Laminate and method of manufacturing the same
The laminate with a low refractive index layer and gap structure protects and maintains the functionality of the optical functional layer, addressing the challenge of adhesive-induced deterioration and enhancing mechanical strength.
Patent Information
- Application Number
- JP2023058427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Protecting the convex surface of an optical functional layer while maintaining its functionality is challenging, as adhesives can cause deterioration or loss of function.
A laminate structure is devised with a low refractive index layer directly on the convex surface of the optical functional layer, forming a gap between them to maintain functionality and provide protection, using a low refractive index layer with a refractive index of 1.30 or less, and incorporating a porous layer to enhance mechanical strength.
The laminate effectively protects the optical functional layer, maintains its functionality, and ensures mechanical strength while allowing for optical effects such as angle-dependent image changes.
Smart Images

Figure 2024145876000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a method for producing the laminate. [Background technology]
[0002] Decorative films are used as a means for improving the design of various products. For example, as disclosed in Patent Documents 1 and 2, depending on the application, decorative films may have an optical functional layer having a function of changing the direction of light. The optical functional layer having the function of changing the direction of light typically has a convex surface. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-028981 A [Patent Document 2] JP 2020-104467 A Summary of the Invention [Problem to be solved by the invention]
[0004] If an attempt is made to protect the convex surface of the optical functional layer with, for example, an adhesive, the function of the optical functional layer may be reduced or lost.
[0005] The present invention has been made to solve the above-mentioned problems, and its main object is to provide a laminate that can achieve both protection of an optical functional layer having a convex surface and suppression of deterioration of the function of the optical functional layer. [Means for solving the problem]
[0006] 1. A laminate according to an embodiment of the present invention comprises an optical functional layer having a first main surface and a second main surface facing each other, with a convex portion formed on the first main surface, and a low refractive index layer having a refractive index of 1.30 or less provided on the first main surface side of the optical functional layer, with a gap formed between the optical functional layer and the low refractive index layer. 2. In the laminate described in 1 above, the protrusions may have vertices. 3. In the laminate according to 1 or 2 above, the ratio of the height of the voids to the height of the protrusions may be 10% or more. 4. In the laminate according to any one of the above items 1 to 3, the low refractive index layer may be in direct contact with the first main surface of the optical functional layer. 5. In the laminate according to any one of the above items 1 to 4, the height of the protrusions may be from 10 nm to 100 μm. 6. In the laminate according to any one of the above items 1 to 5, the pitch of the convex portions may be 1 μm to 1000 μm. 7. In the laminate according to any one of the above items 1 to 6, the low refractive index layer may be a porous layer made of a porous body. 8. The laminate according to any one of 1 to 7 above may have the optical functional layer, the low refractive index layer, and a first pressure-sensitive adhesive layer in this order. 9. The laminate according to any one of the above 1 to 8 may have a second pressure-sensitive adhesive layer, the optical functional layer, and the low refractive index layer in this order. 10. A method for manufacturing a laminate according to an embodiment of the present invention includes preparing an optical functional layer having first and second main surfaces opposing each other, with a convex portion formed on the first main surface; forming a coating film of a material that forms a low refractive index layer on the first main surface of the optical functional layer; and heating the coating film to form a low refractive index layer having a refractive index of 1.30 or less, wherein the heating forms a gap between the optical functional layer and the low refractive index layer. Effect of the Invention
[0007] According to the embodiment of the present invention, it is possible to protect the optical functional layer having a convex surface while suppressing deterioration of the function of the optical functional layer. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an outline of the configuration of a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram illustrating an optical functional layer included in the laminate shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In order to clarify the description, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the embodiment, but they are merely examples and do not limit the interpretation of the present invention. In addition, in the drawings, the same or equivalent elements are given the same reference numerals, and duplicate descriptions may be omitted.
[0010] Fig. 1 is a schematic cross-sectional view showing an outline of the configuration of a laminate according to one embodiment of the present invention, and Fig. 2 is a diagram for explaining an optical functional layer included in the laminate shown in Fig. 1. Note that, for ease of viewing, hatching of the optical functional layer is omitted in Figs. 1 and 2.
[0011] The laminate 100 has an optical functional layer 10 and a low refractive index layer 20. The optical functional layer 10 has a first main surface 10a and a second main surface 10b facing each other. The first main surface 10a is a convex surface, and the second main surface 10b is a flat surface. The optical functional layer 10 is, for example, a lenticular lens in which a plurality of convex portions (e.g., cylindrical lenses) 11 extending linearly on a base 12 are arranged in parallel. The convex portions 11 are arranged in the X direction (left-right direction) of FIG. 1 with their ridge lines directed in the Y direction. The low refractive index layer 20 is provided on the first main surface (convex surface) 10a side of the optical functional layer 10.
[0012] Height H of the convex portion 11 of the optical functional layer 10 1 The height H of the protrusion 11 can be set to any appropriate value. 1is, for example, 10 nm to 100 μm, preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm, and further preferably 10 μm to 20 μm. In this specification, "the height of a convex portion" means the height from the bottom surface of the convex shape to the highest part (for example, the apex t).
[0013] The pitch P of the convex portions 11 of the optical functional layer 10 can be set to any appropriate value. The pitch P of the convex portions 11 is, for example, 1 μm to 1000 μm, preferably 5 μm to 500 μm, more preferably 10 μm to 250 μm, and further preferably 40 μm to 120 μm. In this specification, the "pitch of the convex portions" is the distance between the centers of adjacent convex portions in a planar view. In the illustrated example, the pitch P of the convex portions is the distance between the highest parts (e.g., apexes t) of adjacent convex portions 11. In one embodiment, the pitch P of the convex portions 11 substantially corresponds to the width D of the convex portions 11.
[0014] Height H of the substrate 12 of the optical functional layer 10 2 can be set to any appropriate value. 2 is, for example, 15 μm to 360 μm, preferably 30 μm to 180 μm, and more preferably 60 μm to 120 μm.
[0015] The low refractive index layer 20 is in direct contact with the first main surface 10a of the optical functional layer 10. The low refractive index layer 20 can be provided on the first main surface 10a via an adhesive layer (not shown), for example. By providing the low refractive index layer 20 directly on the first main surface 10a, for example, adverse effects due to the refractive index of the adhesive layer can be avoided. The low refractive index layer 20 can be directly formed on the optical functional layer 10 by, for example, coating or printing a material for forming the low refractive index layer. When the low refractive index layer 20 is directly provided on the first main surface 10a of the optical functional layer 10, the adhesive strength (for example, 180° peel adhesive strength) of the low refractive index layer 20 to the optical functional layer 10 is preferably 1N / 25mm or more, more preferably 3N / 25mm or more, and even more preferably 5N / 25mm or more. The upper surface 20a of the low refractive index layer 20 may have an uneven shape following the unevenness of the convex surface 10a of the optical functional layer 10, or may be a flat surface unlike the illustrated example.
[0016] In the laminate 100, a gap 13 is formed between the optical functional layer 10 and the low refractive index layer 20. The upper end 11a of the convex portion 11 of the optical functional layer 10 is covered with the low refractive index layer 20, and the gap 13 is formed surrounded by the convex portion 11 of the optical functional layer 10 and the low refractive index layer 20. In this way, the low refractive index layer 20 is provided on the convex surface 10a side of the optical functional layer 10 to form the gap 13, thereby maintaining the function of the optical functional layer 10. For example, when the optical functional layer 10 is a lenticular lens, the light collection area when parallel light is incident on the optical functional layer 10 can be reduced. And, by providing the low refractive index layer 20 on the convex surface 10a side of the optical functional layer 10, a protective structure for the optical functional layer 10 can be formed, and for example, mechanical strength can be ensured.
[0017] Height H of protrusion 11 1 Height H of the gap 13 3 The ratio (H 3 ÷H 1× 100, hereinafter referred to as porosity) is, for example, more than 0%, preferably 10% or more, more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. With such a porosity, the function of the optical functional layer 10 can be maintained well. On the other hand, the porosity is, for example, less than 100%, preferably 90% or less, more preferably 80% or less, even more preferably 70% or less, and particularly preferably 60% or less. With such a porosity, the optical functional layer 10 can be well protected, and for example, excellent mechanical strength can be obtained.
[0018] The laminate 100 may have a first pressure-sensitive adhesive layer 31 provided on the first main surface 10a side of the optical functional layer 10. In the illustrated example, the first pressure-sensitive adhesive layer 31 is provided directly on the low refractive index layer 20. By providing the low refractive index layer 20, a protective structure can be formed by the first pressure-sensitive adhesive layer 31 while suppressing the deterioration of the function of the optical functional layer 10 due to the first pressure-sensitive adhesive layer 31, and for example, mechanical strength can be ensured. Although not illustrated, the laminate 100 may have a second pressure-sensitive adhesive layer provided on the second main surface 10b side of the optical functional layer 10. For practical purposes, it is preferable that a release liner (not illustrated) is temporarily attached to the surface of the pressure-sensitive adhesive layer until the laminate is used. By temporarily attaching the release liner, the pressure-sensitive adhesive layer is protected and the laminate can be rolled.
[0019] The optical functional layer typically has a function of changing the direction of light. A laminate including such an optical functional layer can achieve the following effects depending on the type of the optical functional layer. For example, various products can be surface-decorated to improve their design or aesthetics. Specifically, (1) the color of the displayed image can be changed depending on the viewing angle; and / or (2) different images can be displayed depending on the viewing angle. Therefore, the laminate according to the embodiment of the present invention can also be called a decorative film, an optical laminate, or the like. In the example shown in FIG. 1, a decorative portion 40 is provided on the second main surface 10b side of the optical functional layer 10, and for example, a pattern corresponding to the size of the convex portion (e.g., a cylindrical lens) 11 is drawn on the decorative portion 40.
[0020] As the optical functional layer, in addition to the lenticular lens, any suitable film having an uneven surface can be adopted. Representative examples of the optical functional layer 10 include a reflective hologram film, a microlens array film, and a prism film. The uneven surface of the optical functional layer can be appropriately designed according to the purpose. For example, any suitable uneven surface that can exhibit functions such as light diffusion, light scattering, light reflection, and light diffraction can be adopted as the uneven surface of the reflective hologram film. Representative examples include a Fourier transform structure, a light diffraction pattern, and a moth-eye structure in addition to the lenticular lens shown in the figure. In addition, uneven surfaces such as a hairline pattern, a matte pattern, a line pattern, and an interference pattern that do not have a light diffraction function but can exhibit a unique brilliance may be used. The size of the height of the convex parts, the pitch of the convex parts, etc. can be appropriately set according to the uneven surface shape.
[0021] The refractive index of the low refractive index layer 20 is typically 1.30 or less, and its lower limit is more than 1.00. The refractive index of the low refractive index layer 20 is preferably 1.15 to 1.30, more preferably 1.17 to 1.28, even more preferably 1.18 to 1.26, and particularly preferably 1.19 to 1.24. With such a refractive index, it is possible to very effectively suppress the deterioration of the function of the optical functional layer caused by providing a layer on the first main surface (convex surface) side of the optical functional layer. The refractive index refers to a refractive index measured at a wavelength of 550 nm, unless otherwise specified. The refractive index is, for example, a value measured by the method described in the Examples below.
[0022] The total light transmittance of the low refractive index layer 20 is preferably 85% to 99%, more preferably 87% to 98%, and further preferably 89% to 97%. By providing such a low refractive index layer on the first main surface (convex surface) side of the optical functional layer, for example, excellent transparency can be achieved as a whole laminate. As a result, for example, when the laminate is applied to various products, visibility of the product structure, image, etc. on the opposite side to the visible side of the optical functional layer can be ensured. The total light transmittance can be measured, for example, by a haze meter described later.
[0023] The haze of the low refractive index layer 20 is preferably less than 5%, more preferably less than 3%. On the other hand, the haze may be, for example, 0.1% or more, and may be 0.2% or more. By providing such a low refractive index layer on the first main surface (convex surface) side of the optical functional layer, for example, excellent transparency can be achieved for the entire laminate. As a result, for example, when the laminate is applied to various products, visibility of the product structure, image, etc. on the opposite side to the visible side of the optical functional layer can be ensured. For example, the haze can be calculated from the following formula using a value measured by a haze meter (for example, "HM-150" manufactured by Murakami Color Research Laboratory Co., Ltd.). Haze (%) = [Diffuse transmittance (%) / Total light transmittance (%)] x 100 (%)
[0024] The thickness of the low refractive index layer 20 is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and may be 5 μm or less. With such a thickness, the function of the optical functional layer 10 can be well maintained. On the other hand, the thickness of the low refractive index layer 20 is preferably 0.5 μm or more, more preferably 1 μm or more, even more preferably 1.5 μm or more, particularly preferably 2 μm or more, and most preferably 3 μm or more. With such a thickness, the optical functional layer 10 can be well protected, and for example, excellent mechanical strength can be obtained.
[0025] The low refractive index layer may have any suitable structure that can achieve the desired characteristics. Materials for forming the low refractive index layer may be, for example, materials described in International Publication No. 2004 / 113966, JP 2013-254183 A, and JP 2012-189802 A. Representative examples of materials for forming the low refractive index layer include silicon compounds. Examples of silicon compounds include silica-based compounds; hydrolyzable silanes, and their partial hydrolyzates and dehydration condensates; silicon compounds containing silanol groups; and activated silica obtained by contacting silicate with acid or ion exchange resin. Examples of materials for forming the low refractive index layer include organic polymers; polymerizable monomers (e.g., (meth)acrylic monomers and styrene monomers); and curable resins (e.g., (meth)acrylic resins, fluorine-containing resins, and urethane resins). These materials may be used alone or in combination of two or more.
[0026] In one embodiment, the low refractive index layer may contain spaces such as holes and gaps therein. In this case, the porosity of the low refractive index layer is preferably 20 volume % to 60 volume %, more preferably 25 volume % to 55 volume %, further preferably 30 volume % to 50 volume %, and particularly preferably 35 volume % to 45 volume %. With such a porosity, the refractive index of the low refractive index layer can be set in an appropriate range, and strength can be ensured. Here, the porosity is a value calculated from the refractive index measured by an ellipsometer using the Lorentz-Lorenz's formula.
[0027] The size of the pores that can be contained in the low refractive index layer can be adjusted to a desired size depending on the purpose and use. The size of the pores that can be contained in the low refractive index layer is, for example, 2 nm or more, preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 20 nm or more. On the other hand, the size of the pores that can be contained in the low refractive index layer is, for example, 500 nm or less, preferably 200 nm or less, and more preferably 100 nm or less. The size of the pores refers to the diameter of the major axis of the pores among the diameter of the major axis and the diameter of the minor axis.
[0028] The size of the pores can be quantified by the BET test method. In one embodiment, 0.1 g of a measurement sample (for example, the formed low refractive index layer) is placed in the capillary of a specific surface area measurement device (for example, "ASAP2020" manufactured by Micromeritics), and then the measurement sample is dried under reduced pressure for 24 hours at room temperature to remove gas contained in the measurement sample. Then, an adsorption isotherm is drawn by adsorbing nitrogen gas to the measurement sample, and the pore distribution is obtained. This allows the size of the pores to be evaluated.
[0029] The low refractive index layer having a space therein includes, for example, a porous layer made of a porous body and / or a layer containing an air layer at least in a part thereof. The low refractive index layer typically contains aerogel and / or particles (which may be, for example, hollow fine particles and / or porous particles). The low refractive index layer is preferably a nanoporous layer (specifically, a layer in which the diameter of 90% or more of the pores is 10 -1 nm~10 3 The porous layer may be in the range of 1 nm.
[0030] Any suitable particle may be used as the particle. The particle is typically composed of a silica-based compound. Examples of particle shapes include spherical, plate-like, needle-like, string-like, and bunch-of-grapes shapes. Examples of string-like particles include particles in which a plurality of particles having a spherical, plate-like, or needle-like shape are linked together in a string-like shape, short fiber-like particles (for example, short fiber-like particles described in JP-A-2001-188104), and combinations thereof. The string-like particles may be linear or branched. Examples of bunch-of-grapes particles include particles in which a plurality of spherical, plate-like, and needle-like particles are aggregated to form a bunch-of-grapes shape. The shape of the particles can be confirmed, for example, by observation using a transmission electron microscope.
[0031] An example of the low refractive index layer is a structure composed of one or more types of structural units that form a fine void structure, and these structural units are bonded together (for example, chemically bonded via catalytic action). The shape of the structural unit can be, for example, a particulate, fibrous, rod-like, or flat plate-like shape. The structural unit may have only one shape, or may have two or more shapes in combination.
[0032] A specific example of the low refractive index layer is a porous layer composed of a porous body in which particles having micropores (hereinafter referred to as micropore particles) are chemically bonded to each other. Such a porous layer can be obtained, for example, by chemically bonding micropore particles to each other. The shape of the micropore particles is not particularly limited, and may be, for example, spherical or other shapes. In addition, the micropore particles may be, for example, sol-gel beaded particles, nanoparticles (for example, hollow nanosilica nanoballoon particles), nanofibers, etc. Representative micropore particles include inorganic substances. Specific examples of inorganic substances include silicon (Si), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), and zirconium (Zr). These may be used alone or in combination of two or more. In one embodiment, the micropore particles are, for example, micropore particles of a silicon compound, and the porous body is, for example, a silicone porous body. The micropore particles of a silicon compound include, for example, a pulverized product of a gel-like silica compound.
[0033] Another example of the low refractive index layer is a layer containing a fibrous material such as nanofibers, and in which a space is formed by the entanglement of the fibrous material. Further examples of the low refractive index layer include a layer formed using hollow nanoparticles or nanoclay, and a layer formed using hollow nanoballoons or magnesium fluoride. The low refractive index layer may be composed of a single constituent material or a plurality of constituent materials. The low refractive index layer may be composed of a single form of the above examples, or a plurality of forms of the above examples.
[0034] The porous layer may be, for example, an open-cell structure in which the pore structure is continuous. The open-cell structure means that the pore structure is three-dimensionally connected in a porous body (for example, a silicone porous body), and can also be said to be a state in which the spaces of the pore structure are continuous. The open-cell structure of the porous layer can increase the porosity. It is difficult to form an open-cell structure using closed-cell particles having individual pore structures such as hollow particles (for example, hollow silica). However, when silica sol particles (pulverized gel-like silicon compound forming a sol) are used, for example, the silica sol particles can have a three-dimensional dendritic structure, so that the dendritic particles can be precipitated and deposited in the coating film (coated film of sol containing pulverized gel-like silicon compound) to easily form an open-cell structure. The porous layer preferably has a monolith structure in which the open-cell structure includes a plurality of pore distributions. The monolith structure means, for example, a hierarchical structure including a structure in which nano-sized fine pores exist and an open-cell structure in which nano-sized fine pores are aggregated. The monolithic structure, for example, can provide film strength through fine pores while providing high porosity through a coarse open-cell structure, thereby achieving both film strength and high porosity.
[0035] For example, the monolith structure can be formed by controlling the pore distribution of the void structure generated in the gel (gel silicon compound) before pulverizing into silica sol particles. Also, for example, when pulverizing the gel silicon compound, the particle size distribution of the silica sol particles after pulverization can be controlled to a predetermined size, thereby forming a monolith structure. Note that the particle size distribution can be measured by, for example, a particle size distribution evaluation device such as dynamic light scattering method or laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0036] As described above, the porous layer may contain pulverized gel compounds such as gel silicon compounds, and the pulverized particles are chemically bonded to each other. The chemical bond is not particularly limited, and may be, for example, a cross-linked bond, a covalent bond, or a hydrogen bond. The volume average particle size of the pulverized particles in the porous layer is, for example, 0.10 μm or more, preferably 0.20 μm or more, and more preferably 0.40 μm or more. On the other hand, the volume average particle size of the pulverized particles in the porous layer is, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The volume average particle size is an index of the particle size variation of the pulverized particles, and is determined by particle size distribution measurement.
[0037] The low refractive index layer may contain silicon atoms. For example, the silicon atoms contained in the low refractive index layer are preferably siloxane bonded. The ratio of unbonded silicon atoms (specifically, residual silanol) among all silicon atoms contained in the low refractive index layer is, for example, less than 50%, preferably 30% or less, more preferably 15% or less.
[0038] The laminate according to the embodiment of the present invention can be manufactured, for example, by preparing an optical functional layer having a first main surface and a second main surface facing each other and a convex portion formed on the first main surface, forming a coating film of a material forming a low refractive index layer on the first main surface (convex surface) of the optical functional layer, and heating the obtained coating film to form a low refractive index layer. By heating, the coating film can be unevenly distributed on the upper end side of the convex surface of the optical functional layer, and a gap can be formed between the obtained low refractive index layer and the optical functional layer, as shown in FIG.
[0039] In one embodiment, the coating film can be formed using a coating liquid containing microporous particles, and the microporous particles can be chemically bonded to each other by heating (including drying) this coating liquid. The coating liquid containing microporous particles is, for example, a suspension. For example, a catalyst (crosslinking reaction promoter) that promotes crosslinking between microporous particles (for example, a dehydration condensation reaction of residual silanol groups that may be contained in the microporous particles) and / or a substance (catalyst generator) that generates a catalyst (crosslinking reaction promoter) may be added to the coating liquid. Examples of the catalyst include photoactive catalysts and thermally active catalysts. Examples of the substance (catalyst generator) that generates a catalyst include photocatalyst generators and thermal catalyst generators. Examples of the photocatalyst generator include photobase generators (catalysts that generate a basic catalyst by light irradiation) and photoacid generators (substances that generate an acidic catalyst by light irradiation). For example, the microporous particles are pulverized products of a gel-like compound (preferably, a gel-like silicon compound), and the low refractive index layer is a porous layer composed of a porous body (preferably, a silicone porous body) containing the pulverized product of the gel-like compound. Such microporous particles may have a state in which the three-dimensional structure of the gel-like compound before pulverization is dispersed in the three-dimensional basic structure, and a structure based on the three-dimensional basic structure may be formed by using such microporous particles. Specifically, a new structure different from the three-dimensional structure of the gel-like compound may be formed. In this way, the finally obtained low refractive index layer (porous layer) may have a low refractive index similar to that of an air layer, for example. In addition, by chemically bonding the microporous particles to each other, the above-mentioned three-dimensional basic structure may be fixed, and sufficient strength may be ensured in the finally obtained low refractive index layer (porous layer). The specific configuration and details of the formation method of the low refractive index layer (porous layer) are described, for example, in International Publication No. 2019 / 151073. The description of the publication is incorporated herein by reference.
[0040] The coating thickness of the coating liquid may be set to a thickness that allows a gap to be formed between the obtained low refractive index layer and the optical functional layer, and may be appropriately set according to the size of the convex portion of the optical functional layer. For example, the coating thickness may be 2 times or more, 2.5 times or more, or 3 times or more of the height of the convex portion. On the other hand, the coating thickness may be 10 times or less of the height of the convex portion. For example, the coating thickness may be 30 μm or more, or 40 μm or more. On the other hand, the coating thickness may be 200 μm or less. The heating temperature of the coating film (coating liquid) is, for example, 20° C. or more, preferably 50° C. or more. On the other hand, the heating temperature of the coating film (coating liquid) is, for example, 200° C. or less, preferably 150° C. or less. The heating time of the coating film (coating liquid) is, for example, 10 seconds or more. On the other hand, the heating time of the coating film (coating liquid) is, for example, 24 hours or less, preferably 1 hour or less, more preferably 30 minutes or less, and further preferably 10 minutes or less.
[0041] The pressure-sensitive adhesive layer is made of any appropriate pressure-sensitive adhesive. In one embodiment, the first pressure-sensitive adhesive layer 31 is made of a pressure-sensitive adhesive having a hardness that does not penetrate into spaces such as pores and gaps that the low refractive index layer 20 may contain. The storage modulus of the first pressure-sensitive adhesive layer 31 at 23° C. is typically 1.0×10 5 (Pa) ~ 1.0 × 10 7 (Pa). The storage modulus of the first pressure-sensitive adhesive layer 31 at 23° C. is, for example, 1.1×10 5 (Pa) or more, 1.2×10 5 (Pa) or more, 1.3×10 5 (Pa) or more, 1.4×10 5 (Pa) or more, 1.5×10 5 (Pa) or more, 1.6×10 5 (Pa) or more, 1.7×10 5 (Pa) or more, 1.8×10 5 (Pa) or more, 1.9×10 5 (Pa) or more or 2.0×10 5 (Pa) or more and 1.0×10 7 (Pa) or less, 5.0×10 6 (Pa) or less, 1.0×10 6(Pa) or less or 5.0×10 5 (Pa) or less. The storage modulus of the first pressure-sensitive adhesive layer 31 at 23° C. is preferably 1.3×10 5 (Pa) ~ 1.0 × 10 6 (Pa), more preferably 1.5×10 5 (Pa) ~ 5.0 x 10 5 The storage modulus is determined in accordance with the method described in JIS K 7244-1 "Plastics - Test methods for dynamic mechanical properties" by reading the value at 23°C when measuring at a temperature rise rate of 5°C / min in the range of -50°C to 150°C under a frequency condition of 1Hz.
[0042] A representative example of the adhesive constituting the first adhesive layer 31 is an acrylic adhesive (acrylic adhesive composition). A representative example of the acrylic adhesive composition is a (meth)acrylic polymer as a main component (base polymer). The (meth)acrylic polymer may be contained in the adhesive composition at a ratio of, for example, 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more of the solid content of the adhesive composition. The (meth)acrylic polymer contains an alkyl (meth)acrylate as a monomer unit as a main component. Here, (meth)acrylate refers to acrylate and / or methacrylate. Examples of the alkyl group of the alkyl (meth)acrylate include linear or branched chain or cyclic alkyl groups having 1 to 20 carbon atoms. Examples of the monomer constituting the (meth)acrylic polymer include comonomers such as carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylates, and heterocyclic ring-containing (meth)acrylates, in addition to alkyl (meth)acrylates.
[0043] The acrylic adhesive composition may contain an acrylic oligomer in addition to the base polymer (or a prepolymer which is a partial polymer thereof). The acrylic oligomer may typically have a weight average molecular weight of about 1000 to 30000. The acrylic oligomer contains an alkyl (meth)acrylate as a monomer unit as a main component. For example, the acrylic adhesive composition is prepared by mixing the acrylic oligomer, a silane coupling agent and / or a crosslinking agent, other additives, etc., with the base polymer (prepolymer) as necessary. The remainder of the monomer which can constitute the base polymer may be added to the acrylic adhesive composition as necessary. Examples of the silane coupling agent include an epoxy group-containing silane coupling agent. Examples of the crosslinking agent include an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent.
[0044] The thickness of the first pressure-sensitive adhesive layer 31 is, for example, 3 μm to 60 μm, preferably 3 μm to 30 μm, and more preferably 5 μm to 10 μm. If the thickness of the first pressure-sensitive adhesive layer 31 is in this range, it has the advantage of having sufficient adhesive strength while having little effect on the optical functional layer. EXAMPLES
[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The refractive index and storage modulus were measured as follows. Unless otherwise specified, "%" and "parts" in the examples are based on weight. <Refractive index> A laminated film having a measurement object (e.g., a porous layer) formed on an acrylic film was cut into a sample piece measuring 25 mm x 50 mm, and the resulting sample piece was attached to the surface of a glass plate (thickness: 3 mm) via an adhesive. The center of the back surface of the above glass plate (diameter: about 20 mm) was filled with black marker to prepare a sample with no reflection on the back surface of the glass plate. The obtained sample was set in an ellipsometer (JA Woollam Japan: VASE), and light with a wavelength of 550 nm was made to enter the sample at an incident angle of 50 to 80 degrees to measure the refractive index. <Storage modulus> The measurement object (e.g., a pressure-sensitive adhesive layer) was molded to a thickness of about 1.5 mm by lamination or the like. This molded product was punched into a disk shape with a diameter of 7.9 mm to prepare a test piece. This test piece was sandwiched between parallel plates, and viscoelasticity was measured under the following conditions using a dynamic viscoelasticity measuring device ("Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific Co., Ltd.), to determine the storage modulus at 23°C. (Measurement conditions) Deformation mode: Torsion ·Measurement frequency: 1Hz ·Measurement temperature: -50℃~+150℃ Heating rate: 5℃ / min
[0046] [Production Example 1] Preparation of coating liquid for forming porous layer (1) Gelation of silicon compounds 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare mixed solution A. 0.5 g of 0.01 mol / L oxalic acid solution was added to this mixed solution A and stirred at room temperature for 30 minutes to hydrolyze MTMS, producing mixed solution B containing tris(hydroxy)methylsilane. To 5.5 g of DMSO, 0.38 g of 28 wt % ammonia water and 0.2 g of pure water were added, and then the above mixed solution B was further added and stirred at room temperature for 15 minutes to gel tris(hydroxy)methylsilane, thereby obtaining mixed solution C containing a gel-like silicon compound. (2) Aging treatment The mixed solution C containing the gel-like silicon compound prepared as above was incubated as it was at 40° C. for 20 hours for aging treatment. (3) Crushing Next, the gel-like silicon compound aged as described above was crushed into granules of several mm to several cm in size using a spatula. Next, 40 g of isopropyl alcohol (IPA) was added to the mixed liquid C, and after light stirring, the mixture was left to stand at room temperature for 6 hours, and the solvent and catalyst in the gel were decanted. The same decantation process was performed three times to replace the solvent, and a mixed liquid D was obtained. Next, the gel-like silicon compound in the mixed liquid D was crushed (high-pressure media-less crushing). The crushing process (high-pressure media-less crushing) was performed using a homogenizer (manufactured by SMT Co., Ltd., product name "UH-50"), and 1.85 g of the gel-like compound and 1.15 g of IPA in the mixed liquid D were weighed into a 5 cc screw bottle, and then crushed for 2 minutes under the conditions of 50 W and 20 kHz. By this grinding process, the gel-like silicon compound in the mixed liquid D was ground, and the mixed liquid D became a ground sol liquid E. The volume average particle diameter, which indicates the particle size variation of the ground material contained in the sol liquid E, was confirmed to be 0.50 to 0.70 μm using a dynamic light scattering nanotrack particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX150 type), and was found to be 0.50 to 0.70 μm. Furthermore, 0.062 g of a 1.5 wt % concentration MEK (methyl ethyl ketone) solution of a photobase generator (Wako Pure Chemical Industries, Ltd., product name: WPBG266) and 0.036 g of a 5% concentration MEK solution of bis(trimethoxysilyl)ethane were added to 0.75 g of the sol liquid E to obtain a coating liquid for forming a porous layer.
[0047] [Production Example 2-1] Preparation of adhesive 1 (Preparation of Acrylic Oligomer) 60 parts by weight of dicyclopentanyl methacrylate (DCPMA) and 40 parts by weight of methyl methacrylate (MMA) as monomer components, 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) was added as a thermal polymerization initiator and reacted at 70°C for 2 hours, and then the temperature was raised to 80°C and reacted for 2 hours. Thereafter, the reaction liquid was heated to 130°C, and toluene, the chain transfer agent, and unreacted monomers were dried and removed to obtain a solid acrylic oligomer. The weight average molecular weight of the obtained acrylic oligomer was 5100 and the glass transition temperature was 130°C.
[0048] (Preparation of Prepolymer) As monomer components for forming a prepolymer, 43 parts by weight of lauryl acrylate (LA), 44 parts by weight of 2-ethylhexyl acrylate (2EHA), 6 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 7 parts by weight of N-vinyl-2-pyrrolidone (NVP) were mixed, and 0.015 parts by weight of "Omnirad 184" manufactured by IGM Resins was used as a photopolymerization initiator. The mixture was irradiated with ultraviolet light to polymerize the mixture, and a prepolymer (polymerization rate: approximately 10%) was obtained.
[0049] (Preparation of Pressure-Sensitive Adhesive Composition) To 100 parts by weight of the prepolymer, 0.07 parts by weight of 1,6-hexanediol diacrylate (HDDA), 3 parts by weight of the acrylic oligomer, and 0.3 parts by weight of a silane coupling agent ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.) were added as post-addition components, and the mixture was mixed uniformly to prepare a pressure-sensitive adhesive composition.
[0050] (Formation of adhesive layer) A 75 μm thick polyethylene terephthalate (PET) film ("Diafoil MRF75" manufactured by Mitsubishi Chemical) with a silicone-based release layer on the surface was used as a substrate (doubles as a heavy-duty release film), and the above-mentioned photocurable adhesive composition was applied to a thickness of 50 μm to form a coating layer. A 75 μm thick PET film ("Diafoil MRE75" manufactured by Mitsubishi Chemical) with one side treated with silicone release was attached as a cover sheet (doubles as a light-duty release film) to this coating layer. This laminate was laminated from the cover sheet side with an irradiation intensity of 5 mW / cm2 on the irradiation surface directly under the lamp. 2 The adhesive was then photocured by irradiating it with ultraviolet light using a black light that was adjusted in position so as to form a 50 μm-thick adhesive layer.
[0051] [Production Example 2-2] Preparation of adhesive 2 (Preparation of acrylic adhesive solution) In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler, 90.7 parts of butyl acrylate, 6 parts of N-acryloylmorpholine, 3 parts of acrylic acid, 0.3 parts of 2-hydroxybutyl acrylate, and 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator were charged together with 100 g of ethyl acetate, and nitrogen gas was introduced to replace the nitrogen gas while gently stirring, and then the liquid temperature in the flask was kept at around 55°C and polymerization reaction was carried out for 8 hours to prepare an acrylic polymer solution. An acrylic adhesive solution was prepared by blending 0.2 parts of an isocyanate crosslinking agent (Coronate L manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane tolylene diisocyanate), 0.3 parts of benzoyl peroxide (Niper BMT manufactured by Nippon Oil & Fats Co., Ltd.), and 0.2 parts of γ-glycidoxypropyl methoxysilane (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd.) with respect to 100 parts of the solid content of the obtained acrylic polymer solution.
[0052] (Formation of adhesive layer) Next, the acrylic adhesive solution was applied to one side of a silicone-treated polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Polyester Film Corporation, thickness: 38 μm) so that the thickness after drying (thickness of the adhesive layer formed) would be 10 μm, and the film was dried at 150° C. for 3 minutes to form an adhesive layer. The storage modulus of the resulting adhesive was 1.3×10 5 (Pa).
[0053] [Example 1] As the optical functional layer, a lenticular film having a shape as shown in FIG. 2 ("Lenticular Lens" manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd.) was used. The height H of the convex part of the lenticular film 1 The width D of the protrusions (the pitch P of the protrusions) is 80 μm, and the height H 2 The thickness was 95 μm. The porous layer forming coating liquid prepared in Production Example 1 was applied to the convex surface of this lenticular film so that the coating thickness was 50 μm to 60 μm to obtain a coating film. The coating film was then heated at 100° C. for 1 minute to dry and obtain a porous body. The dried porous body was irradiated with ultraviolet light. Specifically, the dried porous body was irradiated with light having a wavelength of 360 nm under the condition of a light irradiation amount (energy) of 500 mJ. Then, an adhesive layer (thickness 50 μm) composed of the adhesive prepared in Production Example 2-1 was attached to the surface of the porous body, and heat aging was performed under the condition of 60° C. and 22 hours to form a porous layer on the lenticular film. In this way, a laminate having a configuration of lenticular film / porous layer / first adhesive layer was produced. The refractive index of the obtained porous layer was 1.15, and the porosity was 60%. By heating (drying), the coating film was unevenly distributed on the upper end side of the convex parts of the lenticular film, and voids were formed between the convex surface of the lenticular film and the porous body, as shown in Figure 1. The maximum thickness of the obtained porous layer was 6 μm, and the height H of the voids was 1.15. 3 The particle size was 10 μm and the porosity was 59%.
[0054] [Comparative Example 1] A laminate was produced in the same manner as in Example 1, except that the coating thickness of the coating solution for forming a porous layer was changed to less than 30 μm. Note that, by heating (drying) the coating film, as shown in FIG. 1, no voids were formed between the convex surfaces of the lenticular film and the porous body (the finally obtained porous layer was formed so as to fill the gaps between the convex portions of the lenticular film), and the maximum thickness of the obtained porous layer was 1.4 μm, and the porosity was 0%.
[0055] [Comparative Example 2] A laminate was produced in the same manner as in Example 1, except that a first pressure-sensitive adhesive layer was directly formed on the convex surface of the optical functional layer (a porous layer was not formed by applying the coating liquid for forming a porous layer and not heating or irradiating with ultraviolet light) and that heat aging was not performed. In the obtained laminate, the first pressure-sensitive adhesive layer was embedded between the convex portions of the lenticular film, and no gaps were formed between the convex surface of the lenticular film and the first pressure-sensitive adhesive layer.
[0056] [Comparative Example 3] A laminate was produced in the same manner as in Example 1, except that a first pressure-sensitive adhesive layer was directly formed on the convex surface of the optical functional layer (a porous layer-forming coating liquid was applied, and heating and ultraviolet irradiation were not performed to form a porous layer), and the pressure-sensitive adhesive prepared in Production Example 2-2 was used as the pressure-sensitive adhesive constituting the first pressure-sensitive adhesive layer, and heat aging was not performed. In the obtained laminate, the first pressure-sensitive adhesive layer did not enter between the convex portions of the lenticular film, and gaps were formed between the convex surface of the lenticular film and the first pressure-sensitive adhesive layer.
[0057] [evaluation] The laminates obtained in the examples and comparative examples were evaluated as follows. The evaluation results are shown in Table 1. (1) Optical properties A pattern was prepared in which thin lines of 40 μm width in different colors (two colors) were printed in a pattern arranged alternately without gaps, corresponding to the size of the convex parts of the lenticular film. The obtained laminate was placed on this pattern, and the pattern was observed from the surface of the laminate. Specifically, the change in the pattern that was visible when the viewing angle to the laminate surface was changed was evaluated. The evaluation criteria were as follows. (Evaluation Criteria) ○ (Good): The pattern changes when observed from different angles, and the pattern can be seen from any angle. × (bad): The pattern does not change even when observed from different angles (2) Mechanical strength The mechanical strength was evaluated by a peel test. For the peel test, in the lamination of the adhesive layer in the production of the laminates of each Example and Comparative Example, an adhesive sheet in which an adhesive layer was laminated onto a PET film measuring 25 mm in width and 300 mm in length was used to obtain a test sample (laminate) measuring 25 mm in width and 300 mm in length. For the obtained test samples, a 180° peel test was performed using a tensile tester (manufactured by Minebea, product name: TCM-1kNB) to peel the porous layer or the first adhesive layer from the lenticular film (optical functional layer) of the laminate in the length direction, and the interlayer adhesive strength (180° peel adhesive strength) (unit: N / 25 mm) between the optical functional layer and the layer adjacent thereto was measured. The measurement was performed under conditions of an atmosphere of 23°C and 50% RH, a peel angle of 180°, and a pulling speed of 300 mm / min. The evaluation criteria are as follows. (Evaluation Criteria) ◎ (Very good): Adhesive strength 5N / 25mm or more ○ (Good): Adhesive strength 1N / 25mm or more but less than 5N / 25mm × (Failure): Adhesive strength less than 1N / 25mm
[0058] [Table 1]
[0059] As is clear from Table 1, according to the examples of the present invention, it is possible to ensure mechanical strength while maintaining the function of the optical functional layer. [Industrial Applicability]
[0060] The laminate according to the embodiment of the present invention can be suitably used, for example, as a decorative film. [Explanation of symbols]
[0061] 10 Optical functional layer 10a First principal surface (convex surface) 10b Second principal surface 11 Convex 12 Base 13 void 20 Low refractive index layer 31 First adhesive layer 100 Laminate
Claims
1. an optical functional layer having a first main surface and a second main surface opposed to each other, the first main surface being formed with a convex portion; a low refractive index layer having a refractive index of 1.30 or less, the low refractive index layer being provided on the first main surface side of the optical functional layer; A gap is formed between the optical functional layer and the low refractive index layer. Laminate.
2. The laminate according to claim 1 , wherein the protrusion has an apex.
3. The laminate according to claim 1 , wherein a ratio of a height of the voids to a height of the protrusions is 10% or more.
4. The laminate according to claim 1 , wherein the low refractive index layer is in direct contact with the first main surface of the optical functional layer.
5. 2. The laminate according to claim 1, wherein the height of the protrusions is from 10 nm to 100 μm.
6. 2. The laminate according to claim 1, wherein the pitch of the protrusions is 1 μm to 1000 μm.
7. The laminate according to claim 1 , wherein the low refractive index layer is a porous layer made of a porous material.
8. The laminate according to claim 1 , comprising the optical functional layer, the low refractive index layer, and a first pressure-sensitive adhesive layer in this order.
9. The laminate according to claim 1 , comprising a second pressure-sensitive adhesive layer, the optically functional layer, and the low refractive index layer in this order.
10. preparing an optical functional layer having a first main surface and a second main surface opposed to each other, the first main surface being formed with a convex portion; forming a coating film of a material for forming a low refractive index layer on the first main surface of the optical functional layer; and and heating the coating film to form a low refractive index layer having a refractive index of 1.30 or less. a gap is formed between the optical functional layer and the low refractive index layer by the heating. A method for manufacturing a laminate.
Citation Information
Patent Citations
Decoration film and method for producing the same
JP2020028981A
Decorative film
JP2020104467A
Cited By
Low refractive index film comprising hollow silica and method for producing same
WO2026163877A1