Sensor element and gas sensor

By using a zirconia outer lead portion with a TM ratio less than 2 and a thin dense layer, the sensor element mitigates cracking and water ingress, enhancing reliability.

JP2024145698APending Publication Date: 2024-10-15NGK INSULATORS LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023058161
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Sensor elements experience cracks due to the presence of a dense layer covering a portion of the outer lead portion, which is exacerbated by the transformation of zirconia from the T phase to the M phase during use, leading to stress and potential failure.

Method used

The sensor element incorporates a first region of the outer lead portion made of zirconia with a TM ratio less than 2 and covered by a dense layer with a thickness of less than 11 μm, along with a porous layer to prevent water ingress and reduce stress.

Benefits of technology

This configuration effectively suppresses the occurrence of cracks in the sensor element by minimizing stress and preventing water corrosion, ensuring reliable operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145698000001_ABST
    Figure 2024145698000001_ABST
Patent Text Reader

Abstract

To suppress a crack of a sensor element.SOLUTION: A sensor element 20 includes an element main body 60 including a front end and a rear end, which are both ends along a longitudinal direction, and a first surface 60a along the longitudinal direction, an external electrode 64 disposed on the front end side of the first surface 60a, an upper connector electrode 71 disposed on the rear end side of the first surface 60a, an external lead wire 75 disposed on the first surface 60a and electrically connecting the external electrode 64 and an upper connector electrode 71 (71b), and a first dense layer 92 disposed on the front end side of the element main body 60 relative to the upper connector electrode 71 on the first surface 60a. The external lead wire 75 includes a first region 77 covered with the first dense layer 92. The first region 77 contains zirconia. A TM ratio, which is a ratio Ht / Hm of a peak height Hm of an M phase to a peak height Ht of a T phase of zirconia in the Raman spectrum measured using Raman spectroscopy, is less than 2. The first dense layer 92 has a thickness of less than 11 μm.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sensor element and a gas sensor. [Background technology]

[0002] Conventionally, a sensor element for detecting the concentration of a specific gas such as NOx in a measurement gas such as an automobile exhaust gas is known (see, for example, Patent Document 1). The sensor element of Patent Document 1 includes an element body, an outer electrode, a connector electrode, an outer lead portion, a porous layer, and a dense layer. The front end side of the element body is exposed to the measurement gas. The outer electrode is disposed on the front end side of the side surface of the element body. The connector electrode is disposed on the rear end side of the side surface of the element body and is electrically connected to the contact portion of the connector. The outer lead portion is disposed on the side surface of the element body and is electrically connected to the outer electrode and the connector electrode. The porous layer is disposed on the side surface of the element body and covers at least a part of the outer lead portion to protect it. The dense layer is disposed on the side surface of the element body so as to divide the porous layer along the longitudinal direction of the element body or to be located on the rear end side of the porous layer, and is located on the front end side of the connector electrode. When moisture in the measured gas moves through the porous layer toward the rear end of the element body due to capillary action, capillary action is less likely to occur in the dense layer, and the presence of the dense layer prevents water from reaching the connector electrode. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 155865 Summary of the Invention [Problem to be solved by the invention]

[0004] In a sensor element in which at least a portion of the outer lead portion is covered with a dense layer as in Patent Document 1, cracks may occur in the sensor element.

[0005] The present invention has been made to solve such problems, and has as its main object to suppress cracks in the sensor element. [Means for solving the problem]

[0006] In order to achieve the above-mentioned main object, the present invention adopts the following means.

[0007] [1] The sensor element of the present invention comprises: A sensor element for detecting a specific gas concentration in a measurement gas, comprising: an element body having a front end and a rear end which are both ends along a longitudinal direction and a side surface which is a surface along the longitudinal direction, the front end side being exposed to the measurement gas; an outer electrode disposed on the front end side of the side surface; a connector electrode disposed on the rear end side of the side surface for electrical connection to an outside; an outer lead portion disposed on the side surface and electrically connecting the outer electrode and the connector electrode; a dense layer covering a portion of the side surface and disposed closer to the front end than the connector electrode; Equipped with the outer lead portion has a first region at least a portion of which is covered with the dense layer, The first region contains zirconia, and a TM ratio, which is a ratio Ht / Hm of a peak height Ht of a T phase of zirconia to a peak height Hm of an M phase of zirconia in a Raman spectrum measured using Raman spectroscopy, is less than 2; The dense layer has a thickness of less than 11 μm. It is something.

[0008] In this sensor element, the outer lead portion has a first region at least partially covered with a dense layer. The first region contains zirconia, and the TM ratio of the zirconia is less than 2. The dense layer has a thickness of less than 11 μm. This makes it possible to suppress the occurrence of cracks in the sensor element. The inventors have confirmed this through experiments and analysis. Note that the value of the TM ratio of zirconia in the first region is the value when the sensor element is in an unused state.

[0009] [2] In the above-described sensor element (the sensor element described in [1] above), the first region may have a TM ratio of not more than 1. This makes it possible to more reliably obtain the effect of suppressing the occurrence of cracks in the sensor element.

[0010] [3] In the sensor element described above (the sensor element according to the above [1] or [2]), the first region may have a TM ratio of 0.1 or less. This can further suppress the occurrence of cracks in the sensor element.

[0011] [4] In the sensor element described above (the sensor element according to any one of [1] to [3] above), the first region may have a TM ratio of 0.01 or more.

[0012] [5] In the above-mentioned sensor element (the sensor element according to any one of [1] to [4] above), the dense layer may have a thickness of 10 μm or less. This makes it possible to more reliably obtain the effect of suppressing the occurrence of cracks in the sensor element.

[0013] [6] In the above-mentioned sensor element (the sensor element described in any one of [1] to [5] above), the outer lead portion may have the first region and the second region, and the dense layer may cover only the first region of the first region and the second region from the front end side to the rear end side of the dense layer. In this way, when the second region is present, the effect of suppressing the occurrence of cracks in the sensor element by the first region can be more reliably obtained. In addition, since the effect of suppressing the occurrence of cracks in the sensor element can be obtained even if the TM ratio of the second region is not less than 2, the degree of freedom in designing the second region is increased.

[0014] [7] A gas sensor of the present invention includes the sensor element according to any one of the above items [1] to [6]. Therefore, the gas sensor can obtain the same effects as those of the above-mentioned sensor element, for example, the effect of suppressing the occurrence of cracks in the sensor element. [Brief description of the drawings]

[0015] [Figure 1] FIG. 4 is a vertical cross-sectional view showing a state in which the gas sensor 10 is attached to a pipe 58. [Diagram 2] FIG. [Diagram 3] FIG. [Figure 4] FIG. [Diagram 5] 4 is a vertical cross-sectional view showing the periphery of a first region 77 covered with a first dense layer 92. FIG. [Figure 6] FIG. 2 is an explanatory diagram illustrating a schematic diagram of a process for calculating a peak height Ht and a peak height Hm from a Raman spectrum SP. [Figure 7] 13 is a cross-sectional view showing the periphery of a first dense layer 92 and a first region 77 in a modified example. [Figure 8] 13 is a cross-sectional view showing the periphery of a first dense layer 92 and a first region 77 in a modified example. [Figure 9] 13 is a cross-sectional view showing the periphery of a first dense layer 92 and a first region 77 in a modified example. [Figure 10] 13 is a cross-sectional view showing the periphery of a first dense layer 92 and a first region 77 in a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a vertical cross-sectional view showing a state in which a gas sensor 10 according to an embodiment of the present invention is attached to a pipe 58. FIG. 2 is a perspective view of a sensor element 20 as viewed from the upper right front. FIG. 3 is a vertical cross-sectional view showing a schematic vertical cross-section of the sensor element 20. FIG. 4 is a top view of the sensor element 20. FIG. 5 is a vertical cross-sectional view showing the periphery of a first region 77 of an outer lead wire 75 covered with a first dense layer 92. In this embodiment, as shown in FIGS. 1 to 5, the longitudinal direction of the element body 60 of the sensor element 20 is defined as a front-rear direction (length direction), the stacking direction (thickness direction) of the solid electrolyte layer of the element body 60 is defined as a top-down direction, and the direction perpendicular to the front-rear direction and the top-down direction is defined as a left-right direction (width direction).

[0017] 1, the gas sensor 10 includes an assembly 15, a nut 47, an outer cylinder 48, a connector 50, lead wires 55, and a rubber plug 57. The assembly 15 includes a sensor element 20, a protective cover 30, and an element sealing body 40. The gas sensor 10 is attached to a pipe 58, such as an exhaust gas pipe of a vehicle, and detects NOx and O contained in exhaust gas as a gas to be measured. 2 The gas sensor 10 is used to measure the concentration of a specific gas (specific gas concentration) such as NOx. In this embodiment, the gas sensor 10 measures the NOx concentration as the specific gas concentration. Of both ends (front end and rear end) along the longitudinal direction of the sensor element 20, the front end side is the side exposed to the measurement gas.

[0018] 1, the protective cover 30 includes a cylindrical inner protective cover 31 with a bottom that covers the front end side of the sensor element 20, and a cylindrical outer protective cover 32 with a bottom that covers the inner protective cover 31. A plurality of holes are formed in each of the inner protective cover 31 and the outer protective cover 32 for passing the measurement gas. An element chamber 33 is formed as a space surrounded by the inner protective cover 31, and a fifth surface 60e (front end surface) of the sensor element 20 is disposed within the element chamber 33.

[0019] The element sealing body 40 is a member that seals and fixes the sensor element 20. The element sealing body 40 includes a cylindrical body 41 having a metal shell 42 and an inner cylinder 43, insulators 44a to 44c (an example of a dense body), powder compacts 45a and 45b, and a metal ring 46. The sensor element 20 is disposed so as to extend along the central axis of the element sealing body 40 (here, an axis extending in the front-rear direction), and penetrates the element sealing body 40 in the axial direction.

[0020] The metal shell 42 is a cylindrical metal member. The metal shell 42 has a thick portion 42a whose inner diameter is smaller at the front side than at the rear side. A protective cover 30 is attached to the metal shell 42 on the same side (front side) as the front end of the sensor element 20. The rear end of the metal shell 42 is welded to a flange portion 43a of the inner cylinder 43. A part of the inner peripheral surface of the thick portion 42a is a bottom surface 42b which is a stepped surface. This bottom surface 42b holds the insulator 44a so that it does not protrude forward. The metal shell 42 has a through hole penetrating the metal shell 42 along the axial direction (here, the front-rear direction), and the sensor element 20 penetrates the inside of this through hole.

[0021] The inner cylinder 43 is a cylindrical metal member and has a flange portion 43a at the front end. The inner cylinder 43 and the metal shell 42 are welded coaxially. The inner cylinder 43 is also formed with a reduced diameter portion 43c for pressing the powder compact 45b in the central axial direction of the inner cylinder 43, and a reduced diameter portion 43d for pressing the insulators 44a to 44c and the powder compacts 45a and 45b forward via the metal ring 46. The inner cylinder 43 has a through hole penetrating the inner cylinder 43 along the axial direction (here, the front-rear direction), and the sensor element 20 passes through the inside of this through hole. The through hole of the metal shell 42 and the through hole of the inner cylinder 43 are in communication with each other in the axial direction, and these constitute the through hole of the cylindrical body 41.

[0022] The insulators 44a to 44c and the powder compacts 45a and 45b are disposed between the inner circumferential surface of the through hole of the cylindrical body 41 and the sensor element 20. The insulators 44a to 44c serve as supporters for the powder compacts 45a and 45b. Examples of materials for the insulators 44a to 44c include ceramics such as alumina, steatite, zirconia, spinel, cordierite, and mullite, and glass. The insulators 44a to 44c are dense members, and the porosity thereof is, for example, less than 1%. Each of the insulators 44a to 44c is a hollow columnar member having a through hole penetrating the insulator along the axial direction (here, the front-rear direction), and the sensor element 20 penetrates through the inside of this through hole. In this embodiment, the through hole of each of the insulators 44a to 44c has a rectangular cross section perpendicular to the axial direction in accordance with the shape of the sensor element 20. The powder compacts 45a and 45b are, for example, formed from powder, and serve as a sealing material. Examples of the material of the powder compacts 45a and 45b include ceramic powder such as alumina powder and boron nitride, in addition to talc, and the powder compacts 45a and 45b may each contain at least one of these. The average particle size of the particles constituting the powder compacts 45a and 45b may be 150 to 300 μm. The powder compact 45a is filled between the insulators 44a and 44b, and is sandwiched and pressed by the insulators 44a and 44b from both sides (front and back) in the axial direction. The powder compact 45b is filled between the insulators 44b and 44c, and is sandwiched and pressed by the insulators 44b and 44c from both sides (front and back) in the axial direction. The insulators 44a to 44c and the powder compacts 45a, 45b are sandwiched and pressed from both sides (front and back) in the axial direction by the bottom surface 42b of the thick portion 42a of the metal shell 42, the reduced diameter portion 43d, and the metal ring 46. The powder compacts 45a, 45b are compressed between the cylindrical body 41 and the sensor element 20 by the pressing forces from the reduced diameter portions 43c, 43d, so that the powder compacts 45a, 45b seal the gap between the element chamber 33 in the protective cover 30 and a space 49 in the outer cylinder 48 and fix the sensor element 20.

[0023] The nut 47 is fixed to the outside of the metallic shell 42 coaxially with the metallic shell 42. A male thread is formed on the outer circumferential surface of the nut 47. This male thread is screwed into a female thread provided on the inner circumferential surface of a fixing member 59 welded to the pipe 58. As a result, the gas sensor 10 is fixed to the pipe 58 such that the front end side of the sensor element 20 and a portion of the protective cover 30 protrude into the pipe 58.

[0024] The outer tube 48 is a cylindrical metal member, and covers the inner tube 43, the rear end side of the sensor element 20, and the connector 50. The rear end of the metal shell 42 is inserted inside the outer tube 48. The front end of the outer tube 48 is welded to the metal shell 42. A plurality of lead wires 55 connected to the connector 50 are drawn out from the rear end of the outer tube 48 to the outside. The connector 50 has housings 51a and 51b, a plurality of contact fittings 52, and a clamp 53. The housings 51a and 51b are members made of ceramics such as alumina, and are arranged above and below the rear end of the sensor element 20. The plurality of contact fittings 52 are all metal members, and are arranged below the housing 51a and above the housing 51b. The clamp 53 is a member formed by bending a plate-shaped metal into a C-shape, and uses elastic force to clamp the housings 51a and 51b from above and below and press them in a direction toward each other. The housings 51a and 51b clamp and fix the rear end of the sensor element 20 via the contact fittings 52 by the elastic force of the clamp 53. The contact fittings 52 are in contact with and electrically connected to the corresponding connector electrodes among the upper connector electrodes 71 and the lower connector electrodes 72 arranged on the surface of the rear end side of the sensor element 20, and are also electrically connected to the corresponding lead wires among the lead wires 55. The lead wires 55 are electrically connected to the connector 50 and to any of the electrodes 64 to 68 and the heater 69 inside the sensor element 20 via any of the upper connector electrodes 71 and the lower connector electrodes 72. The gap between the outer tube 48 and the lead wire 55 is sealed by a rubber plug 57. A space 49 in the outer tube 48 is filled with a reference gas. A sixth surface 60f (rear end surface) of the sensor element 20 is disposed in the space 49.

[0025] As shown in Figs. 2 to 4, the sensor element 20 includes an element body 60, a detection unit 63, a heater 69, a plurality of upper connector electrodes 71, a plurality of lower connector electrodes 72, a porous layer 80, and a dense layer 90. The element body 60 is made of zirconia (ZrO 2 The element body 60 has a laminate in which a plurality of oxygen ion conductive solid electrolyte layers (six in FIG. 3 ) such as oxygen ion conductive solid electrolyte layers are laminated. The element body 60 has a rectangular parallelepiped shape with the longitudinal direction along the front-rear direction, and has first to sixth faces 60a to 60f as outer surfaces on the top, bottom, left, right, front and rear, respectively. The first to fourth faces 60a to 60d are surfaces along the longitudinal direction of the element body 60 and correspond to side faces of the element body 60. The fifth face 60e is the front end face of the element body 60, and the sixth face 60f is the rear end face of the element body 60. The dimensions of the element body 60 may be, for example, a length in the front-rear direction of 25 mm to 100 mm, a width in the left-right direction of 2 mm to 10 mm, and a thickness in the up-down direction of 0.5 mm to 5 mm. The element body 60 is formed with a measurement gas inlet 61 that opens to the fifth face 60e and introduces a measurement gas into the element body 60 itself, and a reference gas inlet 62 that opens to the sixth face 60f and introduces a reference gas (here, air) that serves as a standard for detecting a specific gas concentration into the element body 60 itself.

[0026] The detection section 63 is for detecting the concentration of a specific gas in the measurement gas. The detection section 63 has a plurality of electrodes disposed on the front end side of the element body 60. In this embodiment, the detection section 63 includes an outer electrode 64 disposed on the first surface 60a, and an inner main pump electrode 65, an inner auxiliary pump electrode 66, a measurement electrode 67, and a reference electrode 68 disposed inside the element body 60. The inner main pump electrode 65 and the inner auxiliary pump electrode 66 are disposed on the inner circumferential surface of the space inside the element body 60, and have a tunnel-like structure.

[0027] The principle by which the detection unit 63 detects the concentration of a specific gas in a measurement gas is well known, and therefore a detailed description thereof will be omitted. The detection unit 63 detects the concentration of a specific gas, for example, as follows. The detection unit 63 pumps out or pumps in oxygen in the measurement gas around the inner main pump electrode 65 to the outside (element chamber 33) based on a voltage applied between the outer electrode 64 and the inner main pump electrode 65. The detection unit 63 also pumps out or pumps in oxygen in the measurement gas around the inner auxiliary pump electrode 66 to the outside (element chamber 33) based on a voltage applied between the outer electrode 64 and the inner auxiliary pump electrode 66. As a result, the measurement gas whose oxygen concentration has been adjusted to a predetermined concentration reaches the vicinity of the measurement electrode 67. The measurement electrode 67 functions as a NOx reduction catalyst and reduces the specific gas (NOx) in the measurement gas that has reached it. The detection unit 63 generates, as an electric signal, an electromotive force generated between the measurement electrode 67 and the reference electrode 68 in accordance with the oxygen concentration after reduction, or a current flowing between the measurement electrode 67 and the outer electrode 64 based on the electromotive force. The electric signal thus generated by the detection unit 63 is a signal indicating a value in accordance with the specific gas concentration in the measured gas (a value from which the specific gas concentration can be derived), and corresponds to the detection value detected by the detection unit 63.

[0028] The heater 69 is an electric resistor disposed inside the element body 60. When power is supplied from the outside, the heater 69 generates heat to heat the element body 60. The heater 69 heats and keeps warm the solid electrolyte layer that forms the element body 60, and can adjust the temperature to a temperature (e.g., 800° C.) at which the solid electrolyte layer is activated.

[0029] The upper connector electrodes 71 and the lower connector electrodes 72 are disposed on the rear end side of one of the side surfaces of the element body 60, and are electrodes for electrical conduction with the outside. The upper connector electrodes 71 and the lower connector electrodes 72 are exposed without being covered by the porous layer 80. In this embodiment, the four upper connector electrodes 71 (71a to 71d in FIG. 4) are arranged in the left-right direction and disposed on the rear end side of the first surface 60a (upper surface). The four lower connector electrodes 72 are arranged in the left-right direction and disposed on the rear end side of the second surface 60b (lower surface) facing the first surface 60a (upper surface). The four upper connector electrodes 71 (71a to 71d) and the four lower connector electrodes 72 are electrically connected to the electrodes 64 to 68 and the heater 69 of the detection unit 63, respectively. In this embodiment, the upper connector electrode 71a is electrically connected to the measurement electrode 67, the upper connector electrode 71b is electrically connected to the outer electrode 64, the upper connector electrode 71c is electrically connected to the inner auxiliary pump electrode 66, the upper connector electrode 71d is electrically connected to the inner main pump electrode 65, the three lower connector electrodes 72 are electrically connected to the heaters 69, and one lower connector electrode 72 is electrically connected to the reference electrode 68. The upper connector electrode 71b and the outer electrode 64 are electrically connected via an outer lead wire 75 disposed on the first surface 60a (see FIGS. 3 and 4). The other connector electrodes are electrically connected to the corresponding electrodes or the heater 69 via lead wires or through holes disposed inside the element body 60.

[0030] The outer lead wire 75 is a conductor containing a precious metal such as platinum (Pt) or a high melting point metal such as tungsten (W) or molybdenum (Mo) and zirconia. Zirconia is the same material as the oxygen ion conductive solid electrolyte contained in the element body 60. The outer lead wire 75 is preferably a cermet conductor containing a precious metal or a high melting point metal and zirconia. In this embodiment, the outer lead wire 75 is a cermet conductor containing platinum and zirconia. As shown in Figs. 3, 4, and 5, the outer lead wire 75 has a first region 77 and a second region 78. In this embodiment, the outer lead wire 75 is configured such that the entire portion other than the first region 77 is the second region 78. The second region 78 is covered with a porous layer 80, more specifically, with a first inner porous layer 83 as shown in Fig. 3. The second region 78 has a front end portion 78a disposed in front of the first region 77 and in contact with the first region 77 in the front-rear direction, and a rear end portion 78b disposed behind the first region 77 and in contact with the first region 77 in the front-rear direction. The front end portion 78a of the second region 78 is covered by the front end portion 83a of the first inner porous layer 83 of the porous layer 80, and the rear end portion 78b is covered by the rear end portion 83b of the first inner porous layer 83. The first region 77 is at least partially covered by the dense layer 90, and more specifically, is covered by the first dense layer 92 as shown in FIG. 3. In this embodiment, as shown in FIG. 3 and FIG. 5, the first dense layer 92 and the first region 77 have the same front-rear length, and the front end positions and the rear end positions are the same. Therefore, the first region 77 does not have a protruding portion protruding from the front end side and / or the rear end side of the first dense layer 92.

[0031] The first region 77 has a TM ratio Ht / Hm, which is the ratio of the peak height Ht of the T phase (tetragonal crystal) of zirconia to the peak height Hm of the M phase (monoclinic crystal) of zirconia in a Raman spectrum measured by Raman spectroscopy, of less than 2. The TM ratio of the zirconia in the first region 77 is preferably 1 or less, more preferably 0.1 or less. The TM ratio of the zirconia in the first region 77 may be 0.01 or more. The TM ratio of the zirconia in the second region 78 may be the same as or different from that in the first region 77. The TM ratio of the second region 78 may be larger or smaller than that of the first region 77. The first region 77 and the second region 78 may be made of different materials, and for example, if the first region 77 contains zirconia, the second region 78 may not contain zirconia. In this embodiment, the first region 77 and the second region 78 are made of the same material but have different TM ratios of zirconia.

[0032] The TM ratio of zirconia in the first region 77 of the outer lead wire 75 is a value derived as follows using a Raman spectrum measured by Raman spectroscopy. First, the sensor element 20 is cut along the thickness direction of the outer lead wire 75 so that the cross section of the first region 77 of the outer lead wire 75 is the observation surface, and the cut surface is processed by ion milling to prepare a cross-sectional sample. Next, a laser beam is irradiated onto the observation surface using, for example, a Raman spectrometer to obtain a Raman spectrum. The Raman spectrum has a wavelength of 70 to 800 cm. -1 The intensity is acquired between 0.01 and 0.15, and the maximum and minimum values ​​of the intensity are calculated within this range. Furthermore, the minimum value is subtracted from the overall intensity, and the spectrum is normalized by the value of the maximum value minus the minimum value. FIG. 6 is an explanatory diagram showing a schematic diagram of the calculation of the peak heights Ht and Hm from the Raman spectrum SP, which is an example of the Raman spectrum thus obtained. The horizontal axis of FIG. 6 represents the Raman shift [cm -1 For example, when a Raman spectrum SP as shown in FIG. 6 is obtained, first, the Raman shift is determined to be 145 cm based on the Raman spectrum SP. -1The peak P1 closest to the Raman spectrum SP is identified as a peak derived from the T phase. The intensity Hta of this peak P1 is then calculated based on the Raman spectrum SP. Next, the intensity Htb of the baseline of the peak P1 is calculated. The intensity Htb is calculated based on the Raman shift of 130 cm -1 Nearby area R1 (129cm -1 Over 131cm -1 The difference between the intensity Hta and the intensity Htb is calculated as the peak height Ht of the T phase. -1 The peak P2 located closest to the peak P1 is identified as a peak derived from the M phase. The intensity Hma of this peak P2 is then calculated based on the Raman spectrum SP. Next, the intensity Hmb of the baseline of the peak P2 is calculated. The intensity Hmb is calculated based on the Raman shift of 160 cm -1 Nearby area R2 (159cm -1 Over 161cm -1 The TM ratio Ht / Hm is calculated as the average value of the intensities of the T phase and M phase (regions below). The difference between the intensities Hma and Hmb is then calculated as the peak height Hm of the M phase. The TM ratio = Ht / Hm is calculated based on the peak heights Ht of the T phase and Hm of the M phase thus calculated. The TM ratio of zirconia in the second region 78 is also a value derived in the same manner. Regions R1 and R2 are predetermined regions from among regions where the peaks derived from the T phase and the peaks derived from the M phase do not interfere with each other (regions that do not overlap with either peak).

[0033] The porosity of each of the first region 77 and the second region 78 may be 5% or more. The porosity of each of the first region 77 and the second region 78 may be 40% or less, or less than 15%. The porosity of the first region 77 and the second region 78 may be different. The porosity of the front end portion 78a and the rear end portion 78b of the second region 78 may be different. The line width (thickness) of the outer lead wire 75 may be, for example, 0.1 mm or more and 1.0 mm or less. The line thickness (thickness) of the outer lead wire 75 may be, for example, 1 μm or more and 30 μm or less. An insulating layer (not shown) for insulating the outer lead wire 75 from the solid electrolyte layer of the element body 60 may be disposed between the outer lead wire 75 and the first surface 60a of the element body 60.

[0034] The porosity of the first region 77 and the second region 78 of the outer lead wire 75 is a value derived as follows using an image (SEM image) obtained by observation using a scanning electron microscope (SEM). First, the sensor element 20 is cut along the thickness direction of the outer lead wire 75 so that the cross section of the outer lead wire 75 is the observation surface, and the cut surface is filled with resin and polished to obtain an observation sample. Next, the magnification of the SEM is set to 1000 to 10000 times, and an SEM image of the outer lead wire 75 is obtained by photographing the observation surface of the observation sample. Next, the obtained image is analyzed, and a threshold value is determined by a discriminant analysis method (Otsu's binarization) from the brightness distribution of the brightness data of the pixels in the image. After that, each pixel in the image is binarized into an object part and a pore part based on the determined threshold value, and the area of ​​the object part and the area of ​​the pore part are calculated. Then, the ratio of the area of ​​the pore part to the total area (the total area of ​​the object part and the pore part) is derived as the porosity (unit: %). The porosities of a porous layer 80 and a dense layer 90, which will be described later, are also values ​​derived in a similar manner.

[0035] The porous layer 80 is a porous body that covers part of the side surfaces, i.e., the first and second faces 60a and 60b, of the element body 60 on which the upper and lower connector electrodes 71 and 72 are disposed. In this embodiment, the porous layer 80 covers at least the front end sides of the first and second faces 60a and 60b. The porous layer 80 includes an inner porous layer 81 that covers the first and second faces 60a and 60b, respectively, and an outer porous layer 85 that is disposed on the outside of the inner porous layer 81.

[0036] The inner porous layer 81 includes a first inner porous layer 83 covering the first surface 60a and a second inner porous layer 84 covering the second surface 60b. The first inner porous layer 83 has a front end portion 83a and a rear end portion 83b (see Figs. 2 to 4 and 5). The front end portion 83a covers the area of ​​the first surface 60a from the front end of the first surface 60a to the front end of the first dense layer 92. The rear end portion 83b covers the area of ​​the first surface 60a from the rear end of the first dense layer 92 to the rear end of the first surface 60a, except for the area where the upper connector electrode 71 is present. The widths of the front end portion 83a and the rear end portion 83b of the first inner porous layer 83 are the same as the width of the first surface 60a, and the front end portion 83a and the rear end portion 83b cover the first surface 60a from the left end to the right end of the first surface 60a. The first inner porous layer 83 covers at least a part of the outer electrode 64 and the outer lead wire 75. In this embodiment, as shown in Figs. 3 and 4, the first inner porous layer 83 covers the entire outer electrode 64 and the outer lead wire 75 except for the first region 77 (i.e., the entire second region 78). The first inner porous layer 83 serves as a protective layer that protects the outer electrode 64 and the outer lead wire 75 from components such as sulfuric acid in the measured gas, and suppresses corrosion of these electrodes.

[0037] The second inner porous layer 84 has a front end portion 84a and a rear end portion 84b (see Figs. 2 and 3). The front end portion 84a covers the area of ​​the second surface 60b from the front end of the second surface 60a to the front end of the second dense layer 96. The rear end portion 84b covers the area of ​​the second surface 60b from the rear end of the second dense layer 96 to the rear end of the second surface 60b, except for the area where the lower connector electrode 72 is present. The left-right width of the front end portion 84a and the rear end portion 84b of the second inner porous layer 84 is the same as the left-right width of the second surface 60b, and the front end portion 84a and the rear end portion 84b cover the second surface 60b from the left end to the right end of the second surface 60b.

[0038] The outer porous layer 85 covers at least a part of each of the first to fifth faces 60a to 60e. The outer porous layer 85 covers the first face 60a and the second face 60b by covering the inner porous layer 81. The outer porous layer 85 has a shorter length in the front-rear direction than the inner porous layer 81, and unlike the inner porous layer 81, covers only the front end and the region near the front end of the element body 60. As a result, the outer porous layer 85 covers the peripheral portion of the multiple electrodes 64 to 68 of the detection unit 63 of the element body 60, in other words, the portion of the element body 60 that is disposed in the element chamber 33 and exposed to the measured gas. As a result, the outer porous layer 85 serves as a protective layer that suppresses the occurrence of cracks in the element body 60 due to the adhesion of water or the like in the measured gas.

[0039] The porous layer 80 is made of a ceramic porous body such as a porous alumina body, a porous zirconia body, a porous spinel body, a porous cordierite body, a porous titania body, or a porous magnesia body. In this embodiment, the porous layer 80 is made of a porous alumina body. The thickness of each of the first inner porous layer 83 and the second inner porous layer 84 may be, for example, 5 μm or more and 40 μm or less. The thickness of the outer porous layer 85 may be, for example, 40 μm or more and 800 μm or less. The porosity of the porous layer 80 is 10% or more. The porous layer 80 covers the outer electrode 64 and the measurement gas inlet 61, but if the porosity of the porous layer 80 is 10% or more, the measurement gas can pass through the porous layer 80. The porosity of the inner porous layer 81 may be 10% or more and 50% or less. The porosity of the outer porous layer 85 may be 10% or more and 85% or less. The outer porous layer 85 may have the same porosity as the inner porous layer 81 , or may have a higher porosity than the inner porous layer 81 .

[0040] The dense layer 90 suppresses the capillary phenomenon of water along the longitudinal direction of the element body 60. In this embodiment, the dense layer 90 has a first dense layer 92 and a second dense layer 96. The first dense layer 92 is provided on the first surface 60a on which the upper connector electrode 71 and the first inner porous layer 83 are provided. The first dense layer 92 is provided on the rear end side, i.e., rearward, of the element body 60 from at least a part of the porous layer 80 (here, the outer porous layer 85 and the front end side portion 83a). The first dense layer 92 is provided on the front end side, i.e., forward of the plurality of upper connector electrodes 71, of the element body 60. The first dense layer 92 is provided rearward from the outer electrode 64. The first dense layer 92 is provided rearward from any of the plurality of electrodes 64 to 68 of the detection unit 63 including the outer electrode 64 (see FIG. 3). When water moves backward in the first inner porous layer 83 by capillary action, the first dense layer 92 serves to prevent the water from passing through the first dense layer 92 and thus preventing the water from reaching the upper connector electrode 71. The first dense layer 92 is a dense layer having a porosity of less than 10%. The left-right width of the first dense layer 92 is the same as the left-right width of the first surface 60a, and the first dense layer 92 covers the first surface 60a from the left end to the right end of the first surface 60a. The front end of the first dense layer 92 contacts the rear end of the front end portion 83a of the first inner porous layer 83. The rear end of the first dense layer 92 contacts the front end of the rear end portion 83b of the first inner porous layer 83. The first dense layer 92 covers the first region 77 of the outer lead wire 75, as shown in Figs. 3, 4, and 5.

[0041] The second dense layer 96 is provided on the second surface 60b on which the lower connector electrodes 72 and the second inner porous layer 84 are disposed. The second dense layer 96 is provided on the rear end side, i.e., rearward, of the element body 60 from at least a part of the porous layer 80 (here, the outer porous layer 85 and the front end side portion 84a). The second dense layer 96 is provided on the front end side, i.e., forward of the lower connector electrodes 72, of the element body 60 from the lower connector electrodes 72. The second dense layer 96 is provided rearward from all of the electrodes 64 to 68 of the detection unit 63 including the outer electrode 64 (see FIG. 3). When water moves rearward in the second inner porous layer 84 by capillary action, the second dense layer 96 serves to prevent the water from passing through the second dense layer 96 and thus preventing the water from reaching the lower connector electrode 72. The second dense layer 96 is a dense layer with a porosity of less than 10%. The left-right width of the second dense layer 96 is the same as the left-right width of the second surface 60b, and the second dense layer 96 covers the second surface 60b from the left end to the right end of the second surface 60b. The front end of the second dense layer 96 contacts the rear end of the front end portion 84a of the second inner porous layer 84. The rear end of the second dense layer 96 contacts the front end of the rear end portion 84b of the second inner porous layer 84.

[0042] The first dense layer 92 and the second dense layer 96 differ from the porous layer 80 in that the porosity is less than 10%, but ceramics made of the materials exemplified for the porous layer 80 described above can be used. In this embodiment, the first dense layer 92 and the second dense layer 96 are both made of alumina ceramics. The thickness of the first dense layer 92 is less than 11 μm. The thickness of the first dense layer 92 may be 10 μm or less. The thickness of the first dense layer 92 may be 5 μm or more. The thickness of the first dense layer 92 may be thinner than the thickness of the first inner porous layer 83. The thickness of the first dense layer 92 may be thinner than the thickness of the outer lead wire 75. The thickness of the first dense layer 92 is measured at a portion of the first dense layer 92 located directly above the outer lead wire 75. The porosity of each of the first dense layer 92 and the second dense layer 96 is preferably 8% or less, more preferably 5% or less. The smaller the porosity, the more the first dense layer 92 and the second dense layer 96 can suppress the capillary phenomenon of water along the longitudinal direction of the element body 60 .

[0043] In the longitudinal direction (here, the front-rear direction) of the element body 60, the length Le1 (see FIG. 4) of the first dense layer 92 may be 0.5 mm or more. The length Le1 may be 5 mm or more. The length Le1 may be 25 mm or less, or 20 mm or less. In this embodiment, the length of the first region 77 of the outer lead wire 75 is equal to the length Le1 of the first dense layer 92.

[0044] The first dense layer 92 and the second dense layer 96 are disposed so as to overlap with the inner peripheral surface of any one of the plurality of insulators 44a to 44c in the longitudinal direction of the element body 60. In this embodiment, as shown in Fig. 1, the first dense layer 92 and the second dense layer 96 are disposed so as to overlap with the inner peripheral surface of the insulator 44b among the insulators 44a to 44c in the longitudinal direction of the sensor element 20. The inner peripheral surface of the insulator 44b is a surface of the insulator 44b facing the first dense layer 92 and the second dense layer 96, i.e., a surface exposed toward the first dense layer 92 and the second dense layer 96, and is a surface located on the upper and lower sides of the inner peripheral surface of the insulator 44b having a rectangular cross section.

[0045] Next, a method for manufacturing the gas sensor 10 thus constructed will be described. After the method for manufacturing the sensor element 20 is described, a method for manufacturing the gas sensor 10 incorporating the sensor element 20 will be described.

[0046] A method for manufacturing the sensor element 20 will be described. First, a plurality of (here, six) unfired ceramic green sheets corresponding to the element body 60 are prepared. In each green sheet, notches, through holes, grooves, etc. are provided by punching processing as necessary, and wiring patterns such as electrodes and outer lead wires 75 are screen-printed. In addition, the unfired porous layers that become the first inner porous layer 83 and the second inner porous layer 84 after firing, and the unfired dense layers that become the first dense layer 92 and the second dense layer 96 after firing are also formed on the surfaces of the green sheets that correspond to the first and second surfaces 60a, 60b by screen printing. After that, a plurality of green sheets are stacked. The stacked plurality of green sheets are the unfired element body that becomes the element body after firing, and include the unfired porous layer and the unfired dense layer. Then, this unfired element body is fired to obtain the element body 60 that includes the first inner porous layer 83, the second inner porous layer 84, the first dense layer 92, and the second dense layer 96. Next, the outer porous layer 85 is formed by plasma spraying to obtain the sensor element 20. Note that, in addition to screen printing and plasma spraying, gel casting, dipping, etc. can also be used as a manufacturing method for the porous layer 80, the first dense layer 92, and the second dense layer 96.

[0047] The wiring pattern that will become the outer lead wire 75 after firing can be formed by screen printing using a slurry made by kneading raw material particles (here, platinum particles and zirconia particles) of the outer lead wire 75, an additive, and a solvent. The additive can be, for example, yttrium oxide (Y 2 O 3), calcium oxide (CaO), magnesium oxide (MgO), etc. In this embodiment, the additive is yttrium oxide. The slurry for forming the wiring pattern of the outer lead wire 75 may contain a pore-forming material. The TM ratio of zirconia in the first region 77 of the outer lead wire 75 can be adjusted, for example, by adjusting the content ratio of the additive or the firing temperature of the wiring pattern for the outer lead wire 75 (i.e., the firing temperature of the unfired element body). For example, the higher the content ratio of the additive, the higher the proportion of the crystal system of the T phase of zirconia compared to the M phase at room temperature after firing, and thus the TM ratio tends to be larger. Therefore, the TM ratio can be reduced by reducing the content ratio of the additive. For example, the TM ratio can be reduced by reducing the ratio B / A of the content ratio B (mol%) of yttrium oxide to the content ratio A (mol%) of zirconia in the slurry for forming the wiring pattern for the first region 77. In addition, the lower the firing temperature, the higher the proportion of the M phase crystal system compared to the T phase, and the smaller the TM ratio tends to be. Therefore, the TM ratio can be reduced by setting the firing temperature to a relatively low temperature. In addition, the wiring patterns of the first region 77 and the second region 78 of the outer lead wire 75 can be formed by preparing two types of slurries made of the same material except for the difference in the value of the ratio B / A, and screen-printing the two types of slurries separately. When an additive is used as described above, the first region 77 and the second region 78 after manufacture also contain an additive (for example, at least one of yttrium oxide, calcium oxide, and magnesium oxide). The thickness of the first dense layer 92 can be adjusted, for example, by changing the number of printings when forming the unsintered dense layer that becomes the first dense layer 92, or by adjusting the viscosity of the unsintered dense layer.

[0048] A method for manufacturing the gas sensor 10 incorporating the sensor element 20 will be described. First, the sensor element 20 is inserted axially into the through hole of the cylindrical body 41, and the insulator 44a, the powder compact 45a, the insulator 44b, the powder compact 45b, the insulator 44c, and the metal ring 46 are arranged in this order between the inner circumferential surface of the cylindrical body 41 and the sensor element 20. Next, the metal ring 46 is pressed to compress the powder compacts 45a and 45b, and in this state, the diameter-reduced portions 43c and 43d are formed to manufacture the element sealing body 40, and the gap between the inner circumferential surface of the cylindrical body 41 and the sensor element 20 is sealed. After that, the protective cover 30 is welded to the element sealing body 40, and the nut 47 is attached to obtain the assembly 15. Then, the lead wire 55 passing through the rubber plug 57 and the connector 50 connected thereto are prepared. The prepared connector 50 is connected to the rear end side of the sensor element 20, and the multiple contact metal fittings 52 of the connector 50 are electrically connected to corresponding connector electrodes among the multiple upper connector electrodes 71 and lower connector electrodes 72. Thereafter, the outer cylinder 48 is fixed to the main metal fitting 42 by welding, thereby obtaining the gas sensor 10.

[0049] Next, an example of use of the gas sensor 10 thus constructed will be described. When the gas sensor 10 is attached to the pipe 58 as shown in FIG. 1 and a measurement gas flows through the pipe 58, the measurement gas flows through the protective cover 30 and flows into the element chamber 33, and the front end side of the sensor element 20 is exposed to the measurement gas. When the measurement gas passes through the porous layer 80 and reaches the outer electrode 64 and then reaches the sensor element 20 from the measurement gas inlet 61, the detection unit 63 generates an electric signal corresponding to the NOx concentration in the measurement gas, as described above. This electric signal is extracted through the upper and lower connector electrodes 71 and 72, and the NOx concentration is detected based on the electric signal.

[0050] In the sensor element 20 of the gas sensor 10 thus configured, the outer lead wire 75 has the first region 77 covered with the first dense layer 92 as described above. The first region 77 contains zirconia, and the TM ratio of the zirconia is less than 2. The first dense layer 92 has a thickness less than 11 μm. These features can suppress the occurrence of cracks in the sensor element 20. The inventors have confirmed this through experiments and analysis. The reason why such an effect is obtained is considered to be as follows. When the outer lead wire 75 contains zirconia, the heat generated during use of the sensor element 20 may cause TM transformation of the zirconia (change in crystal structure from T phase (tetragonal) to M phase (monoclinic)), which may cause the volume of the zirconia to expand. If the portion of the outer lead wire 75 covered with the first dense layer 92 expands too much, the stress inside the first dense layer 92 increases, and there is a concern that the sensor element 20 may crack, for example, by cracking the first dense layer 92. In contrast, in the sensor element 20 of this embodiment, the TM ratio of the zirconia in the first region 77 covered by the first dense layer 92 of the outer lead wire 75 is less than 2, so that the proportion of T phase in the zirconia is low and the proportion of M phase is high compared to when the TM ratio is 2 or more. Therefore, the proportion of T phase, which is the source of the change to M phase, is low in the zirconia in the first region 77 of this embodiment, so that the reduction rate of the TM ratio due to TM transformation is small, and the expansion rate of the volume of the first region 77 due to TM transformation is small. In addition, since the thickness of the first dense layer 92 is thin, less than 11 μm, the Young's modulus of the first dense layer 92 is low, so that even if the first region 77 expands, the stress inside the first dense layer 92 is unlikely to become large. It is considered that these factors can suppress the occurrence of cracks in the sensor element 20.

[0051] The smaller the TM ratio of the first region 77, the smaller the rate of decrease in the TM ratio due to TM transformation and the smaller the rate of volume expansion of the first region 77 due to TM transformation, thereby enhancing the effect of suppressing the occurrence of cracks in the sensor element 20. From this viewpoint, the TM ratio of the first region 77 is preferably 1 or less, and more preferably 0.1 or less. Furthermore, the thinner the first dense layer 92 is, the lower the Young's modulus of the first dense layer 92 is, thereby enhancing the effect of suppressing the occurrence of cracks in the sensor element 20 (particularly cracks in the first dense layer 92). From this viewpoint, the thickness of the first dense layer 92 is preferably 10 μm or less.

[0052] In addition, when the first region 77 changes from the T phase to the M phase, the value of the TM ratio decreases, so that the TM transformation of zirconia caused by use of the sensor element 20 may occur, causing the TM ratio of the first region 77 to change from 2 or more to less than 2. Alternatively, the first region 77 may change from the M phase to the T phase caused by use of the sensor element 20, causing the value of the TM ratio to increase, causing the TM ratio of the first region 77 to change from less than 2 to 2 or more. However, in the sensor element 20 of this embodiment, when the sensor element 20 is in an unused state, that is, when the TM transformation of zirconia caused by use of the sensor element 20 is not occurring, the TM ratio of zirconia in the first region 77 is less than 2. In addition, when the sensor element 20 is in an unused state, the TM ratio of zirconia in the first region 77 is preferably 1 or less, and more preferably 0.1 or less. In addition, when a change from M phase to T phase occurs in the first region 77 due to use of the sensor element 20 and the value of the TM ratio increases, the first region 77 will shrink. However, when the first region 77 shrinks, cracks in the sensor element 20 are less likely to occur compared to when the first region 77 expands.

[0053] The first inner porous layer 83 also covers the outer lead wire 75, but since the first inner porous layer 83 has a higher porosity and therefore a lower Young's modulus than the first dense layer 92, the internal stress of the first inner porous layer 83 is unlikely to increase even if the first region 77 expands. For this reason, even if the zirconia in the second region 78 expands due to the TM transformation, cracks are unlikely to occur in the first inner porous layer 83.

[0054] Furthermore, the measured gas may contain water (water, sulfuric acid dissolved in water, etc.), and this water may move through the porous layer 80 by capillary action. If this water reaches the upper and lower connector electrodes 71, 72, there is a concern that the upper and lower connector electrodes 71, 72 and the contact fittings 52 of the connector 50 that contact the upper and lower connector electrodes 71, 72 may rust or corrode. However, in the gas sensor 10 of this embodiment, even if the water in the measured gas moves through the porous layer 80 (particularly through the first inner porous layer 83 and the second inner porous layer 84) toward the rear end side of the sensor element 20 (element body 60) by capillary action, the water reaches the first and second dense layers 92, 96 before reaching the upper and lower connector electrodes 71, 72. Since the first and second dense layers 92, 96 are denser than the first and second inner porous layers 83, 84, capillary action of water is less likely to occur along the longitudinal direction of the element body 60. As a result, water can be prevented from moving beyond the first and second dense layers 92, 96 toward the rear end of the sensor element 20 and reaching the upper and lower connector electrodes 71, 72.

[0055] At this time, since the porosity of the first region 77 covered by the first dense layer 92 is 40% or less, water can be prevented from moving inside the first region 77, around the first dense layer 92, and moving toward the rear end side of the first dense layer 92 of the sensor element 20. This makes it possible to prevent water from reaching the upper connector electrode 71. Furthermore, when the porosity of the first region 77 is less than 15%, water is further prevented from moving inside the first region 77, and therefore water can be further prevented from reaching the upper connector electrode 71.

[0056] In addition, the first and second dense layers 92, 96 are arranged so that the inner circumferential surface of the insulator 44b and the sensor element 20 (element body 60) overlap in the longitudinal direction, respectively, thereby preventing water from moving around the first and second dense layers 92, 96 from the outside of the sensor element 20 toward the rear end side of the sensor element 20. For example, as a comparative example, consider a case in which the first and second dense layers 92, 96 are arranged so that the inner circumferential surface of the powder compact 45a in FIG. 1 and the sensor element 20 overlap in the longitudinal direction. The powder compact 45a is formed from powder as described above, and has water absorption properties. Therefore, in the comparative example, water may move around the first and second dense layers 92, 96 from the outside of the sensor element 20 toward the rear end side of the first and second dense layers 92, 96 by moving inside the powder compact 45a. 1, in the sensor element 20 of this embodiment, the first and second dense layers 92, 96 are arranged so that the inner circumferential surface of the insulator 44b overlaps with the position of the sensor element 20 in the longitudinal direction, and the insulator 44b is dense. This makes it possible to prevent water from moving around the multiple first and second dense layers 92, 96 from the outside of the sensor element 20 to the rear end side of the sensor element 20. This makes it possible to prevent water from reaching the upper and lower connector electrodes 71, 72.

[0057] Here, the correspondence between the components of this embodiment and the components of the present invention will be clarified. The sensor element 20 of this embodiment corresponds to the sensor element of the present invention, the element body 60 corresponds to the element body, the first surface 60a corresponds to the side surface, the outer electrode 64 corresponds to the outer electrode, the upper connector electrode 71 (71b) corresponds to the connector electrode, the outer lead wire 75 corresponds to the outer lead portion, the first dense layer 92 corresponds to the dense layer, and the first region 77 corresponds to the first region. Also, the second region 78 corresponds to the second region.

[0058] According to the sensor element 20 of this embodiment described above in detail, the outer lead wire 75 has the first region 77 at least a part of which is covered with the first dense layer 92. The first region 77 contains zirconia, and the TM ratio of the zirconia is less than 2. The first dense layer 92 has a thickness of less than 11 μm. This makes it possible to suppress the occurrence of cracks in the sensor element 20.

[0059] Moreover, by making the TM ratio of the first region 77 equal to or less than 1, the effect of suppressing the occurrence of cracks in the sensor element 20 can be more reliably obtained. By making the TM ratio of the first region 77 equal to or less than 0.1, the occurrence of cracks in the sensor element 20 can be further suppressed.

[0060] Furthermore, by setting the thickness of the first dense layer 92 to 10 μm or less, the effect of suppressing the occurrence of cracks in the sensor element 20 can be more reliably obtained.

[0061] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention.

[0062] For example, in the contact portion between the first dense layer 92 and the first inner porous layer 83 shown in FIG. 5 in the above-mentioned embodiment, there is no portion where the first dense layer 92 and the first inner porous layer 83 overlap in the thickness direction of the first dense layer 92, i.e., in the vertical direction. However, this is not limited thereto, and the first dense layer 92 may have an overlap portion where the first dense layer 92 overlaps with the first inner porous layer 83 in the thickness direction of the first dense layer 92 in the contact portion with the first inner porous layer 83. FIG. 7 is a cross-sectional view showing the first dense layer 92 and the periphery of the first region 77 of the modified example. In FIG. 7, the first dense layer 92 and the first inner porous layer 83 partially overlap with each other in the thickness direction of the first dense layer 92, i.e., in the vertical direction. Therefore, the first dense layer 92 has an overlap portion 92a which is a part of the first dense layer 92 on the front end side, and an overlap portion 92b which is a part of the first dense layer 92 on the rear end side. The overlapping portion 92a is a portion of the first dense layer 92 that overlaps with the rear end of the front end portion 83a of the first inner porous layer 83 in the vertical direction, and the upper surface of the overlapping portion 92a is in contact with the front end portion 83a. The upper surface of the overlapping portion 92a is inclined with respect to the front-rear direction, and the overlapping portion 92a has a shape in which the thickness becomes thinner as it approaches its own front end. The overlapping portion 92b is a portion of the first dense layer 92 that overlaps with the front end of the rear end portion 83b of the first inner porous layer 83 in the vertical direction, and the upper surface of the overlapping portion 92b is in contact with the rear end portion 83b. The upper surface of the overlapping portion 92b is inclined with respect to the front-rear direction, and the overlapping portion 92b has a shape in which the thickness becomes thinner as it approaches its own rear end. In FIG. 7, the first region 77 and the second region 78 also partially overlap each other in the thickness direction of the first region 77, i.e., in the vertical direction. Therefore, the first region 77 has an overlap portion 77a which is a part of the front end side of the first region 77, and an overlap portion 77b which is a part of the rear end side. The overlap portion 77a is a part of the first region 77 which overlaps with the rear end portion of the front end portion 78a of the second region 78 in the up-down direction, and the upper surface of the overlap portion 77a is in contact with the front end portion 78a. The upper surface of the overlap portion 77a is inclined with respect to the front-to-rear direction, and the overlap portion 77a has a shape which becomes thinner as it approaches its front end.The overlapping portion 77b is a portion of the first region 77 that overlaps with the front end of the rear end portion 78b of the second region 78 in the up-down direction, and the upper surface of the overlapping portion 77b is in contact with the rear end portion 78b. The upper surface of the overlapping portion 77b is inclined with respect to the front-rear direction, and the overlapping portion 77b has a shape in which the thickness becomes thinner as it approaches its rear end. Such overlapping portions 77a, 77b, 92a, and 92b may be formed, for example, for reasons related to the manufacture of the sensor element 20. For example, in the above-mentioned method of manufacturing the sensor element 20, when the pattern of the first region 77 of the outer lead wire 75 is formed by screen printing and then the pattern of the second region 78 is formed, as shown in FIG. 7, a part of the front and rear of the first region 77 is covered from the outside (upper side) of the sensor element 20 by the second region 78, and the overlapping portions 77a and 77b are formed. Similarly, when the pattern of the first dense layer 92 is formed by screen printing and then the pattern of the first inner porous layer 83 is formed, overlapping portions 92a and 92b are formed as shown in FIG.

[0063] Even if the overlapping portions 77a, 77b, 92a, and 92b are present as shown in Fig. 7, the outer lead wire 75 is covered with the first dense layer 92 and has the first region 77 in which the TM ratio of zirconia is less than 2, and the thickness of the first dense layer 92 is less than 11 µm, so that occurrence of cracks in the sensor element 20 can be suppressed as in the above-mentioned embodiment. In this case, it is preferable that the first dense layer 92 covers only the first region 77 out of the first region 77 and the second region 78 from the front end side to the rear end side of the first dense layer 92 including the overlapping portions 92a and 92b. In other words, it is preferable that the second region 78 does not exist directly below the first dense layer 92 from the front end to the rear end of the first dense layer 92 in Fig. 7. In FIG. 7, the front end position of the overlapping portion 92a and the rear end position of the overlapping portion 77a (= the rear end position of the front end portion 78a of the second region 78) are at the same position in the front-rear direction, so the front end portion 78a of the second region 78 does not exist directly below the overlapping portion 92a. In addition, the front end position of the overlapping portion 77b (= the front end position of the rear end portion 78b of the second region 78) is located rearward of the rear end position of the overlapping portion 92b, so the rear end portion 78b of the second region 78 does not exist directly below the overlapping portion 92b. As a result, the second region 78 does not exist directly below the first dense layer 92 from the front end to the rear end of the first dense layer 92. This more reliably achieves the effect of suppressing the occurrence of cracks in the sensor element 20 by the first region 77. For example, as shown in Fig. 8, a part of the front end portion 78a of the second region 78 may be present directly below the overlapping portion 92a of the first dense layer 92, i.e., the overlapping portion 92a and the overlapping portion 77a may overlap in the vertical direction. Rather than the form shown in Fig. 8, it is preferable that the second region 78 does not exist directly below the first dense layer 92 from the front end to the rear end of the first dense layer 92 as shown in Fig. 7. If the second region 78 does not exist directly below the first dense layer 92 from the front end to the rear end of the first dense layer 92, the effect of suppressing the occurrence of cracks in the sensor element 20 can be obtained even if the TM ratio of the second region 78 is not less than 2, so that the degree of freedom in designing the second region 78 is increased. For example, the degree of freedom in designing the TM ratio of the second region 78 and the degree of freedom in designing the material of the second region 78 are increased.Even when the overlapping portions 77a, 77b, 92a, and 92b do not exist, it is preferable that the first dense layer 92 covers only the first region 77 of the first region 77 and the second region 78 from the front end side to the rear end side of the first dense layer 92. For example, the first dense layer 92 shown in FIG. 5 covers only the first region 77 of the first region 77 and the second region 78.

[0064] In FIG. 7, the first dense layer 92 and the first inner porous layer 83 are partially overlapped with each other so that the first inner porous layer 83 is located on the upper side, but the first dense layer 92 may be partially overlapped with each other so that the first dense layer 92 is located on the upper side of the first inner porous layer 83. The same applies to the vertical relationship of the overlap between the second region 78 and the first region 77. For example, FIG. 9 is a cross-sectional view in which the vertical relationship of the overlap between the first dense layer 92 and the first inner porous layer 83 in FIG. 7 is reversed, and the vertical relationship of the overlap between the second region 78 and the first region 77 is reversed. Similarly, FIG. 10 is a cross-sectional view in which the vertical relationship of the overlap in FIG. 8 is reversed. In FIG. 9 and FIG. 10, the same components as those in FIG. 7 and FIG. 8 are denoted by the same reference numerals, and detailed description thereof will be omitted. In FIG. 10, the lower surface of the first dense layer 92 does not overlap with the overlapping portion 77a of the first region 77 in the vertical direction, but the overlapping portion 92a of the first dense layer 92 partially overlaps with the overlapping portion 77a of the first region 77 in the vertical direction. That is, in FIG. 10, like FIG. 8, a part of the front end portion 78a of the second region 78 exists directly below the overlapping portion 92a of the first dense layer 92. In contrast, in FIG. 9, the overlapping portion 92a of the first dense layer 92 does not overlap with the overlapping portion 77a of the first region 77 in the vertical direction. That is, in FIG. 9, like FIG. 7, the front end portion 78a of the second region 78 does not exist directly below the overlapping portion 92a. Therefore, in FIG. 9, the second region 78 does not exist directly below the first dense layer 92 from the front end to the rear end of the first dense layer 92. Therefore, the configuration of FIG. 9 is preferable to the configuration of FIG. 10.

[0065] In the above-described embodiment, the first region 77 shown in FIG. 5 does not have a protruding portion protruding from the first dense layer 92 toward the front end side and / or rear end side, but the first region 77 may have a protruding portion. That is, it is sufficient that at least a part of the first region 77 is covered with the first dense layer 92. For example, the first region 77 in FIG. 7 and FIG. 9 has an overlap portion 77a protruding from the first dense layer 92 toward the front end side, and the overlap portion 77a corresponds to the protruding portion. The first region 77 in FIG. 7 and FIG. 9 has a region 77c protruding from the first dense layer 92 toward the rear end side. The region 77c includes the overlap portion 77b and a region between the overlap portion 92b and the overlap portion 77b in the front-rear direction. This region 77c also corresponds to the protruding portion. Even though the first region 77 has a protruding portion (overlapping portion 77a, region 77c) in this manner, the outer lead wire 75 has the first region 77 which is covered with the first dense layer 92 and in which the TM ratio of zirconia is less than 2, and the thickness of the first dense layer 92 is less than 11 μm, so that the occurrence of cracks in the sensor element 20 can be suppressed, as in the above-described embodiment.

[0066] In the above-described embodiment, the outer lead wire 75 has the first region 77 having a TM ratio of less than 2, and the second region 78 having a TM ratio different from that of the first region 77. However, the TM ratio of the second region 78 may be the same as that of the first region 77. For example, the outer lead wire 75 may not have the second region 78, and the entire outer lead wire 75 may be configured as the first region 77.

[0067] In the above-described embodiment, the first inner porous layer 83 of the sensor element 20 covers the first surface 60a except for the region where the upper connector electrode 71 and the first dense layer 92 are present, but this is not limited thereto. For example, the first inner porous layer 83 may cover the region of the first surface 60a from the front end of the first surface 60a to the front end of the upper connector electrode 71 or a predetermined position further forward than the front end. In addition, a gap region (a region where neither a porous layer nor a dense layer exists) may be provided between the front end portion 83a of the first inner porous layer 83 and the first dense layer 92 and / or between the rear end portion 83b of the first inner porous layer 83 and the first dense layer 92. Alternatively, the first inner porous layer 83 may not include the rear end portion 83b, and the region between the first dense layer 92 and the upper connector electrode 71 may be the gap region. The outer lead wire 75 may be exposed where the gap region is provided. Furthermore, the first inner porous layer 83 does not necessarily have to include the front end portion 83a, the porous layer 80 does not necessarily have to include the outer porous layer 85, and the sensor element 20 does not necessarily have to include the porous layer 80.

[0068] In the above-described embodiment, the first dense layer 92 overlaps with the insulator 44b in the front-rear direction, but this is not limited thereto. The first dense layer 92 may overlap with, for example, the insulator 44a or the insulator 44c in the front-rear direction.

[0069] In the above embodiment, the element body 60 has a rectangular parallelepiped shape, but is not limited thereto. For example, the element body 60 may have a cylindrical or columnar shape. In this case, the element body 60 has only one side surface.

[0070] In the above-described embodiment, the gas sensor 10 includes two powder compacts 45a, 45b and three insulators 44a to 44c, but may include one or more powder compacts and multiple insulators (dense bodies). For example, the insulator 44b may be removed from the gas sensor 10. In this case, since the powder compacts 45a, 45b are adjacent to each other in the front-rear direction, the powder compacts 45a, 45b may be integrated. EXAMPLES

[0071] Specific examples of sensor elements produced will be described below as examples. Experimental Examples 2 to 6, 9, 11, and 12 correspond to examples of the present invention, and Experimental Examples 1, 7, 8, and 10 correspond to comparative examples. Note that the present invention is not limited to the following examples.

[0072] [Experimental Examples 1-12] Sensor elements were fabricated by the same manufacturing method as the gas sensor 10 in Figs. 1 to 5 and 7, and used as Experimental Examples 1 to 12. The element body 60 of each of these sensor elements 20 had dimensions of 52.5 mm in length, 4.25 mm in width, and 1.45 mm in thickness. The first dense layer 92 had a length Le1 of 5 mm and a porosity of 0%. The outer lead wire 75 had a line width of 0.4 mm and a line thickness of 15 µm. In Experimental Examples 1 to 13, the TM ratios of the first region 77 and the second region 78 of the outer lead wire 75 and the thickness of the first dense layer 92 were variously changed as shown in Table 1. The TM ratio of each of the first region 77 and the second region 78 was adjusted by adjusting the ratio B / A of the yttrium oxide content B (mol%) to the zirconia content A (mol%) in the slurry for forming the wiring patterns of each of the first region 77 and the second region 78 described above, or by adjusting the firing temperature of the unsintered element body.

[0073] [TM ratio measurement] For the sensor elements 20 of Experimental Examples 1 to 12, the TM ratios of the first region 77 and the second region 78 were measured by the method described above. The Raman spectrum was measured using a laser Raman spectrometer LabRAM ARAMIS manufactured by Horiba, Ltd., and the operation software LabSpec. The optical system was a Czerny-Turner type spectrometer using the backscattering method, and a semiconductor pumped solid-state laser (DPSS, 532 nm) was used as the light source. Before measuring the sample, calibration was performed using a Si wafer. The Raman spectrum was measured with a hole (confocal hole diameter) of 400 μm and a central wave number of the spectrometer of 520 cm. -1, Slit was 100 μm, grating was 1800 gr / mm, and objective lens was 100x. The measurement was performed in Duoscan mode with a measurement range of 15 × 15 μm. However, when a layer other than the lead wire was included in the measurement range, the measurement range was adjusted according to the thickness of the lead wire. The measurement points for the TM ratio of the first region 77 were the positions directly below the center of the first dense layer 92 in the front and rear and the positions directly below the front and rear ends, and three measurement points were measured at 50 μm intervals on the left and right for each position, for a total of nine measurement points. The TM ratio was calculated for each of the nine measurement points, and the average value was taken as the TM ratio of the first region 77. The measurement points for the TM ratio of the second region were the positions near the first region 77 in the front end portion 78a and the positions near the first region 77 in the rear end portion 78b, for a total of six measurement points, three measurement points were measured at 50 μm intervals on the left and right for each position. The TM ratio was calculated for each of the six measurement points, and the average value was determined as the TM ratio of the second region 78. Table 1 shows the measured TM ratios of the first region 77 and the second region 78 in each of Experimental Examples 1 to 12.

[0074] [Table 1]

[0075] [Crack test] A test was conducted to evaluate the crack resistance of the sensor elements 20 of Experimental Examples 1 to 12. Specifically, 20 sensor elements 20 of Experimental Example 1 were prepared, and these were placed in an autoclave and left for a total of 7 hours under saturated steam at a temperature of 180° C., thereby promoting the TM transformation of zirconia of the outer lead wire 75. At two timings, 5 hours and 7 hours after the initial placement in the autoclave, the 20 sensor elements 20 were visually checked using an optical microscope to see whether or not cracks had occurred, and the number of sensor elements 20 in which cracks had occurred was counted. The number of sensor elements 20 in which cracks had occurred after 5 hours was determined as the first crack number, and the ratio of the number of first cracks to the number of 20 sensor elements 20 was calculated as the first crack rate. The number of sensor elements 20 in which cracks occurred after 7 hours had elapsed (including the number of first cracks) was defined as the second crack number, and the ratio of the number of second cracks to the 20 sensor elements 20 was calculated as the second crack rate. The first crack rate and the second crack rate were calculated similarly for the sensor elements 20 of Experimental Examples 2 to 12. The first crack rate of Experimental Example 1 was defined as a reference value, and when the second crack rate was less than the reference value in Experimental Examples 1 to 12, it was judged as excellent (A), when the second crack rate was equal to or greater than the reference value but the first crack rate was less than the reference value, it was judged as good (B), and when the first crack rate was equal to or greater than the reference value, it was judged as poor (F).

[0076] As can be seen from Table 1, in Experimental Examples 2 to 6, 9, 11, and 12 in which the TM ratio of the first region 77 of the outer lead wire 75 is less than 2 and the thickness of the first dense layer 92 is less than 11 μm, the crack test evaluation was excellent (A) or good (B). In contrast, in Experimental Examples 1, 7, 8, and 10 in which the TM ratio of the first region 77 is 2 or more or the thickness of the first dense layer 92 is 11 μm or more, the crack test evaluation was poor (F). From this, it was confirmed that the occurrence of cracks in the sensor element 20 can be suppressed by making the TM ratio of the first region 77 covered with the first dense layer 92 of the outer lead wire 75 less than 2 and the thickness of the first dense layer 92 less than 11 μm. It is also considered that the TM ratio of the first region 77 is preferably 1 or less and the thickness of the first dense layer 92 is preferably 10 μm or less. Furthermore, among Experimental Examples 2 to 6, 9, 11, and 12 that were evaluated as excellent (A) or good (B) in the crack test, Experimental Examples 4 to 6, 11, and 12 in which the TM ratio of the first region 77 was 0.1 or less were all evaluated as excellent (A) in the crack test. From this, it was confirmed that by having the TM ratio of the first region 77 be 0.1 or less, the occurrence of cracks in the sensor element 20 can be further suppressed.

[0077] Furthermore, as can be seen from Table 1, a comparison of Experimental Examples 2 to 6, 9, 11, and 12, which were rated excellent (A) or good (B) in the crack test, confirmed that in all cases where the TM ratio of the second region 78 of the outer lead wire 75 is the same as the TM ratio of the first region 77 (Experimental Examples 2 to 6), is smaller than the TM ratio of the first region (Experimental Example 9), or is larger than the TM ratio of the first region (Experimental Examples 11 and 12), the effect of suppressing the occurrence of cracks in the sensor element 20 can be obtained as long as the TM ratio of the first region 77 is less than 2 and the thickness of the first dense layer 92 is less than 11 μm. [Industrial Applicability]

[0078] INDUSTRIAL APPLICABILITY The present invention can be used in a gas sensor for detecting the concentration of a specific gas, such as NOx, in a measurement gas, such as an exhaust gas from an automobile. [Explanation of symbols]

[0079] 10 gas sensor, 15 assembly, 20 sensor element, 30 protective cover, 31 inner protective cover, 32 outer protective cover, 33 element chamber, 40 element sealing body, 41 cylindrical body, 42 metal shell, 42a thick portion, 42b bottom surface, 43 inner cylinder, 43a flange portion, 43c, 43d reduced diameter portion, 44a to 44c insulator, 45a, 45b powder compact, 46 metal ring, 47 nut, 48 outer cylinder, 49 space, 50 connector, 51a, 51b housing, 52 contact metal, 53 clamp, 55 lead wire, 57 rubber plug, 58 piping, 59 fixing member, 60 element body, 60a to 60f first surface to sixth surface, 61 measured gas inlet, 62 reference gas inlet, 63 Detection portion, 64 outer electrode, 65 inner main pump electrode, 66 inner auxiliary pump electrode, 67 measurement electrode, 68 reference electrode, 69 heater, 71, 71a to 71d upper connector electrodes, 72 lower connector electrode, 75 outer lead wire, 77 first region, 77a, 77b overlap portion, 77c region, 78 second region, 78a front end portion, 78b rear end portion, 80 porous layer, 81 inner porous layer, 83 first inner porous layer, 83a front end portion, 83b rear end portion, 84 second inner porous layer, 84a front end portion, 84b rear end portion, 85 outer porous layer, 90 dense layer, 92 first dense layer, 92a, 92b overlap portion, 96 second dense layer.

Claims

1. A sensor element for detecting a specific gas concentration in a measurement gas, comprising: an element body having a front end and a rear end which are both ends along a longitudinal direction and a side surface which is a surface along the longitudinal direction, the front end side being exposed to the measurement gas; an outer electrode disposed on the front end side of the side surface; a connector electrode disposed on the rear end side of the side surface for electrical connection to an outside; an outer lead portion disposed on the side surface and electrically connecting the outer electrode and the connector electrode; a dense layer covering a portion of the side surface and disposed closer to the front end than the connector electrode; Equipped with the outer lead portion has a first region at least a portion of which is covered with the dense layer; The first region contains zirconia, and a TM ratio, which is a ratio Ht / Hm of a peak height Ht of a T phase of zirconia to a peak height Hm of an M phase of zirconia in a Raman spectrum measured using Raman spectroscopy, is less than 2; The dense layer has a thickness of less than 11 μm. Sensor element.

2. The first region has a TM ratio of 1 or less. The sensor element according to claim 1 .

3. The first region has a TM ratio of 0.1 or less. The sensor element according to claim 1 or 2.

4. The first region has a TM ratio of 0.01 or more. The sensor element according to claim 1 or 2.

5. The dense layer has a thickness of 10 μm or less. The sensor element according to claim 1 or 2.

6. the outer lead portion has the first region and a second region, The dense layer covers only the first region of the first region and the second region from the front end side to the rear end side of the dense layer. The sensor element according to claim 1 or 2.

7. A gas sensor comprising the sensor element according to claim 1 or 2.

Citation Information

Patent Citations

  • Solid electrolyte

    JP1981042909A

  • Partially stabilized zirconium oxide sintered body

    JP1984035065A

  • Laminated air / Fuel ratio sensor element

    JP1999316211A

  • Nondestructive inspection method and nondestructive inspection device

    JP2006084179A

  • Solid electrolyte for gas sensor, method of producing the same, and gas sensor using the same

    JP2010204088A