exhibit electrical conductivity or semiconductor properties.

[0029] The gallium nitride sputtering target may further comprise a backing plate bonded to the bulk of the target.

[0030] The target may further include a bonding material between the bulk and the backing plate. Various materials can be used as the bonding material, but indium is preferred from the viewpoint of suppressing thermal diffusion and thermal expansion during sputtering.

[0031] The sputtering method may be one or more selected from the group consisting of DC sputtering, RF sputtering, AC sputtering, DC magnetron sputtering, RF magnetron sputtering, ECR sputtering, pulsed laser deposition deposition and ion beam sputtering. Among these, at least one of DC magnetron sputtering and RF magnetron sputtering is preferred because it allows for uniform and high-speed film formation over a large area.

[0032] The gas pressure during sputtering is not particularly limited, but may be, for example, 5 Pa or less, preferably 3 Pa or less, more preferably 2 Pa or less, and particularly preferably 1 Pa or less. The gas pressure during sputtering may be, for example, 0 Pa or more, or 0.1 Pa or more. The lower the gas pressure during sputtering, the more easily the particles (sputtered particles) emitted from the target reach the silicon substrate 1 or the aluminum nitride layer 2 while still having high energy, and the more easily the aluminum nitride layer 2 or the gallium nitride layer 3 is epitaxially rearranged. This makes it easier to obtain the hexagonal aluminum nitride layer 2 or the gallium nitride layer 3.

[0033] In order to improve the crystallinity of the entire laminate, the sputtering target used preferably has an oxygen content of less than 3 at%, more preferably 1 at% or less, or 0.1 at% or less. The oxygen content of the sputtering target is, for example, 0 at% or more, or 0.0000001 at% or more. The sputtering target preferably has a high purity, and the content of metal impurities is preferably less than 0.1 mass%, and more preferably less than 0.01 mass%, for example, 0 at% or more, or 0.0000001 at% or more. The metal impurities herein do not include intentionally added indium, aluminum, etc.

[0034] The area of ​​the target surface of the sputtering target is preferably 18 cm 2 More preferably, it is 100 cm 2 That is all. The larger the area of ​​the target surface, the more stable the discharge becomes, making it possible to perform sputtering at a lower gas pressure and lower power density. Furthermore, the uniformity of the thickness and quality of the aluminum nitride layer 2 or gallium nitride layer 3 also improves.

[0035] (Cleaning process) It is preferable to clean the silicon substrate 1 (substrate cleaning) before film formation. By cleaning the substrate, contaminants on the surface of the silicon substrate 1 are removed, and the aluminum nitride layer 2 and the gallium nitride layer 3, which are homogeneous films, can be obtained over the entire surface of the silicon substrate 1. For example, RCA cleaning can be used for the substrate cleaning. It is preferable to perform RCA cleaning using any of the following: SPM cleaning (cleaning solution: mixed solution of sulfuric acid and hydrogen peroxide (sulfuric acid: hydrogen peroxide = 4:1, 80°C), with a rinse process with pure water after cleaning), SC1 cleaning (cleaning solution: mixed solution of ammonia water, hydrogen peroxide and pure water (ammonia water: hydrogen peroxide: pure water = 1:1:5, 50°C), with a rinse process with pure water after cleaning), SC2 cleaning (cleaning solution: mixed solution of hydrochloric acid, hydrogen peroxide and pure water (hydrochloric acid: hydrogen peroxide: pure water = 1:1:5, 50°C), with a rinse process with pure water after cleaning), and DHF cleaning (cleaning solution: 0.5% hydrofluoric acid (20°C), with a rinse process with pure water after cleaning).

[0036] (Pre-treatment for film formation) The degree of vacuum in the deposition apparatus before deposition is not particularly limited, but is preferably 3×10 -5 Pa or less, and 1×10 -5It is more preferable to set the vacuum level to 3×10 Pa or less. -5 By setting the pressure at or below Pa, residual gas is less likely to be mixed in as an impurity during film formation, improving the crystallinity of the aluminum nitride layer 2 or the gallium nitride layer 3. In the film formation apparatus, it is preferable to perform a baking process on the film formation apparatus before evacuating the apparatus in order to remove residual gas.

[0037] It is preferable to hold the silicon substrate 1 at the film formation temperature for a certain period of time before starting the formation of the gallium nitride layer 3. This makes the temperature of the silicon substrate 1 uniform before film formation, improving the crystallinity of the formed gallium nitride layer 3. For example, the holding time is preferably 1 minute or more, more preferably 5 minutes or more, and even more preferably 10 minutes or more. On the other hand, from the viewpoint of improving productivity, the long holding time is preferably 1 hour or less, and more preferably 30 minutes or less.

[0038] (film formation) The aluminum nitride layer 2 is preferably formed while the silicon substrate 1 is heated. This promotes migration of particles deposited on the silicon substrate 1, and allows the formation of a deposited film in a stable crystalline state. The heating temperature (film formation temperature) of the silicon substrate 1 is preferably 100°C or higher and 1000°C or lower, and more preferably 200°C or higher and 800°C or lower. The deposition of the gallium nitride layer 3 is preferably carried out while the silicon substrate 1 is heated. This promotes migration of particles deposited on the silicon substrate 1, and allows the deposition of a film in a stable crystalline state to be formed. The heating temperature (deposition temperature) of the silicon substrate 1 is preferably 100°C or higher and 1000°C or lower, and more preferably 200°C or higher and 800°C or lower.

[0039] The gas used for film formation preferably contains, for example, nitrogen as a main component. The gas used for film formation preferably further contains argon, which is commonly used. In this case, the partial pressure ratio of nitrogen / (nitrogen + argon) is preferably 0.7 or more and 0.9 or less.

[0040] The power density during discharge is 1W / cm 2 More than 20W / cm 2 It is preferable that the power consumption is less than 1.5 W / cm 2 More than 10W / cm 2 More preferably, it is 2.5 W / cm or less. 2 More than 5W / cm 2 It is more preferable that the power density is 20 W / cm or less. The power density is calculated by dividing the power applied during discharge by the area of ​​the target surface of the sputtering target. 2 If the power density is less than 1 W / cm, even if the sputtering target mainly made of gallium nitride is generally low density, the coarse polycrystalline particles are unlikely to peel off from the sputtering target due to the power applied to the target. 2 At the above level, the plasma is stable, which facilitates discharge, and the film formation speed is increased, improving film productivity. Furthermore, the energy during sputtering is high, improving the adhesion during film formation.

[0041] The deposition time may be adjusted as appropriate depending on the thickness of the aluminum nitride layer 2 or the gallium nitride layer 3. The thickness of the aluminum nitride layer 2 or the gallium nitride layer 3 can be increased as the deposition time is increased.

[0042] <Structure> Next, one embodiment of the structure of the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing one embodiment of the structure of the present disclosure. 2 includes a stacked body 10 and a gallium nitride film 4. The gallium nitride film 4 is provided on the gallium nitride layer 3 of the stacked body 10. The gallium nitride film 4 is a film formed by a CVD method.

[0043] According to this structure 20, the surface of the gallium nitride film 4 is a mirror surface, so that marking can be easily performed on the surface of the gallium nitride film 4. Therefore, the alignment of the mask used in photolithography can be easily performed, and a device including the structure 20 can be efficiently manufactured. In addition, since the surface of the gallium nitride film 4 can have a mirror surface, that is, a surface having projections and recesses to such an extent that light is not diffusely reflected, the microfabrication required for manufacturing the device can be easily performed.

[0044] The gallium nitride film 4 may be any film formed by a CVD method. An example of a CVD method is metal-organic chemical vapor deposition (MOCVD). The MOCVD method is a method in which a carrier gas containing vapor of a raw material is transported to the surface of the gallium nitride layer 3, and the raw material is decomposed by reaction with the heated gallium nitride layer 3, thereby growing a crystal.

[0045] <Semiconductor devices> The semiconductor device of the present disclosure may be any device including a structure 20, and may be applied to, for example, light emitting elements such as LEDs, laser diodes, and power devices such as transistors in HEMT devices. EXAMPLES

[0046] The contents of the present disclosure will be described more specifically below using examples, but the present disclosure is not limited to the following examples.

[0047] Example 1 A disk-shaped silicon substrate with a diameter of 2 inches and a thickness of 725 μm was prepared. The silicon substrate used had a (111) crystal plane on its surface.

[0048] Next, a magnetron sputtering device (product name "MPS-6000", manufactured by ULVAC) was used to form a film on the surface of the silicon substrate, forming an aluminum nitride layer with a thickness of 100 nm. At this time, a metal aluminum sputtering target (purity 99.9999% by mass, manufactured by Kojundo Chemical Laboratory) having the diameter of the sputtering surface shown in Table 1 was prepared as the sputtering target. Then, after RCA cleaning of the silicon substrate, both the silicon substrate and the target were placed in the film formation chamber of the sputtering device. The distance between the target and the silicon substrate was 150 mm. Before the film formation, the chamber was baked to achieve a higher ultimate vacuum. Next, the vacuum level in the deposition chamber (the ultimate vacuum level before deposition) was 1.0×10 -5 The vacuum was drawn until the pressure was below 1 Pa. Next, with the shutter on the silicon substrate side closed, plasma was ignited using nitrogen gas, and film formation was carried out under the film formation conditions shown in Table 1. The distance between the shutter and the silicon substrate was 5 mm. The shutter used was an accessory shutter for the magnetron sputtering device, and had a diameter of 3 inches.

[0049] Next, a film was formed on the surface of the aluminum nitride layer using the magnetron sputtering device to form a gallium nitride layer with a thickness of 100 nm. At this time, a gallium nitride sputtering target (purity 99.999 mass%) having the diameter of the sputtering surface shown in Table 2 was prepared as the sputtering target. This target was then placed in the film formation chamber of the sputtering device. The distance between the target and the silicon substrate was 110 mm. Before the film formation, the chamber was baked to achieve a higher ultimate vacuum. Next, the vacuum level in the deposition chamber (the ultimate vacuum level before deposition) was 1.0×10 -5 The vacuum was drawn until the pressure was below 1 Pa. Next, with the shutter on the silicon substrate side closed, plasma was ignited using nitrogen gas, and film formation was performed under the film formation conditions shown in Table 2. During film formation, the substrate temperature was raised to the temperature shown in Table 2, and then maintained for 10 minutes before film formation. The distance between the shutter and the silicon substrate was 5 mm. The shutter used was an accessory shutter for the magnetron sputtering device, and had a diameter of 3 inches.

[0050] In this way, a stack (silicon substrate / aluminum nitride layer / gallium nitride layer) having a thickness of 0.73 mm was obtained.

[0051] Then, the gallium nitride layer of the obtained laminate was subjected to X-ray rocking curve measurement (XRC measurement) of the (10-12) plane. The XRC measurement was performed using an XRD device (D8-DISCOVER manufactured by Bruker) with a CuKα radiation (λ=0.15418 nm) as the radiation source, using the HIGHRESOLUTION mode, and performing a φ scan under the following measurement conditions. The above measurement was also performed after converting CuKα2 into parallel monochromatic light using a Ge(220) monochromator. (Measurement conditions) Tube voltage: 40kV Tube current: 50mA Measurement interval: 0.02° Measurement time: 1800 seconds Measurement range: φ=0°~360° The XRC measurement was carried out in this manner, and the profile was smoothed using XRD analysis software (manufactured by Bruker, "LEPTOS" Ver. 4.03), after which the half-value width W1 of the diffraction peak was determined. The results are shown in Table 3.

[0052] [Table 1] [Table 2] [Table 3]

[0053] (Example 2 and Comparative Example 1) A laminate was obtained in the same manner as in Example 1, except that the half-width W1 of the diffraction peak was set to the value shown in Table 3 by using the targets and film-forming conditions shown in Tables 1 and 2. In Table 2, "RT" is an abbreviation for room temperature.

[0054] <Evaluation of the laminate> For the laminates of Examples 1 and 2 and Comparative Example 1 obtained as described above, a gallium nitride layer (CVDGaN film) was formed on the gallium nitride layer by CVD, and the surface of the obtained CVDGaN film was visually observed. The results are shown in Table 3.

[0055] From the results shown in Table 3, the entire surface of the CVDGaN film was a mirror surface in the laminates of Examples 1 and 2. In contrast, in the laminate of Comparative Example 1, the entire surface of the CVDGaN film was a non-mirror surface, and no mirror surface was observed on the surface. From this, it was confirmed that with the laminate of the present disclosure, in which the half-width of the diffraction peak in X-ray rocking curve measurement of the (10-12) plane of the gallium nitride layer is less than 14°, when a gallium nitride film is formed on the gallium nitride layer by a CVD method, the surface can be made mirror-finished. [Explanation of symbols]

[0056] 1...silicon substrate, 2...aluminum nitride layer, 3...gallium nitride layer, 4...gallium nitride film, 10...laminated body, 20...structure.

Claims

1. A silicon substrate, an aluminum nitride layer, and a gallium nitride layer in this order, The laminate has a half-width of a diffraction peak in an X-ray rocking curve measurement of a (10-12) plane of the gallium nitride layer of less than 14°.

2. The laminate according to claim 1 , wherein the gallium nitride layer is a layer made of a sputtered film formed by a sputtering method.

3. 2. The laminate according to claim 1, wherein the crystal plane of the surface of the silicon substrate is a (111) plane.

4. The laminate according to any one of claims 1 to 3, A structure comprising a gallium nitride film formed by a CVD method on the gallium nitride layer of the laminate.

5. A semiconductor device comprising the structure of claim 4.

Citation Information

Patent Citations

  • Manufacturing methods of group iii nitride semiconductor and group iii nitride semiconductor light emitting element, group iii nitride semiconductor light emitting element and lamp

    JP2009135197A

  • Nitride semiconductor epitaxial substrate and nitride semiconductor device

    JP2013014450A

  • Vapor growth device and film forming method

    JP2013222884A

  • Method and apparatus for forming gallium nitride film

    JP2013227198A

  • Group IIIA nitride growth systems and methods

    JP2019524982A