Aqueous coating composition, coated film and building coating material
Patent Information
- Application Number
- JP2023058473
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
【0009】 本発明によれば、無機酸化物系の紫外線吸収剤を含む塗膜(例えばクリアー層)において、無機酸化物系の紫外線吸収剤の分散性に優れていることにより可視光透過率(透明性)に優れるとともに、無機酸化物系の紫外線吸収剤の金属成分の酸性環境下における耐溶出性にも優れ、加えて、長期にわたって優れた紫外線吸収性を維持できる塗膜の形成に好適な水性塗料組成物、塗膜および建築塗装材を提供することができる。
Smart Images

Figure 2024145895000001 
Figure 2024145895000002 
Figure 2024145895000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based coating composition, a coating film, and an architectural coating material. [Background technology]
[0002] In exterior building boards, a common coating specification is to coat the base material with a colored paint to form a design layer, and then coat a clear paint to form a surface protective layer (clear layer). The colored paint and clear paint used here are often water-based paints from an environmental perspective. Since exterior building boards are required to have long-term weather resistance, the clear layer is required to prevent ultraviolet rays from reaching the design layer. For this reason, ultraviolet absorbers are often blended into the paint that forms the clear layer. There are organic and inorganic ultraviolet absorbers, but inorganic ones generally have better weather resistance. Inorganic oxides such as titanium oxide, zinc oxide, and cerium oxide are known as inorganic ultraviolet absorbers.
[0003] However, when an inorganic oxide-based ultraviolet absorbent is used, if the dispersibility of the ultraviolet absorbent in the clear layer is insufficient, the clear layer may become cloudy or colored. In addition, when exposed to an acidic liquid such as acid rain for a long period of time, the metal components of the ultraviolet absorbent in the clear layer may be eluted, resulting in a problem of a decrease in the ultraviolet absorption of the clear layer.
[0004] In order to solve these conventional problems, for example, Patent Document 1 discloses a coating composition containing an ultraviolet-blocking material, the coating composition containing polysiloxane as a main component, and the ultraviolet-blocking material being formed by coating zinc oxide or cerium oxide with an inorganic material. Furthermore, Patent Document 2 discloses a coating system comprising: (a) at least one curable silicone resin material; (b) about 1% to about 50% by weight, based on the dry weight of the film after curing the coating system, of at least one inorganic UV absorbing material; and (c) about 1 ppm to about 75 ppm of at least one catalyst. Furthermore, Patent Document 3 discloses an inorganic clear coating composition containing (a) a specific silanol group-containing polyorganosiloxane, (b) a specific silane coupling agent, (c) a curing catalyst selected from the group consisting of tertiary amine compounds and tin-containing compounds, and (d) an inorganic ultraviolet absorber.
[0005] However, since the UV-cutting material of Patent Document 1 has an average particle size of 200 to 400 μm in the coating composition, it is presumed that the material forms aggregates in the coating film and is not uniformly dispersed in the coating film. Patent Documents 2 and 3 also do not disclose clear coatings containing inorganic UV absorbers with excellent acid resistance. Therefore, none of Patent Documents 1 to 3 discloses a clear layer that has excellent dispersibility of the inorganic UV absorber and does not dissolve the metal components of the inorganic UV absorber even when exposed to an acidic liquid for a long period of time. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-159668 A [Patent Document 2] Special Publication No. 2020-517754 [Patent Document 3] JP 2014-009304 A Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the present invention aims to provide an aqueous coating composition, coating film, and architectural coating material that are suitable for forming a coating film containing an inorganic oxide-based UV absorber, which has excellent visible light transmittance (transparency) due to excellent dispersibility of the inorganic oxide-based UV absorber, excellent resistance to leaching of the metal components of the inorganic oxide-based UV absorber in acidic environments, and can maintain excellent UV absorbency over the long term. [Means for solving the problem]
[0008] The features of the present invention are listed below. (1) An aqueous coating composition containing a water-dispersible resin and an inorganic oxide, The aqueous coating composition is applied to a substrate, dried to form a coating film having a dry thickness of 15 μm. A test piece is then immersed in a 5 g / L aqueous sulfuric acid solution for 24 hours in accordance with the acid resistance test specified in JIS K 5658:2010. When the amount of eluted metal components dissolved from the inorganic oxides contained in the coating film into the aqueous sulfuric acid solution is measured by ICP analysis, the amount of eluted metal components is 15 ppm or less. (2) The aqueous coating composition according to (1), wherein the substrate is made of a light-transmitting material and the test piece has a transmittance of light with a wavelength of 365 nm of 15% or less. (3) The aqueous coating composition according to (1), wherein the content of the inorganic oxide in the coating film is 5% by mass or more and 40% by mass or less. (4) The aqueous coating composition according to (1), further comprising a dispersant having an absolute value of the difference between the acid value and the amine value of 35 or less and a sum of the acid value and the amine value of 120 or less. (5) The aqueous coating composition according to (1), wherein the inorganic oxide contains at least one metal component selected from the group consisting of Ti, Zn and Ce. (6) The aqueous coating composition according to (1), wherein the volume average particle diameter of the secondary particles of the inorganic oxide is 20 nm or more and 200 nm or less. (7) The aqueous coating composition according to (1), wherein the inorganic oxide has a surface covered with a hydrophobic coating. (8) A coating film formed by applying the aqueous coating composition according to any one of (1) to (7) above onto a substrate and drying it. (9) An architectural coating material comprising an architectural substrate and a coating film formed by applying the aqueous coating composition according to any one of (1) to (7) above onto the architectural substrate and drying the composition. Effect of the Invention
[0009] According to the present invention, it is possible to provide an aqueous coating composition, coating film and architectural coating material that are suitable for forming a coating film (e.g., a clear layer) containing an inorganic oxide-based UV absorber, which has excellent visible light transmittance (transparency) due to excellent dispersibility of the inorganic oxide-based UV absorber, and which also has excellent resistance to leaching of the metal components of the inorganic oxide-based UV absorber in acidic environments, and which can maintain excellent UV absorbency over the long term. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] One aspect of the present invention is an aqueous coating composition containing a water-dispersible resin and an inorganic oxide. The aqueous coating composition of the present invention will be described in detail below. Note that the aqueous coating composition of the present invention can be embodied in various ways from the following description, and is not limited to the description.
[0011] (Water-based paint composition) The aqueous coating composition of the present invention is preferably an aqueous coating. In the present invention, the "aqueous coating" is a water-based coating containing water as a main solvent. Even if the aqueous coating composition of the present invention is an aqueous coating, it can obtain high water resistance after being sufficiently dried to form a coating film.
[0012] The water used in the aqueous coating composition of the present invention is not particularly limited, and preferred examples include tap water, ion-exchanged water, distilled water, and other pure water. When the aqueous coating composition is to be stored for a long period of time, water that has been sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria. In the aqueous coating composition of the present invention, the amount of water is preferably 20 to 90% by mass.
[0013] (Water dispersible resin) The water-dispersible resin used in the aqueous coating composition of the present invention is not particularly limited as long as it is a resin that is stably dispersed in water.For example, resin can be acrylic resin, silicone resin, acrylic silicone resin, fluororesin, polyester resin, rosin resin, petroleum resin, coumarone resin, phenolic resin, polyurethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, etc., and from the viewpoint of weather resistance, acrylic resin, silicone resin, or acrylic silicone resin, fluororesin are more preferred.
[0014] The water-dispersible resin is preferably used in the state of an emulsion in which the resin is stably dispersed in water, and may contain additives such as emulsifiers as necessary. Examples of methods for preparing an emulsion in which the resin is dispersed in water include a method of preparing an emulsion by performing emulsion polymerization in water using water as a medium. More preferably, an emulsion having a uniform structure obtained by emulsion polymerization, an emulsion having a heterophase structure obtained by a multi-stage emulsion polymerization method, and the like may be used together. Alternatively, an emulsion in which the resin is stably dispersed in water may be prepared as follows. For example, the emulsion may be prepared by self-emulsifying the resin in water while applying a forced shear force by using a high-speed stirrer or the like. Alternatively, an emulsion of the resin may be prepared by performing phase conversion into water for a resin polymerized in an organic solvent medium, and the organic solvent contained in the emulsion may be removed by distillation or the like as necessary.
[0015] Examples of the emulsifier include fatty acid salts such as sodium laurate, higher alcohol sulfate salts such as sodium lauryl sulfate, alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, polyoxyethylene alkyl ether sulfates, ammonium polyoxynonylphenyl ether sulfonate, polyoxyethylene-polyoxypropylene glycol ether sulfates, and further, anionic surfactants such as so-called reactive emulsifiers having a sulfonic acid group or a sulfate group and a polymerizable carbon-carbon unsaturated double bond in the molecule; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene nonylphenyl ethers, sorbitan fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene-polyoxypropylene block copolymers, or reactive nonionic surfactants having a skeleton of these compounds and a polymerizable carbon-carbon unsaturated double bond in the molecule; cationic surfactants such as alkylamine salts and quaternary ammonium salts; and (modified) polyvinyl alcohol.
[0016] The acrylic resin can be prepared by polymerizing one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, and nitriles, and, if necessary, polymerizable unsaturated monomers such as styrene and vinyl group-containing ester compounds (excluding the acrylic component) can also be added. Silicone resins are polymers having polysiloxane bonds in the main skeleton, and can be obtained, for example, by polymerizing one or more types of alkoxysilyl group-containing monomers or oligomers having polysiloxane bonds. The acrylic silicone resin can be prepared by polymerizing one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, and nitriles with an alkoxysilyl group-containing monomer such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane. Alternatively, it may be produced by a method in which a polymerization reaction and a siloxane condensation reaction are made to compete with each other using an alkoxysilyl group-containing monomer, or by a method in which a polymer (silicone portion) having a polysiloxane bond in the main skeleton is synthesized, and then the above-mentioned acrylic or methacrylic monomer is graft-polymerized to the polymer, or an acrylic resin is bonded to the polymer. The fluororesin may be a polymer having a unit based on a fluorine-containing monomer, or a copolymer having a unit based on a fluorine-containing monomer and a unit based on another monomer copolymerizable with the fluorine-containing monomer. The fluorine-containing monomer may be, for example, a unit based on a fluoroolefin or a fluorine-containing (meth)acrylic acid ester. The fluoroolefin may be, for example, trifluoroethylene, tetrafluoroethylene, pentafluoropropylene, hexafluoropropylene, chlorotrifluoroethylene, vinylidene fluoride, etc., and the fluorine-containing (meth)acrylic acid ester may be, for example, trifluoroethyl (meth)acrylate, pentafluoropropyl (meth)acrylate, perfluorocyclohexyl (meth)acrylate, etc.
[0017] (Inorganic oxides) The aqueous coating composition of the present invention contains an inorganic oxide. The inorganic oxide has ultraviolet absorbing properties and preferably contains at least one metal component selected from the group consisting of Ti, Zn and Ce, and more preferably contains at least one selected from the group consisting of titanium oxide, zinc oxide, cerium oxide and a complex thereof. Moreover, from the viewpoint of transparency, titanium oxide, zinc oxide or a complex thereof is even more preferable. From the viewpoint of satisfying both dispersion stability and transparency in a well-balanced manner, the average particle diameter of the primary particles of the inorganic oxide is preferably in the range of 1 to 200 nm, preferably 5 nm or more and 150 nm or less, and more preferably 10 nm or more and 100 nm or less. In the present invention, the "average particle diameter of the primary particles of the inorganic oxide" is a value obtained by observing with a transmission electron microscope, randomly selecting 50 particles, measuring their particle diameters, and averaging them. In the water-based paint composition, if the average particle diameter of the inorganic oxide particles exceeds 200 nm, the transparency decreases. Also, if the average particle diameter of the primary particles is less than 1 nm, the dispersion stability decreases. Also, the content of the inorganic oxide contained in the water-based paint composition is preferably 1 mass % or more and 35 mass % or less, and preferably 2 mass % or more and 25 mass % or less. If it is less than 1 mass %, it is an insufficient amount to exhibit the action as an ultraviolet absorber, and if it exceeds 35 mass %, the long-term dispersion stability in the water-based paint composition is likely to decrease. The content of inorganic oxide relative to the non-volatile content (in the coating film) of the aqueous coating composition is preferably 5% by mass or more and 40% by mass or less, preferably 10% by mass or more and 35% by mass or less, and more preferably 12% by mass or more and 30% by mass or less. If the content is less than 5% by mass, the function as an ultraviolet absorbing agent is insufficient, and if it exceeds 40% by mass, the amount of eluted metal components increases and the transparency of the coating film decreases.
[0018] Furthermore, the inorganic oxide in the aqueous coating composition of the present invention is preferably inorganic fine particles whose surfaces are coated with a hydrophobic coating film using a reactive surface treatment agent. The surface hydrophobic coating film can be at least one selected from, for example, hydrogen dimethicone, fluoroalkyl silane, alkoxy silane, silane coupling agent, and organosilicon compounds such as organopolysiloxane.
[0019] (Dispersant) The aqueous coating composition of the present invention contains a dispersant for dispersing inorganic oxides. The dispersant preferably has an absolute value of the difference between the acid value and the amine value (acid value-amine value) of 35 or less, and a total value of the acid value and the amine value (acid value+amine value) of 120 or less. If the absolute value of the difference between the acid value and the amine value (acid value-amine value) and the total value of the acid value and the amine value (acid value+amine value) are within the above ranges, not only is the dispersion stability of the inorganic oxide excellent, but the inorganic oxide is also excellent in resistance to elution of metal components in an acidic environment, so that excellent ultraviolet absorption can be maintained for a long period of time. If the absolute value of the difference between the acid value and the amine value exceeds 35, when exposed to an acidic environment after the formation of the coating film, the metal components will elute from the inorganic oxide, resulting in poor acid resistance. Therefore, the absolute value of the difference between the acid value and the amine value is preferably 35 or less, more preferably 15 or less. Furthermore, if the total of the acid value and the amine value exceeds 120, when the coating film is exposed to an acidic environment after formation, metal components are eluted from the inorganic oxide, resulting in poor acid resistance. Therefore, the total of the acid value and the amine value is preferably 120 or less, and more preferably 50 to 110.
[0020] The acid value is defined as the number of mg of KOH required to neutralize free fatty acids contained in 1 g of a sample. The acid value of the dispersant is preferably 100 mg KOH / g or less, more preferably 70 mg KOH / g or less, as the active ingredient (non-volatile content) of the dispersant. If the acid value is 100 mg KOH / g or less, the metal components of the inorganic oxide are less likely to dissolve in an acidic environment. The acid value can be measured in accordance with JIS K0070:1992. The amine value is defined as the amount of perchloric acid and the equivalent amount of potassium hydroxide required to neutralize the total basic nitrogen contained in 1 g of sample. The amine value of the dispersant is preferably 100 mg KOH / g or less, more preferably 70 mg KOH / g or less, as the active ingredient (non-volatile content) of the dispersant. If the amine value is 100 mg KOH / g or less, the metal components of the inorganic oxide are less likely to dissolve in an acidic environment. The amine value can be measured in accordance with JIS K7237:1995.
[0021] Specific examples of the dispersants in the aqueous coating composition of the present invention are BYK185 (non-volatile content 90% by mass or more, acid value 0 mgKOH / g, amine value 17 mgKOH / g (acid value calculated as non-volatile content 0 mgKOH / g, amine value 17 mgKOH / g)), BYK187 (non-volatile content 70% by mass, acid value 35 mgKOH / g, amine value 35 mgKOH / g (acid value calculated as non-volatile content 50 mgKOH / g, amine value 50 mgKOH / g)), BYK190 (non-volatile content 40% by mass, acid value 10 mgKOH / g, amine value 0 mgKOH / g (acid value calculated as non-volatile content 25 mgKOH / g, amine value 0 mgKOH / g)), BYK191 (non-volatile content 98% by mass, acid value 30 mgKOH / g, amine value 20mgKOH / g (acid value 31mgKOH / g converted to non-volatile content, amine value 20mgKOH / g)), BYK192 (non-volatile content 98% or more by mass, acid value 0mgKOH / g, amine value 0mgKOH / g (acid value 0mgKOH / g converted to non-volatile content, amine value 0mgKOH / g)), BYK193 (non-volatile content 40% by mass, acid value 0mgKOH / g, amine value 0mgKOH / g (acid value 0mgKOH / g converted to non-volatile content, amine value 0mgKOH / g)), BYK2012 (non-volatile content 40% by mass, acid value 7mgKOH / g, amine value 7mgKOH / g (acid value 17.5mgKOH / g converted to non-volatile content, amine value 17.5mgKOH / g)), BYK2013 (non-volatile content 98.5% by mass or more, acid value 8 mg KOH / g, amine value 18 mg KOH / g (acid value 8 mg KOH / g converted to non-volatile content, amine value 18 mg KOH / g)), BYK2060 (non-volatile content 95% by mass or more, acid value 5 mg KOH / g, amine value 0 mg KOH / g (acid value 5 mg KOH / g converted to non-volatile content, amine value 0 mg KOH / g)), BYK2061 (non-volatile content 100% by mass, acid value 0 mg KOH / g, amine value 3 mg KOH / g), FLOWRENE G-700DMEA (non-volatile content 70% by mass, acid value 38 mg KOH / g, amine value 38 mg KOH / g (acid value 54 mg KOH / g converted to non-volatile content, amine value 54 mgKOH / g), AJISPER PB821 (non-volatile content 100% by mass, acid value 10 mgKOH / g, amine value 17 mgKOH / g), AJISPER PB822 (non-volatile content 100% by mass, acid value 17 mgKOH / g, amine value 14 mgKOH / g), AJISPER PB824 (non-volatile content 100% by mass, acid value 17 mgKOH / g, amine value 21 mgKOH / g), AJISPER PB881 (non-volatile content 100% by mass, acid value 17 mgKOH / g, amine value 17 mgKOH / g), AJISPER PN411 (non-volatile content 100% by mass, acid value 0 mgKOH / g, amine value 6 mgKOH / g), Dispex Ultra FA4420 (non-volatile content 100% by mass, acid value 22 mg KOH / g, amine value 35 mg KOH / g) and others.
[0022] (Inorganic oxide dispersion) From the viewpoint of achieving a good balance between dispersion stability and transparency, the inorganic oxide dispersion obtained by the dispersion treatment preferably has a volume average particle size of secondary particles in the range of 20 to 200 nm, more preferably 30 to 150 nm. Here, the secondary particles refer to primary particles naturally aggregated by van der Waals forces, etc., and the inorganic oxide exists in the form of secondary particles in the water-based coating composition. In particular, when emphasis is placed on dispersion stability, the volume average particle diameter of the secondary particles is preferably 20 nm or more, and when emphasis is placed on transparency, the volume average particle diameter of the secondary particles is preferably 200 nm or less.
[0023] (others) In addition, the aqueous coating composition of the present invention may contain an organic solvent from the viewpoint of ensuring the film-forming properties of the coating film and improving the drying properties of the coating film. The organic solvent is not particularly limited, and organic solvents commonly used in the coating industry can be used. As the solvent, organic solvents having polarity that can be mixed with water are preferable, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono n-propyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono n-butyl ether, diethylene glycol monoiso-butyl ether, diethylene glycol mono tert-butyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, dipropylene glycol monoisobutyl ether, 3-methyl-3-methoxybutanol, triethylene glycol monobutyl ether, acetone, methyl ethyl ketone, diethyl ketone, etc. In the aqueous coating composition of the present invention, the amount of the organic solvent is preferably 0.1 to 20% by mass, and more preferably 0.5 to 10% by mass. The organic solvent may be used alone or in combination of two or more kinds.
[0024] (Amount of metal components dissolved) In the present invention, the aqueous coating composition of the present invention is applied to a substrate, and then dried to form a coating film having a dry thickness of 15 μm. A test piece is then immersed in a 5 g / L aqueous sulfuric acid solution for 24 hours in accordance with the acid resistance test specified in JIS K5658:2010. When the amount of eluted metal components dissolved from the inorganic oxides contained in the coating film into the aqueous sulfuric acid solution is measured by ICP analysis, the amount of eluted metal components is 15 ppm or less.
[0025] In the present invention, acid resistance refers to the property of resisting deterioration of a coating film caused by acid, and specifically refers to the property of suppressing the elution of inorganic metal components from the inorganic oxide of the ultraviolet absorber contained in the coating film over time when a specific acid resistance test is performed on a coating film obtained from the aqueous coating composition. When the acid resistance is low, the metal components are eluted and the ultraviolet absorption property is reduced. The aqueous coating composition of the present invention has a transmittance of 15% or less at a wavelength of 365 nm when the coating film is applied and dried to a thickness of 15 μm. Here, the measurement wavelength is set to 365 nm and the film thickness is set to 15 μm. The ultraviolet transmittance can be measured by applying the aqueous coating composition to a substrate (translucent material) that transmits ultraviolet rays at a wavelength of 365 nm using a bar coater to a predetermined thickness, forming a film, and then measuring the transmittance of the test piece at a wavelength of 365 nm using an ultraviolet-visible spectrophotometer. Examples of the translucent material that transmits ultraviolet rays at a wavelength of 365 nm include glass and quartz. When a translucent material that transmits ultraviolet rays at a wavelength of 365 nm is used, the "transmittance of the test piece at a wavelength of 365 nm" can be read as the "transmittance of the coating film at a wavelength of 365 nm".
[0026] According to the acid resistance test specified in JIS K5658:2010, after immersion in a 5 g / L aqueous sulfuric acid solution for 24 hours, the amount of metal components dissolved from the inorganic oxide contained in the coating film into the aqueous sulfuric acid solution is measured by ICP analysis, and the amount of metal components dissolved is 15 ppm or less, preferably 10 ppm or less, and more preferably 5 ppm or less. If the amount of metal components dissolved is 15 ppm or less, excellent ultraviolet absorption can be maintained for a long period of time. In order to improve the ultraviolet absorption of the coating film, it is necessary to blend a predetermined amount of ultraviolet absorber, and in the present invention, even if the content of inorganic oxide relative to the non-volatile content (in the coating film) of the water-based coating composition is 5 mass% or more, the amount of metal components dissolved can be suppressed to 15 ppm or less.
[0027] (Other Ingredients) Furthermore, the aqueous coating composition of the present invention can be appropriately blended with other components such as pigments, other resins (including water-soluble resins), organic solvents, surface conditioners, wetting agents, dispersants, emulsifiers, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, color separation inhibitors, viscosity adjusters, rheology control agents, leveling agents, defoamers, drying agents, plasticizers, preservatives, antifungal agents, antibacterial agents, insecticides, antiviral agents, neutralizing agents, radical scavengers, antistatic agents, and conductivity imparting agents, etc., depending on the purpose. It can be prepared by mixing various components appropriately selected as necessary.
[0028] (Neutralizer) The neutralizing agent is preferably used so that the pH of the aqueous coating composition is 7 to 10. Examples of the neutralizing agent include alkaline compounds. The neutralizing agents may be used alone or in combination of two or more. Examples of alkaline inorganic compounds that can be used as neutralizing agents include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal hydrogen carbonates such as sodium hydrogen carbonate, alkali metal carbonates such as sodium carbonate, and ammonia. Examples of the alkaline organic compound include amine compounds, specifically amine compounds capable of forming an ion pair with an acid group, such as primary amines such as methylamine, ethylamine, propylamine, isopropylamine, butylamine, t-butylamine, hexylamine, benzylamine, ethanolamine, isopropanolamine, butanolamine, hexanolamine, 1,2-propanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,6-hexanediamine, pyrrolidine, and morpholine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, diethanolamine, diisopropanolamine, N-methylethanolamine, N-ethylethanolamine, N-butylethanolamine, N-butylisopropanolamine, Nt-butylisopropanolamine, N,N-diethylethylenediamine, N,N-dimethyl-1,3-diaminopropane, N,N-diethyl ... Examples of the amines include secondary amines such as minopropane and piperazine, and tertiary amines such as trimethylamine, triethylamine, tripropylamine, triisopropylamine, tributylamine, N-methyldiethylamine, N,N-dimethylpropylamine, triethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, N-butyldiethanolamine, Nt-butyldiethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, N,N-di-t-butylethanolamine, triisopropanolamine, N-methyldiisopropanolamine, N-ethyldiisopropanolamine, N-butyldiisopropanolamine, Nt-butyldiisopropanolamine, N,N-dimethylisopropanolamine, N,N-diethylisopropanolamine, N,N-dibutylisopropanolamine and N,N-di-t-butylisopropanolamine.
[0029] (Radical scavenger) It is preferable to include a radical scavenger from the viewpoint of improving the light stability of the coating film. Also, a substance (so-called polymerization inhibitor) that reacts with free radicals and has a function of preventing a polymerization reaction from occurring is included in the radical scavenger. The use of a radical scavenger is also preferable from the viewpoint of preventing the occurrence of cracks. Examples of the radical scavenger include hindered amine compounds, hydroquinone compounds, phenol compounds, phenothiazine compounds, nitroso compounds, and N-oxyl compounds, and particularly preferred are hindered amine light stabilizers (HALS).
[0030] (Thickener) In the aqueous coating composition of the present invention, from the viewpoint of coating workability, particularly workability during thick film coating, it is preferable to use a thickener as another additive, and a thickener that is commonly used in the coating industry can be used. Examples of thickeners include fatty acid amides, polyethylene, fatty acid esters, polyurethanes, modified ureas, castor oil derivatives, organically modified clay minerals such as organic bentonite and organically modified sepiolite, and hydrophilic silica. Among these, thickeners selected from the group consisting of polyurethanes and modified urethanes are preferred. This can further improve the dripping-off property and storage stability. In the aqueous coating composition of the present invention, the thickener may be used alone or in combination of two or more.
[0031] (Paint film) In addition, one aspect of the present invention is a coating film having a clear layer formed from the above-mentioned aqueous coating composition. The coating film of the present invention will be described in detail below, but is not limited thereto. The coating film of the present invention forms a clear layer using the aqueous coating composition of the present invention. This clear layer suppresses deterioration of the coating film due to deterioration of the pigment in the design layer caused by ultraviolet rays.
[0032] (base material) The substrate is not particularly limited, and examples thereof include metal substrates containing at least a metal or alloy such as steel, galvanized steel (e.g., galvanized iron sheet), tin-plated steel (e.g., tin plate), stainless steel, magnesium alloy, aluminum, aluminum alloy, etc., wood substrates such as wood, inorganic substrates such as gypsum, calcium silicate, glass, ceramic, concrete, cement, mortar, slate, etc., and plastic substrates such as acrylic resin, polyvinyl chloride, polycarbonate, ABS resin, polyethylene terephthalate, polyolefin, etc. In addition, composite substrates such as wood fiber reinforced cement board, fiber reinforced cement board, fiber reinforced cement-calcium silicate board, etc. can also be exemplified. The metal substrate also includes substrates that have been subjected to various surface treatments, for example, oxidation treatment. In addition, plastic substrates whose surfaces are coated with inorganic substances (e.g., plastic substrates coated with glass) are included in inorganic substrates. The substrate may be subjected to a primer treatment, or an old coating film (a coating film already formed when painting) may be present on at least a part of the substrate surface. In addition, the present invention can be applied even if an undercoat film is present on at least a part of the substrate surface.
[0033] (Sealer layer) The substrate may be subjected to a primer treatment, or a sealer layer may be provided. The sealer layer may be used by mixing with other resins. As the resin to be mixed, a resin that is usually used is used. For example, acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, etc. may be mentioned. These resins may be used alone or in combination of two or more. In particular, the use of an acrylic resin such as a styrene acrylic copolymer resin can further improve the storage stability as a coating performance, and the coating appearance, water resistance, and solvent resistance as a coating film performance.
[0034] (Design layer) As the material for forming the design layer, a paint for forming a design layer that is normally used can be used, and a water-based paint can be preferably used. Alternatively, instead of the paint for forming a design layer, a design film that has been previously made into a sheet can be attached to a substrate using an adhesive or the like to form a design layer. Alternatively, a water-based paint of the present invention can be applied to the surface of a previously made sheet of a design film to create a sheet of "design film / coating film of the present invention", and the sheet can be attached to a substrate using an adhesive or the like so that the coating film of the present invention is on the surface side (the design film is on the substrate side). The paint for forming a design layer can be prepared by blending a colorant such as a glittering pigment, a coloring pigment, or a dye with a binder resin such as a urethane resin or an acrylic resin. Furthermore, the paint for forming a design layer can be blended with pigments that are normally used in the paint industry, such as rust-preventive pigments and extender pigments, as necessary. These pigments may be used alone or in combination of two or more. Specifically, examples of color pigments include inorganic pigments such as carbon black, iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, and phthalocyanine blue; and examples of luster pigments include metal pigments made of scaly foil flakes of aluminum, brass, and the like; and pearlescent pigments made of scaly foil flakes of titanium dioxide-coated mica, basic lead carbonate, and the like. The design layer may also be a thin metal film formed by deposition, sputtering, or foil transfer using aluminum, chromium, gold, silver, copper, or the like.
[0035] (Other layers) In order to impart hydrophilicity or water repellency to the surface of the coating film of the present invention, a water repellent coating layer may be provided.
[0036] (Method of producing aqueous coating composition) The aqueous coating composition of the present invention can be prepared, for example, by mixing a water-dispersible resin, an inorganic oxide, water, and, if necessary, various additives appropriately selected. (Application method) The method for applying the aqueous coating composition of the present invention is not particularly limited, and includes known application methods such as brush, roller, dipping, spin coating, flow coating, roll coating, spray coating, blade coating, and air knife coating. The amount of the aqueous coating composition of the present invention to be applied can be varied depending on the type of substrate to be coated and the intended use.
[0037] (Architectural coating materials) The architectural coating material of the present invention forms a clear layer that absorbs ultraviolet rays using the aqueous coating composition of the present invention, so the design layer does not fade, and the coating film formed on the architectural coating material of the present invention has excellent transparency and weather resistance. The thickness of the coating film formed on the architectural coating material of the present invention is preferably 10 to 50 μm.
[0038] (Applications for architectural coating materials) The architectural coating material of the present invention can be used, for example, as an architectural coating material for structures such as buildings and constructions, as well as vehicles (automobiles, etc.), furniture, building materials, electronic devices (home appliances, etc.), and their parts that have a coating film on their surfaces. EXAMPLES
[0039] The present invention will be described in detail with reference to the following examples, but the present invention is not limited to the examples shown below.
[0040] <1. Preparation of inorganic oxide dispersion> Table 1 shows the acid value (mgKOH / g), amine value (mgKOH / g), (acid value - amine value) (mgKOH / g), and (acid value + amine value) (mgKOH / g) of the dispersant used in preparing the inorganic oxide dispersion.
[0041] [Table 1]
[0042] Details of the dispersants listed in Table 1 are as follows: (1) Dispersant 1: Copolymer with affinity for pigments, product name BYK-191 (manufactured by BYK-Chemie) (2) Dispersant 2: fatty acid methyl ester, trade name Dispex Ultra FA4420 (manufactured by BASF) (3) Dispersant 3: Carboxyl group-containing polymer modified product, trade name BG700DMEA (manufactured by Kyoeisha Chemical Co., Ltd.) (4) Dispersant 4: Controlled polymerization acrylic copolymer, trade name BYK-2012 (manufactured by BYK-Chemie) (5) Dispersant 5: Nonionic copolymer with affinity for pigments, trade name BYK-192 (manufactured by BYK-Chemie) (6) Dispersant 6: Neutral polymer, trade name AJISPER PN411 (manufactured by Ajinomoto Fine-Techno Co., Ltd.) (7) Dispersant 7: Structure-controlled copolymer having a pigment affinity group, product name BYK-2013 (manufactured by BYK-Chemie) (8) Dispersant 8: Copolymer with affinity for pigments, product name BYK-194N (manufactured by BYK-Chemie) (9) Dispersant 9: Alkylolammonium salt of copolymer containing acid group, trade name BYK-180 (manufactured by BYK-Chemie) (10) Dispersant 10: Alkylolammonium salt of high molecular weight polymer, trade name ANT1-TERRA250 (manufactured by Big-Chemie)
[0043] Next, dispersants 1 to 10 listed in Table 1, hydrophobic treated zinc oxide (primary particle size: 25 nm, silicone oil surface treated zinc oxide, product name: MZY-505S, manufactured by Teica Corporation) and water were mixed in advance, and then dispersed using a bead mill to prepare inorganic oxide dispersions 1 to 10. Table 2 shows the compositions of inorganic oxide dispersions 1 to 10.
[0044] [Table 2]
[0045] Next, dispersants 1 to 10 listed in Table 1, hydrophobic treated titanium oxide (primary particle size: 20 nm, Al(OH)3 / stearic acid surface treated titanium oxide, product name: TTO-51(C), manufactured by Ishihara Sangyo Kaisha) and water were mixed in advance and then dispersed in a bead mill to prepare inorganic oxide dispersions 11 to 20. Table 3 shows the compositions of inorganic oxide dispersions 11 to 20.
[0046] [Table 3]
[0047] <2. Preparation of Water-Based Coating Composition> The inorganic oxide dispersions 1 to 10 shown in Table 2 were mixed with an aqueous dispersion of a resin, a radical scavenger, a film-forming aid, other additives, and water, and the mixture was thoroughly stirred with a high-speed stirrer to prepare the aqueous coating compositions of Examples 1 to 21 and Comparative Examples 1 to 9. Tables 4 to 6 show the compositions of the aqueous coating compositions of Examples 1 to 21 and Comparative Examples 1 to 9.
[0048] Table 4 shows Examples 1 to 7 and Comparative Examples 1 to 3 in which a fluororesin emulsion (aqueous resin dispersion 1) was used as the aqueous resin dispersion (A). [Table 4]
[0049] Table 5 shows Examples 8 to 14 and Comparative Examples 4 to 6 in which an acrylic silicone resin emulsion (aqueous resin dispersion 2) was used as the aqueous resin dispersion (A). [Table 5]
[0050] Table 6 shows Examples 15 to 21 and Comparative Examples 7 to 9 in which an acrylic emulsion (aqueous resin dispersion 3) was used as the aqueous resin dispersion (A). [Table 6]
[0051] The inorganic oxide dispersions 11 to 20 shown in Table 3, a fluororesin emulsion (aqueous resin dispersion 1), a radical scavenger, a film-forming aid, other additives, and water were mixed and thoroughly stirred with a high-speed stirrer to prepare the aqueous coating compositions of Examples 22 to 28 and Comparative Examples 10 to 12.
[0052] Table 7 shows the compositions of the aqueous coating compositions of Examples 22-28 and Comparative Examples 10-12. [Table 7]
[0053] Details of the raw materials used are shown below. (1) Resin water dispersion 1: Fluorine resin emulsion, non-volatile content: 50% by mass, product name: Lumiflon FE4300 (manufactured by AGC) (2) Resin aqueous dispersion 2: Acrylic silicone resin emulsion, non-volatile content: 44% by mass, product name: U-DOUBLE EF-002 (manufactured by Nippon Shokubai Co., Ltd.) (3) Resin aqueous dispersion 3: Acrylic emulsion, non-volatile content: 43% by mass, product name: Acryset EX-41 (manufactured by Nippon Shokubai Co., Ltd.) (4) Radical scavenger: hindered amine, non-volatile content: 100%, trade name Tinuvin 292 (manufactured by BASF) (5) Film-forming aid: diethylene glycol monobutyl ether, non-volatile content: 0%, product name: Hisorb DB (manufactured by Toho Chemical Industry Co., Ltd.) (6) Others (neutralizers, thickeners) (7) Water (ion-exchanged water)
[0054] <3. Preparation of coated objects (test pieces) with water-based coating compositions> The aqueous coating compositions of Examples 1 to 28 and Comparative Examples 1 to 12 were applied to a glass plate (50 mm × 50 mm × 1 mm thick) using a bar coater to a dry film thickness of 15 μm, and then dried at 130°C for 3 minutes to prepare test pieces coated with the aqueous coating composition of Examples 1 to 28 and Comparative Examples 1 to 12.
[0055] <4. Evaluation of the properties of water-based paint compositions and test pieces> <4-1: Particle size distribution measurement (dispersibility evaluation)> For the particle size distribution of inorganic oxides in the aqueous coating compositions of Examples 1 to 28 and Comparative Examples 1 to 12, a dynamic light scattering particle size distribution measuring device (product name: NANOTRAC WAVE II, Microtrack Bell Co., Ltd.) was used. The measurement conditions were a measurement time of 60 seconds, a refractive index of sample particles of 1.95 (zinc oxide), 2.55 (titanium oxide anatase type), 2.62 (titanium oxide rutile type), and 2.20 (cerium oxide), a dispersion medium of water, and a refractive index of the dispersion medium of 1.33. The volume particle size distribution of the measurement sample (aqueous dilution of the aqueous coating composition) was measured, and the particle size at which the cumulative volume from the small particle size side in the cumulative volume distribution becomes 50% was calculated as the volume average particle size (nm) of the secondary particles of the inorganic oxide from the measurement results. The measurement was performed three times, and the average value was taken as the volume average particle size (nm) of the secondary particles of the inorganic oxide. Dispersibility was judged according to the following criteria. The results are shown in Tables 8 to 11. The judgement of "◯" or "△" indicates a level at which no practical problems will occur. The judgement of "×" indicates a level at which practical problems will occur and the material cannot be actually used. [Criteria for determining dispersibility] "Good": The volume average particle size of the secondary particles is 30 to 150 nm, and the dispersibility is excellent. "△": The volume average particle size of the secondary particles is more than 150 and 200 nm or less, and dispersibility is within a range that does not cause any practical problem. "X": The volume average particle size of the secondary particles is greater than 200 nm, and therefore the dispersibility is poor.
[0056] <4-2: UV transmittance measurement (UV absorbency evaluation)> The ultraviolet transmittance of the obtained test pieces at a wavelength of 365 nm was measured using a UV3100PC ultraviolet-visible near-infrared analyzer photometer (manufactured by Shimadzu Corporation). The ultraviolet absorbance was evaluated from the measured ultraviolet transmittance. The results are shown in Tables 8 to 11. The evaluation results of "◯" and "△" indicate a level at which no practical problems will occur. The evaluation result of "×" indicates a level at which practical problems will occur and the material cannot be actually used. [Judgment criteria] "Good": UV transmittance is 5% or less. "△": UV transmittance is more than 5% and 15% or less. "X": UV transmittance is greater than 15%.
[0057] <4-3: Measurement of the amount of eluted metal components (acid resistance evaluation)> The obtained test pieces were immersed in a 5 g / L aqueous sulfuric acid solution for 24 hours in accordance with the acid resistance test specified in JIS K5658:2010, and the amount of metal components dissolved from the inorganic oxide contained in the coating film into the aqueous sulfuric acid solution was then measured by ICP analysis (measuring device: ICPE-9820, manufactured by Shimadzu Corporation). The acid resistance of the coating was evaluated from the amount of eluted metal components measured by ICP analysis. The results are shown in Tables 8 to 11. The evaluation results of "Good" and "Good" indicate a level at which no practical problems will occur. The evaluation results of "Poor" indicate a level at which practical problems will occur and the coating cannot be actually used. [Judgment criteria] "Good": The amount of metal components eluted is 5 ppm or less. "△": The amount of eluted metal components is more than 5 ppm and 15 ppm or less. "X": The amount of metal components eluted was more than 15 ppm.
[0058] <4-4: Visible light transmittance (transparency evaluation)> The obtained test pieces were visually evaluated for transparency (visible light transmittance). The results are shown in Tables 8 to 11. The evaluation results of "◯" and "△" indicate a level at which no practical problems occur. The evaluation result of "×" indicates a level at which practical problems occur and the material cannot be actually used. [Judgment criteria] "Good": The base (substrate surface) can be clearly observed. "△": The coating film is slightly cloudy, but the base can be clearly observed. "X": The coating film is cloudy and the base cannot be clearly observed.
[0059] Table 8 shows the evaluation results of Examples 1 to 7 and Comparative Examples 1 to 3. [Table 8]
[0060] Table 9 shows the evaluation results of Examples 8 to 14 and Comparative Examples 4 to 6. [Table 9]
[0061] Table 10 shows the evaluation results of Examples 15 to 21 and Comparative Examples 7 to 9. [Table 10]
[0062] Table 11 shows the evaluation results of Examples 22 to 28 and Comparative Examples 10 to 12. [Table 11]
[0063] From the results shown in Tables 8 to 11, the aqueous coating compositions of Examples 1 to 28 were rated as "good" or "good" in terms of dispersibility, transparency, UV absorption, and acid resistance, and presented no practical problems.
[0064] The aqueous coating compositions of Comparative Examples 1, 4, 7 and 10 had an absolute value of (acid value-amine value) exceeding 35, and therefore were rated as "x" for acid resistance.
[0065] The aqueous coating compositions of Comparative Examples 2, 5, 8 and 11 had an absolute value of (acid value + amine value) exceeding 120, and therefore were rated "x" for dispersibility, transparency and acid resistance.
[0066] The aqueous coating compositions of Comparative Examples 3, 6, 9 and 12 had an (acid value + amine value) of more than 120, and therefore were rated "x" for dispersibility, transparency and acid resistance.
[0067] The results of Examples 1 to 28 and Comparative Examples 1 to 12 demonstrate that the aqueous coating composition of the present invention has excellent dispersibility, transparency, and acid resistance, and has long-term ultraviolet absorption properties, all of which pose no practical problems.
Claims
1. An aqueous coating composition containing a water-dispersible resin and an inorganic oxide, The aqueous coating composition is applied to a substrate, dried to form a coating film having a dry thickness of 15 μm. A test piece is then immersed in a 5 g / L aqueous sulfuric acid solution for 24 hours in accordance with the acid resistance test specified in JIS K 5658:2010. When the amount of eluted metal components dissolved from the inorganic oxides contained in the coating film into the aqueous sulfuric acid solution is measured by ICP analysis, the amount of eluted metal components is 15 ppm or less.
2. 2. The aqueous coating composition according to claim 1, wherein the substrate is made of a light-transmitting material, and the test piece has a transmittance of light with a wavelength of 365 nm of 15% or less.
3. 2. The aqueous coating composition according to claim 1, wherein the content of said inorganic oxide in said coating film is 5% by mass or more and 40% by mass or less.
4. 2. The aqueous coating composition according to claim 1, further comprising a dispersant having an absolute value of the difference between the acid value and the amine value of 35 or less and a sum of the acid value and the amine value of 120 or less.
5. The aqueous coating composition according to claim 1, wherein the inorganic oxide contains at least one metal component selected from the group consisting of Ti, Zn and Ce.
6. 2. The aqueous coating composition according to claim 1, wherein the volume average particle size of the secondary particles of the inorganic oxide is 20 nm or more and 200 nm or less.
7. 2. The aqueous coating composition according to claim 1, wherein the inorganic oxide has a surface coated with a hydrophobic coating.
8. A coating film formed by applying the aqueous coating composition according to any one of claims 1 to 7 onto a substrate and drying it.
9. 8. An architectural coating material comprising a building substrate and a coating film formed by applying the aqueous coating composition according to any one of claims 1 to 7 onto the building substrate and drying the composition.
Citation Information
Patent Citations
Preparation method of water-based clear coating composition containing silicone resin emulsion
JP2019137709A
Coating film repair method and coated product
WO2016088846A1
Paint composition
JP2013159668A
Inorganic clear coating composition and method for forming double-layer coating film by using the same
JP2014009304A
Abrasion-resistant coating composition using inorganic metal oxide
JP2020517754A