Method for regenerating solid lewis acid

Regenerating the solid Lewis acid with an oxidizing agent and phosphoric acid treatment addresses the activity reduction issue, allowing efficient production of hydroxymethylfurfural from sugars.

JP2024146568APending Publication Date: 2024-10-15CUYUSYOJI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059551
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The solid Lewis acid used in the synthesis of hydroxymethylfurfural from glucose or fructose becomes coated with caramelization reaction products, leading to reduced activity and inefficiency in the conversion process.

Method used

Regenerate the solid Lewis acid by treating it with an oxidizing agent, preferably a hypochlorite salt, and optionally follow up with phosphoric acid treatment.

Benefits of technology

The regenerated solid Lewis acid maintains high activity, enabling efficient production of hydroxymethylfurfural from sugars by repeated use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a method for regenerating a solid Lewis acid of which activity was deteriorated by being covered with a caramelization reaction product.SOLUTION: In the present invention, a solid Lewis acid that converts glucose or fructose to hydroxymethylfurfural and is surface-coated with a caramelization reaction product is treated with an oxidizing agent. The oxidizing agent may be a hypochlorite. The solid Lewis acid may be a phosphated titanium oxide having a phosphate residue covalently bonded to the surface of an amorphous hydrous titanium oxide that functions as a Lewis acid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for regenerating a solid Lewis acid used in the synthesis of hydroxymethylfurfural from glucose or fructose. [Background technology]

[0002] Hydroxymethylfurfural (hereinafter sometimes referred to as "HMF" in this specification) is an important intermediate chemical that can be synthesized using glucose as a raw material, but its synthetic pathway is very complicated. The raw material glucose is converted to fructose by skeletal isomerization in the presence of an acid catalyst. The resulting fructose is converted to hydroxymethylfurfural by a dehydration reaction with the acid catalyst, and hydroxymethylfurfural is further sequentially hydrolyzed by the acid catalyst in the reaction system to organic acids (formic acid, levulinic acid). For this reason, a new catalyst for highly selectively producing hydroxymethylfurfural is desired.

[0003] By treating amorphous hydrous titanium oxide with phosphoric acid, a phosphorylated titanium oxide is obtained in which phosphoric acid residues are covalently bonded to the surface of the hydrous titanium oxide. This phosphorylated titanium oxide is known as a solid Lewis acid that converts glucose or fructose to HMF (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2012-108472 Summary of the Invention [Problem to be solved by the invention]

[0005] The reaction of converting glucose etc. into HMF using the titanium phosphate compound is carried out in the range of 80 to 180°C, so there was a problem that glucose etc. underwent a caramelization reaction, and the caramelization reaction product (often considered to be humic acid) covered the solid Lewis acid, reducing the activity of the solid Lewis acid. An object of the present invention is to provide a method for regenerating a solid Lewis acid whose activity has been reduced by being coated with a caramelization reaction product. [Means for solving the problem]

[0006] As a result of investigations aimed at solving the above problems, the inventors of the present invention found that a solid Lewis acid coated with a caramelization reaction product can be regenerated by treating it with an oxidizing agent, thereby completing the present invention.

[0007] That is, the present invention relates to a method for regenerating a solid Lewis acid, which converts glucose or fructose into hydroxymethylfurfural and whose surface is covered with a caramelization reaction product, by treating the solid Lewis acid with an oxidizing agent. The oxidizing agent is preferably a hypochlorite. The solid Lewis acid is preferably a titanium oxide phosphate having phosphoric acid residues covalently bonded to the surface of an amorphous hydrous titanium oxide functioning as a Lewis acid. When the solid Lewis acid is the titanium oxide phosphate, it is preferable to treat the titanium oxide with phosphoric acid after the treatment with the oxidizing agent. Effect of the Invention

[0008] By using the method for regenerating a solid Lewis acid of the present invention, even a solid Lewis acid that has been covered with a caramelization reaction product and has reduced activity can be used repeatedly to efficiently produce HMF from sugars. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for regenerating a solid Lewis acid that converts glucose or fructose into HMF and is surface-coated with a caramelization reaction product according to the present invention comprises treating the solid Lewis acid with an oxidizing agent.

[0010] The solid Lewis acid used in the regeneration method is not particularly limited as long as it can convert glucose or fructose into HMF, but specific examples include amorphous hydrous titanium oxide that functions as a Lewis acid, and titanium phosphate oxide in which phosphoric acid residues are covalently bonded to the surface of the amorphous hydrous titanium oxide. The amorphous hydrous titanium oxide can be obtained by reacting an organic titanium compound that is hydrolyzed in an aqueous solution to form an oxide with water, together with an acid catalyst or a base catalyst.

[0011] Examples of the organic titanium compound include inorganic titanium compounds such as titanium hydroxide, titanic acid, titanium trichloride, titanium tetrachloride, titanium tetrabromide, titanium sulfate, and titanium oxysulfate; titanium alkoxide compounds such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetrakis(2-ethylhexyloxy)titanium, and tetrastearyloxytitanium; titanium acylate compounds; titanium chelate compounds such as diisopropoxybis(acetylacetonato)titanium, isopropoxy(2-ethyl-1,3-hexanediolato)titanium, and hydroxybis(lactato)titanium; organic acid titanium compounds such as titanium oxalate and titanium tetraacetate; and water-soluble titanium complexes. Among these, at least one selected from the group consisting of titanium chloride, titanium oxalate, and titanium alkoxide is preferred.

[0012] The number of carbon atoms constituting the alkoxy group in the titanium alkoxide is preferably 1 to 6, more preferably 2 to 4. The alkoxy group may be linear, branched, or cyclic.

[0013] Examples of the acid used in the hydrolysis reaction include hydrochloric acid, sulfuric acid, and nitric acid. Examples of the base used in the hydrolysis reaction include ammonia, sodium hydroxide, and potassium hydroxide. The temperature during the hydrolysis reaction is preferably 10 to 100° C., and more preferably 20 to 30° C. The time required for the hydrolysis reaction can be appropriately set depending on the reaction temperature, reaction scale, and the like, and is preferably 0.5 to 48 hours, and more preferably 10 to 24 hours.

[0014] The titanium oxide phosphate can be obtained by treating the amorphous titanium oxide hydrous with phosphoric acid. The phosphoric acid treatment can be carried out by immersing the amorphous titanium oxide hydrous in an aqueous phosphoric acid solution and stirring it. The temperature during this treatment is preferably 10°C or higher and lower than 100°C, more preferably 20°C or higher and 30°C or lower. The reaction time can be appropriately set depending on the reaction temperature, reaction scale, etc., but is preferably 1 hour to 96 hours, more preferably 24 hours to 72 hours.

[0015] The solid Lewis acid may be doped with a metal element or may be coated with a compound containing a metal element, such as aluminum, gallium, indium, thallium, magnesium, manganese, calcium, niobium, tantalum, zirconium, silicon, zinc, cerium, iron, tungsten, molybdenum, or vanadium.

[0016] The solid Lewis acid may be mixed with a binder to form a molded body, if necessary. Specific examples of the binder include crystalline aluminosilicate molecular sieves such as mordenite, chabazite, erionite, ferrierite, faujasite, levin, ZSM-5, zeolite A, zeolite β, FU-1, Rho, ZK-5, RUB-3, RUB-13, NU-3, NU-4, NU-5, NU-10, NU-13, NU-23, and MCM-22; SAPO-5, SAPO-11, SAPO-17, SAPO-18, SAPO-26, SAPO-31, SAPO-33, SAPO-34, SAPO-35, and SAPO- Examples of the silicoaluminophosphate molecular sieve include crystalline silicoaluminophosphate molecular sieves such as SAPO-42, SAPO-43, SAPO-44, SAPO-47, and SAPO-56; clay compounds such as kaolinite, sericite, talc, mica (muscovite, phlogopite, biotite, lepidolite, vanadium mica, chromium mica, and fluorine mica), montmorillonite, sepiolite, attapulgite, and smectite; silica, alumina (aluminum oxide), titania, zirconia, yttria; polytetrafluoroethylene, silicone, permethylpolysilane, and carbon black. Among these, at least one selected from the group consisting of polytetrafluoroethylene, aluminum oxide, silicone, silica, permethylpolysilane, and carbon black is preferred.

[0017] The amount of the binder is not particularly limited as long as it allows production of a molded body, but is preferably 10 to 100 parts by mass, more preferably 10 to 50 parts by mass, and further preferably 10 to 20 parts by mass, relative to 100 parts by mass of the solid Lewis acid.

[0018] The solid Lewis acid molded body can be obtained, for example, by kneading a binder and a solid Lewis acid, optionally with water, molding, drying, and optionally firing. The kneading is preferably performed under pressure. From the viewpoint of workability, the kneading is preferably performed continuously using a kneader or other kneading machine. The drying conditions are not limited as long as moisture can be removed, and can be performed, for example, at a temperature range of 80°C to 150°C for 1 to 10 hours. After the drying, the product is adjusted to a desired size and, if necessary, fired. The firing temperature and time vary depending on the type of solid Lewis acid molded body. The firing can be performed, for example, at 400°C to 700°C for 1 to 10 hours.

[0019] The molded product of the solid Lewis acid may be in the form of powder, granules, pellets, thin film, nanotubes, etc., as necessary. Molded products in various shapes can be obtained by, for example, extrusion molding, compression molding (e.g., tablet molding, etc.), rolling molding, spray drying, etc.

[0020] More specific examples of the molded article of the solid Lewis acid include a method in which a binder precursor such as tetraethoxysilane, the organotitanium compound, and phosphoric acid or a precursor thereof are mixed to form a liquid or slurry, which is then subjected to casting, slush molding, coating, or the like, followed by hydrolysis; and a method in which a binder precursor such as tetraethoxysilane and the organotitanium compound are mixed to form a liquid or slurry, which is then subjected to casting, slush molding, coating, or the like, followed by hydrolysis, followed by phosphoric acid treatment.

[0021] The caramelization reaction is a phenomenon that occurs due to an oxidation reaction caused by sugars, and brown compounds containing a wide variety of compounds are the caramelization reaction products.

[0022] The oxidizing agent is not particularly limited, but specific examples thereof include peroxides such as hydrogen peroxide, sodium peroxide, barium peroxide, and anhydrous perbenzoic acid; oxygen species such as oxygen and ozone; inorganic nitrogen compounds such as dinitrogen tetroxide, dinitrogen trioxide, and dinitrogen monoxide; peroxyacids and peroxyacid salts such as sodium peroxodisulfate, potassium peroxodisulfate, sodium peroxomonosulfate, peroxyacetic acid, and ammonium peroxodisulfate; halogens and compounds thereof such as F2, Cl2, Br2, I2, and iron chloride (FeCl3); Examples of the oxidizing agent include permanganate and permanganate such as chromium; chromium compounds such as chromic anhydride, chromium dioxide dichloride, sodium chromate, sodium dichromate, and sodium chlorochromate; lead compounds such as lead dioxide and lead acetate; mercury compounds such as mercury acetate; metal acetates such as bismuth acetate; nitrates such as ammonium nitrate, potassium nitrate, and copper nitrate; and halogenated acids and halogenated acid salts such as sodium hypochlorite, sodium hypobromite, sodium hypoiodite, sodium chlorate, periodic acid, potassium periodate, sodium perchlorate, and sodium hydrogen iodate. Among these, the halogenated acids or halogenated acid salts are preferred, hypochlorite is more preferred, and sodium hypochlorite is even more preferred. The oxidizing agent may be used alone or in combination of two or more.

[0023] The oxidizing agent is preferably dissolved in water and used as an aqueous solution. The concentration of the aqueous solution is not particularly limited, but is preferably 1.0 to 30 mass / volume %, more preferably 3.0 to 10.0 mass / volume %.

[0024] The method of treating the solid Lewis acid with the oxidizing agent is not particularly limited, but specific examples include a method of immersing the solid Lewis acid in an aqueous oxidizing agent solution, a method of stirring the solid Lewis acid in an aqueous oxidizing agent solution, a method of irradiating an aqueous oxidizing agent solution containing the solid Lewis acid with ultrasonic waves, and a method of passing the aqueous oxidizing agent solution through a column packed with the solid Lewis acid. The treatment is carried out at room temperature or under heating conditions. The heating conditions are not particularly limited as long as they are less than 100°C, but are preferably in the range of 50 to 90°C, and more preferably in the range of 60 to 80°C.

[0025] When the solid Lewis acid is a phosphoric acid titanium oxide, it is preferable to treat the solid Lewis acid with phosphoric acid after the treatment with the oxidizing agent. The phosphoric acid treatment may be carried out in the same manner as in the treatment of the amorphous hydrous titanium oxide with phosphoric acid.

[0026] Next, the present invention will be described in more detail using examples, but the scope of the present invention is not limited to the examples.

[0027] <Production Example> 20 ml of titanium tetraisopropoxide was added to 100 ml of distilled water and stirred at room temperature for 3 hours. The white precipitate was removed by filtration, added to 200 ml of 1.0 M aqueous hydrochloric acid, and stirred for 1 hour to promote condensation of the oxide framework. This filtration, addition, and stirring (condensation) process was repeated two more times (for a total of three times). The resulting precipitate was washed with distilled water until neutral, and then dried in an oven at 80°C to obtain amorphous hydrous titanium oxide. The amorphous hydrous titanium oxide was added to an aqueous phosphoric acid solution (0.1 M) and stirred at room temperature for 48 hours. The white solid was filtered off and washed with distilled water until neutral to obtain the solid Lewis acid 1. EXAMPLES

[0028] The solid Lewis acid catalyst was packed in a cylindrical column with a diameter of 7.6 mm and a height of 150 mm, and the temperature was maintained at 145° C., and a 10% glucose solution was passed through. After a 5-hour reaction, an average of 79.2 mM / h of HMF was obtained. After that, because brown matter was attached and the catalytic activity was significantly reduced, a sodium hypochlorite solution was passed through for 16 hours, distilled water was passed through for washing for 24 hours, a 1M phosphoric acid solution was passed through for 48 hours, and a 10% glucose solution was passed through, and the reaction was carried out again. As a result, 95.6 mM / h of HMF was obtained, which was comparable to the activity of the catalyst before use. [Industrial Applicability]

[0029] The regeneration method of the present invention is useful for industrially producing HMF from sugars such as glucose.

Claims

1. A method for regenerating a solid Lewis acid, which converts glucose or fructose into hydroxymethylfurfural and is surface-coated with a caramelization reaction product, comprising treating the solid Lewis acid with an oxidizing agent.

2. 2. The method for regenerating a solid Lewis acid according to claim 1, wherein the oxidizing agent is a hypochlorite.

3. 3. The method for regenerating a solid Lewis acid according to claim 1, wherein the solid Lewis acid is a titanium oxide phosphate having phosphoric acid residues covalently bonded to the surface of an amorphous hydrous titanium oxide functioning as a Lewis acid.

4. 4. The method for regenerating a solid Lewis acid according to claim 3, further comprising treating the solid Lewis acid with phosphoric acid after the treatment with the oxidizing agent.

Citation Information

Patent Citations