Flame-retardant polyester resin composition and electronic electromechanical component using the same

The flame-retardant polyester resin composition addresses rigidity and moldability issues by incorporating specific amounts of polyalkylene glycol derivatives and inorganic fibers, ensuring high rigidity, flame retardancy, and stable moldability with improved product appearance.

JP2024146336APending Publication Date: 2024-10-15TOYOBO MC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023059172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Flame-retardant polyester resin compositions face issues with decreased rigidity, moldability, and retention stability due to polymer decomposition caused by the inclusion of flame retardants, particularly when highly filled with inorganic fillers, leading to problems like lower physical properties and deteriorated appearance of molded products.

Method used

A flame-retardant polyester resin composition containing 20-65% thermoplastic polyester, 0.05-1% polyalkylene glycol and/or polyalkylene glycol derivative, 3-20% flame retardant, and 28-55% inorganic fiber, with specific amounts of polyalkylene glycol derivatives and reactive compounds, enhancing rigidity, flame retardancy, and moldability while maintaining retention stability.

Benefits of technology

The composition achieves high rigidity and flame retardancy with improved moldability and retention stability, resulting in excellent appearance of molded products by optimizing the resin's fluidity and reducing the need for extreme molding conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146336000001
    Figure 2024146336000001
  • Figure 2024146336000002
    Figure 2024146336000002
  • Figure 2024146336000003
    Figure 2024146336000003
Patent Text Reader

Abstract

To provide a high rigid flame-retardant polyester resin composition highly filled with an inorganic filler (particularly an inorganic fiber material) in addition to a flame retardant, the composition having good moldability and retention stability and also having excellent appearance of a molded article, in addition to rigidity and flame retardance.SOLUTION: A polyester resin composition includes: 20-65 mass% of thermoplastic polyester (A); 0.05-1 mass% of polyalkylene glycol and / or polyalkylene glycol derivative (B); 3-20 mass% of a flame retardant (C); 28-55 mass% of an inorganic fiber material (D); and 0.05-1 mass% of a reactive compound (E).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flame-retardant polyester resin composition and an electronic / electrical part using the same. In particular, the present invention relates to a flame-retardant polyester resin composition having a high deflection temperature under load, excellent retention stability, and excellent appearance of a molded product, and an electronic / electrical part using the same. [Background technology]

[0002] Polyester resins have excellent mechanical properties, heat resistance, chemical resistance, and the like, and therefore flame-retardant polyester resin compositions prepared by blending polyester resins with flame retardants have been widely used in various parts that require flame retardancy, such as automobile parts, electric and electronic parts, and industrial machine parts.

[0003] In particular, electric and electronic parts, such as the housings of electronic devices, are required to have not only flame retardancy but also rigidity and good molded product appearance (including dimensional stability such as low warpage).

[0004] However, since the inclusion of a flame retardant causes polymer decomposition, resin compositions containing a flame retardant have problems such as a decrease in rigidity, a decrease in the retention stability of the resin in the cylinder of the molding machine during molding, which causes a decrease in physical properties during continuous molding, and a deterioration in the appearance of the molded product (deterioration of surface gloss, dimensional stability, etc.) compared to resin compositions not containing a flame retardant. In particular, resin compositions highly filled with inorganic fillers are more likely to cause polymer decomposition because the cylinder temperature is increased to ensure fluidity during molding. Note that retention stability refers to the thermal stability of a resin that has been retained in the cylinder of a molding machine for a certain period of time, and retention stability decreases if polymer decomposition progresses during retention.

[0005] Prior documents related to the present application include the following Patent Documents 1 and 2. Patent Document 1 relates to a polyester resin composition, and Patent Document 2 relates to a flame-retardant electronic component with excellent dimensional stability. These Patent Documents 1 and 2 disclose a method of improving physical properties by increasing the crystallinity of the resin in a molded product by including a crystallization promoter. However, the resin composition described in Patent Document 1 does not include a flame retardant, and does not take into account the deterioration of physical properties caused by the flame retardant and the effect on retention stability. In addition, the resin composition described in Patent Document 2 includes a flame retardant, and although the improvement of moldability is mentioned, the effect on retention stability is not taken into account. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 4-363356 [Patent Document 2] JP 2001-302895 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to provide a flame-retardant polyester resin composition having high rigidity and containing a high content of an inorganic filler (particularly an inorganic fiber material) in addition to a flame retardant, which has good moldability and retention stability in addition to rigidity and flame retardancy, and also has excellent appearance of molded products. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by incorporating a specific amount of polyalkylene glycol and / or a polyalkylene glycol derivative in a highly rigid flame-retardant polyester resin composition that is highly filled with an inorganic filler (particularly an inorganic fiber material) in addition to a flame retardant, and have thus completed the present invention.

[0009] That is, the present invention relates to the following flame-retardant polyester resin composition and electronic / electrical parts. 1. A flame-retardant polyester resin composition comprising 20 to 65 mass% of a thermoplastic polyester (A), 0.05 to 1 mass% of a polyalkylene glycol and / or a polyalkylene glycol derivative (B), 3 to 20 mass% of a flame retardant (C), 28 to 55 mass% of an inorganic fiber material (D), and 0.05 to 1 mass% of a reactive compound (E). 2. Shear rate 10 s -1 The melt viscosity at is 1×10 3 Pa s~5×10 3 2. The flame-retardant polyester resin composition according to item 1, wherein the flame-retardant polyester resin composition has a viscosity of 1 Pa·s. 3. The flame-retardant polyester resin composition according to item 1 or 2, wherein the thermoplastic polyester (A) is polyethylene terephthalate. 4. The flame-retardant polyester resin composition according to any one of items 1 to 3, wherein the flame retardant (C) is a bromine-based compound (C1), and further contains an antimony compound (C2) as a flame-retardant auxiliary. 5. The flame-retardant polyester resin composition according to any one of items 1 to 4, wherein at least one of the molecular terminals of the polyalkylene glycol derivative is a carboxylate. 6. The flame-retardant polyester resin composition according to any one of items 1 to 5, further comprising 2 mass % or less of talc (F). 7. The flame-retardant polyester resin composition according to any one of items 1 to 6, which has a deflection temperature under load of 225° C. or higher as measured under a load of 1.82 MPa in accordance with ISO 75. 8. An electronic or electrical part comprising a molded article of the flame-retardant polyester resin composition according to any one of items 1 to 7 above. Effect of the Invention

[0010] The polyester resin composition of the present invention achieves a high degree of both rigidity and flame retardancy by being highly filled with an inorganic fiber material in addition to a flame retardant, and by containing a specific amount of polyalkylene glycol and / or a polyalkylene glycol derivative, the composition has good moldability and retention stability and also has excellent appearance of molded products.

[0011] The flame-retardant polyester resin composition of the present invention ensures flowability in the high shear rate range by containing a specific amount of flame retardant. In addition, the resin composition has a significantly improved flowability in the low shear rate range by containing a specific amount of polyalkylene glycol and / or polyalkylene glycol derivative. This allows the temperature of the molding machine cylinder to be set lower than before and molding to be performed under relatively mild molding conditions, resulting in good moldability and retention stability in addition to rigidity and flame retardancy, and excellent appearance of the molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The flame-retardant polyester resin composition of the present invention and electronic / electrical parts using the same will be described in detail below. In this specification, a numerical range indicated by "to" means a range including the numerical values ​​before and after "to" as the lower and upper limits (i.e., "not less than or equal to").

[0013] The flame-retardant polyester resin composition of the present invention is characterized by containing 20 to 65 mass% of a thermoplastic polyester (A), 0.05 to 1 mass% of a polyalkylene glycol and / or a polyalkylene glycol derivative (B), 3 to 20 mass% of a flame retardant (C), 28 to 55 mass% of an inorganic fiber material (D), and 0.05 to 1 mass% of a reactive compound (E).

[0014] The flame-retardant polyester resin composition of the present invention having the above-mentioned characteristics achieves a high degree of both rigidity and flame retardancy by being highly filled with an inorganic fiber material in addition to a flame retardant, and by containing a specific amount of polyalkylene glycol and / or a polyalkylene glycol derivative, the composition has good moldability and retention stability and also has excellent appearance of the molded product.

[0015] Hereinafter, each component constituting the flame-retardant polyester resin composition of the present invention will be described.

[0016] [Thermoplastic polyester (A)] Examples of the thermoplastic polyester (A) include amorphous polyester resins such as amorphous semi-aromatic polyesters and amorphous fully aromatic polyesters; crystalline polyester resins such as crystalline semi-aromatic polyesters and crystalline fully aromatic polyesters; and random copolymers, block copolymers, graft copolymers, etc. of these exemplified polymers. These thermoplastic polyester resins can be used alone or in combination of two or more. When combining two or more resins, a compatibilizer or the like may be added as necessary. The types of these thermoplastic polyesters may be appropriately selected depending on the purpose of the final product (molded body). Among these thermoplastic polyesters, crystalline polyester resins are preferred in the present invention.

[0017] Specific examples of the crystalline polyester resin include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, polybutylene naphthalate, poly1,4-cyclohexylene dimethylene terephthalate, polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate, etc. In addition, crystalline copolymer polyesters such as polyethylene isophthalate / terephthalate, polybutylene terephthalate / isophthalate, polybutylene terephthalate / decane dicarboxylate, and polycyclohexane dimethylene terephthalate / isophthalate, etc. are also included. Among these crystalline polyester resins, polyethylene terephthalate is preferred from the viewpoint of heat resistance.

[0018] Polyethylene terephthalate is basically a homopolymer of ethylene terephthalate units. In addition, other components can be copolymerized up to about 5 mol % within the range that does not impair various properties. Examples of other components include copolymerization components used in copolymerized polyester resins described below.

[0019] Examples of the copolymerized polyester resin include polyester resins containing at least one selected from the group consisting of terephthalic acid, isophthalic acid, sebacic acid, adipic acid, trimellitic acid, 2,6-naphthalenedicarboxylic acid, ethylene glycol, diethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, 1,2-propanediol, 1,3-propanediol, and 2-methyl-1,3-propanediol as a copolymerization component.

[0020] Among these, a copolymer polyester having 50 mol% or more of terephthalic acid as a dicarboxylic acid component and 50 mol% or more of ethylene glycol as a glycol component is more preferable. Here, examples of the acid component other than terephthalic acid include aromatic or aliphatic polybasic acids such as isophthalic acid, naphthalenedicarboxylic acid, adipic acid, sebacic acid, and trimellitic acid, and esters thereof. Examples of the glycol component other than ethylene glycol include diethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, 1,2-propanediol, 1,3-propanediol, and 2-methyl-1,3-propanediol. Among these, isophthalic acid and neopentyl glycol are preferable in terms of availability and characteristics of the final product.

[0021] The molecular weight of the polyethylene terephthalate is not limited, but the intrinsic viscosity (a 0.1 g sample is dissolved in 25 ml of a mixed solvent of phenol / tetrachloroethane (mass ratio 6 / 4) and measured at 30°C using an Ubbelohde viscometer; dl / g) is preferably 0.5 to 1.1 dl / g, and more preferably 0.6 to 1.0 dl / g.

[0022] When the intrinsic viscosity of the polyethylene terephthalate is within the above range, the resin has good rigidity and a molded product with high strength can be easily obtained. In addition, good fluidity of the resin can be easily ensured. The intrinsic viscosity can be adjusted by blending polyethylene terephthalates having different intrinsic viscosities. For example, the intrinsic viscosity can be adjusted to 0.9 dL / g by blending polyethylene terephthalate having an intrinsic viscosity of 1.0 dL / g with polyethylene terephthalate having an intrinsic viscosity of 0.7 dL / g.

[0023] The content of the thermoplastic polyester (A) in the flame-retardant polyester resin composition may be from 20 to 65% by mass, and preferably from 30 to 60% by mass.

[0024] [Polyalkylene glycol and / or polyalkylene glycol derivative (B)] The polyalkylene glycol and / or polyalkylene glycol derivative is not limited to, but may be, for example, the compounds represented by the following formulas (1) and (2).

[0025] [ka]

[0026] [ka]

[0027] In the general formulas (1) and (2), l and m are 0 or 1, n is an integer of 2 to 30, R 1 , R 3 is an aliphatic or aromatic hydrocarbon group having 1 to 7 carbon atoms, provided that when m=0, R 1 R represents a hydrogen atom. 2 is an aliphatic hydrocarbon group having 2 to 6 carbon atoms, R 4 , R 5 is an aliphatic hydrocarbon group having 1 to 7 carbon atoms, provided that when l=0, R 4 indicates a hydrogen atom.

[0028] Examples of the polyalkylene glycol included in the component (B) include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyneopentyl glycol, polyethylene glycol / polypropylene glycol copolymer, and polyethylene glycol / polytetramethylene glycol copolymer.

[0029] Examples of the polyalkylene glycol derivatives included in the component (B) include those in which the molecular terminals (one or both) of the above polyalkylene glycols are esterified with acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, benzoic acid, etc., and the above polyalkylene glycols as methyl ethers, ethyl ethers, butyl ethers, etc. Among these polyalkylene glycol derivatives, particularly preferred are those in which at least one of the molecular terminals is a carboxylate ester.

[0030] The (B) component may be a polyalkylene glycol, a polyalkylene glycol derivative, or a mixture thereof. In the case of a mixture, the mixing ratio of the two is not limited, and any mixing ratio can be used.

[0031] The average molecular weight of the (B) component is not limited, but is preferably not more than 5000, more preferably from 200 to 3000, and even more preferably from 300 to 1500. When the average molecular weight is within the above range, good compatibility and a crystallization promoting effect in the flame-retardant polyester resin composition are easily obtained, and gas generation during molding is easily suppressed.

[0032] The content of the (B) component in the flame-retardant polyester resin composition may be 0.05 to 1 mass%, preferably 0.08 to 0.9 mass%, more preferably 0.1 to 0.8 mass%. In addition, when the (B) component is a mixture of polyalkylene glycol and a polyalkylene glycol derivative, these contents are the total amount of both. If the (B) component is less than 0.05 mass%, it is difficult to obtain flowability in the low shear rate range, and it is difficult to stabilize the surface gloss. If the (B) component is more than 1 mass%, the physical properties (especially the retention stability) of the flame-retardant polyester resin composition are reduced, and there is a problem of dimensional stability, such as the generation of burrs on the molded product during molding. In the present invention, the content of the (B) component is 0.05 to 1 mass%, so that the flowability of the resin composition in the low shear rate range can be significantly improved.

[0033] [Flame retardant (C)] The flame retardant (C) is not limited, but may be any known halogen-based flame retardant, non-halogen-based flame retardant, flame retardant assistant, etc. that can generally impart flame retardancy to a resin composition, and these may be used alone or in combination of two or more. Examples of the flame retardant (C) include triazine compounds and / or derivatives thereof, phosphorus compounds, bromine compounds, antimony compounds, etc.

[0034] The content of the flame retardant (C) in the flame-retardant polyester resin composition may be from 3 to 20% by mass, and within this range, from 5 to 15% by mass is preferred.

[0035] Examples of triazine compounds and / or derivatives thereof include melamine, melamine cyanurate, melamine phosphate, guanidine sulfamate, etc. Among these, melamine cyanurate is preferred. When using a triazine compound and / or derivatives thereof, the content is preferably 5 to 50 parts by weight per 100 parts by weight of the component (A). If the content is less than 5 parts by weight, it is difficult to obtain a flame retardant effect, and if the content exceeds 50 parts by weight, it is not preferred because the physical properties of the final product may be deteriorated.

[0036] The phosphorus-based compound includes organic phosphorus compounds.

[0037] Examples of organic phosphorus compounds include phosphate esters, melamine phosphate, etc. Examples of phosphate esters include phosphates, phosphonates, phosphinates, etc., and more specifically, examples of such phosphate esters include trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, octyl diphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, triphenyl phosphate, trixylenyl phosphate, tris-isopropylphenyl phosphate, diethyl-N,N-bis(2-hydroxyethyl)aminomethylphosphonate, bis(1,3-phenylenediphenyl)phosphate, aromatic condensed phosphate esters, etc. Among these, aromatic condensed phosphate esters such as 1,3-[bis(2,6-dimethylphenoxy)phosphophenyloxy]benzene and 1,4-[bis(2,6-dimethylphenoxy)phosphophenyloxy]benzene are preferred from the viewpoints of hydrolysis resistance, thermal stability, flame retardancy, and the like.

[0038] When a phosphorus-based compound is used, the content is preferably 1 to 20 parts by weight per 100 parts by weight of the component (A). If it is less than 1 part by weight, it is difficult to obtain a flame retardant effect, and if it exceeds 20 parts by weight, it is not preferable because the physical properties of the final product may be deteriorated.

[0039] Examples of the brominated compound (C1) include brominated phenoxy resin, brominated epoxy resin, brominated epoxy oligomer, TBA (tetrabromobisphenol A) carbonate oligomer, ethylene bis (tetrabromophthalic) imide, hexabromobenzene, and decabromodiphenyl ether. Among them, at least one of brominated phenoxy resin and TBA carbonate oligomer is preferred. When using a brominated compound, the content is preferably 5 to 60 parts by weight per 100 parts by weight of the (A) component. If the content is less than 5 parts by weight, it is difficult to obtain a flame retardant effect, and if the content exceeds 60 parts by weight, it is not preferred because the physical properties of the final product may be deteriorated.

[0040] In the present invention, a flame retardant assistant may be used together with the flame retardant (C). Examples of the flame retardant assistant include antimony compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, and sodium pyroantimonate, as well as tin dioxide, zinc metaborate, aluminum hydroxide, magnesium hydroxide, zirconium oxide, molybdenum oxide, red phosphorus compounds, ammonium polyphosphate, melamine cyanurate, and tetrafluoroethylene. Among these, at least one of antimony trioxide and antimony pentoxide is preferable among antimony compounds. Examples of red phosphorus compounds include red phosphorus coated with a resin and a composite compound with aluminum. When a flame retardant assistant is used, the content is preferably 2 to 20 parts by weight relative to 100 parts by weight of the (A) component. If the content is less than 2 parts by weight, there is no flame retardant effect, and if the content exceeds 20 parts by weight, it is not preferable because physical properties may be deteriorated. In the present invention, a preferred embodiment is to use a bromine compound (C1) as the flame retardant (C) in combination with an antimony compound (C2) as the flame retardant assistant.

[0041] [Inorganic fiber materials (D)] The inorganic fiber material (D) is one that most effectively improves physical properties such as strength, rigidity, and heat resistance, and examples thereof include glass fiber, carbon fiber, alumina fiber, silicon carbide fiber, and zirconia fiber. Among these, glass fiber and carbon fiber are preferred. These inorganic fiber materials are preferably surface-treated in advance with a coupling agent such as an organosilane compound, an organotitanium compound, an organoborane compound, or an epoxy compound. When glass fiber surface-treated with a coupling agent is blended, it is preferred because a final product with excellent mechanical properties and appearance properties can be obtained. These inorganic fiber materials (D) can be used alone or in combination of two or more.

[0042] When the inorganic fiber material (D) is glass fiber, chopped strands cut to a fiber length of about 1 to 20 mm can be preferably used. Glass fibers having a circular or noncircular cross section can be used as the cross section of the glass fiber. From the viewpoint of physical properties, glass fibers having a noncircular cross section are preferable as the cross section of the glass fiber. Glass fibers having a noncircular cross section include those having a substantially elliptical, substantially oval, or substantially cocoon-shaped cross section perpendicular to the longitudinal direction of the fiber, and the flatness is preferably 1.5 to 8. The flatness here is the ratio of the major axis to the minor axis when a rectangle having the minimum area circumscribing the cross section perpendicular to the longitudinal direction of the glass fiber is assumed, and the length of the long side of this rectangle is the major axis and the length of the short side is the minor axis. The thickness of the glass fiber is not particularly limited, but the minor axis is about 1 to 20 μm and the major axis is about 2 to 100 μm.

[0043] The fiber length (number average fiber length) of the glass fiber in the flame-retardant polyester resin composition of the present invention is preferably 140 to 700 μm, more preferably 180 to 400 μm. The glass fiber length in this range provides high strength, high rigidity, and stable flowability. If the glass fiber length is outside the above range, it becomes difficult to orient and fill the polyester resin surface, and the fiber end faces are exposed on the surface, which may reduce the abrasion resistance of the molded product.

[0044] The glass fiber is preferably treated with a coupling agent such as a silane or titanate, and is particularly preferably treated with a silane coupling agent. Here, examples of the silane coupling agent include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, and γ-mercaptopropyltrimethoxysilane. Among these, γ-glycidoxypropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane are particularly preferred.

[0045] The amount of inorganic fiber material (D) in the polyester resin composition may be 28 to 55% by mass, and is preferably 30 to 53% by mass, more preferably 33 to 50% by mass, and even more preferably 35 to 48% by mass. If the amount exceeds 55% by mass, the productivity decreases, and if it is less than 28% by mass, the reinforcing effect of the inorganic fiber material may not be fully exhibited.

[0046] The flame-retardant polyester resin composition of the present invention can be used in combination with an inorganic filler other than the inorganic fiber material (D). In addition to the reinforcing filler, a conductive filler, a magnetic filler, a flame-retardant filler, or a thermally conductive filler can be used for different purposes. Specific examples include glass beads, glass flakes, glass balloons, silica, talc, kaolin, wollastonite, mica, alumina, hydrotalcite, montmorillonite, hydroxyapatite, graphite, carbon nanotubes, fullerene, zinc oxide, indium oxide, tin oxide, iron oxide, titanium oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, red phosphorus, calcium carbonate, potassium titanate, lead zirconate titanate, barium titanate, aluminum nitride, boron nitride, zinc borate, aluminum borate, barium sulfate, magnesium sulfate, zinc sulfide, iron, aluminum, copper, and silver. These inorganic fillers can be used alone or in combination of two or more. The shape is not particularly limited, and shapes other than fibrous shapes such as needle-like, spherical, plate-like, amorphous, etc. The content of the inorganic filler other than these inorganic fiber materials (D) can be appropriately set so as to meet the above-mentioned purposes.

[0047] [Reactive compound (E)] The reactive compound (E) is a compound having a functional group capable of reacting with a hydroxyl group or a carboxyl group of the thermoplastic polyester (A), and the reactive functional group is preferably at least one selected from the group consisting of an epoxy group (glycidyl group), an acid anhydride group, a carbodiimide group, and an isocyanate group, and the functional group is contained in one molecule at least two times. The functional group is more preferably an epoxy group (glycidyl group).

[0048] When the reactive compound (E) is a compound having an epoxy group, a polyfunctional epoxy compound having two or more epoxy groups can be mentioned. Specifically, polyethylene glycol diglycidyl ether, 1,6-dihydroxynaphthalene diglycidyl ether, 1,3-bis(oxiranylmethoxy)benzene, 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, diglycerol triglycidyl ether, 1-chloro-2,3-epoxypropane-formaldehyde-2,7-naphthalenediol polycondensate, and pentaerythritol polyglycidyl ether, each having four epoxy groups, are mentioned. Among these, a polyfunctional epoxy compound having heat resistance in the skeleton is preferable. In particular, a bifunctional or tetrafunctional epoxy compound having a naphthalene structure in the skeleton, or a trifunctional epoxy compound having a triazine structure in the skeleton is preferable. Considering the degree of increase in the solution viscosity of the thermoplastic polyester (A), the effect of efficiently reducing the acid value of the thermoplastic polyester (A), and the degree of gelation due to aggregation and solidification of the epoxy itself, a difunctional or trifunctional epoxy compound is preferred.

[0049] Other examples include copolymers containing two or more glycidyl groups per molecule, having a weight average molecular weight of 4,000 to 25,000, and comprising (X) 20 to 99% by mass of a vinyl aromatic monomer, (Y) 1 to 80% by mass of glycidyl (meth)acrylate, and (Z) 0 to 79% by mass of a vinyl group-containing monomer other than (X) that does not contain an epoxy group.

[0050] The reactive compound (E) used in the present invention is preferably a styrene-based copolymer that contains two or more glycidyl groups per molecule, has a weight average molecular weight of 4000 to 25000, and is composed of 20 to 99% by mass of a vinyl aromatic monomer (X), 1 to 80% by mass of glycidyl (meth)acrylate (Y), and 0 to 79% by mass of a vinyl group-containing monomer other than (X) that does not contain an epoxy group, because it has good compatibility with the thermoplastic polyester (A) and has a wider molecular weight distribution. More preferably, it is a copolymer composed of 20 to 99% by mass of (X), 1 to 80% by mass of (Y), and 0 to 40% by mass of (Z), and even more preferably, it is a copolymer composed of 25 to 90% by mass of (X), 10 to 75% by mass of (Y), and 0 to 35% by mass of (Z). These compositions affect the concentration of functional groups that contribute to the reaction with the thermoplastic polyester (A), so it is preferable to appropriately control them within the above range.

[0051] Examples of the (X) vinyl aromatic monomer include styrene, α-methylstyrene, etc. Examples of the (Y) glycidyl alkyl (meth)acrylate include glycidyl (meth)acrylate, (meth)acrylic acid ester having a cyclohexene oxide structure, (meth)acrylic glycidyl ether, etc., and among these, glycidyl (meth)acrylate is preferred in terms of high reactivity. Examples of the (Z) other vinyl group-containing monomers include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 22 carbon atoms (the alkyl group may be linear or branched), such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, and methoxyethyl (meth)acrylate; (meth)acrylic acid polyalkylene glycol esters; (meth)acrylic acid alkoxyalkyl esters; (meth)acrylic acid hydroxyalkyl esters; (meth)acrylic acid dialkylaminoalkyl esters; (meth)acrylic acid benzyl esters; (meth)acrylic acid phenoxyalkyl esters; (meth)acrylic acid isobornyl esters; and (meth)acrylic acid alkoxysilylalkyl esters. In addition, (meth)acrylamide, (meth)acryldialkylamide, vinyl esters such as vinyl acetate, vinyl ethers, (meth)allyl ethers and other aromatic vinyl monomers, and α-olefin monomers such as ethylene and propylene can also be used as the (Z) other vinyl group-containing monomer.

[0052] The weight average molecular weight of the copolymer is preferably 4000 to 25000. The weight average molecular weight is more preferably 5000 to 15000. If the weight average molecular weight is less than 4000, the unreacted copolymer may volatilize during the molding process or bleed out onto the surface of the molded article, causing surface contamination. On the other hand, if the weight average molecular weight exceeds 25000, not only will the reaction with the thermoplastic polyester (A) be slowed down, resulting in an insufficient molecular weight increasing effect, but also the compatibility between the copolymer and the thermoplastic polyester (A) will be poor, increasing the possibility of a decrease in the inherent properties of the thermoplastic polyester (A), such as heat resistance.

[0053] The epoxy value of the copolymer is 400 to 2500 equivalents / 1×10 6 g, and more preferably 500 to 1500 equivalents / 1×10 6 g, and more preferably 600 to 1000 equivalents / 1×10 6 g. The epoxy value is 400 equivalents / 1×10 6 If the viscosity is less than 2500 equivalents / 1×10 6 If it exceeds g, the thickening effect becomes excessive and the moldability may be adversely affected.

[0054] When the reactive compound (E) is a compound having a carbodiimide group, a polycarbodiimide compound can be used. The polycarbodiimide compound is advantageous in that it efficiently reduces the acid value.

[0055] The polycarbodiimide compound that can be used in the present invention may be any polycarbodiimide having two or more carbodiimide groups (-N=C=N- structure) in one molecule, and examples thereof include aliphatic polycarbodiimides, alicyclic polycarbodiimides, aromatic polycarbodiimides, and copolymers thereof. Preferred are aliphatic polycarbodiimide compounds or alicyclic polycarbodiimide compounds.

[0056] The polycarbodiimide compound can be obtained, for example, by the decarbonation reaction of a diisocyanate compound. Examples of the diisocyanate compound that can be used here include 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,5-naphthylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane diisocyanate, tetramethylxylylene diisocyanate, and 1,3,5-triisopropylphenylene-2,4-diisocyanate. These may be used alone or in the form of copolymerization of two or more. In addition, a branched structure may be introduced, or a functional group other than a carbodiimide group or an isocyanate group may be introduced by copolymerization. Furthermore, the terminal isocyanate may be used as it is, but the degree of polymerization may be controlled by reacting the terminal isocyanate, or a part of the terminal isocyanate may be blocked.

[0057] As the polycarbodiimide compound, alicyclic polycarbodiimides derived from dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, etc. are particularly preferred, and polycarbodiimides derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate are particularly preferred.

[0058] The polycarbodiimide compound preferably contains 2 to 50 carbodiimide groups per molecule in terms of stability and handling. More preferably, the polycarbodiimide compound contains 5 to 30 carbodiimide groups per molecule. The number of carbodiimide groups in a polycarbodiimide molecule (i.e., the number of carbodiimide groups) corresponds to the degree of polymerization if the polycarbodiimide is obtained from a diisocyanate compound. For example, the degree of polymerization of a polycarbodiimide obtained by linking 21 diisocyanate compounds in a chain is 20, and the number of carbodiimide groups in the molecular chain is 20. Usually, a polycarbodiimide compound is a mixture of molecules of various lengths, and the number of carbodiimide groups is expressed as an average value. If the polycarbodiimide compound has the number of carbodiimide groups in the above range and is solid around room temperature, it can be powdered, so it is excellent in workability and compatibility when mixed with the thermoplastic polyester (A), and is also preferable in terms of uniform reactivity and bleed-out resistance. The number of carbodiimide groups can be measured, for example, using a conventional method (a method of dissolving with an amine and performing back titration with hydrochloric acid).

[0059] The polycarbodiimide compound has an isocyanate group at its terminal, and the isocyanate group content is preferably 0.5 to 4 mass% from the viewpoint of stability and ease of handling. More preferably, the isocyanate group content is 1 to 3 mass%. In particular, it is preferable that the polycarbodiimide is derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate and has an isocyanate group content in the above range. The isocyanate group content can be measured by a conventional method (a method of dissolving in an amine and performing back titration with hydrochloric acid).

[0060] When the reactive compound (E) is a compound having an isocyanate group, examples of the reactive compound include the above-mentioned polycarbodiimide compounds containing an isocyanate group and the above-mentioned isocyanate compounds which are raw materials for polycarbodiimide compounds.

[0061] When the reactive compound (E) is a compound having an acid anhydride group, a compound containing 2 to 4 anhydrides per molecule is preferred in terms of stability and ease of handling. Examples of such compounds include phthalic anhydride, trimellitic anhydride, and pyromellitic anhydride.

[0062] The amount of the reactive compound (E) in the polyester resin composition may be 0.05 to 1 mass %, and within that, it is preferably 0.1 to 0.9 mass parts, more preferably 0.1 to 0.8 mass parts, and even more preferably 0.1 to 0.7 mass parts.

[0063] If the reactive compound (E) is less than 0.05 parts by mass, the targeted molecular chain extension effect is insufficient, and if it exceeds 1 part by mass, the thickening effect becomes excessive, which tends to adversely affect moldability and affect the mechanical properties of the final product. If the reactive compound (E) is an epoxy compound, if it exceeds 1 part by mass, the epoxy compound may coagulate and harden, which may cause unevenness on the surface of the molded product. If the reactive compound (E) is a carbodiimide compound, if it exceeds 1 part by mass, the basicity of the polycarbodiimide compound may cause hydrolysis of the thermoplastic polyester (A), which tends to affect the mechanical properties.

[0064] [Talc (F)] The flame-retardant polyester resin composition of the present invention may further contain talc (F) as a crystallization accelerator in addition to the components (A) to (E). The content of talc (F) is not limited, but is preferably 2% by mass or less in the flame-retardant polyester resin composition. When talc (F) is contained, the lower limit of the content may be 0.1% by mass or more.

[0065] The average particle size of the primary particles of talc (F) is preferably 1 to 15 μm, more preferably 2 to 10 μm. If the average particle size exceeds the above range, it is difficult for the average particle size of the secondary particles of talc (F) to be 30 μm or less, and the bending modulus and appearance of the molded product may be deteriorated. On the other hand, if the average particle size is less than the above range, dispersion failure is likely to occur. The average particle size can be measured from the particle size value of a cumulative amount of 50% by weight read from a particle size cumulative distribution curve measured by a laser diffraction method (e.g., LA920W manufactured by Horiba, Ltd.) or a liquid layer sedimentation type light transmission method (e.g., CP type manufactured by Shimadzu Corporation). In the present invention, it is a value measured by the former method (laser diffraction method).

[0066] Talc (F) can be obtained by mechanically pulverizing naturally occurring talc and then classifying it more precisely. It is also possible to further classify the talc that has been roughly classified once. As a mechanical pulverization method, talc can be pulverized using a pulverizer such as a jaw crusher, a hammer crusher, a roll crusher, a screen mill, a jet pulverizer, a colloid mill, a roller mill, or a vibration mill. The pulverized talc can be wet- or dry-classified once or repeatedly using a device such as a cyclone, a cyclone air separator, a microseparator, a cyclone air separator, or a sharp-cut separator in order to adjust the average particle size to the above-mentioned preferred particle size. When producing the talc used in the present invention, it is preferable to pulverize the talc to a specific particle size and then perform a classification operation using a sharp-cut separator.

[0067] The talc (F) in the present invention does not require any particular surface treatment, but for the purpose of improving adhesion or dispersibility with the thermoplastic polyester (A), it may be surface-treated with various organic titanate coupling agents, organic silane coupling agents, unsaturated carboxylic acids or modified polyolefins grafted with their anhydrides, fatty acids, fatty acid metal salts, fatty acid esters, etc. It may also be granular talc granulated into granules using a water-soluble polymer binder.

[0068] [Optional Additives] In addition to the above, the flame-retardant polyester resin composition of the present invention may contain, if necessary, known heat stabilizers, antioxidants, ultraviolet absorbers, light stabilizers, plasticizers, lubricants, crystal nucleating agents, release agents, antistatic agents, inorganic pigments, organic pigments, dyes, or other polymers.

[0069] The flame-retardant polyester resin composition of the present invention preferably contains the components (A), (B), (C), (D), and (E) in total amount of 80 mass% or more, more preferably 90 mass% or more, and even more preferably 95 mass% or more.

[0070] [Method of producing flame-retardant polyester resin composition] The method for producing the flame-retardant polyester resin composition of the present invention is not limited, but the composition can be produced by blending the above-mentioned components (A), (B), (C), (D), and (E) and other blends in any blending order so as to obtain a predetermined blend composition, and then mixing and melt-kneading the mixture in a tumbler, Henschel mixer, etc. Examples of the melt-kneading method include methods using a single-screw extruder, twin-screw extruder, kneader, Banbury mixer, roll, etc., which are well known to those skilled in the art, and among these, it is preferable to use a twin-screw extruder.

[0071] In addition, inorganic fiber material (D) that is easily damaged during extrusion processing is preferably fed from the side port of the twin-screw extruder to prevent damage to the glass fiber, but this is not particularly limited. In addition, the silane coupling agent may be added simultaneously with the raw material components other than (D), but it is preferable to add it to the (D) component in advance before adding it.

[0072] In addition, in order to remove volatile components and decomposed low-molecular-weight components during processing and to increase the reactivity between the inorganic fiber material (D) and the thermoplastic polyester (A), it is desirable to perform suction using a vacuum pump between the side opening for feeding the inorganic fiber material (D) and the die head at the tip of the extruder.

[0073] [Physical properties of flame-retardant polyester resin composition] In a preferred embodiment, the flame-retardant polyester resin composition of the present invention has a melting point of the resin composition +10°C, a capillary diameter of 1.0 × length of 10.0 mm, a shear rate of 10 s -1 The melt viscosity measured at 1×10 3 Pa s~5×10 3 This means that the content of the component (B) in the flame-retardant polyester resin composition of the present invention is 0.05 to 1 mass %, and thus the fluidity of the resin composition in the low shear rate range is significantly improved.

[0074] In a preferred embodiment, the flame-retardant polyester resin composition of the present invention satisfies the excellent property that the deflection temperature under load of a multipurpose test piece measured under a load of 1.82 MPa in accordance with ISO75 is 225°C or higher. EXAMPLES

[0075] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0076] Examples 1 to 4 and Comparative Examples 1 to 5 The characteristics and physical properties shown in the examples and comparative examples were measured by the following test methods. (1) Reduced viscosity of polyester resin (dL / g): 0.1 g of the sample was dissolved in 25 mL of a mixed solvent of phenol / tetrachloroethane (mass ratio 6 / 4), and the viscosity was measured at 30° C. using an Ubbelohde viscosity tube. (2) Melt viscosity: The melt viscosity of the flame-retardant polyester resin composition was measured using a "Capillograph 1D" manufactured by Toyo Seiki Seisakusho Co., Ltd. Specifically, the melt viscosity was measured under the following conditions: capillary diameter 1.0 mm, length 40 mm, cylinder diameter 9.55 mm, temperature: melting point + 10°C, shear rate 10 s -1 The melt viscosity at this time was measured. (3) Deflection temperature under load (HDT): A multipurpose test piece according to ISO-3167 was molded using an injection molding machine (Toshiba Machine Co., Ltd., IS80), and the HDT was measured at a load of 1.82 MPa in accordance with ISO-75. (4) Flammability test: In accordance with UL94, flammability was evaluated using test pieces 1 / 32 inch thick. UL94 evaluates self-extinguishing flame retardancy with an index of 5VA>5VB>V-0>V-1>V-2, with 5VA being the most flame retardant. (5) Bending strength (initial): Measurements were performed in accordance with ISO-178. Test pieces were prepared by continuous injection molding of ISO dumbbell pieces using an injection molding machine (Toshiba Machine Co., Ltd., IS80) at a cylinder temperature of 275°C, a mold temperature of 140°C, and a cycle time of 40 seconds. (6) Bending strength (when retained): The bending strength was measured in the same manner as in (5), except that the sample was allowed to remain in the cylinder for 15 minutes. (7) Appearance of molded product: Test pieces injection molded under the following molding conditions were evaluated according to the following criteria.

[0077] [Molding condition 1] Using a 100 mm x 100 mm x 2 mm thick embossed plate mold, injection molding was performed in an injection molding machine with a cylinder temperature of 275°C, a mold temperature of 140°C, and a cycle time of 40 seconds.

[0078] [Molding condition 2] Injection molding was performed in the same manner as in molding condition 1, except that the cycle time was changed to 30 seconds.

[0079] [Evaluation Criteria] ○: Meets all of the following (1) to (3). (1) There is no glass fiber floating on the entire surface of the plate, and the surface gloss is excellent. (2) No burrs are generated. (3) No gas burns are observed.

[0080] △: In the above (1), slight floating of glass fibers was observed on the end face away from the gate, but (2) and (3) were satisfied.

[0081] ×: Any of the following (4) to (6) applies. (4) The lifting of glass fibers is clearly observed at the end face away from the gate. (5) Burrs are generated. (6) Gas burns are observed.

[0082] The raw materials used in the examples and comparative examples are as follows.

[0083] Polyethylene terephthalate resin (A-1): Toyobo Co., Ltd., reduced viscosity 0.75 dL / g Polyethylene glycol dibenzoate (B-1): KRM4004, manufactured by Sanyo Chemical Industries, Ltd., called "PEGDBE."

[0084] Brominated flame retardant (C-1): Great Lakes, PDBS-80 (polybrominated styrene) Flame retardant assistant (C-2): PATOX-MK (antimony trioxide) manufactured by Nihon Seiko Co., Ltd. Glass fiber (D-1): Nippon Electric Glass Co., Ltd., ECS03T-120H Epoxy compound (E-1): Denacol EX-830 (polyethylene glycol diglycidyl ether), manufactured by Nagase ChemteX Corporation Carbodiimide (E-2): Carbodilite LA-1, manufactured by Nisshinbo Chemical Co., Ltd. Talc (F-1): Hayashi Kasei Co., Ltd., Micron White #5000 The following other additives were used:

[0085] Antioxidant: BASF, Irganox 1010 Release agent: Recorb WE40, manufactured by Clariant Japan Co., Ltd. The flame-retardant polyester resin compositions of the Examples and Comparative Examples were obtained by weighing the above raw materials according to the blending ratios (mass%) shown in Table 1 and melt-kneading them in a 35φ twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.) at a cylinder temperature of 275°C and a screw rotation speed of 100 rpm. The raw materials other than the glass fiber were fed into the twin-screw extruder from a hopper, and the glass fiber was fed by side feeding from a vent port.

[0086] The resulting polyester resin composition pellets were used to obtain molded articles for each evaluation sample in an injection molding machine.

[0087] The evaluation results are shown in Table 1.

[0088] [Table 1]

[0089] From Table 1, it can be seen that the flame-retardant polyester resin compositions of Examples 1 to 4 obtained good results in all items, and were well-balanced in terms of strength, rigidity, heat resistance, flame retardancy, retention stability, and moldability (appearance of molded product).

[0090] On the other hand, in Comparative Example 1, the (B) component was excessive, so the retention stability was poor, and gas burns were observed in the molded product. In Comparative Example 2, the (B) component was not included, so the fluidity was insufficient, and glass floating was observed at the end of the molded product, resulting in a poor appearance. In Comparative Example 3, the reactive compound (E) was not included, so the retention stability was poor, and burrs and gas burns were observed in the molded product. In Comparative Example 4, the (B) component was included, but in an insufficient amount, so the fluidity was insufficient like in Comparative Example 2, and glass floating was observed at the end of the molded product, resulting in a poor appearance. In Comparative Example 5, the (B) component was included in an amount exceeding the predetermined amount, so the retention stability was poor like in Comparative Example 1, and gas burns were observed in the molded product. [Industrial Applicability]

[0091] The polyester resin composition of the present invention achieves a high degree of both rigidity and flame retardancy, and further has good moldability and retention stability, and can give molded products with excellent molded appearance. Therefore, it can be used in a wide range of applications such as electric and electronic parts, machine mechanism parts, and automobile parts that require rigidity and heat resistance (high HDT), and therefore it will make an enormous contribution to the industrial world.

Claims

1. A flame-retardant polyester resin composition comprising: 20 to 65 mass% of a thermoplastic polyester (A); 0.05 to 1 mass% of a polyalkylene glycol and / or a polyalkylene glycol derivative (B); 3 to 20 mass% of a flame retardant (C); 28 to 55 mass% of an inorganic fiber material (D); and 0.05 to 1 mass% of a reactive compound (E).

2. Shear rate 10 s -1 The melt viscosity at 3 Pa·s to 5×10 3 The flame-retardant polyester resin composition according to claim 1, having a viscosity of Pa·s.

3. The flame-retardant polyester resin composition according to claim 1, wherein the thermoplastic polyester (A) is polyethylene terephthalate.

4. 2. The flame-retardant polyester resin composition according to claim 1, wherein the flame retardant (C) is a bromine-based compound (C1) and further contains an antimony compound (C2) as a flame-retardant auxiliary.

5. The flame-retardant polyester resin composition according to claim 1 , wherein at least one of the molecular terminals of the polyalkylene glycol derivative is a carboxylate.

6. The flame-retardant polyester resin composition according to claim 1 , further comprising 2 mass% or less of talc (F).

7. 2. The flame-retardant polyester resin composition according to claim 1, which has a deflection temperature under load of 225° C. or higher as measured at a load of 1.82 MPa in accordance with ISO 75.

8. An electronic or electrical part comprising a molded article of the flame-retardant polyester resin composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Polyester resin composition

    JP1993043783A

  • Flame-retardant polyester resin composition improved in melt stability

    JP1996283550A

  • Thermoplastic polyester resin composition

    JP1999049939A

  • Flame-retardant thermoplastic polyester resin composition

    JP2009074019A

  • Flame-retardant thermoplastic polyester resin composition and molded article

    JP2010037375A