Optical laminate and image display device including optical laminate

The optical laminate addresses the challenge of achieving thinness and bending resistance in image display devices by using liquid crystal retardation layers and a robust adhesive layer, ensuring durability under harsh conditions.

JP2024146143APending Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023058874
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing image display devices face challenges in achieving thinness and maintaining bending resistance, particularly under high temperature and high humidity conditions, due to the fragility of retardation layers and adhesive layers used in polarizing plates.

Method used

The optical laminate incorporates a polarizing plate with a first and second retardation layer made of liquid crystal compounds, an adhesive layer with a Martens hardness of 150 N/mm² to 250 N/mm², and a VOC value of 100 ppm or less, or a polymerization rate of 98.5% or more, to enhance bending resistance and durability.

Benefits of technology

The laminate achieves a thin profile with excellent bending resistance, even under high temperature and high humidity environments, by using a combination of liquid crystal alignment solidified layers and a robust adhesive layer that minimizes volatile component generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146143000001_ABST
    Figure 2024146143000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate that is thin and excels in flex resistance.SOLUTION: An optical laminate according to an embodiment of the present invention comprises, in order stated: a polarizing plate including a polarizer; a first retardation layer which is the orientation solidifying layer of a liquid crystal compound; an adhesive layer whose Martens hardness is 150 N / mm2 to 250 N / mm2; a second retardation layer which is the orientation solidifying layer of a liquid crystal compound; and an adhesive layer whose VOC value is 100 ppm or less. In one embodiment, the polymerization rate of the adhesive layer is 98.5% or greater.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate and an image display device including the optical laminate. [Background technology]

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (for example, organic EL display devices and inorganic EL display devices), have rapidly become widespread. In image display devices, a polarizing plate and a retardation plate are typically used. In practice, a retardation layer-attached polarizing plate in which a polarizing plate and a retardation plate are integrated is widely used (for example, Patent Document 1). As the demand for thinner image display devices increases, the demand for thinner retardation layer-attached polarizing plates also increases. In order to make the retardation layer-attached polarizing plate thinner, the retardation layer is being made thinner, and a retardation layer made of a liquid crystal material is being used. Furthermore, as the use of image display devices expands, the demands for image display devices are becoming more diverse. For example, in smartphones, there is a demand for foldable devices. Therefore, there is a strong demand for a retardation layer-attached polarizing plate that can realize such an image display device. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3325560 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide an optical laminate that is thin and has excellent flex resistance. [Means for solving the problem]

[0005] 1. The optical laminate of the embodiment of the present invention comprises a polarizing plate including a polarizer; a first retardation layer which is a layer in which a liquid crystal compound is aligned and solidified; and a liquid crystal layer having a Martens hardness of 150 N / mm 2 ~250N / mm 2 the second retardation layer being a layer for solidifying the alignment of a liquid crystal compound; and a pressure-sensitive adhesive layer having a VOC value of 100 ppm or less, in this order. 2. The optical laminate of another embodiment of the present invention includes a polarizing plate including a polarizer; a first retardation layer which is an alignment-solidified layer of a liquid crystal compound; and a liquid crystal layer having a Martens hardness of 150 N / mm 2 ~250N / mm 2 the second retardation layer being a layer for solidifying the alignment of a liquid crystal compound; and a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more, in this order. 3. In the optical laminate according to 1 or 2 above, the adhesive layer may have a thickness of 0.3 μm to 3 μm. 4. In the optical laminate according to any one of the above 1 to 3, the pressure-sensitive adhesive layer may have a thickness of 10 μm to 100 μm. 5. The optical laminate according to any one of 1 to 4 above may have a total thickness of 180 μm or less. 6. In the optical laminate described in any one of 1 to 5 above, the first retardation layer may have an in-plane retardation Re(550) of 100 nm to 190 nm and satisfy Re(450) / Re(550)<1, and the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer may be 40° to 50°. 7. In the optical laminate described in any one of 1 to 5 above, the first retardation layer has Re(550) of 200 nm to 300 nm, the second retardation layer has Re(550) of 100 nm to 200 nm, the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is 10° to 20°, and the angle between the slow axis of the second retardation layer and the absorption axis of the polarizer is 70° to 80°. 8. In another aspect of the present invention, there is provided an image display device. The image display device according to an embodiment of the present invention comprises the optical laminate according to any one of 1 to 6 above. Effect of the Invention

[0006] According to an embodiment of the present invention, it is possible to provide an optical laminate that is thin and has excellent flex resistance. The optical laminate of the embodiment of the present invention can have excellent flex resistance even in a high-temperature and high-humidity environment. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention.

[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0010] A. Overall configuration of optical laminate FIG. 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. The optical laminate 100 of the illustrated example includes a polarizing plate 10, a first retardation layer 21 which is an alignment solidified layer of a liquid crystal compound (hereinafter also referred to as a liquid crystal alignment solidified layer), an adhesive layer 30, a second retardation layer 22 which is a liquid crystal alignment solidified layer, and a pressure-sensitive adhesive layer 40, in this order. The polarizing plate 10 typically includes a polarizer 11 and protective layers 12 and 13 arranged on both sides of the polarizer 11. In the illustrated example, lamination of the protective layers 12 and 13 with the polarizer 11 and lamination of the polarizing plate 10 with the first retardation layer 21 can each be performed via an adhesive layer (not shown). The adhesive layer may be an adhesive layer formed of any suitable adhesive, or may be an adhesive layer formed of any suitable adhesive. These laminations may be performed directly without an adhesive layer depending on the purpose.

[0011] In the illustrated example, protective layers are laminated on both sides of the polarizer 11, but one of the protective layers (for example, the protective layer 13 disposed on the inner side) may be omitted and a protective layer may be laminated only on one side of the polarizer. The first retardation layer 21 and the second retardation layer 22 are liquid crystal alignment solidified layers, and are laminated via an adhesive layer 30. The adhesive layer 30 is formed by laminating an adhesive composition having a Martens hardness of 150 N / mm 2 ~250N / mm 2The optical laminate 100 is provided with the adhesive layer 40 as the outermost layer, and can be attached to an image display device (substantially, an image display cell). In one embodiment of the present invention, the adhesive layer 40 has a VOC value of 100 ppm or less. In another embodiment of the present invention, the adhesive layer 40 has a polymerization rate of 98.5% or more. For practical purposes, it is preferable that a release liner is temporarily attached to the surface of the adhesive layer 40 until the optical laminate 100 is used. By temporarily attaching the release liner, the adhesive layer is protected until actual use, and the optical laminate can be rolled. In this specification, the "liquid crystal alignment solidified layer" refers to a layer in which liquid crystal compounds are aligned in a predetermined direction within the layer and the alignment state is fixed. The "alignment solidified layer" is a concept that includes an alignment hardened layer obtained by hardening a liquid crystal monomer as described later.

[0012] The retardation layer, which is a liquid crystal alignment solidified layer, can achieve an in-plane retardation equivalent to that of a resin film with a thickness that is significantly thinner than that of a resin film. Therefore, it can contribute to making the optical laminate thinner. On the other hand, since the liquid crystal alignment solidified layer is a brittle layer, a hard adhesive layer that can support the liquid crystal alignment solidified layer is used. Martens hardness is 150 N / mm 2If the adhesive layer having the above properties is used as an adhesive layer for the first retardation layer and the second retardation layer, which are liquid crystal alignment solidified layers, the durability of the retardation layer can be improved. On the other hand, a hard adhesive layer tends to crack easily due to bending stress when bending. The optical laminate of the embodiment of the present invention further includes a pressure-sensitive adhesive layer. By including the pressure-sensitive adhesive layer, the bending resistance can be improved. In addition, in a high-temperature and high-humidity environment (for example, a temperature of 60°C and a humidity of 90% RH), the adhesive layer is easily deteriorated and cracks are more likely to occur, which is a problem. The present inventors have found that one cause of deterioration of the adhesive layer is volatile components from the pressure-sensitive adhesive layer. Furthermore, they have found that it is difficult to sufficiently block contact between the adhesive layer and the volatile components because the liquid crystal alignment solidified layer is thin. The optical laminate of the embodiment of the present invention uses a pressure-sensitive adhesive layer having a VOC value of 100 ppm or less, or a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more. These pressure-sensitive adhesive layers not only improve the bending resistance of the adhesive layer, but also suppress the generation of volatile components from the pressure-sensitive adhesive layer even when the optical laminate is placed in a high-temperature and high-humidity environment. Martens hardness is 150N / mm 2 ~250N / mm 2 The optical laminate of the embodiment of the present invention, which uses a combination of an adhesive layer having a VOC value of 100 ppm or less, or a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more, is not only thin and has excellent bending resistance, but also has excellent bending resistance in high-temperature and high-humidity environments.

[0013] The total thickness of the optical laminate is 180 μm or less, preferably 50 μm to 170 μm, more preferably 70 μm to 160 μm, and further preferably 90 μm to 155 μm. In this specification, the total thickness of the optical laminate refers to the sum of the thicknesses of the polarizing plate, the first retardation layer, the second retardation layer, the adhesive layer, and the adhesive layer for laminating these (i.e., the total thickness of the optical laminate does not include the thickness of the pressure-sensitive adhesive layer 40 provided as the outermost layer and the thickness of the release liner that may be temporarily attached to the surface of the pressure-sensitive adhesive layer).

[0014] The components of the optical laminate will be described in more detail below.

[0015] B. Polarizing plate B-1.Polarizer A polarizer is typically composed of a resin film containing a dichroic material (typically, iodine). As the resin film, any appropriate resin film that can be used as a polarizer can be adopted. The resin film is typically a polyvinyl alcohol resin (hereinafter, referred to as "PVA resin") film. The resin film may be a single-layer resin film or a laminate of two or more layers.

[0016] A specific example of a polarizer composed of a single-layer resin film is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based resin film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, not only can dirt and antiblocking agents on the surface of the PVA-based resin film be washed off, but also the PVA-based resin film can be swelled to prevent uneven dyeing.

[0017] Specific examples of polarizers obtained using a laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. At the same time, by increasing the orientation of the PVA in advance, problems such as a decrease in the orientation or dissolution of the PVA when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and the decrease in the orientation of the polyvinyl alcohol molecules can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment process in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction by the drying shrinkage treatment.The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP-A-2012-73580 (Patent No. 5414738) and Japanese Patent No. 6470455. The entire disclosures of these publications are incorporated herein by reference.

[0018] The thickness of the polarizer is preferably 1 μm to 25 μm, more preferably 1 μm to 15 μm, even more preferably 1 μm to 10 μm, still more preferably 1 μm to 8 μm, and particularly preferably 2 μm to 5 μm. In one embodiment, the thickness of the polarizer is 8 μm or less. In an embodiment of the present invention, even when a polarizer having the above thickness is used, it is possible to provide an optical laminate that is thin and has excellent bending resistance.

[0019] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, more preferably 41% to 46%. The degree of polarization P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more. The single transmittance is typically a Y value measured using an ultraviolet-visible spectrophotometer and subjected to luminosity correction. The degree of polarization is typically calculated by the following formula based on the parallel transmittance Tp and crossed transmittance Tc measured using an ultraviolet-visible spectrophotometer and subjected to luminosity correction. Degree of polarization (%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0020] B-2.Protective layer The protective layer is formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0021] The optical laminate is typically placed on the viewing side of an image display device, and the protective layer 12 is typically placed on the viewing side. Therefore, the protective layer (outer protective layer) may be subjected to surface treatment such as hard coat treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment, as necessary.

[0022] The thickness of the protective layer is preferably 40 μm or less, more preferably 10 μm to 40 μm, and further preferably 10 μm to 30 μm. When a surface treatment is applied, the thickness of the outer protective layer (protective layer 12) includes the thickness of the surface treatment layer.

[0023] C. Retardation layer As described above, the first retardation layer and the second retardation layer are layers in which the liquid crystal compound is oriented and solidified. By using a liquid crystal compound, it is possible to realize an in-plane retardation equivalent to that of a resin film with a thickness that is much thinner than that of a resin film. Since the retardation layer, which is an orientation of a liquid crystal compound, is thin and brittle, problems with bending resistance may occur. Furthermore, volatile components from the pressure-sensitive adhesive layer are likely to reach the adhesive layer, and cracking of the adhesive layer in a high-temperature and high-humidity environment may become a problem. As described above, in the optical laminate of the embodiment of the present invention, a pressure-sensitive adhesive layer having a VOC of 100 ppm or less or a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more is used as the pressure-sensitive adhesive layer. Martens hardness of 150 N / mm 2 ~250N / mm 2 An optical laminate comprising an adhesive layer having a VOC value of 100 ppm or less, or a pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more, is not only thin and has excellent bending resistance, but also has excellent bending resistance in a high-temperature and high-humidity environment.

[0024] The retardation layer typically has a circular polarization function or an elliptically polarizing function. In one embodiment, the first retardation layer preferably has Re(550) of 100 nm to 190 nm, satisfies the relationship of Re(450) / Re(550)<1, and the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50°. In this embodiment, the second retardation layer preferably has a refractive index characteristic of nz>nx=ny (hereinafter also referred to as embodiment 1). In another embodiment of the present invention, the Re(550) of the first retardation layer is 200 nm to 300 nm, and the Re(550) of the second retardation layer is 100 nm to 200 nm. In addition, the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is 10° to 20°, and the angle between the slow axis of the second retardation layer and the absorption axis of the polarizer is 70° to 80° (hereinafter also referred to as embodiment 2).

[0025] C-1.Embodiment 1 As described above, in the first embodiment, the first retardation layer preferably has Re(550) of 100 nm to 190 nm, satisfies Re(450) / Re(550)<1, and the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50°. In this embodiment, the second retardation layer preferably has a refractive index characteristic that satisfies the relationship nz>nx=ny.

[0026] C-1-1. First retardation layer In this embodiment, the first retardation layer can function as a λ / 4 plate. The in-plane retardation Re(550) of the first retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and further preferably 130 nm to 160 nm.

[0027] The Nz coefficient of the first retardation layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3. If such a relationship is satisfied, when the obtained optical laminate is used in an image display device, an extremely excellent reflection hue can be achieved.

[0028] The thickness of the first retardation layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 7 μm, and further preferably 1 μm to 5 μm.

[0029] The first retardation layer may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes according to the wavelength of the measurement light. In one embodiment, the first retardation layer preferably exhibits an inverse dispersion wavelength characteristic. In this case, Re(550) / Re(650) is preferably greater than 1, more preferably greater than 1 and 1.2 or less, and further preferably 1.01 to 1.15. In addition, Re(450) / Re(550) of the first retardation layer is preferably less than 1, more preferably 0.8 or more and less than 1, and further preferably 0.8 or more and 0.95 or less. With such a configuration, it is possible to realize very excellent antireflection characteristics. With such a configuration, it is possible to realize very excellent antireflection characteristics.

[0030] In this embodiment, the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and further preferably about 45°. If the angle is within this range and the first retardation layer is a λ / 4 plate as described above, an optical laminate having excellent circular polarization properties (resulting in excellent antireflection properties) can be obtained.

[0031] As described above, the first retardation layer is preferably an alignment solidified layer of a liquid crystal compound. By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly increased compared to non-liquid crystal materials, so the thickness of the retardation layer to obtain a desired in-plane retardation can be significantly reduced. As a result, the optical laminate can be further thinned.

[0032] C-1-2. Second retardation layer As described above, the second retardation layer may be a so-called positive C plate whose refractive index characteristics show the relationship nz>nx=ny. If a positive C plate is used as the second retardation layer, it is possible to effectively prevent reflection in an oblique direction, and the anti-reflection function can be made to have a wide viewing angle. In this case, the thickness direction retardation Rth(550) of the second retardation layer is preferably -50 nm to -300 nm, more preferably -70 nm to -250 nm, further preferably -90 nm to -200 nm, and particularly preferably -100 nm to -180 nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. That is, the in-plane retardation Re(550) of another retardation layer may be less than 10 nm.

[0033] The second retardation layer having a refractive index characteristic of nz>nx=ny may be formed of any appropriate material. The second retardation layer is preferably made of a film containing a liquid crystal material fixed in a homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method of forming the retardation layer include the liquid crystal compound and the method of forming the retardation layer described in

[0020] to

[0028] of JP-A-2002-333642. In this case, the thickness of the second retardation layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.

[0034] C-2. Second embodiment In the second embodiment, the first retardation layer preferably has Re(550) of 200 nm to 300 nm, and the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is 10° to 20°. The second retardation layer preferably has Re(550) of 100 nm to 200 nm, and the angle between the slow axis of the second retardation layer and the absorption axis of the polarizer is 70° to 80°. In this embodiment, either the first retardation layer or the second retardation layer can function as a λ / 4 plate, and the other can function as a λ / 2 plate. For example, when the first retardation layer functions as a λ / 2 plate and the second retardation layer functions as a λ / 4 plate, the Re(550) of the first retardation layer is preferably 200 nm to 300 nm, more preferably 200 nm to 270 nm, even more preferably 210 nm to 260 nm, and particularly preferably 230 nm to 260 nm. The Re(550) of the second retardation layer is preferably 100 nm to 200 nm, more preferably 100 nm to 170 nm, even more preferably 110 nm to 150 nm, and particularly preferably 110 nm to 130 nm.

[0035] The thickness of the first retardation layer can be adjusted, for example, to obtain a desired in-plane retardation of the λ / 2 plate. The thickness of the first retardation layer is, for example, 2.0 μm to 4.0 μm. The thickness of the second retardation layer can be adjusted, for example, to obtain a desired in-plane retardation of the λ / 4 plate. The thickness of the second retardation layer is, for example, 0.5 μm to 2.5 μm.

[0036] In this embodiment, the angle formed between the slow axis of the first retardation layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and even more preferably 12° to 16°. Also, the angle formed between the slow axis of the second retardation layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and even more preferably 72° to 76°. In this embodiment, the first retardation layer and the second retardation layer may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light.

[0037] In the first retardation layer and the second retardation layer, at least one of them typically exhibits a refractive index characteristic showing a relationship of nx > ny = nz. Note that "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny > nz or ny < nz may occur. The Nz coefficient of the retardation layer is preferably 0.9 to 1.5, more preferably 0.9 to 1.3.

[0038] Although the case where the first retardation layer functions as a λ / 2 plate and the second retardation layer functions as a λ / 4 plate has been described, the first retardation layer may function as a λ / 4 plate and the second retardation layer may function as a λ / 2 plate. Also, the angle formed between the slow axis of the first retardation layer and the absorption axis of the polarizer may be about 75°, and the angle formed between the slow axis of the second retardation layer and the absorption axis of the polarizer may be about 15°.

[0039] D. Adhesive layer As described above, the adhesive layer has a Martens hardness of 150 N / mm 2 ~250 N / mm 2 That is, the adhesive layer used in the embodiment of the present invention has a Martens hardness of 150 N / mm 2 ~250 N / mm 2An adhesive composition having the above structure may be used. As described above, an adhesive layer formed using an adhesive composition having high hardness is prone to cracking due to bending stress. The optical laminate of the embodiment of the present invention includes an adhesive layer having a VOC value of 100 ppm or less, or an adhesive layer having a polymerization rate of 98.5% or more as the adhesive layer. If such an adhesive layer is included, the generation of volatile components from the adhesive layer can be suppressed, and an optical laminate having excellent bending resistance even in a high-temperature and high-humidity environment can be obtained.

[0040] The Martens hardness of the adhesive layer (more specifically, the adhesive composition forming the adhesive layer) is 150 N / mm 2 ~250N / mm 2 and more preferably 155 N / mm 2 ~240N / mm 2 and more preferably 160 N / mm 2 ~230N / mm 2 and particularly preferably 160 N / mm 2 ~220N / mm 2 If the Martens hardness of the adhesive layer is within the above range, the impact resistance can be excellent. On the other hand, the occurrence of cracks due to bending stress during bending can be significant. The optical laminate according to the embodiment of the present invention can provide an optical laminate having excellent bending resistance even in a high temperature and high humidity environment. In the present specification, the Martens hardness can be measured by the following method. <Martens hardness> The adhesive that forms the adhesive layer is applied to glass using a bar coater, and sandwiched between two pieces of glass via a spacer with a thickness of 1 μm. The adhesive is then cured by irradiating it with UV light using a UV light irradiator, forming a single adhesive layer with a thickness of 1 μm between the pieces of glass, which is used as the analysis sample. The obtained analysis sample is fixed to a support, one side of the glass is removed, and nanoindentation measurement is performed under the following conditions. Measurement device: Nanoindentation (ELIONIX, product name "ENT-NEXUS") Indenter used: Berkovich (triangular pyramid) Measurement method: Single indentation measurement Measurement temperature: room temperature (25℃) Pressing load: 500μN Push-in / pull-out time: 10 seconds Maximum load holding time: 1 second

[0041] The thickness of the adhesive layer is preferably 0.3 μm to 3 μm, more preferably 0.5 μm to 2.5 μm, and further preferably 0.7 μm to 2 μm. If the thickness of the adhesive layer is within the above range, the first retardation layer and the second retardation layer can be appropriately adhered to each other. According to the embodiment of the present invention, even if the thickness of the adhesive layer is within the above range, an optical laminate having excellent bending resistance can be provided.

[0042] The adhesive layer may have the above Martens hardness, and any suitable adhesive may be used. For example, an active energy ray curable adhesive may be used. As the active energy ray curable adhesive, any suitable active energy ray curable adhesive may be used, and examples of such adhesives include ultraviolet ray curable adhesives and electron beam curable adhesives.

[0043] The active energy ray curable adhesive typically contains a monofunctional component, a polyfunctional component (curing component), and a photopolymerization initiator. The monofunctional component and the polyfunctional component are typically radical polymerizable compounds. Preferred monofunctional components include, for example, higher alkyl esters of (meth)acrylic acid and modified products thereof. Specific examples include isostearyl acrylate, lauryl acrylate, acryloylmorpholine, unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone, and the like. Preferred polyfunctional components include, for example, monomers and / or oligomers having two or more functional groups such as (meth)acrylate groups and (meth)acrylamide groups. Specific examples include polyethylene glycol diacrylate, trimethylpropane triacrylate, and glycerin triacrylate. Specific examples of monofunctional or polyfunctional components other than those mentioned above include tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, phenoxydiethylene glycol acrylate, cyclic trimethylolpropane formal acrylate, dioxane glycol diacrylate, EO-modified diglycerin tetraacrylate, γ-butyrolactone acrylate, N-methylpyrrolidone, hydroxyethyl acrylamide, N-methylol acrylamide, N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide, and 9-vinyl carbazole. In one embodiment, the monofunctional or polyfunctional component has a ring structure. Specific examples include acryloylmorpholine, γ-butyrolactone acrylate, unsaturated fatty acid hydroxyalkyl ester-modified ε-caprolactone, N-methylpyrrolidone, and 9-vinyl carbazole. The monofunctional or polyfunctional components may each be used alone or in combination of two or more.

[0044] The active energy ray curable adhesive may further contain a cationic polymerizable compound as required. The cationic polymerizable compound may be monofunctional or polyfunctional. Examples of the monofunctional cationic polymerizable compound include p-tert-butylphenyl glycidyl ether and 3-ethyl-3-[(2-ethylhexyl)oxy]oxetane. Examples of the polyfunctional cationic polymerizable compound include 3-ethyl-3-{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane. A silane coupling agent may be used as the cationic polymerizable compound. Examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane.

[0045] The active energy ray curable adhesive may further contain any suitable additive. For example, a plasticizer (e.g., an oligomer component), a crosslinking agent, a diluent, etc. These additives are used in any suitable content depending on the purpose.

[0046] Details of the active energy ray-curable adhesive are described, for example, in JP 2018-017996 A. The disclosure of this publication is incorporated herein by reference.

[0047] E. Adhesive layer In one embodiment of the present invention, the pressure-sensitive adhesive layer has a VOC value of 100 ppm or less. In another embodiment of the present invention, the pressure-sensitive adhesive layer has a polymerization rate of 98.5% or more. Even when these pressure-sensitive adhesive layers are placed in a high-temperature, high-humidity environment (for example, a temperature of 60° C. and a humidity of 90% RH), they can suppress the volatilization of components that deteriorate the adhesive layer from the pressure-sensitive adhesive layer. The deterioration of the adhesive layer due to volatile components from the pressure-sensitive adhesive layer can be suppressed, and as a result, an optical laminate having excellent flex resistance even in a high-temperature, high-humidity environment can be provided.

[0048] The VOC value of the adhesive layer is 100 ppm or less, preferably 95 ppm or less, more preferably 90 ppm or less, still more preferably 85 ppm or less, and particularly preferably 80 ppm or less. The VOC value of the adhesive layer may be 0 ppm. If the VOC value of the adhesive layer is within the above range, the generation of volatile components from the adhesive layer can be suppressed even in a high-temperature and high-humidity environment. In this specification, the VOC value is measured by the following method. <Measurement of VOC value> Cut out the optical laminate into a size of 100 mm × 50 mm to obtain a test piece. Place it on a table with the release liner laminated on the adhesive layer of the test piece facing up, and arrange it so that the sensor part of the VOC monitor (for example, manufactured by Toyo Medic Co., Ltd., product name "ppbRAE3000") is located at a height of 40 mm from the surface on the adhesive layer side of the test piece (the surface after peeling off the release liner). Then, peel off the release liner from the adhesive layer and perform the measurement for 60 seconds. Among the measurements for 60 seconds, take the maximum value as the VOC value.

[0049] The polymerization rate of the adhesive layer is 98.5% or more, more preferably 98.6% or more, still more preferably 99% or more. The polymerization rate of the adhesive layer may be 100%. If the polymerization rate of the adhesive layer is within the above range, the generation of volatile components from the adhesive layer can be suppressed even in a high-temperature and high-humidity environment. The polymerization rate of the adhesive layer can be calculated using the following formula from the weights of the adhesive layer before and after drying the adhesive layer at 130 °C for 3 hours. Weight ratio (%) = Weight of the adhesive layer after drying / Weight of the adhesive layer after drying × 100

[0050] The thickness of the adhesive layer is preferably 10 μm to 100 μm, more preferably 15 μm to 80 μm, and still more preferably 20 μm to 60 μm.

[0051] The adhesive layer may be formed using any suitable adhesive composition as long as the VOC value or weight ratio is within the above range. Specific examples of adhesives constituting the adhesive layer include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, etc., an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more. From the viewpoints of transparency, processability, durability, etc., an acrylic adhesive (acrylic adhesive composition) is preferred.

[0052] The acrylic pressure-sensitive adhesive typically contains a (meth)acrylic polymer as a main component, and the (meth)acrylic polymer may be contained in the pressure-sensitive adhesive composition in an amount of, for example, 50% by weight or more, preferably 70% by weight or more, and more preferably 90% by weight or more of the solid content of the pressure-sensitive adhesive composition.

[0053] The (meth)acrylic polymer contains alkyl (meth)acrylate as a main component as a monomer unit. Here, (meth)acrylate refers to acrylate and / or methacrylate. The alkyl (meth)acrylate may be contained in a proportion of preferably 80% by weight or more, more preferably 90% by weight or more, in the monomer components forming the (meth)acrylic polymer. Examples of the alkyl group of the alkyl (meth)acrylate include linear or branched alkyl groups having 1 to 18 carbon atoms. The average carbon number of the alkyl group is preferably 3 to 9, more preferably 3 to 6.

[0054] The acrylic adhesive may preferably contain a silane coupling agent and / or a crosslinking agent. Examples of the silane coupling agent include an epoxy group-containing silane coupling agent. Examples of the crosslinking agent include an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent. Furthermore, the acrylic adhesive composition may contain an antioxidant and / or a conductive agent. Details of the adhesive layer or the acrylic adhesive composition are described in, for example, JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712 A, and the descriptions in these publications are incorporated herein by reference.

[0055] In one embodiment, the pressure-sensitive adhesive layer is subjected to an annealing treatment. The pressure-sensitive adhesive layer that has been subjected to the annealing treatment can have a reduced ratio of volatile components contained in the pressure-sensitive adhesive layer. Therefore, even if the pressure-sensitive adhesive composition itself contains volatile components, it can be suitably used as the pressure-sensitive adhesive layer of the optical laminate of the embodiment of the present invention. The annealing treatment can be performed under any appropriate conditions so that the pressure-sensitive adhesive layer has the above VOC value and / or weight ratio. For example, the annealing treatment can be performed by placing the pressure-sensitive adhesive layer sandwiched between release liners in an oven. The heating temperature and heating time can be set in any appropriate range depending on the composition and thickness of the pressure-sensitive adhesive composition that forms the pressure-sensitive adhesive layer. The treatment temperature of the annealing treatment is, for example, 100°C to 140°C, preferably 105°C to 135°C, more preferably 110°C to 130°C, and even more preferably 115°C to 125°C. The treatment time for the annealing step is, for example, 1 to 5 minutes, preferably 1.5 to 4.5 minutes, more preferably 2 to 4 minutes, and further preferably 2.5 to 3.5 minutes.

[0056] The storage modulus of the adhesive layer at 23° C. is preferably 0.1×10 5 Pa~1.5×10 5 Pa, more preferably 0.2×10 5 Pa~1.0×10 5 Pa, and more preferably 0.3×105 Pa~0.8×10 5 When the pressure-sensitive adhesive layer has a storage modulus at 23° C. within the above range, an optical laminate that is thin and has excellent flex resistance can be provided. The storage modulus at 23° C. can be measured using a dynamic viscoelasticity measuring device.

[0057] F. Image display device The optical laminate of the embodiment of the present invention can be applied to an image display device. Therefore, the embodiment of the present invention includes an image display device using such an optical laminate. Representative examples of image display devices include liquid crystal displays and electroluminescence (EL) displays (e.g., organic EL displays, inorganic EL displays). The image display device according to the embodiment of the present invention includes the optical laminate on the viewing side. The optical laminate can be laminated so that the polarizing plate is on the viewing side and the adhesive layer is on the image display cell (e.g., liquid crystal cell, organic EL cell, inorganic EL cell) side (so that the polarizer is on the viewing side). EXAMPLES

[0058] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.

[0059] <Production Example 1: Preparation of Adhesive Composition 1> 20 parts by weight of acryloylmorpholine (ACMO) (KJ Chemicals, trade name "ACMO"), 10 parts by weight of FA1DDM (unsaturated fatty acid hydroxyalkyl ester modified epsilon-caprolactone; Daicel, trade name "PLACCEL FA1DDM"), 60 parts by weight of EAF5710 (mixture of fluorene-based acrylate and reactive acrylate; Osaka Gas Chemicals, trade name "Oxol EA-F5710"), 5 parts by weight of UP1190 (acrylic acid-based polymer; Toa Gosei, trade name "ARUFON UP-1190"), Omnirad907 (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one; IGM Three parts by weight of Omnirad907 (manufactured by Nippon Kayaku Co., Ltd.) and two parts by weight of DETX-S (2,4-diethylthioxanthone; manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE DETX-S") were mixed at 25°C for one hour to obtain adhesive composition 1.

[0060] <Production Example 2: Preparation of Adhesive Composition 2> Adhesive composition 2 was obtained in the same manner as in Production Example 1, except that the composition was changed as follows. "Adhesive composition 2": 27.5 parts by weight of ACMO, 17.5 parts by weight of FA1DDM, 45 parts by weight of EAF5710, 5 parts by weight of UP1190, 3 parts by weight of Omnirad907, 2 parts by weight of DETX-S

[0061] <Production Example 3: Preparation of Adhesive Composition 3> Adhesive composition 3 was obtained in the same manner as in Production Example 1, except that the composition was changed as follows. "Adhesive composition 3": 20 parts by weight of HEAA (N-(2-hydroxyethyl)acrylamide; manufactured by KJ Chemicals, trade name "HEAA"), 25 parts by weight of ACMO, 35 parts by weight of 1,9-NDA (1,9-nonanediol diacrylate; manufactured by Kyoeisha Chemical, trade name "Light Acrylate 1,9ND-A"), 15 parts by weight of UG4010 (acrylic acid ester polymer; manufactured by Toagosei, trade name "ARUFON UG-4010"), 4 parts by weight of Omnirad907, and 1 part by weight of Omnirad184 (1-hydroxycyclohexyl phenyl ketone; manufactured by IGM Resins, trade name "Omnirad184").

[0062] <Production Example 4: Preparation of Adhesive Composition 4> Adhesive composition 4 was obtained in the same manner as in Production Example 1, except that the composition was changed as follows. "Adhesive composition 4": 35 parts by weight of ACMO, 25 parts by weight of FA1DDM, 30 parts by weight of EAF5710, 5 parts by weight of UP1190, 3 parts by weight of Omnirad907, 2 parts by weight of DETX-S

[0063] <Production Example 5: Preparation of Adhesive Composition 5> Adhesive composition 5 was obtained in the same manner as in Production Example 1, except that the composition was changed as follows. "Adhesive composition 5": 15 parts by weight of HEAA, 2 parts by weight of M5300 (acrylic acid ester of ω-carboxy-polycaprolactone; manufactured by Toagosei Co., Ltd., trade name "Aronix M-5300"), 30 parts by weight of ACMO, 40 parts by weight of 1,9-NDA, 10 parts by weight of UP1190, 3 parts by weight of Omnirad907, and 2 parts by weight of DETX-S.

[0064] <Production Example 6: Preparation of adhesive layer 1> 1. Preparation of Prepolymer Composition In a flask, 60 parts by weight of n-octyl acrylate (NOAA), 30 parts by weight of butyl acrylate (BA), 8 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 2 parts by weight of N-vinyl-2-pyrrolidone (NVP) were added to a monomer mixture containing 0.05 parts by weight of 2,2-dimethoxy-1,2-diphenyl-1-one (manufactured by IGM Resins, product name "Omnirad651") as a photopolymerization initiator, and 0.05 parts by weight of 1-hydroxy-cyclohexyl-phenyl-ketone (manufactured by IGM Resins, product name "Omnirad184") to obtain a mixture. The obtained mixture was irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a part of the monomer components in the mixture, and a prepolymer composition (containing monomer components that have not undergone a polymerization reaction) with a polymerization rate of about 10% was obtained.

[0065] 2. Preparation of Pressure-Sensitive Adhesive Composition 100 parts by weight of the obtained prepolymer composition, 0.08 parts by weight of a crosslinking agent (dipentaerythritol hexaacrylate (DPHA)), 0.05 parts by weight of a photopolymerization initiator (2,2-dimethoxy-1,2-diphenyl-1-one; manufactured by IGM Resins, product name "Omnirad651"), and 0.3 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-403") were mixed to obtain a pressure-sensitive adhesive composition.

[0066] 3. Formation of adhesive layer The obtained pressure-sensitive adhesive composition was applied onto the release-treated surface of a release liner (manufactured by Mitsubishi Chemical Corporation, product name "Diafoil MRF#38", thickness 38 μm) having a release-treated surface on one side to form a coating film. Next, a release-treated surface of a release liner (manufactured by Mitsubishi Chemical Corporation, product name "Diafoil MRN#38", thickness 38 μm) having a release-treated surface on one side was attached to the side of the coating film on which the release liner was not laminated. Next, ultraviolet light (irradiation source: black light, irradiation intensity: 5 mW / cm2) was applied to the coating film between the release liners. 2 ) to photocure the coating film and form a pressure-sensitive adhesive layer (thickness: 25 μm). Next, the pressure-sensitive adhesive layer sandwiched between the release liners was placed in an oven and annealed at 120° C. for 3 minutes to obtain pressure-sensitive adhesive layer 1.

[0067] <Production Example 7: Preparation of adhesive layer 2> An adhesive layer 2 (thickness: 25 μm) was obtained in the same manner as in Production Example 6, except that the annealing treatment was not carried out.

[0068] <Production Example 8: Preparation of adhesive layer 3> 1. Preparation of Acrylic-Based Polymer A mixture containing 44 parts by weight of 2-ethylhexyl acrylate (2EHA), 43 parts by weight of lauryl acrylate (LA), 6 parts by weight of 4-hydroxybutyl acrylate (4HBA), 7 parts by weight of N-vinyl-2-pyrrolidone (NVP), and 0.015 parts by weight of a photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 184") was polymerized by irradiating ultraviolet light to obtain a prepolymer composition (polymerization rate: about 10%). Note that the prepolymer composition contains monomer components that have not undergone a polymerization reaction.

[0069] 2. Preparation of Pressure-Sensitive Adhesive Composition Next, 100 parts by weight of the prepolymer composition, 0.08 parts by weight of 1,6-hexanediol diacrylate (HDDA), 1 part by weight of an acrylic oligomer, and 0.3 parts by weight of a silane coupling agent (product name "KBM403", manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed together to prepare a photocurable adhesive composition.

[0070] 3. Formation of adhesive layer The obtained pressure-sensitive adhesive composition was applied onto the release-treated surface of a polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Corporation, product name "Diafoil MRF#75", thickness 75 μm) one side of which had been treated for release with silicone, to form a coating film. Next, the release-treated surface of a PET film (manufactured by Mitsubishi Chemical Corporation, product name "Diafoil MRF#75", thickness 75 μm) one side of which had been treated for release with silicone was attached to the coating film on the PET film. Next, ultraviolet light (illumination source: black light, irradiation intensity: 5 mW / cm2) was applied to the coating film. 2 ) to cure the coating film. The thickness of the resulting pressure-sensitive adhesive layer 3 was 50 μm.

[0071] <Production Example 9: Preparation of adhesive layer 4> An adhesive layer 4 (thickness: 50 μm) was obtained in the same manner as in Production Example 6, except that no annealing treatment was performed and the thickness was set to 50 μm.

[0072] [Example 1] 1. Preparation of Polarizer The substrate was a long amorphous isophthalic acid copolymerized polyethylene terephthalate (IPA copolymerized PET) film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of 75° C. One side of the substrate was subjected to a corona treatment, and an aqueous solution containing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (polymerization degree 1200, acetoacetyl-modification degree 4.6%, saponification degree 99.0 mol% or more, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: Gohsefimer Z200) in a ratio of 9:1 was applied to the corona-treated surface and dried at 25° C. to form a PVA-based resin layer with a thickness of 13 μm, and a laminate was produced. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the laminate was immersed in a dyeing solution at 30°C (an aqueous solution containing 7.0 parts by weight of potassium iodide and 1.0 part by weight of solid iodine per 100 parts by weight of water) to dye the laminate so that the transmittance of the resulting polarizer was 42% or more (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 35 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4.0% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. for 3 seconds (cleaning treatment). Next, it was dried in an oven at 60° C. for 60 seconds to obtain a laminate having a PVA-based resin layer (polarizer) with a thickness of 5 μm.

[0073] 2. Preparation of Polarizing Plates An acrylic resin film (thickness 20 μm) having a lactone ring structure was attached as a protective layer to the surface of the polarizer obtained above (the surface opposite to the resin substrate) via a UV-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was 1.0 μm, and the layers were attached using a roller. Then, the adhesive was cured by irradiating the protective layer with UV light.

[0074] 3. Preparation of the first retardation layer 55 parts by weight of the compound represented by formula (I), 25 parts by weight of the compound represented by formula (II), and 20 parts by weight of the compound represented by formula (III) were added to 400 parts by weight of cyclopentanone (CPN), and then heated to 60°C and stirred to dissolve. Then, the solution of the above-mentioned compound was returned to room temperature, and 3 parts by weight of Irgacure 907 (manufactured by BASF Japan Ltd.), 0.2 parts by weight of Megafac F-554 (manufactured by DIC Corporation), and 0.1 parts by weight of p-methoxyphenol (MEHQ) were added to the solution of the above-mentioned compound, and further stirred. The solution after stirring was transparent and uniform. The obtained solution was filtered through a 0.20 μm membrane filter to obtain a polymerizable composition. Also, a polyimide solution for an alignment film was applied to a glass substrate having a thickness of 0.7 mm by spin coating, and a coating film was obtained by drying at 100° C. for 10 minutes and then baking at 200° C. for 60 minutes. The obtained coating film was subjected to a rubbing treatment using a commercially available rubbing device to form an alignment film. Next, the polymerizable composition obtained above was applied to the substrate (substantially the alignment film) by spin coating, and dried at 100° C. for 2 minutes. After the obtained coating film was cooled to room temperature, it was heated with a high-pressure mercury lamp at 30 mW / cm 2The film was irradiated with ultraviolet light at an intensity of 100 nm for 30 seconds to obtain a retardation layer (thickness 3 μm) which is an alignment solidification layer of the liquid crystal compound. The in-plane retardation Re(550) of the retardation layer was 130 nm. The retardation layer also had a Re(450) / Re(550) of 0.851, which showed reverse dispersion wavelength characteristics. The retardation layer can function as a λ / 4 plate. [ka] [ka]

[0075] 4. Preparation of the second retardation layer A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (the numbers 65 and 35 in the formula indicate the mole percent of the monomer unit, and are conveniently represented as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a PET substrate that had been subjected to a vertical alignment treatment using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, thereby forming a retardation layer (thickness 4 μm) exhibiting a refractive index characteristic of nz>nx=ny on the substrate. [ka]

[0076] 5. Fabrication of Optical Laminates The resin substrate was peeled off from the polarizing plate obtained in 2. Next, the first retardation layer was attached to the surface of the polarizer from which the resin substrate was peeled off via an ultraviolet-curing adhesive. At this time, the first retardation layer and the second retardation layer were attached so that the absorption axis of the polarizer and the slow axis of the first retardation layer formed an angle of 45°. Next, the first retardation layer and the second retardation layer were laminated via an adhesive layer (thickness 1 μm) formed using the adhesive composition obtained in Production Example 1, and a retardation layer-attached polarizing plate having a configuration of protective layer (acrylic resin film having a lactone ring structure) / ultraviolet-curing adhesive layer / polarizer / ultraviolet-curing adhesive layer / first retardation layer / adhesive layer (adhesive layer formed with adhesive composition 1) / second retardation layer was obtained. Next, one of the release liners was peeled off from the adhesive layer 1 obtained in Production Example 7, and the surface of the adhesive layer 1 from which the release liner was peeled off was laminated with the surface of the polarizing plate with a retardation layer facing the second retardation layer to obtain an optical laminate.

[0077] [Examples 2 to 4] An optical laminate was obtained in the same manner as in Example 1, except that the adhesive composition forming the adhesive layer and the pressure-sensitive adhesive layer were changed as shown in Table 1.

[0078] (Comparative Examples 1 to 4 and Reference Examples 1 to 6) An optical laminate was obtained in the same manner as in Example 1, except that the adhesive composition forming the adhesive layer and the pressure-sensitive adhesive layer were changed as shown in Table 1.

[0079] [evaluation] The optical laminates obtained in the Examples, Comparative Examples, and Reference Examples, and the adhesive compositions and pressure-sensitive adhesives used therein were subjected to the following evaluations. The results are shown in Table 1. 1. Thickness The thickness of 10 μm or less was measured using an interference film thickness meter (manufactured by Otsuka Electronics, product name "MCPD-3000"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C").

[0080] 2.VOC value The optical laminates obtained in the Examples, Comparative Examples, and Reference Examples were cut into a size of 100 mm x 50 mm to prepare test specimens. The test specimen was placed on a table with the protective layer side facing down and the release liner attached to the adhesive layer facing up, and the sensor part of a portable VOC monitor (manufactured by Toyo Medic Co., Ltd., product name "ppbRAE3000") was positioned at a height of 40 mm from the adhesive layer side surface of the test specimen (the surface of the adhesive layer after the release liner is peeled off). Next, the release liner was peeled off from the adhesive layer, and measurements were performed for 60 seconds. The maximum value of the measurements over 60 seconds was taken as the VOC value.

[0081] 3. Polymerization rate Samples were taken from the pressure-sensitive adhesive layers of the Examples, Comparative Examples, and Reference Examples, and their weights were measured.The samples were then dried at 130°C for 3 hours, and the weights of the samples after drying were measured.The polymerization rate was calculated from the weights of the samples before and after drying using the following formula. Weight rate (%) = weight of sample after drying / weight of sample after drying x 100

[0082] 4. Martens hardness Adhesive compositions 1 to 5 were applied onto glass using a bar coater and sandwiched between two pieces of glass via a spacer having a thickness of 1 μm. Then, UV light was irradiated using a UV light irradiator (visible light (gallium-encapsulated metal halide lamp) irradiation device: manufactured by Fusion UV Systems, Inc., product name "Light HAMMER10", bulb: V bulb, peak irradiance: 1600 mW / cm 2 , cumulative dose 1000 / mJ / cm 2 The adhesive was cured by 380-440 nm wavelength, and a 1 μm thick adhesive layer was formed between the glass plates to obtain an analysis sample. The obtained analysis sample was fixed, one side of the glass plate was removed, and nanoindentation measurements were performed under the following conditions. Measurement device: Nanoindentation (ELIONIX, product name "ENT-NEXUS") Indenter used: Berkovich (triangular pyramid) Measurement method: Single indentation measurement Measurement temperature: room temperature (25℃) Pressing load: 500μN Push-in / pull-out time: 10 seconds Maximum load holding time: 1 second

[0083] 5. Bending test The optical laminates obtained in the Examples, Comparative Examples, and Reference Examples were cut into a length of 100 mm and a width of 30 mm so that the angle between the horizontal direction of the cut optical laminate and the absorption axis of the polarizer was approximately 135°. The release liner was peeled off from the pressure-sensitive adhesive layer of the cut optical laminate, and an acrylic resin film (thickness 20 μm) having a lactone ring structure was bonded to the pressure-sensitive adhesive layer to prepare a test specimen. The vertical center of the prepared test piece was aligned with the center of the bending part of the test piece (the bending line) on two plates of a double-joint clamshell type tabletop durability tester (manufactured by Yuasa System Co., Ltd., product name "DR11MR4-CS"), and the acrylic resin film having a lactone ring structure laminated on the adhesive layer of the test piece was fixed with double-sided tape so that it was on the plate side. The durability tester was placed in an environment of room temperature 60°C and humidity 90% RH, and the bending test was repeated with a curvature radius of 1.5 mm and a folding speed of 30 rpm (30 folding and unfolding operations per minute). After the test, the test piece was observed with an optical microscope (magnification: 10 times) to observe the presence or absence of cracks in the adhesive layer between the first retardation layer and the second retardation layer. If there was no crack or the crack length was less than 100 μm, it was evaluated as no crack, and if the crack length was 100 μm or more, it was evaluated as having a crack.

[0084] [Table 1]

[0085] As is clear from Table 1, the optical laminates of the examples of the present invention had excellent flex resistance even in a high-temperature and high-humidity environment. [Industrial Applicability]

[0086] The optical laminate according to the embodiment of the present invention can be suitably used in image display devices such as liquid crystal display devices, organic EL display devices, and inorganic EL display devices. [Explanation of symbols]

[0087] 10 Polarizing plate 11 Polarizer 12 Protective layer 13 Protective layer 21 First retardation layer 22 Second retardation layer 30 Adhesive layer 40 Adhesive layer 100 Optical laminate

Claims

1. A polarizing plate including a polarizer; A first retardation layer which is a layer in which a liquid crystal compound is aligned and solidified; Martens hardness is 150N / mm 2 ~250N / mm 2 an adhesive layer which is a second retardation layer which is a layer in which a liquid crystal compound is aligned and solidified; and a pressure-sensitive adhesive layer having a VOC value of 100 ppm or less, in this order.

2. A polarizing plate including a polarizer; A first retardation layer which is a layer in which a liquid crystal compound is aligned and fixed; Martens hardness is 150N / mm 2 Up to 250N / mm 2 an adhesive layer which is a second retardation layer which is a layer in which a liquid crystal compound is aligned and solidified; A pressure-sensitive adhesive layer having a polymerization rate of 98.5% or more; and

3. 3. The optical laminate according to claim 1, wherein the adhesive layer has a thickness of 0.3 μm to 3 μm.

4. The optical laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm to 100 μm.

5. The optical laminate according to claim 1 or 2, having a total thickness of 180 μm or less.

6. the first retardation layer has an in-plane retardation Re(550) of 100 nm to 190 nm and satisfies Re(450) / Re(550)<1; 3. The optical laminate according to claim 1, wherein an angle between a slow axis of the first retardation layer and an absorption axis of the polarizer is 40° to 50°.

7. The first retardation layer has an Re(550) of 200 nm to 300 nm, and the second retardation layer has an Re(550) of 100 nm to 200 nm, the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is 10° to 20°; 3. The optical laminate according to claim 1, wherein the angle between the slow axis of the second retardation layer and the absorption axis of the polarizer is 70° to 80°.

8. An image display device comprising the optical laminate according to claim 1 or 2.

Citation Information

Patent Citations

  • Polarizing plate with retardation layers and organic el display device

    JP2019191571A

  • Optical laminate and organic el display device

    JP2020003650A

  • Composite polarizer and method of manufacturing the same

    JP2020194091A

  • Foldable polarizing plate