Dispersion liquid, method for producing dispersion liquid, method for producing elastomer composition, and method for manufacturing gas seal member for high-pressure hydrogen equipment

A dispersion liquid with a specific particle size distribution of fibrous carbon nanostructures in elastomers enhances the durability of gas seal members in high-pressure hydrogen equipment by preventing blister failure, addressing the durability challenge.

JP2024146538AInactive Publication Date: 2024-10-15ZEON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059508
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Gas seal members used in high-pressure hydrogen equipment are prone to blister failure due to repeated contact with high-pressure hydrogen and rapid depressurization, necessitating improved durability.

Method used

A dispersion liquid containing an elastomer, fibrous carbon nanostructures, and a solvent is formulated with a specific particle size distribution to create gas seal members that suppress blister failure, using a dispersion process to achieve enhanced durability.

Benefits of technology

The solution effectively suppresses blister failure in gas seal members for high-pressure hydrogen equipment, ensuring improved durability and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146538000001_ABST
    Figure 2024146538000001_ABST
Patent Text Reader

Abstract

To provide a dispersion liquid or the like by which a gas seal member for high-pressure hydrogen equipment which has excellent durability and can sufficiently suppress the occurrence of blister rupture.SOLUTION: A dispersion liquid used for a gas seal member for high-pressure hydrogen equipment includes an elastomer, a fibrous carbon nano structure, and a solvent which dissolves the elastomer. The dispersion liquid contains the fibrous carbon nano structure by larger than 0.5 pt.mass and less than 3 pts.mass per 100 pts.mass of the elastomer, where the particle size distribution of the fibrous carbon nano structure in the dispersion liquid satisfies the following conditions (1) and (2): (1) D50≤20 μm (2) D90-D10≤45 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersion used in a gas sealing member for high-pressure hydrogen equipment, a method for producing the dispersion, a method for producing an elastomer composition used in a gas sealing member for high-pressure hydrogen equipment, and a method for producing a gas sealing member for high-pressure hydrogen equipment. [Background technology]

[0002] 2. Description of the Related Art Gas seal members such as packings and gaskets have been used to prevent gas leakage. Such gas seal members are sometimes used in high-pressure hydrogen equipment such as hydrogen stations for fuel cell vehicles.

[0003] Gas seal members used in high-pressure hydrogen equipment are exposed to high-pressure hydrogen of, for example, 35 MPa or more and 105 MPa or less, and are therefore required to suppress the occurrence of failure modes caused by high-pressure hydrogen, such as extrusion failure and blister failure. Here, "extrusion rupture" refers to rupture caused by the gas seal member protruding from a specified installation position (for example, an installation groove) due to contact with high-pressure hydrogen and becoming caught in gaps around the installation position. "Blister rupture" refers to rupture caused by hydrogen that has permeated the inside of the gas seal member due to contact with high-pressure hydrogen, remaining inside the gas seal member during rapid decompression, and expanding, causing the gas seal member to burst.

[0004] For example, Patent Document 1 discloses a gas seal member that can suppress both the occurrence of extrusion damage and blister damage by forming the gas seal member by crosslinking an elastomer composition containing an elastomer and a fibrous carbon nanostructure such as a carbon nanotube. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2021 / 193667 Summary of the Invention [Problem to be solved by the invention]

[0006] Gas seal members used in high-pressure hydrogen equipment are required to have even greater durability because they are prone to blister damage caused by repeated contact with high-pressure hydrogen and rapid depressurization.

[0007] An object of the present invention is to provide a dispersion etc. capable of producing a gas seal member for high-pressure hydrogen equipment having even greater durability. [Means for solving the problem]

[0008] The inventors have conducted intensive research to achieve the above-mentioned object, and have discovered that by dispersing a dispersion containing an elastomer, fibrous carbon nanostructures, and a solvent that dissolves the elastomer so that the particle size distribution of the fibrous carbon nanostructures falls within a predetermined range, and then using this dispersion to manufacture a gas sealing member, it is possible to provide a gas sealing member for high-pressure hydrogen equipment that is even more durable and primarily suppresses the occurrence of blister breakage, and thus completed the present invention.

[0009] [1] The dispersion of the present invention is a dispersion used for a gas sealing component for high-pressure hydrogen equipment, and contains an elastomer, fibrous carbon nanostructures, and a solvent that dissolves the elastomer, and contains 0.5 parts by mass or more and less than 3 parts by mass of the fibrous carbon nanostructures per 100 parts by mass of the elastomer, and the particle size distribution of the fibrous carbon nanostructures in the dispersion satisfies the following conditions (1) and (2). (1) D50≦20μm (2) D90-D10≦45μm Here, D50, D10, and D90 each indicate the particle diameter when the particle size distribution of the fibrous single-layer nanostructure in the dispersion is measured, and D50 is the diameter of the particle where the cumulative value of the particles is 50% (= the median value, also called the median diameter), D10 is the diameter of the particle where the cumulative value of the particles is 10%, and D90 is the diameter of the particle where the cumulative value of the particles is 90%. According to the present invention, by setting the particle size distribution of the fibrous carbon nanostructures in the dispersion liquid within the above range, the occurrence of blister breakage can be sufficiently suppressed, and the durability of gas sealing members for high-pressure hydrogen equipment can be further improved.

[0010] [2] In the dispersion liquid of the above [1], it is preferable that the following condition (3) is satisfied, since this can further suppress the occurrence of blister breakage. (3) D90-D10≦35μm

[0011] [3] In the dispersion of [1] or [2] above, the elastomer may be at least one rubber selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, ethylene propylene diene rubber, silicone rubber, and fluororubber. This configuration can further suppress the occurrence of blister breakage.

[0012] [4] In any one of the dispersions [1] to [3] above, the fibrous carbon nanostructures preferably contain single-walled carbon nanotubes. With this configuration, the occurrence of blister breakage can be further suppressed.

[0013] [5] The method for producing a dispersion liquid according to the present invention is a method for producing a dispersion liquid used for a gas seal member for high-pressure hydrogen equipment, and includes a dispersion step of mixing and dispersing an elastomer, fibrous carbon nanostructures, and a solvent that dissolves the elastomer to obtain a dispersion liquid, the dispersion liquid containing 0.5 parts by mass or more and less than 3 parts by mass of the fibrous carbon nanostructures per 100 parts by mass of the elastomer, and the dispersion step is performed so that the particle size distribution of the fibrous carbon nanostructures in the dispersion liquid satisfies the following conditions (1) and (2), where D10, D50, and D90 are as described above. (1) D50≦20μm (2) D90-D10≦45μm

[0014] [6] A method for producing an elastomer composition according to the present invention is a method for producing an elastomer composition used for a gas sealing member for high-pressure hydrogen equipment, comprising the steps of: preparing a dispersion liquid obtained by any one of the dispersion liquids [1] to [4] above or the dispersion liquid production method [5] above; and removing the solvent from the dispersion liquid to obtain the elastomer composition.

[0015] [7] Furthermore, the method for producing a gas sealing member for high-pressure hydrogen equipment according to the present invention includes the steps of obtaining a crosslinkable elastomer composition comprising the elastomer composition obtained by the method for producing an elastomer composition according to the above [6] and a crosslinking agent, and obtaining a crosslinked product by crosslinking the crosslinkable elastomer composition. The crosslinked product is then appropriately molded or processed to be used as a gas sealing member for high-pressure hydrogen equipment. According to these manufacturing methods, it is possible to provide a gas seal member for high-pressure hydrogen equipment that is excellent in durability and can sufficiently prevent the occurrence of blister breakage. Effect of the Invention

[0016] According to the present invention, it is possible to provide a dispersion capable of producing a gas sealing member for high-pressure hydrogen equipment that can sufficiently suppress the occurrence of blister breakage and has excellent durability, a method for producing the dispersion, a method for producing an elastomer composition, and a method for producing a gas sealing member for high-pressure hydrogen equipment. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is an explanatory diagram showing a schematic configuration of a hydrogen station. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail. <High pressure hydrogen equipment> The gas seal member for high-pressure hydrogen equipment obtained by using the dispersion of the present invention can be used as a gas seal member such as a packing or gasket in high-pressure hydrogen equipment such as a hydrogen station for a fuel cell vehicle. An example of such high-pressure hydrogen equipment is high-pressure hydrogen equipment that includes a container filled with high-pressure hydrogen and a gas sealing member for high-pressure hydrogen equipment that comes into contact with the high-pressure hydrogen filled in the container to prevent leakage of the high-pressure hydrogen. Here, "high-pressure hydrogen equipment" means equipment that handles high-pressure hydrogen (e.g., 35 MPa or more and 105 MPa or less), and specific examples include hydrogen production equipment (e.g., hydrogen production equipment 111 in FIG. 1 described later), hydrogen gas compressors (e.g., hydrogen gas compressor (booster) 112 in FIG. 1 described later), gas accumulators (e.g., gas accumulator (pressure accumulator) 113 in FIG. 1 described later), dispensers (e.g., dispenser 114 in FIG. 1 described later), and fuel cells mounted on vehicles (e.g., vehicle (fuel cell vehicle) 120 in FIG. 1 described later) used in hydrogen stations.

[0019] <Gas seal materials for high-pressure hydrogen equipment> The gas seal member for high-pressure hydrogen equipment is a gas seal member used in the above-mentioned high-pressure hydrogen equipment, and can be obtained by crosslinking and molding a composition (crosslinkable elastomer composition) obtained by adding a crosslinking agent to an elastomer composition under specified conditions to form a crosslinked product.

[0020] <Elastomer composition> The elastomer composition contains an elastomer and a fibrous carbon nanostructure, and the fibrous carbon nanostructure is present in an amount of 0.5 parts by mass or more and less than 3 parts by mass per 100 parts by mass of the elastomer. This elastomer composition can be obtained by preparing a dispersion containing an elastomer, the fibrous carbon nanostructure, and a solvent that dissolves the elastomer (preparation step), and removing the solvent from this dispersion (solvent removal step).

[0021] <Dispersion> The dispersion of the present invention is used for a gas seal member for high-pressure hydrogen equipment, and is required to contain 0.5 parts by mass or more and less than 3 parts by mass of fibrous carbon nanostructures per 100 parts by mass of elastomer. In addition, as will be described later, the particle size distribution of the fibrous carbon nanostructures in the dispersion satisfies the following conditions (1) and (2). (1) D50≦20μm (2) D90-D10≦45μm

[0022] <Elastomer> The elastomer contained in the dispersion is not particularly limited, and any known elastomer used in forming a gas seal member for high-pressure hydrogen equipment can be used. Specifically, the elastomer can be, for example, natural rubber, butadiene rubber, styrene butadiene rubber, isoprene rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (H-NBR), fluororubber, chloroprene rubber, ethylene propylene rubber, halogenated butyl rubber, polyisobutylene rubber, silicone rubber, ethylene propylene diene rubber (EPDM), etc. These may be used alone or in combination of two or more. Among the above, the elastomer is preferably at least one rubber selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, ethylene propylene diene rubber, silicone rubber and fluororubber.

[0023] Here, the elastomer contained in the gas seal member used in a hydrogen gas compressor (booster) (e.g., -20°C to 180°C: 95 MPa) is preferably fluororubber (e.g., FKM), the elastomer contained in the gas seal member used in a gas accumulator (pressure accumulator) (e.g., -20°C to 50°C: 95 MPa) is preferably nitrile rubber (NBR) or hydrogenated nitrile rubber (H-NBR), and the elastomer contained in the gas seal member used in a dispenser (e.g., -40°C to 50°C: 82 MPa) is preferably ethylene propylene diene rubber (EPDM).

[0024] <Fibrous carbon nanostructures> Examples of fibrous carbon nanostructures contained in this dispersion include cylindrical carbon nanostructures such as carbon nanotubes (CNTs, hereinafter referred to as "CNTs" as appropriate), and non-cylindrical carbon nanostructures such as carbon nanostructures in which a six-membered carbon ring network is formed into a flattened cylinder. By incorporating fibrous carbon nanostructures in the elastomer composition, the strength of the gas seal member for high-pressure hydrogen equipment can be ensured, and the occurrence of extrusion damage and blister damage can be suppressed.

[0025] The average length of the fibrous carbon nanostructure is not particularly limited, but is usually 100 μm or more and 1000 μm or less, preferably 150 μm or more, more preferably 250 μm or more, preferably 750 μm or less, and more preferably 500 μm or less. If the average length is within the above range, the occurrence of blister breakage can be effectively suppressed.

[0026] The type of fibrous carbon nanostructure is not particularly limited, and may be composed only of single-walled carbon nanotubes (single-walled CNTs), may be composed only of multi-walled carbon nanotubes (multi-walled CNTs), may be a mixture of single-walled CNTs and multi-walled CNTs, or may be a mixture of carbon nanotubes (CNTs) and fibrous carbon nanostructures other than CNTs. Here, single-walled CNTs are preferably used as the fibrous carbon nanostructures, since they are less susceptible to hydrogen adsorption and have a high reinforcing effect compared to multi-walled CNTs. In order to further suppress the occurrence of both extrusion failure and blister failure in a gas sealing member formed using the elastomer composition, the proportion of single-walled CNTs per 100 fibrous carbon nanostructures is preferably 50 or more, more preferably 70 or more, even more preferably 90 or more, and particularly preferably 100.

[0027] In the elastomer composition, it is preferable to use a fibrous carbon nanostructure containing single-walled CNTs as the fibrous carbon nanostructure, because the use of a fibrous carbon nanostructure containing single-walled CNTs in this manner can further suppress the occurrence of blister breakage.

[0028] The fibrous carbon nanostructure preferably has a t-plot obtained from an adsorption isotherm that shows an upwardly convex shape. By using a fibrous carbon nanostructure having a t-plot obtained from an adsorption isotherm that shows an upwardly convex shape, a gas seal member capable of further suppressing the occurrence of blister breakage can be formed. It is more preferable that the fibrous carbon nanostructure is not subjected to an opening treatment for the CNTs and that the t-plot shows an upwardly convex shape.

[0029] Generally, adsorption is a phenomenon in which gas molecules are removed from the gas phase to a solid surface, and is classified into physical adsorption and chemical adsorption depending on the cause. The nitrogen gas adsorption method used to obtain t-plots utilizes physical adsorption. Normally, if the adsorption temperature is constant, the number of nitrogen gas molecules adsorbed to a fibrous carbon nanostructure increases with increasing pressure. Also, a plot of relative pressure (the ratio of the pressure P at adsorption equilibrium to the saturated vapor pressure P0) on the horizontal axis and the amount of nitrogen gas adsorption on the vertical axis is called an "isotherm." When the amount of nitrogen gas adsorption is measured while increasing the pressure, it is called an "adsorption isotherm," and when the amount of nitrogen gas adsorption is measured while decreasing the pressure, it is called a "desorption isotherm."

[0030] The t-plot is obtained by converting the relative pressure into the average thickness t (nm) of the nitrogen gas adsorption layer in an adsorption isotherm measured by a nitrogen gas adsorption method. That is, the t-plot of the fibrous carbon nanostructure is obtained by determining the average thickness t of the nitrogen gas adsorption layer corresponding to the relative pressure from a known standard isotherm in which the average thickness t of the nitrogen gas adsorption layer is plotted against the relative pressure P / P0, and performing the above conversion (t-plot method by de Boer et al.).

[0031] Here, in a sample having pores on the surface, the growth of the nitrogen gas adsorption layer is classified into the following processes (1) to (3). The slope of the t-plot changes depending on the processes (1) to (3) below. (1) The process of forming a monolayer of nitrogen molecules on the entire surface (2) Formation of multilayer adsorption and the associated capillary condensation filling process in the pores (3) The formation of multilayer adsorption on an apparently non-porous surface whose pores are filled with nitrogen

[0032] In the t-plot of the fibrous carbon nanostructure, in the region where the average thickness t of the nitrogen gas adsorption layer is small, the plot is located on a straight line passing through the origin, whereas as t increases, the plot is shifted downward from the straight line, and preferably shows an upwardly convex shape. Such a t-plot shape indicates that the ratio of the internal specific surface area to the total specific surface area of ​​the fibrous carbon nanostructure is large, and that a large number of openings are formed in the carbon nanostructures constituting the fibrous carbon nanostructure. As a result of the formation of a large number of openings, it is presumed that the gas that has penetrated into the inside of the fibrous carbon nanostructure can easily pass through and escape from the fibrous carbon nanostructure (i.e., the gas seal member including the fibrous carbon nanostructure is less likely to cause blister destruction).

[0033] The bending point of the t-plot of the fibrous carbon nanostructure is preferably in the range of 0.2≦t(nm)≦1.5, more preferably in the range of 0.45≦t(nm)≦1.5, and even more preferably in the range of 0.55≦t(nm)≦1.0. When the bending point of the t-plot is in the above range, the properties of the fibrous carbon nanostructure are further improved, and the occurrence of blister breakage can be further suppressed. Here, the "position of the bending point" is the intersection point of the approximation line A in the above-mentioned process (1) and the approximation line B in the above-mentioned process (3) in the t-plot.

[0034] Furthermore, the ratio (S2 / S1) of the internal specific surface area S2 to the total specific surface area S1 obtained from the t-plot of the fibrous carbon nanostructure is preferably 0.05 or more, more preferably 0.06 or more, even more preferably 0.08 or more, and preferably 0.30 or less. If S2 / S1 is 0.05 or more and 0.30 or less, the properties of the fibrous carbon nanostructure can be further improved, and the occurrence of blister breakage can be further suppressed. The total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure are not particularly limited. 2 / g or more 1400m 2 / g or less, and 2 / g or more 1200m 2 / g or less. 2 / g or more 540m 2 It is preferable that the molecular weight is not more than 1 / g. Here, the total specific surface area S1 and the internal specific surface area S2 of the fibrous carbon nanostructure can be obtained from the t-plot. Specifically, first, the total specific surface area S1 can be obtained from the slope of the approximation line in step (1), and the external specific surface area S3 can be obtained from the slope of the approximation line in step (3). Then, the internal specific surface area S2 can be calculated by subtracting the external specific surface area S3 from the total specific surface area S1.

[0035] Incidentally, the measurement of the adsorption isotherm of the fibrous carbon nanostructure, the creation of t-plots, and the calculation of the total specific surface area S1 and the internal specific surface area S2 based on the analysis of the t-plots can be performed, for example, using a commercially available measuring device, "BELSORP (registered trademark)-mini" (manufactured by BEL Japan Co., Ltd.).

[0036] The BET specific surface area of ​​the fibrous carbon nanostructure is 600m 2 / g or more, and 2 / g or more is more preferable, and 1250m 2 / g or more is more preferable, and 2 / g or less, and 2 When the BET specific surface area of ​​the fibrous carbon nanostructure is within the above range, it is possible to obtain a sufficient reinforcing effect and to adequately disperse the fibrous carbon nanostructure in the crosslinked product, thereby further suppressing the occurrence of blister breakage. In the present invention, the term "BET specific surface area" refers to a nitrogen adsorption specific surface area measured by the BET method.

[0037] According to the super growth method described below, CNTs as fibrous carbon nanostructures are obtained as aggregates (oriented aggregates) oriented in a direction approximately perpendicular to a substrate on the surface of which is provided a catalyst layer for carbon nanotube growth. The mass density of the fibrous carbon nanostructures as the aggregates is 0.002 g / cm. 3 More than 0.2g / cm 3 It is preferable that the mass density is 0.2 g / cm or less. 3 If the mass density is less than 0.002 g / cm, the bonds between the fibrous carbon nanostructures are weak, and the fibrous carbon nanostructures can be uniformly dispersed in the elastomer. 3 If the above conditions are met, the integrity of the fibrous carbon nanostructure can be improved and it can be prevented from falling apart, making it easier to handle.

[0038] The fibrous carbon nanostructures having the above-mentioned properties can be efficiently manufactured by, for example, forming a catalyst layer on the substrate surface by a wet process in a method (super-growth method; see International Publication No. 2006 / 011655) in which a trace amount of oxidant (catalyst activation material) is present in the system when supplying raw material compounds and a carrier gas onto a substrate having a catalyst layer for producing carbon nanotubes on its surface to synthesize CNTs by chemical vapor deposition (CVD). Carbon nanotubes obtained by the super-growth method may be referred to as "SGCNTs" below.

[0039] The fibrous carbon nanostructure produced by the super-growth method may be composed of only SGCNTs, or may be composed of SGCNTs and non-cylindrical carbon nanostructures. Specifically, the fibrous carbon nanostructure may include a single-layer or multi-layer flat cylindrical carbon nanostructure (hereinafter, sometimes referred to as "graphene nanotape (GNT)") having tape-shaped portions over its entire length in which the inner walls are close to or bonded to each other.

[0040] <Solvent> The solvent contained in the dispersion is not particularly limited as long as it is a solvent capable of dissolving the elastomer, and examples thereof include ketones such as methyl ethyl ketone (hereinafter MEK) and acetone, and ethers such as tetrahydrofuran (hereinafter THF). The solvent may be used alone or in combination of two or more. For example, when FEPM is used as the elastomer, examples of the solvent include THF. When FKM is used as the elastomer, examples of the solvent include MEK. When NBR is used as the elastomer, examples of the solvent include MEK.

[0041] <Dispersion liquid preparation process> The dispersion of the present invention is a dispersion used for gas sealing components for high-pressure hydrogen equipment, and can be obtained by mixing and dispersing an elastomer, fibrous carbon nanostructures, and a solvent that dissolves the elastomer (dispersion process) so that the particle size distribution of the fibrous carbon nanostructures in the dispersion satisfies the following conditions (1) and (2), and preferably also satisfies condition (3).

[0042] <Dispersion process> The dispersion can be obtained, for example, by preparing a fibrous carbon nanostructure dispersion by dispersing fibrous carbon nanostructures in a solvent through a dispersion process using an ultrasonic homogenizer or a wet jet mill, and then adding and mixing the elastomer to be blended to the fibrous carbon nanostructure dispersion to dissolve the elastomer.

[0043] <Mixing and Dispersion Processing> The particle size distribution of the fibrous carbon nanostructures in the dispersion satisfies the following conditions (1) and (2), and preferably also satisfies (3). (1) D50≦20μm (2) D90-D10≦45μm (3) D90-D10≦35μm Here, D50, D10, and D90 each indicate the particle diameter when the particle size distribution of the fibrous single-layer nanostructure in the dispersion is measured, and D50 is the diameter of the particle where the cumulative value of the particles is 50% (= the median value, also called the median diameter), D10 is the diameter of the particle where the cumulative value of the particles is 10%, and D90 is the diameter of the particle where the cumulative value of the particles is 90%.

[0044] The particle size distribution (D10, D50, D90) of the fibrous carbon nanostructure can be determined by diluting the dispersion obtained by the dispersion process with a solvent such as methyl ethyl ketone, and measuring the particle size at a transmittance of 88% using a laser diffraction particle size distribution meter (e.g., HORIBA LA-950).

[0045] To satisfy the above conditions, examples of dispersion treatment conditions and treatment devices include ultrasonic homogenizers, bead mills, wet jet mills, and high-speed rotary shear dispersers. By applying a moderately strong shear force, the fibrous carbon nanostructures can be sufficiently dispersed, and a molded body with improved material uniformity can be formed. These may be used alone or in combination of two or more. Specifically, in a bead mill using zirconia beads as a dispersion medium, the dispersion treatment conditions may be a peripheral speed of 8 to 12 m / s, and the dispersion treatment can be performed using a probe-type ultrasonic device with an output of 200 to 600 W and an ultrasonic amplitude of 20 to 40 μm.

[0046] <Method of producing elastomer composition> The elastomer composition can be obtained by preparing the above-mentioned dispersion and removing the solvent from the dispersion. If necessary, the elastomer composition can be obtained by further adding the additives described below to the obtained composition. The method for removing the solvent from the obtained dispersion is not particularly limited, but for example, a coagulation method, a casting method, or a drying method can be used.

[0047] <Elastomer composition> Since the elastomer composition is obtained using the above-mentioned dispersion, the elastomer and fibrous carbon nanostructures contained in the dispersion can be contained in the same amount and state. Therefore, the content of the fibrous carbon nanostructures in the elastomer composition is 0.5 parts by mass or more and less than 3 parts by mass per 100 parts by mass of elastomer, and the fibrous carbon nanostructures can maintain the state (particle size, etc.) at the time of dispersion in the solvent. By configuring the fibrous carbon nanostructures in this way, the strength of the gas seal member for high-pressure hydrogen equipment can be sufficiently increased and the occurrence of blister breakage can be suppressed.

[0048] <Additives> The elastomer composition may contain any additives, including, but not limited to, known additives such as reinforcing materials and antioxidants. The reinforcing material is not particularly limited, and silica, carbon black, etc. can be used. The antioxidant is not particularly limited, and examples of the antioxidant that can be used include amine-based antioxidants (e.g., 4,4'-bis(a,a-dimethylbenzyl)diphenylamine) and imidazole-based antioxidants (e.g., zinc salt of 2-mercaptobenzimidazole). These additives may be used alone or in combination of two or more. The amount of the additives may be any amount as long as the desired effect is not inhibited.

[0049] When the elastomer composition contains the above-mentioned additives, it can be obtained by mixing or kneading the additives in a desired compounding ratio with the composition obtained by removing the solvent from the dispersion. Kneading can be performed using, for example, a mixer, a single-screw kneader, a twin-screw kneader, a roll, a Brabender, an extruder, etc. The above-mentioned additives may be added together with the crosslinking agent when producing the crosslinkable elastomer described below, or may be added in advance to the elastomer composition before the crosslinking agent is added.

[0050] <Crosslinkable elastomer composition> As described above, the crosslinkable elastomer composition can be obtained by adding a crosslinking agent (if necessary, a crosslinking assistant agent is added, the same in the present specification) to the elastomer composition. When the crosslinking agent is added to the elastomer composition, it can be obtained by kneading in the same manner as in the case of the above-mentioned additives. The crosslinking agent is not particularly limited, but a known crosslinking agent capable of crosslinking the elastomer component contained in the elastomer composition can be used. More specifically, the crosslinking agent may be, for example, sulfur, a peroxide-based crosslinking agent (for example, 1,3-bis(t-butylperoxyisopropyl)benzene), triallyl isocyanurate, or the like. The crosslinking assistant is not particularly limited, but for example, zinc oxide, or the like can be used. These crosslinking agents (as well as crosslinking assistants) may be used alone or in combination of two or more. The amount of the crosslinking agent (as well as crosslinking assistant) may be any amount as long as it does not inhibit the development of the desired effect.

[0051] <Gas seal materials> The gas seal member is a member used in high-pressure hydrogen equipment, and can be obtained by preparing the above-mentioned crosslinkable elastomer composition, molding it into a desired shape, and crosslinking it. Specifically, the gas seal member can be formed, for example, by putting the crosslinkable elastomer composition into a mold, crosslinking it, and molding it. The shape of the gas seal member can be any shape depending on the application, and may be, for example, a ring-shaped gas seal member (O-ring) or a hollow disk-shaped gas seal member. There are no particular restrictions on the crosslinking conditions, but for example, conditions of temperature: 140°C to 250°C, pressure: 1 MPa to 20 MPa, and time: 1 minute to 180 minutes are preferable.

[0052] <High pressure hydrogen equipment> The high-pressure hydrogen equipment is configured to include a container filled with high-pressure hydrogen of 35 MPa or more and 105 MPa or less, and the above-mentioned gas seal member. The gas seal member used in the high-pressure hydrogen equipment is in contact with the high-pressure hydrogen filled in the container. The pressure of the high-pressure hydrogen can be, for example, 60 MPa or more or 70 MPa or more. The pressure of the high-pressure hydrogen can be, for example, 100 MPa or less or 95 MPa or less.

[0053] FIG. 1 is a schematic diagram showing the configuration of a hydrogen station. 1, the hydrogen station 100 includes a hydrogen production device 111, a hydrogen gas compressor (booster) 112, a gas accumulator (pressure accumulator) 113, and a dispenser 114, and each piece of equipment is connected by hydrogen piping 118. Furthermore, piping equipment (not shown) such as valves and joints are provided along each hydrogen piping 118 as necessary. In an on-site hydrogen station 100, fuel (naphtha or kerosene) is supplied from an external source, and hydrogen is produced using this fuel in a hydrogen production device 111 that includes a fuel reformer 111A and a hydrogen purification device 111B that increases the purity of the hydrogen. The hydrogen produced in the hydrogen production device 111 is converted into high-pressure hydrogen at a predetermined temperature (e.g., -20°C to 180°C) and pressure (e.g., 95 MPa) in a hydrogen gas compressor (booster) 112, and the pressurized hydrogen is supplied to a vehicle (fuel cell vehicle) 120 equipped with a hydrogen tank (not shown) via a gas accumulator (pressure accumulator) 113 for temporarily storing the high-pressure hydrogen and a dispenser 114 for supplying the high-pressure hydrogen stored in the gas accumulator (pressure accumulator) 113 to the vehicle (fuel cell vehicle) 120. At this time, hydrogen is supplied from dispenser 114 to vehicle (fuel cell vehicle) 120 by the hydrogen pressure difference. For example, the temperature and pressure in gas accumulator (pressure accumulator) 113 are set to -20°C to 50°C and 95 MPa, respectively, and the temperature and pressure in dispenser 114 are set to -40°C to 50°C and 82 MPa, respectively, and hydrogen is filled into the hydrogen tank in vehicle (fuel cell vehicle) 120 by the pressure difference.

[0054] Dispenser 114 is equipped with hydrogen supply hose 115 for supplying hydrogen to a hydrogen tank of vehicle (fuel cell vehicle) 120, and hydrogen supply hose 115 is fitted with hydrogen supply plug 116 that is detachably connected to receptacle 121 of vehicle 120. Thus, by connecting hydrogen supply plug 116 to receptacle 121, hydrogen can be supplied to vehicle (fuel cell vehicle) 120. Additionally, an emergency breakaway coupling 117 is provided midway along the hydrogen supply hose 115. Therefore, in the event of an emergency (for example, if the vehicle (fuel cell vehicle) 120 erroneously starts moving), the supply of hydrogen from the hydrogen station 100 to the vehicle (fuel cell vehicle) 120 can be stopped by operating this emergency breakaway coupling 117.

[0055] Gas sealing members for high-pressure hydrogen equipment are provided, for example, at the connection parts between each piece of equipment (hydrogen production equipment 111, hydrogen gas compressor (booster) 112, gas accumulator (pressure accumulator) 113, dispenser 114) and hydrogen piping 118, and between the container body and the lid in each piece of equipment (hydrogen production equipment 111, hydrogen gas compressor (booster) 112, gas accumulator (pressure accumulator) 113, dispenser 114). EXAMPLES

[0056] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In the examples and comparative examples, the particle size distribution of carbon nanotubes as fibrous carbon nanostructures in the dispersion and the high-pressure hydrogen durability test were measured or evaluated using the following methods.

[0057] <Particle size distribution of dispersion liquid> The dispersion obtained by the dispersion treatment was diluted with methyl ethyl ketone, and the particle size of the carbon nanotubes was measured at a transmittance of 88% using a laser diffraction particle size distribution analyzer (HORIBA, LA-950), and D50, D10, and D90 were obtained, and D90-D10 was calculated. Here, D50 is the diameter of the particle size where the cumulative value of the particles is 50% (= median value, also called median diameter), and similarly, D10 is the diameter of the particle where the cumulative value is 10%, and D90 is the diameter of the particle where the cumulative frequency is 90%.

[0058] <High pressure hydrogen durability test> A cross-linked molded gas seal member, size P22 O-ring, was sandwiched between two backup rings and attached to a metal unit, then inserted into a sample holder, and the hydrogen gas line, pressure gauge, thermometer, heater, etc. were set up. Hydrogen gas was heated to 110°C and the sample holder to 180°C, and the hydrogen gas pressure was increased to 90MPa. After that, a high-pressure retention test was conducted with one cycle lasting 3 minutes, and the pressure of leaked hydrogen was observed. When the pressure of leaked hydrogen rose suddenly, it was determined that the O-ring had been destroyed, and the number of times at that time was determined as the durability. After the specified number of cycles of high-pressure retention tests were conducted, the O-ring was removed and observed for cracks or destruction, and the state of the O-ring after the test was determined. The state of the O-ring after the test was determined as A: no cracks, B: no through cracks, and C: through cracks.

[0059] <Example 1> To 9000 g of methyl ethyl ketone (MEK) as a solvent, 100 parts (1000 g) of fluororubber (manufactured by Chemours, product name "GF600S") was added, and the mixture was stirred to dissolve the fluororubber, thereby obtaining a fluororubber dissolved solution. Next, one part (10 g) of SGCNT (manufactured by Zeon Corporation, product name "ZEONANO SG101") as carbon nanotubes was added to the fluororubber dissolved solution, and the mixture was stirred using a stirrer (manufactured by PRIMIX Corporation, Labo-lution (registered trademark), stirring part: Homo Disper). Furthermore, a bead mill (manufactured by Asada Iron Works, product name "Nano Mill NM-G1.4L", zirconia beads (average diameter of dispersion media: 0.65 mm) as dispersion media, dispersion treatment conditions: peripheral speed 8 m / s, discharge amount 80 g / min) and a probe-type ultrasonic device (manufactured by Mitsui Electric Seiki Co., Ltd., product name "UX300") were used to perform dispersion treatment at an output of 600 W and ultrasonic amplitude of 40 μm (dispersion step), thereby obtaining a fluororubber dissolved solution (corresponding to a dispersion liquid) to which SGCNT had been added. The obtained dispersion was used to perform a laser diffraction particle size distribution measurement of the dispersion, and the median diameters D50 and D90-D10 of the carbon nanotubes in the dispersion were determined. The results are shown in Table 1. Thereafter, the obtained dispersion was dropped into 3000 g of a solution of ion-exchanged water:isopropyl alcohol = 1:1 to cause coagulation, obtaining a black solid. Then, the obtained black solid was dried under reduced pressure at 170 °C for 8 hours (solvent removal step) to obtain a mixture of fluororubber and SGCNT (corresponding to the elastomer composition).

[0060] <Kneading> Using an open roll, 101 g of a mixture of fluororubber and SGCNT, 10 g of carbon black as a reinforcing material (manufactured by Tokai Carbon Co., Ltd., product name "Thermax (registered trademark) N990"), 50 g of silica (manufactured by Nippon Aerosil Co., Ltd., product name "Aerosil R972V"), 4 parts of triallyl isocyanurate as a crosslinking agent (manufactured by Nippon Kasei Co., Ltd., product name "TAIC (registered trademark)"), and 3.75 parts of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (manufactured by NOF Corporation, trade name "Perhexa (registered trademark) 25B-40") were kneaded to obtain a fluororubber composition (corresponding to a crosslinkable elastomer composition). <Manufacture of O-ring> The obtained fluororubber composition was put into a mold and crosslinked at a temperature of 160 °C and a pressure of 10 MPa for 10 minutes to obtain an O-ring (size P22). Then, using the obtained O-ring, a high-pressure hydrogen durability test was carried out. The results are shown in Table 1.

[0061] <Example 2> In the preparation of the mixture of fluororubber and SGCNT, except that the dispersion treatment of the fluororubber solution added with SGCNT was changed only to a bead mill (manufactured by Asada Iron Works Co., Ltd., product name "Nanomill NM-G1.4L", zirconia beads as a dispersion medium (average diameter of the dispersion medium: 0.65 mm), conditions of dispersion treatment: peripheral speed 8 m / s, discharge rate 80 g / min), the same procedure as in Example 1 was followed to prepare and evaluate an O-ring. The results are shown in Table 1.

[0062] <Example 3> In preparing the mixture of fluororubber and SGCNT, a mixture of fluororubber and SGCNT was prepared in the same manner as in Example 1, except that the amount of SGCNT added was changed to 0.5 parts (5 g). In the kneading, a fluororubber composition was obtained in the same manner, except that 100.5 g of the mixture of fluororubber and SGCNT was used, and 10 g of carbon black (manufactured by Tokai Carbon Co., Ltd., product name "Thermax (registered trademark) N990") and 55 g of silica (manufactured by Nippon Aerosil Co., Ltd., product name "Aerosil R972V") were used as reinforcing materials, and an O-ring was prepared and evaluated. The results are shown in Table 1.

[0063] <Example 4> In preparing the mixture of fluororubber and SGCNT, except that the amount of SGCNT added was changed to 2 parts (20 g), a mixture of fluororubber and SGCNT was prepared in the same manner as in Example 1. In the kneading, a fluororubber composition was obtained in the same manner except that 102 g of the mixture of fluororubber and SGCNT was used, and 10 g of carbon black (manufactured by Tokai Carbon Co., Ltd., product name "Thermax (registered trademark) N990") and 40 g of silica (manufactured by Nippon Aerosil Co., Ltd., product name "Aerosil R972V") were used as reinforcing materials, and an O-ring was prepared and evaluated. The results are shown in Table 1.

[0064] <Comparative Example 1> In preparing the mixture of fluororubber and SGCNT, a mixture of fluororubber and SGCNT was prepared in the same manner as in Example 1, except that the amount of SGCNT added was changed to 3 parts (30 g). In the kneading, a fluororubber composition was obtained in the same manner, except that 103 g of the mixture of fluororubber and SGCNT was used, and 10 g of carbon black (manufactured by Tokai Carbon Co., Ltd., product name "Thermax (registered trademark) N990") and 30 g of silica (manufactured by Nippon Aerosil Co., Ltd., product name "Aerosil R972V") were used as reinforcing materials, and an O-ring was prepared and evaluated. The results are shown in Table 1.

[0065] <Comparative Example 2> In the kneading, 100 g of fluororubber was used, and 10 g of carbon black (manufactured by Tokai Carbon Co., Ltd., product name "Thermax (registered trademark) N990") and 60 g of silica (manufactured by Nippon Aerosil Co., Ltd., product name "Aerosil R972V") were used as reinforcing materials, but a fluororubber composition was obtained in the same manner, and an O-ring was produced and evaluated. The results are shown in Table 1.

[0066] [Table 1]

[0067] From Table 1, it can be seen that in Examples 1 to 4, which have a predetermined amount of fibrous carbon nanostructures and a predetermined particle size distribution range, the number of cycles of high-pressure hydrogen durability was high and there were few cracks in the O-rings after the test. On the other hand, in the cases where the fibrous carbon nanostructure was not included or the amount was inappropriate, the number of cycles of durability was low, and the O-rings after the test showed penetration and cracks. [Industrial Applicability]

[0068] According to the present invention, it is possible to provide a gas sealing member for high-pressure hydrogen equipment which is more durable than ever before and can sufficiently suppress the occurrence of blister breakage. Furthermore, according to the present invention, it is possible to provide high-pressure hydrogen equipment in which blister damage of the gas seal members is unlikely to occur even when used over a long period of time, and which enables reduction in maintenance costs. [Explanation of symbols]

[0069] 100 Hydrogen Station 111 Hydrogen production equipment 111A Fuel Reformer 111B Hydrogen purification equipment 112 Hydrogen gas compressor (booster) 113 Gas storage machine (pressure storage machine) 114 Dispenser 115 Hydrogen supply hose 116 Hydrogen supply plug 117 Breakaway Coupling 118 Hydrogen piping 120 Vehicles (Fuel Cell Vehicles) 121 Receptacle

Claims

1. A dispersion liquid used in a gas seal member for high-pressure hydrogen equipment, The present invention includes an elastomer, a fibrous carbon nanostructure, and a solvent that dissolves the elastomer, The fibrous carbon nanostructure is contained in an amount of 0.5 parts by mass or more and less than 3 parts by mass per 100 parts by mass of the elastomer, A dispersion in which the particle size distribution of the fibrous carbon nanostructures in the dispersion satisfies the following conditions (1) and (2). (1) D50≦20μm (2) D90-D10≦45μm Here, D50, D10, and D90 each indicate the particle diameter when the particle size distribution of the fibrous single-layer nanostructure in the dispersion liquid is measured, and D50 is the diameter of the particle at which the accumulated value of the particles is 50% (= the median value, also called the median diameter), D10 is the diameter of the particle at which the accumulated value of the particles is 10%, and D90 is the diameter of the particle at which the accumulated value of the particles is 90%.

2. The dispersion according to claim 1 , which satisfies the following condition (3): (3) D90-D10≦35μm

3. 3. The dispersion according to claim 1, wherein the elastomer is at least one rubber selected from the group consisting of nitrile rubber, hydrogenated nitrile rubber, ethylene propylene diene rubber, silicone rubber and fluororubber.

4. The dispersion according to claim 1 or 2, wherein the fibrous carbon nanostructures include single-walled carbon nanotubes.

5. A method for producing a dispersion liquid used in a gas seal member for high-pressure hydrogen equipment, comprising the steps of: A dispersion step of mixing and dispersing an elastomer, a fibrous carbon nanostructure, and a solvent capable of dissolving the elastomer to obtain a dispersion liquid, The dispersion contains 0.5 parts by mass or more and less than 3 parts by mass of the fibrous carbon nanostructure per 100 parts by mass of the elastomer, The dispersion step is a method for producing a dispersion liquid, in which a mixing and dispersion treatment is carried out so that the particle size distribution of the fibrous carbon nanostructures in the dispersion liquid satisfies the following conditions (1) and (2). (1) D50≦20μm (2) D90-D10≦45μm Here, D50, D10, and D90 each indicate the particle diameter when the particle size distribution of the fibrous single-layer nanostructure in the dispersion liquid is measured, and D50 is the diameter of the particle at which the accumulated value of the particles is 50% (= the median value, also called the median diameter), D10 is the diameter of the particle at which the accumulated value of the particles is 10%, and D90 is the diameter of the particle at which the accumulated value of the particles is 90%.

6. A method for producing an elastomer composition for use in a gas seal member for high-pressure hydrogen equipment, comprising the steps of: A step of preparing a dispersion according to claim 1 or 2, or a dispersion obtained by the method for producing a dispersion according to claim 5; a solvent removal step of removing the solvent from the dispersion to obtain the elastomer composition; A method for producing an elastomer composition comprising:

7. A method for producing a gas seal member for high-pressure hydrogen equipment, comprising the steps of: A step of obtaining a crosslinkable elastomer composition comprising the elastomer composition obtained by the method for producing an elastomer composition according to claim 6 and a crosslinking agent; and obtaining a crosslinked product by crosslinking the crosslinkable elastomer composition, The cross-linked product is used as a gas seal member for high-pressure hydrogen equipment, in accordance with the method for producing a gas seal member for high-pressure hydrogen equipment.

Citation Information

Patent Citations

  • Gas sealing member for high-pressure hydrogen devices, and high-pressure hydrogen device

    WO2021193667A1