Decorative film and method for manufacturing decorative film

The decorative film with a base film, glitter, and adhesive layers, along with specific mass ratios and elongation rates, addresses issues of uneven coloring and streaks in vacuum forming, ensuring a uniform and durable decorative finish on complex substrates.

JP2024146383APending Publication Date: 2024-10-15DAI NIPPON TORYO CO LTD

Patent Information

Application Number
JP2023059246
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing decorative films used for vacuum forming on complex-shaped substrates, such as automobile parts, often result in uneven coloring, transparency of the base material, and decorative streaks, leading to design defects and material deterioration.

Method used

A decorative film comprising a base film layer, a glitter layer with a specific mass ratio of glitter pigment to binder resin (7.5:100 to 30:100), and an adhesive layer, with an elongation rate of 30% or more, ensuring uniform application and adhesion, and optionally including a clear layer with low ultraviolet transmittance and a primer layer with high gel fraction to enhance appearance.

Benefits of technology

The film prevents uneven coloring, transparency, and decorative irregularities, maintaining an excellent appearance even after vacuum forming, with improved adhesion and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146383000001_ABST
    Figure 2024146383000001_ABST
Patent Text Reader

Abstract

To provide a decorative film excellent even in appearance without causing ornament unevenness, such as uneven color, the transparency of a base and a stripe even when decorated by vacuum molding, etc.SOLUTION: A decorative film for decorating a base material includes a base material film layer 1, a bright layer 2 and an adhesive layer 4. The bright layer 2 includes brilliant pigment and a binder resin; the mass ratio of the brilliant pigment to the binder resin in the bright layer 2 is 7.5:100-30:100; and the elongation rate of the decorative film at a temperature when applying the decorative film to the base material is 30% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative film and a manufacturing method for the decorative film, and in particular to a decorative film that has excellent appearance and does not produce decorative unevenness such as color unevenness, show-through of the base, or streaks even when decorated by vacuum forming or the like. [Background technology]

[0002] Shiny designs such as pearl and metallic are often used in automobiles and automobile parts, electrical appliances, small items, interior goods, etc., because they can give a sense of luxury. When applying a shiny design with paint, the painting process often requires multiple steps to form a multi-layered film that includes multiple coating layers such as a shiny layer, a primer layer, and a clear layer, which creates issues such as securing a large-scale painting site, complicated process management, and increased CO2 emissions in each baking process. For this reason, in recent years, various methods have been considered for applying a shiny design to a substrate using decorative films instead of paint.

[0003] Japanese Patent Laid-Open Publication No. 2004-299220 (Patent Document 1) describes an invention relating to a metallic-toned laminate film having a guard film layer (A), a clear coating layer (B), a lustrous material (C3) containing aluminum flakes, and a colored coating layer (C) containing an orientation control material (C4). It describes how, by adding the orientation control material (C4), it is possible to control the orientation of the aluminum flakes so as to achieve a high SV value and a high IV value, thereby providing a metallic-toned laminate film that has excellent processability when decorating molded products and can impart design properties to the decorated molded products that are equal to or better than those achieved by conventional painting methods.

[0004] Japanese Patent Laid-Open Publication No. 2015-66855 (Patent Document 2) describes an invention of a decorative sheet having a base layer and a metallic gloss layer, the metallic gloss layer being formed from a resin composition containing a binder resin containing 50% or more by mass of an acrylic resin and a resin-coated metallic pigment. It describes that by using a resin-coated metallic pigment in which a metallic pigment is pre-coated with a resin as the pigment used in the metallic gloss layer, even when an acrylic resin is used as the binder resin, the metallic pigment can be dispersed with high uniformity in the metallic gloss layer, and excellent metallic gloss and adhesion can be imparted to the decorative sheet.

[0005] JP 2021-160222 A (Patent Document 3) describes an invention of a decorative film having a reflective layer formed by applying a paint containing an elastic photoluminescent pigment to the surface of a film substrate. The elastic photoluminescent pigment stretches in the direction along with the decorative film when the decorative film is stretched along the direction in which the surface of the decorative film expands. Therefore, regardless of the shape of the surface covered by the decorative film (i.e., even if the surface covered by the decorative film is a curved or bent surface), the covered surface exhibits a uniform reflectance. As a result, when the decorative film is attached to, for example, the body of an automobile with many curved surfaces, a surface without uneven color or decorative unevenness is obtained.

[0006] JP 2021-133615 A ​​(Patent Document 4) describes an invention for a decorative vapor deposition sheet including a cover resin layer and a metal vapor deposition layer, in which the cover resin layer has a thickness of about 50 micrometers or more, the metal vapor deposition layer has a granular structure, and the breaking elongation of the decorative vapor deposition sheet at 20°C is about 120% or more and the breaking elongation of the decorative vapor deposition sheet at 160°C is about 350% or more. It describes that this makes it possible to reduce or suppress defects such as breakage of the metal vapor deposition layer or the entire sheet even when applied to a molding method that requires high temperatures, etc. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2004-299220 A [Patent Document 2] JP 2015-66855 A [Patent Document 3] JP 2021-160222 A [Patent Document 4] JP 2021-133615 A Summary of the Invention [Problem to be solved by the invention]

[0008] Patent Documents 1 to 4 describe useful inventions relating to a method of decorating a base material using a decorative sheet including a glittering layer. However, it is difficult to control the arrangement of glittering pigments having a specific shape such as a scale shape. In particular, when decorating base materials with complex shapes such as plastic parts for automobiles using vacuum forming or the like, there are problems such as uneven coloring, the transparency of the base material, and uneven decoration such as streaks, which can easily lead to design defects and deterioration of the base material after decoration.

[0009] SUMMARY OF THE PRESENTLY PREFERRED EMBODIMENTS An object of the present invention is to provide a decorative film which, even when decorated by vacuum forming or the like, does not cause uneven decoration such as color unevenness, show-through of the base, or streaks, and which also has an excellent appearance. [Means for solving the problem]

[0010] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that in a decorative film for decorating a substrate, which comprises a substrate film layer, a glittering layer, and an adhesive layer, by adjusting the mass ratio of the glittering pigment to the binder resin in the glittering layer to be within the range of 7.5:100 to 30:100, and by adjusting the elongation of the decorative film to be 30% or more at the temperature when the decorative film is applied to the substrate, it is possible to provide a decorative film that does not produce decorative unevenness such as color unevenness, show-through of the base, or streaks, even when decorated by vacuum forming, and that also has an excellent appearance, and has thus completed the present invention.

[0011] Therefore, the decorative film of the present invention is a decorative film for decorating a substrate, The decorative film has (A) a base film layer, (B) a glossy layer, and (C) an adhesive layer, The (B) glittering layer contains a glittering pigment and a binder resin, and a mass ratio of the glittering pigment to the binder resin in the (B) glittering layer is within a range of 7.5:100 to 30:100; The decorative film is characterized in that the decorative film has an elongation percentage of 30% or more at the temperature when the decorative film is applied to the base material.

[0012] In a preferred embodiment of the decorative film of the present invention, the glass transition point of the (A) base film layer is within a range of −20° C. to 140° C., When the glass transition point (° C.) of the (A) base film layer is Tg(A) and the glass transition point (° C.) of the (B) glossy layer is Tg(B), Tg(A) and Tg(B) satisfy the following relational formula (1): -20℃ ≦ Tg(A)-Tg(B) ≦ 50℃ ··· Formula (1) Meet the following.

[0013] In another preferred embodiment of the decorative film of the present invention, the decorative film further has a clear layer (D) on the glossy layer (B), The (D) clear layer has an ultraviolet ray transmittance of 30% or less.

[0014] In another preferred embodiment of the decorative film of the present invention, a primer layer (E) is further provided between the base film layer (A) and the glossy layer (B), The (E) primer layer has a gel fraction of 80% or more.

[0015] In another preferable embodiment of the decorative film of the present invention, the luster pigment includes a vapor-deposited aluminum pigment and / or a resin-coated metal pigment.

[0016] The decorative film manufacturing method of the present invention is a decorative film for decorating a substrate, the decorative film having (A) a substrate film layer, (B) a glossy layer, and (C) an adhesive layer, The process includes providing a glossy layer (B) and an adhesive layer (C) on a base film layer (A), The (B) glittering layer contains a glittering pigment and a binder resin, and a mass ratio of the glittering pigment to the binder resin in the (B) glittering layer is within a range of 7.5:100 to 30:100; The method for producing a decorative film is characterized in that the decorative film has an elongation percentage of 30% or more at a temperature when the decorative film is applied to the base material. Effect of the Invention

[0017] According to the present invention, it is possible to provide a decorative film that is excellent in appearance and does not cause decorative unevenness such as color unevenness, show-through of the base, or streaks even when decorated by vacuum forming or the like. [Brief description of the drawings]

[0018] [Figure 1] 1 is a schematic diagram showing one embodiment of a decorative film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention relates to a decorative film and a method for producing the decorative film.

[0020] The decorative film of the present invention is a film for decorating a substrate. Here, "decoration" means providing a design to the substrate or imparting a texture different from that of the substrate. The design means a shape, a pattern, a color, or a combination of these.

[0021] In the present invention, the substrate means an object to which the decorative film is applied. Substrates include various articles, but since the decorative film of the present invention can impart a glittering design to the substrate, automobiles and automobile parts, electrical appliances, small items, interior goods, etc. are suitable substrates to which the decorative film of the present invention is applied. In addition, the materials of the substrate are also diverse, for example, plastic substrates, metal substrates, etc.

[0022] The decorative film of the present invention has a multi-layer structure and includes a base film layer, a glittering layer, and an adhesive layer. In this specification, the base film layer may be referred to as (A) base film layer, the glittering layer may be referred to as (B) glittering layer, and the adhesive layer may be referred to as (C) adhesive layer.

[0023] In the present invention, the base film layer means a film layer that supports the glossy layer and the like among the layers that constitute the decorative film.

[0024] The base film layer is preferably composed of a resin film. The resin used in the film is preferably a thermoplastic resin, such as acrylonitrile-butadiene-styrene resin (ABS resin), acrylonitrile-styrene-acrylic acid ester resin, acrylic resin, polyolefin resin such as polypropylene and polyethylene, polycarbonate resin, vinyl chloride resin such as polyvinyl chloride (PVC), polyethylene terephthalate (PET) resin, polyphenylene ether (PPE) resin, etc. Among these, acrylic resin, ABS resin, and PVC resin are particularly preferable. The resin may be used alone or in combination of two or more kinds.

[0025] The glass transition point of the base film layer is preferably −20° C. to 140° C., more preferably 20° C. to 130° C., and particularly preferably 50° C. to 120° C. By setting the glass transition point of the base film layer to 140° C. or lower, the formability of the decorative sheet is excellent, particularly when a base material having a complex shape is decorated with the decorative sheet by heating in vacuum forming or the like, and by setting the glass transition point of the base film layer to −20° C. or higher, particularly 50° C. or higher, the blocking resistance and durability of the decorative film are improved.

[0026] In this specification, the glass transition point (Tg) of the base film layer is the spectrum peak in a temperature change curve of loss tangent (tan δ) measured at a measurement frequency of 1 Hz using a solid viscoelasticity measuring device based on JIS K7244-4.

[0027] Specifically, the loss modulus and storage modulus of the base film layer are measured at each temperature under the following measurement conditions using a solid viscoelasticity measuring device (e.g., RSA-GII (manufactured by TA Instruments)), the loss tangent is calculated from the loss modulus and storage modulus, a temperature change curve of the loss tangent is created, and the spectrum peak value of the loss tangent is read. <Measurement conditions> Temperature range: -50℃~200℃ Heating rate: 5℃ / min Measurement length: 20.0 mm Measurement width: 5.0mm Frequency: 1Hz Distortion: 0.05%

[0028] The base film layer may be one layer or two or more layers.

[0029] The thickness of the base film layer is preferably 10 to 1000 μm, and more preferably 50 to 1000 μm. When the base film layer is made up of multiple layers, the numerical range described here refers to the total thickness of the base film layers.

[0030] Examples of molding methods that can be used to produce the film include injection molding, blow molding, extrusion molding, vacuum molding, pressure molding, and TOM (Three Dimension Overlay Method) molding.

[0031] In the present invention, the glossy layer is a layer that is required to impart a glossy design to a substrate, among the layers that constitute the decorative film.

[0032] The glittering layer contains a glittering pigment and a binder resin, and the mass ratio of the glittering pigment to the binder resin in the glittering layer is within the range of 7.5:100 to 30:100. In addition, the mass ratio of the glittering pigment to the binder resin in the glittering layer is more preferably within the range of 10:100 to 25:100. If the ratio of the glittering pigment per 100 parts by mass of the binder resin is less than 7.5 parts by mass, the gaps between the particles of the glittering pigment will widen during the molding of the decorative film when the decorative film is applied to the substrate, which will cause the color of the base to show through or cause color unevenness. In addition, if the ratio of the glittering pigment per 100 parts by mass of the binder resin exceeds 30 parts by mass, the ratio of the glittering pigment to the binder resin will be too high, leading to poor appearance and reduced adhesion to the substrate film layer.

[0033] Examples of the luster pigment include metal pigments such as aluminum, indium, nickel, chromium, tin, copper, silver, platinum, gold and stainless steel, and glass flakes.

[0034] The luster pigment is preferably in the form of flakes, and more preferably is an aluminum flake.

[0035] The flake-shaped bright pigment preferably has an average particle size of 5 to 35 μm and an average aspect ratio of 10 to 1000. The flake-shaped bright pigment more preferably has an average particle size of 7 to 25 μm. The flake-shaped bright pigment more preferably has an average aspect ratio of 20 to 1000. The flake-shaped bright pigment also has an average thickness of, for example, 5 to 3000 nm.

[0036] In this specification, the particle size of the luster pigment is the average value of the major axis diameter (the maximum length of a straight line connecting two points on the periphery) and the minor axis diameter (the minimum length of a straight line connecting two points on the periphery) of the particle plane in an image observed by SEM (scanning electron microscope). Here, when the particle plane is circular, the diameter of the circle is the particle size. The average particle size of the luster pigment is the average particle size of the luster pigment contained in the luster layer. In addition, in the present invention, the average aspect ratio of the luster pigment is the ratio (D / T) of the average particle size (D) to the average thickness (T). In addition, in the present invention, the particle size and thickness of the luster pigment were measured using SEM (scanning electron microscope), and the average particle size and average thickness were obtained for 100 or more particles.

[0037] The luster pigment preferably includes a vapor-deposited aluminum pigment and / or a resin-coated metal pigment.

[0038] The vapor-deposited aluminum pigment is a pigment prepared by crushing and adjusting the particle size of a thin aluminum film obtained by uniformly depositing aluminum. The vapor-deposited aluminum pigment is preferably a silica-coated vapor-deposited aluminum pigment. The silica-coated vapor-deposited aluminum pigment is a vapor-deposited aluminum pigment whose surface is coated with a silica film. The amount of silica coating is preferably 0.1 to 25 g, and particularly preferably 5 to 20 g, per 100 g of the vapor-deposited aluminum pigment.

[0039] Resin-coated metal pigments are metal pigments whose surfaces are coated with resin. Here, the metal pigment is preferably in the form of flakes, more preferably aluminum flakes. Examples of the resin include acrylic resin, polyester resin, and urethane resin, and acrylic resin is preferred. The amount of resin coating is preferably 0.1 to 25 g per 100 g of metal pigment, and particularly preferably 5 to 20 g.

[0040] The amount of the luster pigment in the luster layer is preferably 7.5 to 30% by mass, and more preferably 10 to 25% by mass. The luster pigment may be used alone or in combination of two or more kinds.

[0041] Examples of the binder resin include acrylic resin, silicone resin, acrylic silicone resin, styrene-acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenolic resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin (e.g., vinyl chloride resin), amine resin, and ketimine resin.

[0042] The binder resin preferably contains an acrylic resin and / or a cellulose resin. By using an acrylic resin as the binder resin, the chemical resistance and weather resistance of the coating film can be improved. In addition, by using a cellulose resin as the binder resin, the drying property of the coating film is improved, and the orientation of the glittering pigment in the glittering layer can be easily controlled, so that the glittering layer can be easily formed without color unevenness or decorative unevenness.

[0043] The acrylic resin is preferably a polymer or copolymer containing an acrylic acid ester and / or a methacrylic acid ester as a main component, where the main component means a component contained in an amount of 50 mol % or more.

[0044] The acrylic resin preferably has a small amount of hydroxyl groups, and preferably has a hydroxyl value of less than 40 mgKOH / g. In particular, in the case of a one-component paint, it is more preferable that the acrylic resin has a hydroxyl value of 5 mgKOH / g or less. In addition, in the case where the glossy layer contains multiple acrylic resins, the amount of the acrylic resins having a hydroxyl value of less than 40 mgKOH / g is preferably 90% by mass or more of the total acrylic resins.

[0045] In this specification, the hydroxyl value of an acrylic resin is the number of milligrams of potassium hydroxide required to completely acetylate the free hydroxyl groups in 1 g of a sample with acetic anhydride and then neutralize them.

[0046] The weight average molecular weight of the acrylic resin is preferably from 3,000 to 300,000, and more preferably from 4,000 to 200,000.

[0047] In this specification, the weight average molecular weight of a resin is a value measured by gel permeation chromatography, and polystyrene is used as the standard substance.

[0048] The amount of the acrylic resin in the shiny layer is preferably 5 to 95% by mass, and more preferably 10 to 90% by mass. The acrylic resin may be used alone or in combination of two or more kinds.

[0049] Examples of cellulose resins include cellulose ether, cellulose ester, nitrocellulose, cellulose sulfate, cellulose phosphate, and cellulose acetate nitrate. Examples of cellulose ethers include methyl cellulose, ethyl cellulose, benzyl cellulose, trityl cellulose, cyanoethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, aminoethyl cellulose, and oxyethyl cellulose (also called hydroxyethyl cellulose). Examples of cellulose esters include cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, cellulose propionate, and cellulose butyrate.

[0050] In addition, examples of cellulose resins include acrylic modified cellulose derivatives, polyester modified cellulose derivatives, and polyurethane modified cellulose derivatives. The acrylic modified cellulose derivatives are compounds obtained by graft polymerizing acrylic components such as (meth)acrylates to cellulose derivatives such as cellulose ethers and cellulose esters. The polyester modified cellulose derivatives are compounds obtained by binding polyester components (i.e., components having multiple ester bonds in the main chain) such as polytrimethylene terephthalate, polyethylene terephthalate, and polybutylene terephthalate to cellulose derivatives such as cellulose ethers and cellulose esters. The polyurethane modified cellulose derivatives are compounds obtained by reacting hydroxyl groups of cellulose derivatives such as cellulose ethers and cellulose esters with, for example, isocyanate prepolymers.

[0051] As the cellulose resin, nitrocellulose is particularly preferable. The nitrocellulose preferably has a nitrogen content of 10% by mass or more.

[0052] The weight-average molecular weight of the cellulose resin is preferably 20,000 to 150,000, and more preferably 30,000 to 140,000. The cellulose resin preferably includes a cellulose resin having a weight-average molecular weight of 20,000 or more and less than 80,000, preferably 30,000 to 70,000, and a cellulose resin having a weight-average molecular weight of 80,000 or more and 150,000 or less, preferably 80,000 to 130,000. In this specification, the cellulose resin having a weight-average molecular weight of 20,000 or more and less than 80,000 may be referred to as cellulose resin (CE-1), and the cellulose resin having a weight-average molecular weight of 80,000 or more and 150,000 or less may be referred to as cellulose resin (CE-2). By combining cellulose resin (CE-1) and cellulose resin (CE-2) with different molecular weights, it becomes easier to obtain a decorative film with excellent brilliance, and the film's resistance to oil and grease contamination is improved.

[0053] The mass ratio of the cellulose resin (CE-1) to the cellulose resin (CE-2) is preferably from 95:5 to 5:95, and more preferably from 90:10 to 50:50.

[0054] The amount of the cellulose resin in the glossy layer is preferably 1 to 80% by mass, more preferably 2 to 70% by mass. The cellulose resin may be used alone or in combination of two or more kinds.

[0055] The glittering layer may contain, as other components, appropriate amounts as necessary, such as pigments that do not fall under the category of glittering pigments, dispersants, antioxidants, anti-settling agents, defoamers, silane coupling agents, adhesion imparting agents, anti-algae agents, anti-fungal agents, preservatives, insecticides, antibacterial agents, antiviral agents, ultraviolet absorbers, radical scavengers, antistatic agents, and conductivity imparting agents.

[0056] The glass transition point of the shiny layer is preferably 40°C to 120°C.

[0057] In this specification, the glass transition point (Tg) of the shiny layer is the spectrum peak in a temperature change curve of loss tangent (tan δ) measured at a measurement frequency of 1 Hz using a solid viscoelasticity measuring device based on JIS K7244-4.

[0058] Specifically, the loss modulus and storage modulus of the shiny layer are measured at each temperature under the following measurement conditions using a solid viscoelasticity measuring device (e.g., RSA-GII (manufactured by TA Instruments)), the loss tangent is calculated from the loss modulus and storage modulus, a temperature change curve of the loss tangent is created, and the spectral peak value of the loss tangent is read. <Measurement conditions> Temperature range: -50℃~200℃ Heating rate: 5℃ / min Measurement length: 20.0 mm Measurement width: 5.0mm Frequency: 1Hz Distortion: 0.05%

[0059] The glossy layer may be a single layer or two or more layers.

[0060] The glossy layer has a thickness of preferably 2 to 40 μm, more preferably 5 to 20 μm. When the glossy layer is made up of multiple layers, the numerical range described here refers to the total thickness of the glossy layer.

[0061] Examples of coating methods that can be used to produce the glossy layer include brush coating, roller coating, trowel coating, spatula coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, and dipping coating.

[0062] In the decorative film of the present invention, when the glass transition point (° C.) of the base film layer is Tg(A) and the glass transition point (° C.) of the shiny layer is Tg(B), Tg(A) and Tg(B) satisfy the following relational formula (1): -20℃ ≦ Tg(A)-Tg(B) ≦ 50℃ ··· Formula (1) If the glass transition point (° C.) of the base film layer and the glass transition point (° C.) of the shiny layer do not satisfy the relational expression (1), peeling or the like is likely to occur between the base film layer and the shiny layer.

[0063] In the present invention, the adhesive layer is a layer composed of an adhesive. The adhesive layer and the adhesive may be called a pressure-sensitive adhesive layer and a pressure-sensitive adhesive, respectively. Examples of the adhesive include a urethane adhesive, an acrylic adhesive, an epoxy adhesive, and a rubber adhesive, and among these, an acrylic adhesive is preferred.

[0064] The thickness of the adhesive layer is preferably 20 to 200 μm.

[0065] The adhesive layer can be formed by applying an adhesive to the surface of the substrate. Since the decorative film of the present invention is applied to the substrate via the adhesive layer, the adhesive layer is located on at least one surface of the decorative film of the present invention.

[0066] When the decorative film of the present invention is composed of a base film layer, a glittering layer, and an adhesive layer, examples of the multilayer structure of the decorative film of the present invention include adhesive layer / base film layer / glittering layer, base film layer / glittering layer / adhesive layer, etc. In this specification, when the multilayer structure is expressed as, for example, adhesive layer / base film layer / glittering layer, it means that the decorative film of the present invention has a multilayer structure in which the adhesive layer, base film layer, and glittering layer are arranged in this order.

[0067] The decorative film of the present invention may further include a clear layer. In this specification, the clear layer may be referred to as a (D) clear layer. From the viewpoint of protecting the glossy layer, the clear layer is preferably located on the glossy layer in the decorative film of the present invention, and is preferably located on the side of the glossy layer where the base film layer is not located, and is also preferably located on the surface of the decorative film.

[0068] In the present invention, the clear layer means a layer having a visible light transmittance of 30% or more, preferably 40% or more, and more preferably 50% or more.

[0069] In this specification, the visible light transmittance means the total light transmittance in the visible region (360 nm to 750 nm), and can be measured in accordance with JIS K 7375:2008.

[0070] The clear layer preferably has an ultraviolet ray transmittance of 30% or less, more preferably 25% or less.

[0071] In this specification, the ultraviolet transmittance means the transmittance of light in the wavelength range of 280 nm to 400 nm, and can be measured using a spectrophotometer (for example, UV-2450 manufactured by Shimadzu Corporation).

[0072] The clear layer usually contains a resin. The amount of resin in the clear layer is preferably 40 to 99.5% by mass, more preferably 50 to 99% by mass. When the clear layer is composed of multiple layers, the numerical range described here refers to the amount of resin in each clear layer.

[0073] Examples of resins that can be used in the clear layer include acrylic resins, silicone resins, acrylic silicone resins, styrene-acrylic copolymer resins, polyester resins, fluororesins, rosin resins, petroleum resins, coumarone resins, phenolic resins, urethane resins, melamine resins, urea resins, epoxy resins, cellulose resins, xylene resins, alkyd resins, aliphatic hydrocarbon resins, butyral resins, maleic acid resins, fumaric acid resins, vinyl resins (vinyl chloride resins, etc.), amine resins, ketimine resins, etc. The resins may be used alone or in combination of two or more.

[0074] The clear layer may contain, as other components, appropriately as necessary, a pigment, a dispersant, an antioxidant, an antisettling agent, an antifoaming agent, a silane coupling agent, an adhesion imparting agent, an anti-algae agent, an anti-fungal agent, a preservative, an insecticide, an antibacterial agent, an antiviral agent, an ultraviolet absorbing agent, a radical scavenger, an antistatic agent, a conductivity imparting agent, and the like.

[0075] The glass transition point of the clear layer is preferably 40° C. to 120° C., and more preferably 50° C. to 110° C. When the glass transition point is 40° C. or higher, the durability of the coating film, such as chemical resistance, and blocking resistance are improved. In addition, when the glass transition point is higher than 120° C., problems may occur in terms of followability when applying the decorative film to a substrate having a complex shape by vacuum forming or the like.

[0076] In this specification, the glass transition point (Tg) of the clear layer is a spectrum peak in a temperature change curve of loss tangent (tan δ) measured at a measurement frequency of 1 Hz using a solid viscoelasticity measuring device based on JIS K7244-4.

[0077] Specifically, the loss modulus and storage modulus of the clear layer are measured at each temperature under the following measurement conditions using a solid viscoelasticity measuring device (e.g., RSA-GII (manufactured by TA Instruments)), the loss tangent is calculated from the loss modulus and storage modulus, a temperature change curve of the loss tangent is created, and the spectral peak value of the loss tangent is read. <Measurement conditions> Temperature range: -50℃~200℃ Heating rate: 5℃ / min Measurement length: 20.0 mm Measurement width: 5.0mm Frequency: 1Hz Distortion: 0.05%

[0078] The clear layer may be one layer or two or more layers.

[0079] The clear layer has a thickness of preferably 5 to 40 μm, more preferably 10 to 30 μm. When the clear layer is made up of a plurality of layers, the numerical range described here refers to the total thickness of the clear layers.

[0080] Examples of coating methods that can be used to produce the clear layer include brush coating, roller coating, trowel coating, spatula coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, and dipping coating.

[0081] In the decorative film of the present invention, when the glass transition point (° C.) of the base film layer is Tg(A) and the glass transition point (° C.) of the clear layer is Tg(D), Tg(A) and Tg(D) satisfy the following relational formula (2): -20℃ ≦ Tg(A)-Tg(D) ≦ 50℃ ··· Formula (2) If the glass transition point (° C.) of the base film layer and the glass transition point (° C.) of the clear layer do not satisfy the relational expression (2), peeling or the like is likely to occur between the base film layer and the clear layer.

[0082] When the decorative film of the present invention is composed of a base film layer, a glossy layer, an adhesive layer and a clear layer, examples of the multilayer structure of the decorative film of the present invention include adhesive layer / base film layer / glossy layer / clear layer, adhesive layer / glossy layer / clear layer / base film layer, clear layer / base film layer / glossy layer / adhesive layer, etc.

[0083] FIG. 1 is a schematic diagram showing one embodiment of the decorative film of the present invention. The decorative film shown in FIG. 1 includes a base film layer 1, a glossy layer 2 arranged on the base film layer 1, and a clear layer 3 arranged on the glossy layer 2, and has an adhesive layer 4 on the surface of the base film layer 1 on the side on which the glossy layer 2 is not arranged. The decorative film in FIG. 1 is a decorative film having a multilayer structure of an adhesive layer / base film layer / glossy layer / clear layer. Although not shown, a primer layer described later may be present between the base film layer 1 and the glossy layer 2.

[0084] The decorative film of the present invention may further include a primer layer. In this specification, the primer layer may be referred to as a (E) primer layer.

[0085] In the present invention, the primer layer means a layer that is first provided on the base film layer and does not correspond to the glossy layer, adhesive layer, or clear layer. From the viewpoint of improving the adhesion between the base film layer and the glossy layer, it is preferable that the primer layer is located between the base film layer and the glossy layer in the decorative film of the present invention.

[0086] The primer layer preferably has a gel fraction of 80% or more, more preferably 82 to 100%. The gel fraction is an index showing the degree of resistance of the primer layer to organic solvents. If a glittering layer is formed on a primer layer with a low gel fraction, the paint for forming the glittering layer may be soaked into the primer layer more than expected, which may disturb the orientation of the glittering pigment and make it difficult to impart a desired glittering design. According to a preferred embodiment of the decorative film of the present invention, by using a primer layer with a gel fraction of 80% or more, it is possible to easily achieve both adhesion between the base film layer and the glittering layer and a desired glittering design.

[0087] In this specification, the gel fraction of the primer layer refers to the mass proportion of the primer layer that remains without dissolving when the primer layer in a completely dried and cured state is immersed in an organic solvent. Specifically, when the mass of the primer layer before immersion is M1 and the mass of the primer layer after immersion is M2, the gel fraction of the primer layer can be calculated from the following formula. Gel fraction (%) = M2 / M1 × 100 Here, immersion refers to immersing the primer layer in a mixed solution of toluene and acetone (mass ratio 1:1) in an amount of 100 g per 1 g of primer layer under reflux for 5 hours. The mass of the primer layer after immersion is the mass of the primer layer after drying at 105°C for 30 minutes after immersion.

[0088] The gel fraction of the primer layer can be adjusted by appropriately adjusting the glass transition point (Tg) or hydroxyl value of the resin used in the paint for forming the primer layer and the functional group content of the curing agent, or by using a curing accelerator or a reaction catalyst in the paint for forming the primer layer. For example, a primer layer having a gel fraction of 80% or more can be obtained by using a resin having a Tg of 40 to 120°C, preferably 50 to 100°C, a resin having a hydroxyl value of 25 to 250 mgKOH / g, preferably 50 to 200 mgKOH / g, and adjusting the content of functional groups in the curing agent (e.g., isocyanate groups, epoxy groups, aziridine groups, etc.) to 2 to 10 mass% and preferably 3 to 8 mass% of the solid content of the paint. For the paint used to form the primer layer, the glass transition point (Tg) of the resin means the glass transition temperature calculated by the FOX equation, and the hydroxyl value of the resin is the number of milligrams of potassium hydroxide required to neutralize the free hydroxyl groups in 1 g of sample after they have been completely acetylated with acetic anhydride.

[0089] The primer layer usually contains a resin. The amount of the resin in the primer layer is preferably 30 to 99% by mass, and more preferably 50 to 95% by mass. When the primer layer is composed of multiple layers, the numerical range described here refers to the amount of the resin in each primer layer.

[0090] Examples of resins that can be used in the primer layer include acrylic resins, silicone resins, acrylic silicone resins, styrene-acrylic copolymer resins, polyester resins, fluororesins, rosin resins, petroleum resins, coumarone resins, phenolic resins, urethane resins, melamine resins, urea resins, epoxy resins, cellulose resins, xylene resins, alkyd resins, aliphatic hydrocarbon resins, butyral resins, maleic acid resins, fumaric acid resins, vinyl resins, amine resins, ketimine resins, etc. The resins may be used alone or in combination of two or more.

[0091] The primer layer may contain, as other components, appropriately as necessary, a pigment, a dispersant, an antioxidant, an antisettling agent, an antifoaming agent, a silane coupling agent, an adhesion imparting agent, an anti-algae agent, an anti-fungal agent, a preservative, an insecticide, an antibacterial agent, an antiviral agent, an ultraviolet absorbing agent, a radical scavenger, an antistatic agent, a conductivity imparting agent, and the like.

[0092] The primer layer may be one layer or two or more layers.

[0093] The primer layer preferably has a thickness of 3 to 15 μm. When the primer layer is made up of multiple layers, the numerical range described here refers to the total thickness of the primer layers.

[0094] Examples of coating methods that can be used to produce the primer layer include brush coating, roller coating, trowel coating, spatula coating, flow coater coating, spray coating (e.g., air spray coating, airless spray coating), shower coater coating, and dipping coating.

[0095] When the decorative film of the present invention is composed of a base film layer, a glossy layer, an adhesive layer and a primer layer, examples of the multilayer structure of the decorative film of the present invention include adhesive layer / base film layer / primer layer / glossy layer, base film layer / primer layer / glossy layer / adhesive layer, etc.

[0096] When the decorative film of the present invention is composed of a base film layer, a glossy layer, an adhesive layer, a clear layer and a primer layer, examples of the multilayer structure of the decorative film of the present invention include adhesive layer / base film layer / primer layer / glossy layer / clear layer, clear layer / base film layer / primer layer / glossy layer / adhesive layer, etc.

[0097] The decorative film of the present invention has an elongation rate of 30% or more, preferably 80% or more, and more preferably 90% or more at the temperature when applied to the substrate. By adjusting the elongation rate of the decorative film of the present invention and setting the mass ratio of the glittering pigment to the binder resin within the range of 7.5:100 to 30:100 as described above, it is possible to suppress the occurrence of color unevenness and decorative unevenness even when decorating the substrate by vacuum molding or the like. Furthermore, by ensuring the elongation rate of the decorative film of the present invention, it is also possible to suppress the occurrence of cracks and peeling during molding of the decorative film when applying the decorative film to the substrate. For these reasons, the decorative film has an excellent appearance after being applied to the substrate. In addition, although there is no particular limit on the upper limit of the elongation rate of the decorative film of the present invention, for example, the elongation rate at the temperature when applied to the substrate is 400% or less.

[0098] The temperature when the decorative film of the present invention is applied to a substrate (more specifically, when the decorative film of the present invention is attached to a substrate) is, for example, 80°C to 120°C.

[0099] The means for applying the decorative film of the present invention to a substrate (more specifically, the means for attaching the decorative film of the present invention to a substrate) is not particularly limited, and examples include vacuum forming, overlay vacuum forming, hand application, blow molding, insert molding, in-mold molding, etc.

[0100] In this specification, the elongation percentage (%) of the decorative film is the elongation percentage of the sample at the yield point when a tensile test is performed on the sample using a tensile tester (e.g., AGS-X (manufactured by SHIMADZU)) under the measurement conditions described below, or, in the case where defects such as cracks or cracks occur on the surface of the decorative film before the yield point is reached, the maximum elongation percentage of the sample at which no defects such as cracks or cracks are visually observed on the surface of the decorative film. <Measurement conditions> Tensile speed: 5mm / min Test temperature: The temperature at which the decorative film is applied to the substrate (molding temperature) Sample size: 10mm x 30mm (thickness is the thickness of the decorative film applied to the substrate.)

[0101] The elongation of the decorative film can be adjusted by changing the molecular weight, Tg, etc. of the resin contained in each layer that constitutes the decorative film. For example, if the elongation at the temperature when the decorative film is applied to the substrate is less than 30%, the elongation can be increased by increasing the molecular weight of the resin or decreasing the Tg.

[0102] The base film layer has an elongation rate of 30% or more, and preferably 80% or more, at the temperature when the decorative film is applied to the base, the glossy layer has an elongation rate of 20% or more, and preferably 80% or more, at the temperature when the decorative film is applied to the base, and the clear layer has an elongation rate of 20% or more, and preferably 80% or more, at the temperature when the decorative film is applied to the base.

[0103] In this specification, the elongation percentage (%) of the base film layer, the glossy layer and the clear layer is the elongation percentage of the sample at break when a tensile test of the sample is performed using a tensile tester (e.g., AGS-X (manufactured by SHIMADZU)) under the measurement conditions described below. For each layer, prepare a sample of 10 mm x 30 mm (the thickness is the thickness of the layer that constitutes the decorative film). For example, a glossy layer can be formed on a polypropylene (PP) substrate, which is a poor adherend, and then peeled off from the PP substrate to prepare a single film. <Measurement conditions> Tensile speed: 5mm / min Test temperature: The temperature at which the decorative film is applied to the substrate (molding temperature)

[0104] Next, a method for producing the decorative film of the present invention will be described.

[0105] The method for producing the decorative film of the present invention includes a step of providing a glossy layer and an adhesive layer on a base film layer. Here, the order of providing the glossy layer and the adhesive layer on the base film layer is arbitrary, but it is preferable to provide the adhesive layer after disposing the glossy layer on the base film layer.

[0106] One embodiment of the method for producing a decorative film of the present invention includes a process for producing a decorative film, the process including a step of applying paint to a base film layer to produce a glossy layer, and a step of applying an adhesive to the surface of the base film layer on the side on which the glossy layer is not located to produce an adhesive layer.

[0107] In addition, the manufacturing method of the decorative film of the present invention may also include a step of providing a glossy layer, a clear layer, and an adhesive layer on the base film layer. Here, the order of providing the glossy layer, the clear layer, and the adhesive layer on the base film layer is arbitrary, but it is preferable to provide the adhesive layer after disposing the glossy layer and the clear layer on the base film layer in this order.

[0108] In this case, one embodiment of the method for manufacturing a decorative film of the present invention includes a step of applying paint to a base film layer to produce a glossy layer, a step of applying paint to the glossy layer to produce a clear layer, and a step of applying an adhesive to the surface of the base film layer on the side where the glossy layer is not located to produce an adhesive layer.

[0109] In addition, the method for producing the decorative film of the present invention may also include a step of providing a glossy layer, a primer layer, and an adhesive layer on the base film layer. Here, the order in which the glossy layer and the adhesive layer are provided on the base film layer may be arbitrary, but it is preferable to provide the adhesive layer after disposing the primer layer and the glossy layer on the base film layer in this order.

[0110] In this case, one embodiment of the method for manufacturing a decorative film of the present invention includes a step of applying paint to a base film layer to prepare a primer layer, a step of applying paint to the primer layer to prepare a glossy layer, and a step of applying an adhesive to the surface of the base film layer on the side where the primer layer is not located to prepare an adhesive layer.

[0111] The method for producing the decorative film of the present invention may also include a step of providing a glossy layer, a primer layer, a clear layer, and an adhesive layer on the base film layer. Here, the order in which the glossy layer, the clear layer, and the adhesive layer are provided on the base film layer may be arbitrary, but it is preferable to provide the adhesive layer after arranging the primer layer, the glossy layer, and the clear layer on the base film layer in this order.

[0112] In this case, one embodiment of the method for manufacturing a decorative film of the present invention includes a step of applying paint to a base film layer to prepare a primer layer, a step of applying paint to the primer layer to prepare a glossy layer, a step of applying paint to the glossy layer to prepare a clear layer, and a step of applying an adhesive to the surface of the base film layer on the side where the primer layer is not located to prepare an adhesive layer. EXAMPLES

[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0114] [Example of decorative film manufacturing] <Preparation of glittering paint> Various aluminum flakes were dispersed in the below-described paint No. 1 by a known method to prepare paints for the bright layer of Examples 1 to 8 and Comparative Example 1. In addition, paint No. 2 was used to prepare paints for the bright layer of Examples 9, 11, and Comparative Example 2 in the same manner. Furthermore, paint No. 3 was used to prepare paints for the bright layer of Examples 10 and 15 in the same manner. Paint No. 4 was used to prepare paints for the bright layer of Example 12 in the same manner, and paint No. 5 was used to prepare paints for the bright layer of Examples 13 and 14 in the same manner.

[0115] <Paint No.1> The cellulose resin A, acrylic resin A, and acrylic resin B were mixed in a solid content mass ratio of cellulose resin A / acrylic resin A / acrylic resin B = 36 / 28 / 36 so that the Tg of the glossy layer would be as shown in Table 1, and dispersed by a known method to prepare a paint. The materials used are as follows. Cellulose resin A: Product name CAB-381-01, Tg 123°C, weight average molecular weight 50,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin A: Tg 80℃, weight average molecular weight 67,600, solid content 43% by mass, hydroxyl value 0 Acrylic resin B: Tg 62°C, weight average molecular weight 48,000, solid content 45% by mass, hydroxyl value 3.7 <Paint No.2> Cellulose resin B, acrylic resin C, and acrylic resin D were mixed in a solid mass ratio of cellulose resin B / acrylic resin C / acrylic resin D = 2 / 49 / 49 so that the Tg of the glittering layer was as shown in Table 2, and dispersed by a known method to prepare a paint before mixing with a curing agent. Isocyanate curing agent A was added to the paint so that the equivalent ratio was 1.0 and mixed to prepare a paint. The materials used are as follows. Cellulose resin B: Product name CAB-321-01, Tg 127°C, weight average molecular weight 12,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin C: Tg 88°C, weight average molecular weight 33,000, solid content 43% by mass, hydroxyl value 34, Acrylic resin D: Tg 33°C, weight average molecular weight 80,000, solid content 49% by mass, hydroxyl value 0 Isocyanate curing agent A: Product name Sumidur N3800, solid content 100% by mass, NCO group content 11.0% by mass, manufactured by Sumika Covestro Urethane Co., Ltd. <Paint No.3> Cellulose resin B, acrylic resin C, and acrylic resin D were mixed in a solid mass ratio of cellulose resin B / acrylic resin C / acrylic resin D = 2 / 49 / 49 so that the Tg of the glittering layer was as shown in Table 2, and dispersed by a known method to prepare a paint before mixing with a curing agent. Isocyanate curing agent B was added to the paint so that the equivalent ratio was 1.0 and mixed to prepare a paint. The materials used are as follows. Cellulose resin B: Product name CAB-321-01, Tg 127°C, weight average molecular weight 12,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin C: Tg 88°C, weight average molecular weight 33,000, solid content 43% by mass, hydroxyl value 34 Acrylic resin D: Tg 33°C, weight average molecular weight 80,000, solid content 49% by mass, hydroxyl value 0 Isocyanate curing agent B: Product name Desmodur XP2860, solid content 100% by mass, NCO group content 20.0% by mass, manufactured by Sumika Covestro Urethane Co., Ltd. <Paint No.4> Cellulose resin C and acrylic resin E were mixed in a solid mass ratio of cellulose resin C / acrylic resin E = 1 / 99 so that the Tg of the glittering layer was as shown in Table 2, and dispersed by a known method to prepare a paint before mixing with a curing agent. Isocyanate curing agent C was added to the paint so that the equivalent ratio was 1.0 and mixed to prepare a paint. The materials used are as follows. Cellulose resin C: Product name CAB551-0.2, Tg 100°C, weight average molecular weight 70,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin E: Tg 20°C, weight average molecular weight 35,000, solid content 54% by mass, hydroxyl value 27 Isocyanate curing agent C: Product name Sumidur N-75, solid content 75% by mass, NCO group content 22.0% by mass, manufactured by Sumika Covestro Urethane Co., Ltd. <Paint No.5> Cellulose resin A, acrylic resin F, and acrylic resin D were mixed in a solid mass ratio of cellulose resin A / acrylic resin F / acrylic resin D = 10 / 55 / 35 so that the Tg of the glittering layer was as shown in Table 2, and dispersed by a known method to prepare a paint before mixing with a curing agent. Isocyanate curing agent A was added to the paint so that the equivalent ratio was 1.0 and mixed to prepare a paint. The materials used are as follows. Cellulose resin A: Product name CAB-381-01, Tg 123°C, weight average molecular weight 50,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin F: Tg 90°C, weight average molecular weight 42,000, solid content 50% by mass, hydroxyl value 16 Acrylic resin G: Tg 65°C, weight average molecular weight 27,000, solid content 50% by mass, hydroxyl value 10 Isocyanate curing agent A: Product name Sumidur N3800, solid content 100% by mass, NCO group content 11.0% by mass, manufactured by Sumika Covestro Urethane Co., Ltd.

[0116] Aluminum flake A: solid content 70% by mass, average particle size 14.2 μm, average aspect ratio 71, resin-coated aluminum, manufactured by Toyo Aluminum Co., Ltd. Aluminum flake B: solid content 64% by mass, average particle size 9 μm, average aspect ratio 60, resin-coated aluminum, manufactured by Toyo Aluminum Co., Ltd. Aluminum flake C: solid content 70% by mass, average particle size 33 μm, average aspect ratio 41, resin-coated aluminum, manufactured by Toyo Aluminum Co., Ltd.

[0117] <Preparation of clear paint> The paint No. 6 described below was used as the paint for the clear layer in Example 8.

[0118] <Paint No.6> Cellulose resin B, acrylic resin C, and acrylic resin D were mixed in a solid mass ratio of cellulose resin B / acrylic resin C / acrylic resin D = 2 / 49 / 49 so that the Tg of the clear layer was as shown in Table 1, and dispersed by a known method to prepare a paint before mixing with a curing agent. Isocyanate curing agent A was added to the paint so that the equivalent ratio was 1.0, and mixed to prepare a paint. The materials used are as follows. Cellulose resin B: Product name CAB-321-01, Tg 127°C, weight average molecular weight 12,000, solid content 100% by mass, manufactured by Eastman Chemical Japan Acrylic resin C: Tg 88°C, weight average molecular weight 33,000, solid content 43% by mass, hydroxyl value 34, Acrylic resin D: Tg 33°C, weight average molecular weight 80,000, solid content 49% by mass, hydroxyl value 0 Isocyanate curing agent A: Product name Sumidur N3300, solid content 100% by mass, NCO group content 21.8% by mass, manufactured by Sumika Covestro Urethane Co., Ltd.

[0119] <Preparation of decorative film> The above-mentioned glittering paint was applied onto the (A) base film layer using an air spray so that a (B) glittering layer having a film thickness when dried (hereinafter referred to as "dry film thickness") of 10 μm was obtained, and then the layer was dried at 80° C. for 30 minutes to form the (B) glittering layer. However, in Example 6, the film thickness of the (B) glittering layer was 5 μm, and in Example 7, the film thickness of the (B) glittering layer was 40 μm.

[0120] For Example 8, the above-mentioned clear coating was applied onto the (B) shiny layer using an air spray so as to obtain a (D) clear layer having a film thickness when dried (hereinafter referred to as the dry film thickness) of 20 μm, and then the layer was dried at 80° C. for 30 minutes to form the (D) clear layer.

[0121] For the (A) base film layer on which the (B) glossy layer was formed and the (A) base film layer on which the (B) glossy layer and (D) clear layer were formed, Nitto Denko's "No. 5015" was then bonded as an adhesive layer to the surface of the (A) base film layer on the side on which the (B) glossy layer was not formed, to produce a decorative film. The decorative films produced here were a decorative film having a three-layer structure of adhesive layer / base film layer / lustrous layer and a decorative film having a four-layer structure of adhesive layer / base film layer / lustrous layer / clear layer.

[0122] [Example of manufacturing a molded product decorated with a decorative film] The pressure was reduced using a vacuum forming device (product name: NGF, manufactured by Fuse Vacuum), the decorative film was heated using a near-infrared lamp, and the film was molded and pressure-bonded onto a PP molded substrate to obtain a decorated article.

[0123] The resulting decorative films and decorated articles were evaluated according to the following test methods.

[0124] ●Glass transition temperature (Tg): The loss modulus and storage modulus of each layer were measured at each temperature under the following measurement conditions using a solid viscoelasticity measuring device (e.g., RSA-GII (manufactured by TA Instruments)). The loss tangent was calculated from the loss modulus and storage modulus, a temperature change curve of the loss tangent was created, and the spectrum peak value of the loss tangent was determined as the glass transition point (Tg). <Measurement conditions> Temperature range: -50℃~200℃ Heating rate: 5℃ / min Measurement length: 20.0 mm Measurement width: 5.0mm Frequency: 1Hz Distortion: 0.05%

[0125] ●Decorative film elongation rate: A 10 mm x 30 mm sample (the thickness is the thickness of the decorative film in the table) was prepared from the decorative film, and a tensile test was performed on the sample using a tensile tester (AGS-X, manufactured by SHIMADZU) under the measurement conditions below to measure the elongation (%) of the decorative film. <Measurement conditions> Tensile speed: 5mm / min Test temperature: The temperature at which the decorative film is applied to the substrate (molding temperature)

[0126] ●Formability of decorative film: The formability of the decorative film means the property of being able to conform to the surface shape of a substrate when the decorative film is applied to the substrate. The formability of the decorative film was visually evaluated according to the following criteria. The decorative films rated as ⊚ or ◯ were free of defects such as cracks or fissures on the surface and had excellent appearance. (standard) ◎:Can conform to curved substrates with dimensions of 200mm length x 100mm width x 2mm thickness ○: Able to follow when a flat plate of length 200 mm x width 100 mm x thickness 2 mm is used as a molded substrate ×: The decorative film was unable to conform to the shape of the substrate even when it was a flat molded substrate, and defects such as cracks and fractures were observed on the surface of the decorative film.

[0127] Appearance of the decorated item (visual inspection): The appearance of the entire surface of the decorated article was visually evaluated according to the following criteria: The base material used was a curved molded substrate measuring 200 mm in length, 100 mm in width, and 2 mm in thickness. (standard) ◯: The decorative film applied to the molded substrate gave the resulting decorated article a high sense of brilliance. In addition, no unevenness in color or decoration was observed in the decorated article. Δ: The resulting decorated article had no uneven color or decoration, but the design, such as the sense of brilliance, was slightly reduced. ×: Color unevenness or decoration unevenness was observed in the resulting decorated article.

[0128] Adhesion: The surface of the decorated article was subjected to an adhesion test according to the JIS K-5400-8.5.2 cross-cut tape method, and evaluated according to the following criteria. (standard) ○: No abnormalities such as peeling or chipping are observed ×: If abnormality is observed

[0129] Chemical resistance The chemical resistance test of the decorated article was conducted in accordance with "JIS K 5600-6-1", liquid resistance (general method) test method, drip method. The test liquid was a 0.1N aqueous solution of sodium hydroxide, which was placed in a thermostatic chamber maintained at 50±2°C and left for 3 hours, after which the test specimen was rinsed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. Similarly, a 0.1N aqueous solution of sulfuric acid was used as the test liquid, which was left for 24 hours under standard conditions (25±2°C, 50±5% RH), after which the test panel was rinsed with water and wiped, and the coating surface condition of the test area was visually evaluated according to the following criteria. (standard) ◎: No change on the coating surface ○: Slight discoloration is observed on the coating surface. ×: Discoloration was observed on the coating surface.

[0130] Example 1 (A) ABS film (acrylonitrile-butadiene-styrene copolymer resin film) was used as the base film layer. A glittering paint was prepared by mixing aluminum flake A with paint No. 1 in an amount of 7.5 parts by mass of glittering pigment per 100 parts by mass of resin. A decorative film was produced according to the above <Production of decorative film>. The thickness of the decorative film was 1010 μm. Also, a decorated article was produced according to the above-mentioned "Production Example of Molded Article Decorated with Decorative Film". The heating temperature condition of the decorative film was 140°C. The above evaluations were carried out, and the results are shown in Table 1.

[0131] Example 2 A glittering paint was prepared by mixing aluminum flake A with 12.5 parts by mass of glittering pigment per 100 parts by mass of resin in paint No. 1. Except for this, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 1.

[0132] Example 3 A glittering paint was prepared by mixing aluminum flake A with 100 parts by mass of resin and 30.0 parts by mass of glittering pigment into paint No. 1. Except for this, the same procedure as in Example 1 was followed to obtain a decorative article. The above evaluations were carried out, and the results are shown in Table 1.

[0133] Example 4 A glittering paint was prepared by mixing aluminum flakes B in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin in paint No. 1. Except for this, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 1.

[0134] Example 5 A glittering paint was prepared by mixing aluminum flake C with 12.5 parts by mass of glittering pigment per 100 parts by mass of resin in paint No. 1. Except for this, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 1.

[0135] Example 6 A glittering paint was prepared by mixing aluminum flake A with paint No. 1 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin, and the thickness of the glittering layer (B) formed from the glittering paint was set to 5 μm. Otherwise, a decorative article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 1.

[0136] Example 7 A glittering paint was prepared by mixing aluminum flake A with paint No. 1 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin, and the thickness of the glittering layer (B) formed from the glittering paint was set to 40 μm. A decorated article was obtained in the same manner as in Example 1 except for the above. The above evaluations were carried out, and the results are shown in Table 1.

[0137] Example 8 A glittering paint was prepared by mixing 12.5 parts by mass of aluminum flake A with 100 parts by mass of resin in paint No. 1. In addition, paint No. 6 was used as a paint for the clear layer, and a clear layer (D) was provided as a protective layer on the glittering layer (B). Otherwise, a decorative article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 1.

[0138] Comparative Example 1 A glittering paint was prepared by mixing aluminum flake A with 100 parts by mass of resin and 5.0 parts by mass of glittering pigment into paint No. 1. Except for this, the same procedure as in Example 1 was followed to obtain a decorative article. The above evaluations were carried out, and the results are shown in Table 1.

[0139] [Table 1]

[0140] In the table, the item "Tg difference (TgA-TgB or TgD)" shows, for Examples 1 to 7 and Comparative Example 1, the value of Tg(A)-Tg(B) where Tg(A) is the glass transition point (°C) of the (A) base film layer and Tg(B) is the glass transition point (°C) of the (B) glossy layer, and for Example 8, the value of Tg(A)-Tg(D) where Tg(A) is the glass transition point (°C) of the (A) base film layer and Tg(D) is the glass transition point (°C) of the (D) clear layer. The item "molding temperature" indicates the heating temperature conditions of the decorative film when producing a decorated article, and indicates the temperature when the decorative film is applied to a substrate.

[0141] Example 9 A glittering paint was prepared by mixing aluminum flake A with 12.5 parts by mass of glittering pigment per 100 parts by mass of resin in paint No. 2. Except for this, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0142] Example 10 (A) An acrylic film (manufactured by Mitsubishi Chemical) was used as the base film layer. Aluminum flake A was mixed with paint No. 2 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 120°C. Otherwise, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0143] Example 11 (A) A polyvinyl chloride (PVC) film (manufactured by Okamoto) was used as the base film layer. Aluminum flake A was mixed with paint No. 2 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 80°C. Otherwise, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0144] Example 12 (A) Thermoplastic polyurethane (TPU) film (manufactured by Okura Kogyo Co., Ltd.) was used as the base film layer. Aluminum flake A was mixed with paint No. 4 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 80°C. Otherwise, the decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0145] (Example 13) (A) A polycarbonate film (manufactured by Teijin) was used as the base film layer. Aluminum flake A was mixed with paint No. 5 in an amount of 12.5 parts by mass of the luster pigment per 100 parts by mass of the resin content to prepare a luster paint. The heating temperature condition of the decorative film when producing the decorated article was 150°C. Otherwise, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0146] Example 14 (A) A PVC film (manufactured by Lonseal) was used as the base film layer. Aluminum flake A was mixed with paint No. 5 in an amount of 12.5 parts by mass of the glittering pigment per 100 parts by mass of the resin content to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 120°C. Otherwise, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0147] Example 15 (A) An ABS film (manufactured by Okamoto) with a glass transition point of 114.3°C was used as the base film layer. Aluminum flake A was mixed with paint No. 3 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 120°C. Otherwise, the decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0148] Comparative Example 2 (A) A polycarbonate film (manufactured by Teijin) was used as the base film layer. Aluminum flake A was mixed with paint No. 2 in an amount of 12.5 parts by mass of glittering pigment per 100 parts by mass of resin to prepare a glittering paint. The heating temperature condition of the decorative film when producing the decorated article was 160°C. Otherwise, a decorated article was obtained in the same manner as in Example 1. The above evaluations were carried out, and the results are shown in Table 2.

[0149] [Table 2]

[0150] In the table, the "Tg difference (TgA-TgB)" column shows the value of Tg(A)-Tg(B) when the glass transition point (°C) of (A) base film layer is Tg(A) and the glass transition point (°C) of (B) glossy layer is Tg(B). The item "molding temperature" indicates the heating temperature conditions of the decorative film when producing a decorated article, and indicates the temperature when the decorative film is applied to a substrate.

Claims

1. A decorative film for decorating a substrate, The decorative film has (A) a base film layer, (B) a glossy layer, and (C) an adhesive layer, The (B) glittering layer contains a glittering pigment and a binder resin, and a mass ratio of the glittering pigment to the binder resin in the (B) glittering layer is within a range of 7.5:100 to 30:100; A decorative film, characterized in that the decorative film has an elongation percentage of 30% or more at a temperature when the decorative film is applied to the substrate.

2. The (A) base film layer has a glass transition temperature in the range of −20° C. to 140° C., When the glass transition point (° C.) of the (A) base film layer is Tg(A) and the glass transition point (° C.) of the (B) glossy layer is Tg(B), Tg(A) and Tg(B) satisfy the following relational formula (1): -20℃ ≦ Tg (A) - Tg (B) ≦ 50℃ ... Formula (1) The decorative film according to claim 1 , wherein the above-mentioned is satisfied.

3. The decorative film further has a clear layer (D) on the glossy layer (B), 3. The decorative film according to claim 1, wherein the clear layer (D) has an ultraviolet ray transmittance of 30% or less.

4. The film further includes a primer layer (E) between the base film layer (A) and the glossy layer (B), 3. The decorative film according to claim 1, wherein the primer layer (E) has a gel fraction of 80% or more.

5. 3. The decorative film according to claim 1, wherein the luster pigment comprises a vapor-deposited aluminum pigment and / or a resin-coated metal pigment.

6. A method for producing a decorative film for decorating a substrate, the decorative film having (A) a substrate film layer, (B) a glossy layer, and (C) an adhesive layer, The method includes a step of providing a glossy layer (B) and an adhesive layer (C) on a base film layer (A), The (B) glittering layer contains a glittering pigment and a binder resin, and a mass ratio of the glittering pigment to the binder resin in the (B) glittering layer is within a range of 7.5:100 to 30:100; A method for producing a decorative film, characterized in that the decorative film has an elongation of 30% or more at a temperature when the decorative film is applied to the substrate.

Citation Information

Patent Citations

  • Metallic-tone laminated film and decorated molded body using the same

    JP2004299220A

  • Decorative sheet and decorative resin molded body

    JP2015066855A

  • Vapor deposition sheet for decoration

    JP2021133615A

  • Decorative film

    JP2021160222A

Cited By

  • Decorative sheet and resin molded article

    JP2025171927A

  • Decorative sheets and resin molded products

    JP7758134B1