Optical laminate and image display device

The optical laminate structure with specific adhesive sheet properties mitigates display defects by dispersing pressure, enhancing the durability of image display devices against small object impacts.

JP2024146590APending Publication Date: 2024-10-15NITTO DENKO CORP

Patent Information

Application Number
JP2023059587
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Image display devices using optical laminates are prone to display defects when small objects collide or press the screen with a narrow contact area, causing damage to the optical films.

Method used

An optical laminate structure comprising a first optical film, a first adhesive sheet with a thickness of 30 μm to 1000 μm and elongation at break of 500% or less, and a second adhesive sheet, which disperses pressure and reduces stress on the second optical film, thereby minimizing damage.

Benefits of technology

The proposed laminate structure effectively suppresses display defects and damage to optical films even under pressure, ensuring the integrity and functionality of the image display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146590000001_ABST
    Figure 2024146590000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate suitable for suppressing display failure even when a small object collides with a screen or presses the screen in narrow contact area in an image display device manufactured by using the optical laminate.SOLUTION: An optical laminate 10A has a configuration in which a first optical film 1, a first adhesive sheet 2, a second optical film 3, and a second adhesive sheet 4 are laminated in this order. Thickness T1 of the first adhesive sheet 2 is 30 μ m or more and 1000 μ m or less. In addition, breaking elongation of the first adhesive sheet is 500% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate and an image display device. [Background technology]

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices and inorganic EL display devices), have rapidly become widespread. These various image display devices have a laminated structure of, for example, an image display cell, such as a liquid crystal cell or an EL light-emitting element, and an optical laminate. The optical laminate includes an optical film, such as a retardation film and a polarizing film, and an adhesive sheet. The adhesive sheet is mainly used for bonding between films included in the optical laminate, or for bonding between the image display cell and the optical laminate.

[0003] Patent Document 1 discloses a pressure-sensitive adhesive composition for optical films, and an optical film having a pressure-sensitive adhesive layer obtained from this composition provided on at least one surface thereof. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-158702 A Summary of the Invention [Problem to be solved by the invention]

[0005] When an image display device is used or transported, a large load may be applied to the image display device due to a small object colliding with or pressing against the screen with a small contact area. When the above-mentioned load is applied to an image display device manufactured using an optical laminate, damage may occur to the optical film contained in the optical laminate. Damage to the optical laminate may cause display defects in the image display device.

[0006] Therefore, an object of the present invention is to provide an optical laminate that is suitable for suppressing display defects in an image display device manufactured using the optical laminate, even when a small object collides with or presses the screen with a small contact area. [Means for solving the problem]

[0007] The present invention relates to An optical laminate in which a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet are laminated in this order, The thickness T of the first adhesive sheet 1 is 30 μm or more and 1000 μm or less, and the breaking elongation of the first pressure-sensitive adhesive sheet is 500% or less.

[0008] Further, the present invention relates to There is provided an image display device including the above optical laminate. Effect of the Invention

[0009] According to the present invention, an optical laminate can be provided that is suitable for suppressing display defects in an image display device manufactured using the optical laminate, even when a small object collides with or presses the screen with a small contact area. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of an optical laminate according to this embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a method for producing the first pressure-sensitive adhesive sheet. [Diagram 3] FIG. 3 is a schematic diagram illustrating another example of the method for producing the first pressure-sensitive adhesive sheet. [Figure 4A] FIG. 4A is a cross-sectional view illustrating a schematic example of the second optical film. [Figure 4B] FIG. 4B is a cross-sectional view diagrammatically illustrating another example of the second optical film. [Diagram 5]FIG. 5 is a cross-sectional view that illustrates another example of the optical laminate according to this embodiment. [Figure 6] FIG. 6 is a cross-sectional view that illustrates an example of an image display device according to this embodiment. [Figure 7] FIG. 7 is a cross-sectional view that typically shows the optical laminates according to Examples 1 to 4 and 6 and Comparative Examples 1 to 4. As shown in FIG. [Figure 8] FIG. 8 is a cross-sectional view that illustrates an optical laminate according to Example 5. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The optical laminate according to the first aspect of the present invention is An optical laminate in which a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet are laminated in this order, The thickness T of the first adhesive sheet 1 is 30 μm or more and 1000 μm or less, and the breaking elongation of the first pressure-sensitive adhesive sheet is 500% or less.

[0012] In a second aspect of the present invention, for example, in the optical laminate relating to the first aspect, the first adhesive sheet is formed from a photocurable adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group.

[0013] In a third aspect of the present invention, for example, in the optical laminate related to the second aspect, the photocurable pressure-sensitive adhesive composition (I) contains a crosslinking agent, and the amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) is 0.4 parts by weight or more and 20 parts by weight or less relative to 100 parts by weight in total of the monomer group and the partial polymer.

[0014] In a fourth aspect of the present invention, for example, in the optical laminate according to any one of the first to third aspects, the optical laminate has a thickness T of 200 μm or more.

[0015] In a fifth aspect of the present invention, for example, in the optical laminate according to any one of the first to fourth aspects, the second optical film includes a plurality of layers, The plurality of layers includes a polarizer and at least one film disposed between the polarizer and the second adhesive sheet, The photoelastic coefficient of the at least one film is 4×10 -11 m 2 / N or less.

[0016] An image display device according to a sixth aspect of the present invention comprises: The optical laminate according to any one of the first to fifth aspects is provided.

[0017] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention.

[0018] First, the meanings of the terms used in this specification will be explained. "Main surface" means the surface having the widest area of ​​the film or layer. "(Meth)acrylic" means acrylic and methacrylic. For example, "(meth)acrylate" means acrylate and methacrylate. "Main component" means the component with the largest content in the composition. "Substantially free" means that the content of a substance such as a compound, polymer, or solvent is, for example, 0.1% by weight or less, preferably 0.05% by weight or less, and more preferably 0.01% by weight or less. "Main unit" means a unit that occupies 50% by weight or more, preferably 60% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more of all the structural units contained in the polymer. "Long-chain alkyl group" means an alkyl group having 6 to 30 carbon atoms. "Substantially parallel" means that the angle between two directions is 0°±7°, preferably 0°±5°, and even more preferably 0°±3°. "Substantially perpendicular" means that the angle between the two directions is 90°±7°, preferably 90°±5°, and more preferably 90°±3°.

[0019] [Embodiment of Optical Laminate] The optical laminate according to this embodiment includes a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet laminated in this order. 1 is 30 μm or more and 1000 μm or less. In addition, the first adhesive sheet has a breaking elongation of 500% or less.

[0020] 1 is a cross-sectional view showing a schematic example of an optical laminate according to the present embodiment. The optical laminate 10A includes a first optical film 1, a first adhesive sheet 2, a second optical film 3, and a second adhesive sheet 4. The optical laminate 10A has a structure in which the first optical film 1, the first adhesive sheet 2, the second optical film 3, and the second adhesive sheet 4 are laminated in this order.

[0021] The first optical film 1 is in contact with the first adhesive sheet 2. The first optical film 1 is disposed in contact with one main surface of the first adhesive sheet 2. In FIG. 1, the first optical film 1 is in contact with the entire one main surface of the first adhesive sheet. However, the first optical film 1 may be in contact with only a portion of the one main surface of the first adhesive sheet 2.

[0022] The first adhesive sheet 2 is formed on the second optical film 3. The first adhesive sheet 2 is formed on one main surface of the second optical film 3. In FIG. 1, the first adhesive sheet 2 is formed on the entire one main surface of the second optical film 3. However, the first adhesive sheet 2 may be formed on only a portion of the one main surface of the second optical film 3.

[0023] The second adhesive sheet 4 is formed on the second optical film 3. In detail, the second adhesive sheet 4 is formed on the main surface of the second optical film 3 opposite to the main surface on which the first adhesive sheet 2 is formed. In FIG. 1, the second adhesive sheet 4 is formed on the entire one main surface of the second optical film 3. However, the second adhesive sheet 4 may be formed on only a portion of the one main surface of the second optical film 3.

[0024] (First adhesive sheet) As described above, the thickness T of the first adhesive sheet 21 is 30 μm or more and 1000 μm or less, preferably 40 μm or more and 800 μm or less, more preferably 45 μm or more and 700 μm or less, further preferably 50 μm or more and 500 μm or less, and particularly preferably 80 μm or more and 300 μm or less. 1 By setting the thickness to 30 μm or more and 1000 μm or less, even if a strong pressure is applied in the thickness direction of the optical laminate 10A, the pressure can be dispersed. Therefore, the stress applied to the second optical film 3 is unlikely to become large, and damage to the second optical film 3 can be further suppressed. As a result, the optical laminate 10A can suppress display defects.

[0025] As described above, the breaking elongation of the first adhesive sheet 2 is 500% or less, preferably 400% or less, more preferably 350% or less, even more preferably 200% or less, and particularly preferably 100% or less. The lower limit of the breaking elongation of the first adhesive sheet 2 is, for example, 10%. When the breaking elongation of the first adhesive sheet 2 is 500% or less, the first adhesive sheet 2 is less likely to deform even when a strong pressure is applied in the thickness direction of the optical laminate 10A. As a result, damage to the second optical film 3 can be further suppressed.

[0026] The first adhesive sheet 2 is formed from a photocurable adhesive composition (I) or a solvent-based adhesive composition (II). The photocurable adhesive composition (I) is an adhesive composition that forms the first adhesive sheet 2 by being irradiated with light. The solvent-based adhesive composition (II) is, for example, an adhesive composition containing a polymer and a solvent. The photocurable adhesive composition (I) and the solvent-based adhesive composition (II) are described in detail below.

[0027] (Photocurable adhesive composition) The photocurable pressure-sensitive adhesive composition (I) contains, for example, a monomer group and / or a partial polymer of the monomer group. The monomer group in the photocurable pressure-sensitive adhesive composition (I) preferably contains a (meth)acrylic monomer. The photocurable pressure-sensitive adhesive composition (I) may contain a (meth)acrylic component, i.e., a (meth)acrylic monomer and a polymer thereof, as a main component. That is, the content of the (meth)acrylic monomer and a partial polymer thereof in the photocurable pressure-sensitive adhesive composition (I) may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, a (meth)acrylic first pressure-sensitive adhesive sheet 2 containing a (meth)acrylic polymer and a crosslinked product thereof as a main component can be formed. However, the photocurable pressure-sensitive adhesive composition (I) is not limited to the above example.

[0028] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate and octadecyl (meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl (meth)acrylate.

[0029] In 100 parts by weight of the monomer group, the amount of the (meth)acrylic acid alkyl ester may be, for example, 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, 85 parts by weight or more, 90 parts by weight or more, or even 95 parts by weight or more. In calculating the amount of a specific monomer, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0030] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of the carboxyl group-containing monomer are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The amount of the carboxyl group-containing monomer in 100 parts by weight of the monomer group may be, for example, 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4.8 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or even 0.5 parts by weight or less. The lower limit of the amount is, for example, 0.1 parts by weight or more, and in some cases, may be 0.5 parts by weight or more. The monomer group may not include a carboxyl group-containing monomer.

[0031] The monomer group may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may contribute to improving the cohesive strength of the adhesive sheet. Examples of the hydroxyl group-containing monomer are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxyl group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. In 100 parts by weight of the monomer group, the amount of the hydroxyl group-containing monomer may be, for example, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 7.5 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or even 0.5 parts by weight or less. The lower limit of the amount may be, for example, 0.01 parts by weight or more, 0.03 parts by weight or more, or even 0.05 parts by weight or more. The monomer group may not contain a hydroxyl group-containing monomer.

[0032] The monomer group may include an ether group-containing monomer. The ether group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may include an ether group-containing monomer. The ether group-containing monomer can contribute to improving the adhesive strength between the first optical film 1 and the first pressure-sensitive adhesive sheet 2.

[0033] The ether group-containing monomer is preferably an alkoxy group-containing monomer. Examples of the alkoxy group-containing monomer include an alkylene oxide adduct represented by the following chemical formula (1). R in formula (1) 1 R in formula (1) is a hydrogen atom or a methyl group. 2 R is an alkyl group. The alkyl group may be linear or branched.2 R is preferably a linear alkyl group. 2 Examples of n are a methyl group and an ethyl group. In formula (1), n ​​is an integer of 1 to 30, preferably an integer of 1 to 12, and more preferably an integer of 1 to 5. [ka]

[0034] Examples of the alkylene oxide adduct shown in formula (1) are 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate and methoxypolyethylene glycol (meth)acrylate, preferably 2-methoxyethyl acrylate (MEA).

[0035] The ether group-containing monomer is not limited to the alkylene oxide adduct. The ether group-containing monomer may have a ring structure, and the ring structure may have an ether group. Examples of the ring structure having an ether group include a tetrahydrofuran ring and a dioxane ring. Examples of the ether group-containing monomer having a ring structure are cyclic trimethylolpropane formal (meth)acrylate and tetrahydrofurfuryl (meth)acrylate.

[0036] In 100 parts by weight of the monomer group, the amount of the ether group-containing monomer may be, for example, 1 part by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or even 90 parts by weight or more. The upper limit of the amount is, for example, 99 parts by weight or less, and in some cases, may be 50 parts by weight or less. The monomer group may not contain an ether group-containing monomer.

[0037] In the photocurable pressure-sensitive adhesive composition (I), each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The partial polymer can contribute to the stable formation of a coating layer described later by appropriately increasing the viscosity of the photocurable pressure-sensitive adhesive composition (I).

[0038] The photocurable pressure-sensitive adhesive composition (I) usually contains a photopolymerization initiator. Examples of the photopolymerization initiator include photoradical generators that generate radicals when exposed to visible light and / or ultraviolet light having a wavelength shorter than 450 nm.

[0039] Examples of photopolymerization initiators include benzoin ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; substituted benzoin ethers such as anisole methyl ether; substituted acetophenones such as 2,2-diethoxyacetophenone and 2,2-dimethoxy-2-phenylacetophenone; α-hydroxyalkylphenones such as 1-hydroxycyclohexyl-phenyl ketone; substituted alpha-ketol such as 2-methyl-2-hydroxypropiophenone; aromatic sulfonyl chlorides such as 2-naphthalenesulfonyl chloride; photoactive oximes such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime; and benzophenone compounds such as benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone. Thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, 2,4-diethylthioxanthone and other thioxanthone compounds; 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine , 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, 2,4-trichloromethyl-(4'-methoxystyryl)-6-triazine and other triazine-based compounds;Oxime ester compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], O-(acetyl)-N-(1-phenyl-2-oxo-2-(4'-methoxy-naphthyl)ethylidene)hydroxylamine; phosphine compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide; quinone compounds such as 9,10-phenanthrenequinone, camphorquinone, ethylanthraquinone; borate compounds; carbazole compounds; imidazole compounds; and titanocene compounds. The photocurable pressure-sensitive adhesive composition (I) may contain one or more photopolymerization initiators.

[0040] The amount of the photopolymerization initiator in the photocurable pressure-sensitive adhesive composition (I) is, for example, 0.02 to 10 parts by weight, and may be 0.05 to 5 parts by weight, based on 100 parts by weight in total of the monomer group and its partial polymer.

[0041] The photocurable pressure-sensitive adhesive composition (I) may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. An example of the polyfunctional monomer is a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0042] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N DDA), 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and other polyfunctional acrylates (such as ester compounds of polyhydric alcohols and (meth)acrylic acid); allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0043] The crosslinking agent may contain a crosslinking agent other than the above-mentioned polyfunctional monomer. Examples of the other crosslinking agent include an isocyanate-based crosslinking agent. The photocurable pressure-sensitive adhesive composition (I) may contain an isocyanate-based crosslinking agent as a crosslinking agent, and preferably contains both the above-mentioned polyfunctional monomer and an isocyanate-based crosslinking agent. The isocyanate-based crosslinking agent can contribute to improving the adhesive strength between the first optical film 1 and the first pressure-sensitive adhesive sheet 2.

[0044] As the isocyanate-based crosslinking agent, a compound having at least two isocyanate groups (isocyanate compound) can be used. The number of isocyanate groups contained in the isocyanate compound is preferably 3 or more. The upper limit of the number of isocyanate groups is not particularly limited, and is, for example, 5. Examples of the isocyanate compound include an aromatic isocyanate compound, an alicyclic isocyanate compound, and an aliphatic isocyanate compound.

[0045] Examples of aromatic isocyanate compounds include phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenylether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0046] Examples of alicyclic isocyanate compounds include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0047] Examples of the aliphatic isocyanate compound include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), pentamethylene diisocyanate (PDI), 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0048] Examples of the isocyanate-based crosslinking agent include polymers (dimers, trimers, pentamers, etc.) of the above-mentioned isocyanate compounds, adducts obtained by adding them to polyhydric alcohols such as trimethylolpropane, urea-modified products, biuret-modified products, allophanate-modified products, isocyanurate-modified products, carbodiimide-modified products, and urethane prepolymers obtained by adding them to polyether polyols, polyester polyols, acrylic polyols, polybutadiene polyols, polyisoprene polyols, and the like.

[0049] The isocyanate-based crosslinking agent preferably includes an aliphatic isocyanate compound and / or a derivative of an aliphatic isocyanate compound. The isocyanate-based crosslinking agent is particularly preferably at least one selected from the group consisting of pentamethylene diisocyanate (PDI)-based crosslinking agents (PDI and its derivatives) and hexamethylene diisocyanate (HDI)-based crosslinking agents (HDI and its derivatives). Specific examples of PDI-based crosslinking agents include isocyanurate-modified PDI. Specific examples of HDI-based crosslinking agents include isocyanurate-modified HDI and biuret-modified HDI.

[0050] The amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) varies depending on the molecular weight, the number of functional groups, etc., but is preferably 0.4 parts by weight or more and 20 parts by weight or less, more preferably 0.4 parts by weight or more and 10 parts by weight or less, and even more preferably 0.5 parts by weight or more and 5 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. By appropriately adjusting the amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I), it is possible to further suppress display defects in the image display device. In addition, by appropriately adjusting the amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I), it is possible to improve the adhesive strength between the first pressure-sensitive adhesive sheet 2 and the first optical film 1 and / or the second optical film 3.

[0051] In addition, when the photocurable pressure-sensitive adhesive composition (I) contains an isocyanate-based crosslinking agent, the amount of the isocyanate-based crosslinking agent is, for example, 0.02 parts by weight or more, and may be 0.05 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, or even 1 part by weight or more, relative to 100 parts by weight in total of the monomer group and its partial polymer.

[0052] When an isocyanate-based crosslinking agent is added, the pressure-sensitive adhesive sheet may become hard, especially in a high-temperature environment. In such a case, the stress relaxation property of the pressure-sensitive adhesive sheet is impaired, so that the expansion and contraction stress of the optical film is easily transmitted to the interface between the pressure-sensitive adhesive sheet and the adherend, and peeling tends to occur. When the adhesive strength between the pressure-sensitive adhesive sheet and the optical film can be secured by a means other than the addition of an isocyanate-based crosslinking agent, it is preferable that the photocurable pressure-sensitive adhesive composition (I) does not contain an isocyanate-based crosslinking agent.

[0053] The photocurable pressure-sensitive adhesive composition (I) may contain additives other than those mentioned above, such as a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antiaging agent, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber.

[0054] The content of the solvent in the photocurable pressure-sensitive adhesive composition (I) is, for example, 5% by weight or less, and may be 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or even 0.5% by weight or less. The photocurable pressure-sensitive adhesive composition (I) may be substantially free of a solvent.

[0055] The viscosity of the photocurable pressure-sensitive adhesive composition (I) is preferably 5 to 150 poise. The photocurable pressure-sensitive adhesive composition (I) having a viscosity in the above range is particularly suitable for forming a coating layer, which will be described later.

[0056] The polymerization rate of the monomer group in the first adhesive sheet 2 is preferably 90% or more. The polymerization rate may be 95% or more, 98% or more, or even 99% or more.

[0057] The gel fraction of the first adhesive sheet 2 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.

[0058] [Method of manufacturing the first adhesive sheet] When the first adhesive sheet 2 is formed from the photocurable adhesive composition (I), the first adhesive sheet 2 can be produced, for example, by the following method. FIG. 2 is a schematic diagram for explaining an example of a method for producing a first adhesive sheet. As shown in FIG. 2(a), a first laminate 15 is produced, which includes a base sheet 21, a coating layer 22 containing the photocurable adhesive composition (I), and a release liner 23 in this order. Next, the first laminate 15 is irradiated with light 14. At this time, the light 14 passes through the base sheet 21 and reaches the coating layer 22, curing the coating layer 22. The light 14 is typically irradiated onto the first laminate 15 from the side of the base sheet 21. However, the light 14 may also be irradiated from the side of the release liner 23. As a result, the first adhesive sheet 2 is formed from the coating layer 22, as shown in FIG. 2(b). That is, a second laminate 16 is obtained, which includes the base sheet 21, the first adhesive sheet 2, and the release liner 23 in this order.

[0059] When the first adhesive sheet 2 is formed from the photocurable adhesive composition (I), the first adhesive sheet 2 can be produced by, for example, another method. FIG. 3 is a schematic diagram for explaining another example of a method for producing a first adhesive sheet. As shown in FIG. 3(a), a first laminate 15 is produced, which includes a base sheet 21, a coating layer 22 containing the photocurable adhesive composition (I), and a release liner 23 in this order. Next, the first laminate 15 is irradiated with light 14. As shown in FIG. 3(a), the light 14 is irradiated from both the release liner 23 and the base sheet 21 sides. As a result, the first adhesive sheet 2 is formed from the coating layer 22, as shown in FIG. 3(b). That is, a second laminate 16 is obtained, which includes the base sheet 21, the first adhesive sheet 2, and the release liner 23 in this order.

[0060] The first adhesive sheet 2 formed from the coating layer 22 may be sandwiched between the base sheet 21 and the release liner 23 and constitute a part of the second laminate 16 until the release liner 23 is peeled off.

[0061] An example of the substrate of the release liner 23 (hereinafter, "liner substrate") is a resin film. Examples of resins that may be included in the liner substrate are polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0062] The release liner 23 may have transparency to light 14 , or may have the same degree of transparency to light 14 as the base sheet 21 .

[0063] The thickness of the release liner 23 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0064] The release liner 23 may include a layer other than the liner substrate. The release liner 23 may include a release layer. The release liner 23 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 23 can be used such that the release layer is on the coating layer 22 side.

[0065] The release layer is typically a cured layer of a release agent composition containing a release agent. As the release agent, various types of release agents can be used, such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder. The release liner 23 may be provided with a cured layer of a release agent composition containing a silicone-based release agent as a main component (hereinafter, "silicone release layer"). The silicone release layer is particularly suitable for achieving both adhesion to the first adhesive sheet 2 and releasability.

[0066] The silicone-based release agent is, for example, various curable silicone materials such as addition reaction type, condensation reaction type, ultraviolet curable type, electron beam curable type, and solventless type, and an addition reaction curable silicone material is preferred. An addition reaction curable silicone material is particularly suitable for forming a release layer that has both adhesion and releasability to the first adhesive sheet 2. The curable silicone material may be a silicone-modified resin in which reactive silicone is introduced into an organic resin such as a urethane, epoxy, or alkyd resin by graft polymerization or the like.

[0067] An example of the addition reaction curing silicone material is a polyorganosiloxane having a vinyl group or an alkenyl group in the molecule. The addition reaction curing silicone material may not have a hydrosilyl group. Examples of the alkenyl group are 3-butenyl, 4-pentenyl, 5-hexenyl, 6-heptenyl, 7-octenyl, 8-nonenyl, 9-decenyl, 10-undecenyl, and 11-dodecenyl. Examples of the polyorganosiloxane are polyalkylalkylsiloxanes such as polydimethylsiloxane, polydiethylsiloxane, and polymethylethylsiloxane, polyalkylarylsiloxane, and copolymers of multiple types of Si atom-containing monomers such as poly(dimethylsiloxane-diethylsiloxane). The polyorganosiloxane is preferably polydimethylsiloxane.

[0068] A release agent composition containing a silicone-based release agent as a main component (hereinafter referred to as "silicone release agent composition") usually contains a crosslinking agent. An example of the crosslinking agent is polyorganosiloxane having a hydrosilyl group. The crosslinking agent may have two or more hydrosilyl groups in one molecule.

[0069] The silicone release agent composition may contain a curing catalyst. An example of the curing catalyst is a platinum catalyst. An example of the platinum catalyst is chloroplatinic acid, an olefin complex of platinum, or an olefin complex of chloroplatinic acid. The amount of the platinum catalyst used is, for example, 10 to 1000 ppm (weight basis, platinum equivalent) based on the total solid content of the composition.

[0070] The silicone release agent composition may contain additives. Examples of additives are release control agents and adhesion promoters. Examples of release control agents are unreactive silicone resins, and more specific examples are organosiloxanes such as octamethylcyclotetrasiloxane, and MQ resins. The amount of the release control agent and adhesion promoter used is, for example, 1 to 30% by weight in total based on the total solid content of the composition. Further examples of additives are fillers, antistatic agents, antioxidants, ultraviolet absorbers, plasticizers, and colorants. The amount of the further additives used is, for example, 10% by weight or less in total based on the total solid content of the composition.

[0071] The silicone release agent composition may contain an organic solvent. Examples of the organic solvent include hydrocarbon solvents such as cyclohexane, n-hexane, and n-heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; and alcohol solvents such as methanol, ethanol, and butanol. Two or more organic solvents may be contained. The amount of the organic solvent used is preferably 80 to 99.9% by weight of the silicone release agent composition.

[0072] The release layer can be formed, for example, by heating and drying a coating film containing the release agent composition formed on a liner substrate. Various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating can be applied to apply the release agent composition. For example, hot air drying can be applied to apply the heating and drying. The heating temperature and time vary depending on the heat resistance of the liner substrate, but are usually about 80 to 150°C and 10 seconds to 10 minutes. If necessary, irradiation with active energy rays such as ultraviolet rays may be used in combination.

[0073] The thickness of the release layer is, for example, 10 to 300 nm. The upper limit of the thickness may be 200 nm or less, 150 nm or less, 120 nm or less, 110 nm or less, 100 nm or less, less than 100 nm, 90 nm or less, 80 nm or less, 70 nm or less, less than 70 nm, or even 65 nm or less. The lower limit of the thickness may be 15 nm or more, 20 nm or more, 25 nm or more, 30 nm or more, 35 nm or more, 40 nm or more, 45 nm or more, or even 50 nm or more.

[0074] The release liner 23 may be in the form of a sheet or a continuous piece.

[0075] An example of the base sheet 21 is a resin film. Examples of the resin contained in the base sheet 21 are the same as the examples of the resin that can be contained in the liner base material.

[0076] The base sheet 21 preferably has excellent light 14 transmittance.

[0077] The thickness of the base sheet 21 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0078] The base sheet 21 may have a release layer on the surface on the side of the coating layer 22. Examples of the release layer that the base sheet 21 may have and the manufacturing method thereof are the same as the examples of the release layer that the release liner 23 may have and the manufacturing method thereof. Both the release liner 23 and the base sheet 21 may have a release layer. In this case, both release layers may be formed from a release agent composition containing the same release agent as a main component. In addition, the thicknesses of both release layers may be different, and for example, the release layer provided on the base sheet 21 may be thicker.

[0079] For base sheet 21 , a sheet having a greater peel strength from first adhesive sheet 2 than release liner 23 can usually be selected.

[0080] The base sheet 21 may be in the form of a sheet or a long piece.

[0081] The first laminate 15 can be formed, for example, by forming a coating layer 22 on a base sheet 21 (or a release liner 23) and then arranging a release liner 23 (or a base sheet 21) on the formed coating layer 22. Alternatively, the first laminate 15 may be formed by applying, in a pouring manner, a photocurable pressure-sensitive adhesive composition (I) into the space between the base sheet 21 and the release liner 23 that are held at a predetermined distance such that their main surfaces face each other.

[0082] The coating layer 22 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0083] The thickness of the coating layer 22 can be adjusted depending on the intended thickness of the first adhesive sheet 2, and may be, for example, 5 to 500 μm, 5 to 250 μm, 5 to 150 μm, 5 to 100 μm, 5 to 50 μm, 5 to 30 μm, 5 to 25 μm, or even 5 to 20 μm.

[0084] The light 14 irradiated to the first laminate 15 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light 14 may contain light having a wavelength in the same region as the absorption wavelength of the photopolymerization initiator contained in the photocurable pressure-sensitive adhesive composition. The light 14 may be irradiated with light having a short wavelength of 300 nm or less cut by a filter or the like, and cutting the short wavelength light is suitable for suppressing deterioration of the base sheet 21 caused by the light 14. The light source of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of the ultraviolet irradiation lamp are ultraviolet LED, low pressure mercury lamp, medium pressure mercury lamp, high pressure mercury lamp, ultra-high pressure mercury lamp, metal halide lamp, xenon lamp, microwave excited mercury lamp, black light lamp, chemical lamp, germicidal lamp, low pressure discharge mercury lamp, and excimer laser. Two or more ultraviolet irradiation lamps may be combined.

[0085] The illumination with light 14 may be continuous or intermittent.

[0086] The illuminance of the light 14 is, for example, 1 to 20 mW / cm 2 The irradiation time of the light 14 is, for example, 5 minutes to 5 hours. The integrated light amount of the light 14 on the first laminate 15 is, for example, 100 to 5000 mJ / cm 2 2 It is.

[0087] (Solvent-based pressure-sensitive adhesive composition) As described above, the solvent-based adhesive composition (II) is, for example, an adhesive composition containing a polymer and a solvent. When the first adhesive sheet 2 is formed from the solvent-based adhesive composition (II), examples of the adhesive constituting the first adhesive sheet 2 include acrylic adhesives, rubber-based adhesives, vinyl alkyl ether-based adhesives, silicone-based adhesives, polyester-based adhesives, polyamide-based adhesives, urethane-based adhesives, fluorine-based adhesives, epoxy-based adhesives, and polyether-based adhesives. The adhesives constituting the first adhesive sheet 2 are used alone or in combination of two or more kinds. However, from the viewpoints of transparency, processability, durability, adhesion, and the like, it is preferable to use an acrylic adhesive (composition) containing a (meth)acrylic polymer alone. In other words, it is preferable that the first adhesive sheet 2 contains a (meth)acrylic polymer as a polymer.

[0088] [(Meth)acrylic polymer (A)] The (meth)acrylic polymer (A) preferably has as its main unit a structural unit derived from a (meth)acrylic monomer (A1) having an alkyl group having 1 to 30 carbon atoms on its side chain. The alkyl group may be linear or branched. The (meth)acrylic polymer (A) may have one or more structural units derived from the (meth)acrylic monomer (A1). Examples of the (meth)acrylic monomer (A1) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and the like. acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, and n-tetradecyl (meth)acrylate.

[0089] The (meth)acrylic polymer (A) may have a structural unit derived from a (meth)acrylic monomer (A1) having a long-chain alkyl group on the side chain. An example of the monomer (A1) is n-dodecyl (meth)acrylate (lauryl (meth)acrylate).

[0090] The (meth)acrylic polymer (A) may have a structural unit derived from a (meth)acrylic monomer (A1) which, when made into a homopolymer, has a glass transition temperature (Tg) in the range of −70 to −20° C. An example of the monomer (A1) is n-butyl acrylate.

[0091] The (meth)acrylic polymer (A) may have a structural unit other than the structural unit derived from the (meth)acrylic monomer (A1). The structural unit is derived from a monomer (A2) copolymerizable with the (meth)acrylic monomer (A1). The (meth)acrylic polymer (A) may have one or more types of the structural unit.

[0092] An example of the monomer (A2) is an aromatic ring-containing monomer. The aromatic ring-containing monomer may be an aromatic ring-containing (meth)acrylic monomer. Examples of the aromatic ring-containing monomer are phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, hydroxyethylated β-naphthol (meth)acrylate, and biphenyl (meth)acrylate. The content of the constituent unit derived from the aromatic ring-containing monomer in the (meth)acrylic polymer (A) is, for example, 0 to 50% by weight, and may be 1 to 30% by weight, 5 to 25% by weight, 8 to 20% by weight, 10 to 18% by weight, 12 to 16% by weight, or even 12 to 16% by weight. The (meth)acrylic polymer (A) having a structural unit derived from an aromatic ring-containing monomer can contribute to improving the compatibility of the (meth)acrylic polymer (A) with the crosslinking agent (B) and its self-polymer.

[0093] Another example of the monomer (A2) is a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a hydroxyl group-containing (meth)acrylic monomer. Examples of the hydroxyl group-containing monomer are hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate and 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxyl group can react with various crosslinking agents. From the viewpoint of increasing the uniformity of the crosslinked structure to be formed, the content of the structural unit derived from the hydroxyl group-containing monomer in the (meth)acrylic polymer (A) may be 1% by weight or less, 0.5% by weight or less, or even 0.1% by weight or less, or may be 0% by weight (no such structural unit may be included).

[0094] Monomer (A2) may be a carboxyl group-containing monomer, an amino group-containing monomer, or an amide group-containing monomer. Examples of carboxyl group-containing monomers are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of amino group-containing monomers are N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. Examples of the amide group-containing monomer include acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propane(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl group-containing lactam-based monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam.

[0095] Monomer (A2) may be a polyfunctional monomer. Examples of polyfunctional monomers are polyfunctional acrylates such as hexanediol di(meth)acrylate (1,6-hexanediol di(meth)acrylate), butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, epoxy acrylate, polyester acrylate and urethane acrylate; and divinylbenzene. The polyfunctional acrylate is preferably 1,6-hexanediol diacrylate or dipentaerythritol hexa(meth)acrylate.

[0096] The total content of the structural units derived from the carboxyl group-containing monomer, the amino group-containing monomer, the amide group-containing monomer and the polyfunctional monomer in the (meth)acrylic polymer (A) is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 8% by weight or less. When the (meth)acrylic polymer (A) has the structural units, the total content is, for example, 0.01% by weight or more, and may be 0.05% by weight or more. The (meth)acrylic polymer (A) may not contain a structural unit derived from a polyfunctional monomer. When the (meth)acrylic polymer (A) has a structural unit derived from a carboxyl group-containing monomer, particularly acrylic acid, and / or a structural unit derived from an amide group-containing monomer, the self-polymerization of the crosslinking agent (B), for example, can be enhanced. The improvement in the self-polymerization property of the crosslinking agent (B) can particularly contribute to suppressing peeling of the pressure-sensitive adhesive sheet in a humid environment and stabilizing the physical properties of the pressure-sensitive adhesive sheet in a system having a high content of the crosslinking agent (B).

[0097] Examples of the other monomer (A2) include (meth)acrylic acid alkoxyalkyl esters such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate; epoxy group-containing monomers such as glycidyl (meth)acrylate and methylglycidyl (meth)acrylate; vinylsulfonate sodium salts; (meth)acrylic acid esters having an alicyclic hydrocarbon group, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; vinyl esters, such as vinyl acetate and vinyl propionate; aromatic vinyl compounds, such as styrene and vinyl toluene; olefins or dienes, such as ethylene, propylene, butadiene, isoprene, and isobutylene; vinyl ethers, such as vinyl alkyl ether; and vinyl chloride.

[0098] The total content of the structural units derived from the other monomer (A2) in the (meth)acrylic polymer (A) is, for example, 30% by weight or less, and may be 10% by weight or less, and is preferably 0% by weight (not including such structural units).

[0099] The (meth)acrylic polymer (A) can be formed by polymerizing one or more of the above-mentioned monomers by a known method. A monomer and a partial polymer of the monomer may be polymerized. The polymerization can be carried out, for example, by solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, or active energy ray polymerization. Since a pressure-sensitive adhesive sheet having excellent optical transparency can be formed, solution polymerization and active energy ray polymerization are preferred. The polymerization is preferably carried out while avoiding contact between the monomer and / or the partial polymer and oxygen, and for this purpose, for example, polymerization in an inert gas atmosphere such as nitrogen or polymerization in a state in which oxygen is blocked by a resin film or the like can be adopted. The (meth)acrylic polymer (A) formed may be any of a random copolymer, a block copolymer, a graft copolymer, and the like.

[0100] The polymerization system for forming the (meth)acrylic polymer (A) may contain one or more polymerization initiators. The type of polymerization initiator can be selected depending on the polymerization reaction, and may be, for example, a thermal polymerization initiator or a photopolymerization initiator.

[0101] Examples of the solvent used in the solution polymerization include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. However, the solvent is not limited to the above examples. The solvent may be a mixed solvent of two or more solvents.

[0102] The polymerization initiator used in the solution polymerization is, for example, an azo-based polymerization initiator, a peroxide-based polymerization initiator, or a redox-based polymerization initiator. The peroxide-based polymerization initiator is, for example, dibenzoyl peroxide or t-butyl permaleate. Among them, the azo-based polymerization initiator disclosed in JP-A-2002-69411 is preferable. The azo-based polymerization initiator is, for example, 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate) dimethyl, or 4,4'-azobis-4-cyanovaleric acid. However, the polymerization initiator is not limited to the above examples. The amount of the azo-based polymerization initiator used is, for example, 0.05 to 0.5 parts by weight, or may be 0.1 to 0.3 parts by weight, based on 100 parts by weight of the total amount of the monomers.

[0103] The active energy rays used in the active energy ray polymerization are, for example, ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, and ultraviolet rays. The active energy rays are preferably ultraviolet rays. Polymerization by irradiation with ultraviolet rays is also called photopolymerization. The polymerization system for the active energy ray polymerization typically contains a photopolymerization initiator. The polymerization conditions for the active energy polymerization are not limited as long as a (meth)acrylic polymer (A) is formed.

[0104] Examples of the photopolymerization initiator include a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, and a thioxanthone-based photopolymerization initiator, although the photopolymerization initiator is not limited to the above examples.

[0105] Examples of the benzoin ether-based photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride. An example of the photoactive oxime-based photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. An example of the benzoin-based photopolymerization initiator is benzoin. An example of the benzyl-based photopolymerization initiator is benzil. An example of the benzophenone-based photopolymerization initiator is benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexylphenyl ketone. An example of the ketal-based photopolymerization initiator is benzyl dimethyl ketal. An example of the thioxanthone-based photopolymerization initiator is thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.

[0106] The amount of the photopolymerization initiator used is, for example, 0.01 to 1 part by weight, and may be 0.05 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomers.

[0107] The weight average molecular weight (Mw) of the (meth)acrylic polymer (A) is, for example, 1,000,000 to 2,800,000, and from the viewpoint of the durability and heat resistance of the pressure-sensitive adhesive sheet, may be 1,200,000 or more, or even 1,400,000 or more. The weight average molecular weight (Mw) of the polymer and oligomer in this specification is a value (polystyrene equivalent) based on measurement by GPC (gel permeation chromatography).

[0108] The content of the (meth)acrylic polymer (A) in the pressure-sensitive adhesive composition (II) is, for example, 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more, in terms of solid content ratio. The upper limit of the content is, for example, 99% by weight or less, and may be 97% by weight or less, 95% by weight or less, 93% by weight or less, or even 90% by weight or less.

[0109] [Crosslinking agent (B)] The crosslinking agent (B) is typically a polyfunctional crosslinking agent having two or more crosslinking reactive groups per molecule. The crosslinking agent (B) may be a trifunctional or higher crosslinking agent having three or more crosslinking reactive groups per molecule. The trifunctional or higher crosslinking agent (B) is likely to form a self-polymer. The upper limit of the number of crosslinking reactive groups per molecule is, for example, 5.

[0110] The crosslinking agent (B) is, for example, an isocyanate-based crosslinking agent. The isocyanate-based crosslinking agent contains an isocyanate group as a crosslinking reactive group. The isocyanate-based crosslinking agent (B) may be an aromatic isocyanate compound, an alicyclic isocyanate compound, or an aliphatic isocyanate compound.

[0111] Examples of aromatic isocyanate compounds that can be used for the crosslinking agent (B) are phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenylether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0112] Examples of alicyclic isocyanate compounds that can be used in the crosslinking agent (B) include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0113] Examples of aliphatic isocyanate compounds that can be used in the crosslinking agent (B) are trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate and 2,4,4-trimethylhexamethylene diisocyanate.

[0114] The crosslinking agent (B) may be a derivative of the above-mentioned isocyanate compound. Examples of the derivative include a multimer (dimer, trimer, pentamer, etc.), an adduct obtained by adding to a polyhydric alcohol such as trimethylolpropane, a urea-modified product, a biuret-modified product, an allophanate-modified product, an isocyanurate-modified product, a carbodiimide-modified product, and a urethane prepolymer obtained by adding to a polyether polyol, a polyester polyol, an acrylic polyol, a polybutadiene polyol, a polyisoprene polyol, etc.

[0115] The crosslinking agent (B) is preferably an aromatic isocyanate compound and its derivative, more preferably tolylene diisocyanate and its derivative (in other words, a tolylene diisocyanate-based (TDI-based) crosslinking agent). The TDI-based crosslinking agent is superior in reaction uniformity compared to xylylene diisocyanate and its derivative (in other words, a xylylene diisocyanate-based (XDI-based) crosslinking agent). An example of the TDI-based crosslinking agent is an adduct of tolylene diisocyanate and a polyfunctional alcohol, and a more specific example is a trimethylolpropane / tolylene diisocyanate trimer adduct.

[0116] Commercially available products can be used for the crosslinking agent (B). Examples of commercially available products include Millionate MT, Millionate MTL, Millionate MR-200, Millionate MR-400, Coronate L, Coronate HL and Coronate HX (all of which are manufactured by Tosoh Corporation; all are trade names), as well as Takenate D-102, Takenate D-103, Takenate D-110N, Takenate D-120N, Takenate D-140N, Takenate D-160N, Takenate D-165N, Takenate D-170HN, Takenate D-178N, Takenate 500 and Takenate 600 (all of which are manufactured by Mitsui Chemicals; all are trade names). As the crosslinking agent (B), Coronate L, Takenate D-102 and Takenate D-103 (all of which are trimethylolpropane / tolylene diisocyanate trimer adducts) can be preferably used.

[0117] The amount of the crosslinking agent (B) in the pressure-sensitive adhesive composition (I) is 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, 9 parts by weight or more, 10 parts by weight or more, more than 10 parts by weight, or even 11 parts by weight or more, based on 100 parts by weight of the (meth)acrylic polymer (A). The upper limit of the amount is, for example, 30 parts by weight or less, 28 parts by weight or less, 25 parts by weight or less, 23 parts by weight or less, 20 parts by weight or less, 19 parts by weight or less, 18 parts by weight or less, or even 15 parts by weight or less.

[0118] The pressure-sensitive adhesive composition (I) may contain one or more crosslinking agents (B).

[0119] The pressure-sensitive adhesive sheet formed from the pressure-sensitive adhesive composition (II) may have an interpenetrating network (IPN) structure of the crosslinked product of the (meth)acrylic polymer (A) and the self-polymer of the crosslinking agent (B). The IPN structure is suitable for improving the durability of the pressure-sensitive adhesive sheet.

[0120] Other examples of the crosslinking agent (B) are peroxide-based crosslinking agents, epoxy-based crosslinking agents, imine-based crosslinking agents, and polyfunctional metal chelates. However, the crosslinking agent (B) is preferably an isocyanate-based crosslinking agent. When the pressure-sensitive adhesive composition (II) contains a crosslinking agent (B) other than an isocyanate-based crosslinking agent, the total amount of the crosslinking agent (B) is preferably 0.1 to 5 parts by weight, more preferably 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, and 0.1 to 1 part by weight, in that order, relative to 100 parts by weight of the (meth)acrylic polymer (A). The pressure-sensitive adhesive composition (II) may not contain a crosslinking agent (B) other than an isocyanate-based crosslinking agent, such as an epoxy-based crosslinking agent.

[0121] [Additives] The pressure-sensitive adhesive composition (II) may contain other additives. Examples of additives include silane coupling agents, polyfunctional alcohols, colorants such as pigments and dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, rework improvers, softeners, antioxidants, antiaging agents, light stabilizers, UV absorbers, polymerization inhibitors, antistatic agents (alkali metal salts, ionic liquids, ionic solids, etc., which are ionic compounds), inorganic fillers, organic fillers, powders such as metal powders, particles, and foil-like materials. The additives can be blended in an amount of, for example, 10 parts by weight or less, preferably 5 parts by weight or less, and more preferably 1.5 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer (A).

[0122] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.

[0123] When the pressure-sensitive adhesive composition (II) contains a silane coupling agent, the blending amount thereof is, for example, 5 parts by weight or less, and may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, based on 100 parts by weight of the (meth)acrylic polymer (A). The pressure-sensitive adhesive composition (I) may not contain a silane coupling agent.

[0124] The pressure-sensitive adhesive composition (II) may contain a polyfunctional alcohol. The molecular weight of the polyfunctional alcohol may be, for example, 240 or less, 230 or less, 220 or less, 210 or less, 200 or less, 190 or less, 180 or less, 170 or less, 160 or less, or even 150 or less. The lower limit of the molecular weight may be, for example, 60 or more, 80 or more, 90 or more, or even 100 or more.

[0125] Examples of polyfunctional alcohols include alkylene glycols such as ethylene glycol and propylene glycol and polymers thereof, ether glycols such as diethylene glycol and polymers thereof, trimethylolethane, trimethylolpropane, glycerin, and sugar alcohols such as pentaerythritol and sorbitol. The polyfunctional alcohol is preferably trimethylolpropane, glycerin, and diethylene glycol and polymers thereof, and more preferably trimethylolpropane.

[0126] The polyfunctional alcohol may be three or more functional. Examples of trifunctional polyfunctional alcohols are trimethylolpropane and glycerin.

[0127] The polyfunctional alcohol may not have a reactive group other than the hydroxyl group that is reactive with the crosslinking agent (B). The reactive group is, for example, at least one selected from an amino group, a carboxyl group, and an epoxy group, and is particularly an amino group.

[0128] The amount of the polyfunctional alcohol in the pressure-sensitive adhesive composition (II) is, for example, 0.5 parts by weight or more and 20 parts by weight or less, based on 100 parts by weight of the (meth)acrylic polymer (A). The upper limit of the amount may be 15 parts by weight or less, 10 parts by weight or less, 8 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, or even 3 parts by weight or less.

[0129] The adhesive composition (II) may not contain a crosslinking accelerator such as a catalyst. An example of the crosslinking accelerator is a polyether, polyether polyol, or phosphoric acid ester having a reactive group reactive with the crosslinking agent (B). The reactive group is, for example, at least one selected from a hydroxyl group, an amino group, a carboxyl group, and an epoxy group, and is particularly a hydroxyl group or an amino group. The adhesive composition (II) may not contain a polyether polyol having an amino group, and may not contain a phosphoric acid ester having a hydroxyl group. The solvent-based adhesive (II) may not contain a photocuring agent such as an ultraviolet curing agent.

[0130] [Method of manufacturing the first adhesive sheet] When the first pressure-sensitive adhesive sheet 2 is formed from the solvent-based pressure-sensitive adhesive composition (II), the first pressure-sensitive adhesive sheet 2 contains, for example, a crosslinked product of the (meth)acrylic polymer (A). The first pressure-sensitive adhesive sheet 2 can be formed from the solvent-based pressure-sensitive adhesive composition (II) by the following method.

[0131] A method for producing the first adhesive sheet 2 includes, for example, applying a solvent-based adhesive composition (II) containing a (meth)acrylic polymer (A) and a crosslinking agent to a substrate to form a coating film, and drying the resulting coating film.

[0132] As the substrate, for example, a release film can be used. The first adhesive sheet 2 formed on the release film can be transferred to, for example, an optical film. The substrate may be the first optical film 1 or the second optical film 3. In this case, the first adhesive sheet 2 can be formed on the first optical film 1 or the second optical film 3, and an optical film with the first adhesive sheet can be obtained.

[0133] After the first adhesive sheet 2 is transferred to the first optical film 1 or the second optical film 3, the release film can be used as a separator until the first adhesive sheet 2 is put to practical use, thereby simplifying the process.

[0134] Examples of materials constituting the release film include suitable thin sheets such as porous materials such as plastic films, paper, cloth, and nonwoven fabrics, nets, foam sheets, metal foils, and laminates thereof, among which plastic films are preferably used because of their excellent surface smoothness.

[0135] The plastic film is not particularly limited, and examples thereof include a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a polymethylpentene film, a polyvinyl chloride film, a vinyl chloride copolymer film, a polyethylene terephthalate film, a polybutylene terephthalate film, a polyurethane film, and an ethylene-vinyl acetate copolymer film.

[0136] The thickness of the release film is usually 5 to 200 μm, preferably about 5 to 100 μm. The release film is subjected to a release treatment such as a silicone-based, fluorine-based, or long-chain alkyl-based treatment. The release film may be subjected to a release and antifouling treatment using a fatty acid amide-based release agent or silica powder, or an antistatic treatment such as a coating type, kneading type, or deposition type.

[0137] A solution (adhesive solution) containing the solvent-based adhesive composition (II) may be applied to the substrate. The solid content of the adhesive solution is, for example, 5 to 50% by weight, and preferably 10 to 40% by weight. The adhesive solution can be prepared by appropriately adding the same solvent as the polymerization solvent or a different solvent to the solvent-based adhesive composition (II) depending on the polymerization form of the (meth)acrylic polymer (A).

[0138] Various methods are used to apply the solvent-based pressure-sensitive adhesive composition (II) to the substrate, and examples of such methods include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and extrusion coating using a die coater, etc. The amount of the solvent-based pressure-sensitive adhesive composition (II) to be applied can be appropriately adjusted depending on the intended thickness of the first pressure-sensitive adhesive sheet 2.

[0139] The coating film is dried to harden the coating film, forming the first adhesive sheet 2. The drying temperature of the coating film is, for example, 130° C. or less, preferably 125° C. or less, more preferably 120° C. or less, even more preferably 110° C. or less, and particularly preferably 100° C. or less. The drying temperature of the coating film may be 60° C. or more, or 80° C. or more. When the drying temperature is 60° C. or more, for example, the reaction of the isocyanate-based crosslinking agent proceeds smoothly, the cohesive force of the first adhesive sheet 2 can be improved, and display unevenness of the image display device tends to be reduced. When the drying temperature is 130° C. or less, for example, the reaction speed of the isocyanate-based crosslinking agent can be appropriately adjusted, and transparency tends to be ensured.

[0140] The drying time of the coating film can be appropriately adjusted depending on the composition of the solvent-based pressure-sensitive adhesive composition (II), and is preferably 30 to 300 seconds, more preferably 40 to 240 seconds, and particularly preferably 60 to 180 seconds.

[0141] As described above, the first adhesive sheet 2 is formed from the photocurable adhesive composition (I) or the solvent-based adhesive composition (II). In other words, the first adhesive sheet 2 is a cured product of the photocurable adhesive composition (I) or a cured product of the solvent-based adhesive composition (II). The first adhesive sheet 2 is preferably formed from the photocurable adhesive composition (I). That is, the first adhesive sheet 2 is preferably formed from the photocurable adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group. The first adhesive sheet 2 formed from the photocurable adhesive composition (I) tends to have excellent smoothness of its surface. The smoothness of the first adhesive sheet 2 can improve the adhesion between the first adhesive sheet 2 and the first optical film 1 and / or the second optical film 3. In addition, the smooth first adhesive sheet 2 tends to suppress the occurrence of appearance defects such as color unevenness. In other words, by using the first adhesive sheet 2 formed from the photocurable adhesive composition (I), the image display device can achieve the effect of suppressing the occurrence of appearance defects such as color unevenness, in addition to the effect of being suitable for suppressing display defects even when a small object collides with or presses the screen with a small contact area.

[0142] (Second adhesive sheet) Thickness T of the second adhesive sheet 4 2 is, for example, 5 μm or more and 100 μm or less, preferably 8 μm or more and 80 μm or less, more preferably 10 μm or more and 50 μm or less, and further preferably 12 μm or more and 30 μm or less. By appropriately adjusting the thickness of the second adhesive sheet 4, the adhesion between the second optical film 3 and the second adhesive sheet 4 can be improved.

[0143] The breaking elongation of the second adhesive sheet 4 is, for example, 500% or more. The breaking elongation of the second adhesive sheet 4 is preferably 700% or more, more preferably 800% or more, and even more preferably 1000% or more. The upper limit of the breaking elongation of the second adhesive sheet 4 is, for example, 2000%.

[0144] A known adhesive can be used for the second adhesive sheet 4. The second adhesive sheet 4 may be an adhesive sheet formed from a photocurable adhesive composition (I), or may be an adhesive sheet formed from a solvent-based adhesive composition (II). The first adhesive sheet 2 may be used for the second adhesive sheet 4. The second adhesive sheet 4 is preferably an adhesive sheet formed from a photocurable adhesive composition (I).

[0145] (Daiichi Optical Film) 1, the first optical film 1 has two main surfaces facing each other. One of the main surfaces is exposed to the outside of the optical laminate 10A, for example. The other main surface of the first optical film 1 faces the first adhesive sheet 2 and is the surface of the first optical film 1 on which the first adhesive sheet is laminated.

[0146] The first optical film 1 may be composed of a single layer or may be a laminate of multiple layers. In other words, the first optical film 1 may be composed of a single film or may be a laminate of multiple films. Each film constituting the first optical film 1 may be bonded via any adhesive and any pressure-sensitive adhesive sheet. The first optical film 1 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The first optical film 1 may include a polarizing film. The first optical film 1 may be a laminate film including a polarizing film and / or a retardation film.

[0147] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with the main surface of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0148] Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine and dichroic dyes; and polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride. Polarizers typically consist of polyvinyl alcohol films (polyvinyl alcohol films include partially saponified ethylene-vinyl acetate copolymer films) and dichroic substances such as iodine.

[0149] The thickness of the polarizer is, for example, 80 μm or less, and may be 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness of the polarizer is not particularly limited, and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change, and can contribute to improving the durability of the optical laminate, particularly the durability at high temperatures.

[0150] As the material of the protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different from each other. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curing resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more types of optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0151] The thickness of the protective film can be appropriately determined, but is generally about 10 to 200 μm in terms of strength, workability such as handleability, thinness, and the like.

[0152] The polarizer and the protective film are usually adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include an isocyanate-based adhesive, a polyvinyl alcohol-based adhesive, a gelatin-based adhesive, a vinyl-based latex, a water-based polyurethane, and a water-based polyester. Examples of adhesives other than the above-mentioned adhesives include an ultraviolet-curable adhesive and an electron beam-curable adhesive. The electron beam-curable polarizing plate adhesive exhibits suitable adhesion to various protective films. The adhesive may contain a metal compound filler.

[0153] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0154] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for the purposes of anti-reflection, anti-sticking, diffusion, anti-glare, etc.

[0155] The polarizing film may be a circular polarizing film.

[0156] The retardation film may be one obtained by stretching a polymer film or one obtained by aligning and fixing a liquid crystal material. The retardation film has birefringence, for example, in the in-plane and / or thickness direction.

[0157] Examples of retardation films include anti-reflection retardation films (see JP 2012-133303 A,

[0221] ,

[0222] ,

[0228] ), viewing angle compensation retardation films (see JP 2012-133303 A,

[0225] ,

[0226] ), and tilted orientation retardation films for viewing angle compensation (see JP 2012-133303 A,

[0227] ).

[0158] As the retardation film, as long as it substantially has the above-mentioned functions, for example, the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, and the like are not particularly limited, and a known retardation film can be used.

[0159] The thickness of the retardation film is preferably 20 μm or less, more preferably 10 μm or less, further preferably 1 to 9 μm, and particularly preferably 3 to 8 μm.

[0160] The retardation film is composed of, for example, two layers, a quarter-wave plate and a half-wave plate, in which liquid crystal material is oriented and fixed.

[0161] (Second optical film) 1, the second optical film 3 has two main surfaces facing each other. One of the main surfaces faces the first adhesive sheet 2, and is the surface of the second optical film 3 on which the first adhesive sheet 2 is laminated. The other main surface of the second optical film 3 faces the second adhesive sheet 4, and is the surface of the second optical film 3 on which the second adhesive sheet 4 is laminated.

[0162] The second optical film 3 may be composed of a single layer or may be a laminate of multiple layers. In other words, the second optical film 3 may be composed of a single film or may be a laminate of multiple films. Each film constituting the second optical film 3 may be bonded via any adhesive and any pressure-sensitive adhesive sheet. When the second optical film 3 is a laminate of multiple films, the second optical film 3 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The second optical film 3 may be a laminate including a polarizing film and / or a retardation film.

[0163] The second optical film 3 may include a laminate of a plurality of retardation films. The second optical film 3 may include a laminate of a first retardation film and a second retardation film. The first retardation film may be bonded to the second retardation film via any adhesive and any pressure-sensitive adhesive sheet.

[0164] The second optical film 3 includes, for example, a plurality of layers. The plurality of layers is, for example, a laminate including a polarizer and at least one film. The at least one film included in the second optical film 3 may be disposed between the polarizer and the second adhesive sheet. That is, the second optical film 3 may include at least one film disposed at a position closer to the second adhesive sheet than the polarizer.

[0165] Fig. 4A is a cross-sectional view showing a schematic example of the second optical film. As shown in Fig. 4A, the second optical film 3A is formed by laminating a film A31, a polarizer 32, a film B33, and a film C34 in this order. The films A31 and B33 may be protective films for the polarizer. The film C34 may be a retardation film. However, the films A to C may be films having functions other than those described above. For example, the film A and / or the film B may have a function as a retardation film.

[0166] The photoelastic coefficients of the films B33 and C34 arranged between the polarizer 32 and the second adhesive sheet 4 are each 4×10 -11 m 2 The photoelastic coefficient is preferably 2×10 -11 m 2 / N or less, more preferably 1×10 -11 m 2 / N or less, and more preferably 5×10 -12 m 2 / N or less. The lower limit of the photoelastic coefficient is not particularly limited, but is, for example, 2×10 -13 m 2 / N or more, preferably 5 × 10 -13 m 2 / N or more, more preferably 1×10 -12 m 2 / N or more. At least one retardation film may be disposed between the polarizer 32 and the second adhesive sheet 4.

[0167] In the following description, the film B33 may be referred to as the first retardation film 33 and the film C34 as the second retardation film 34, in the case where both the film B33 and the film C34 function as retardation films.

[0168] (Polarizing plate) The polarizing plate 30 is, for example, a laminate of a polarizer 32 and a protective film 31 disposed on the viewing side of the polarizer 32. The protective film 31 is typically attached to the viewing side of the polarizer 32 via any appropriate adhesive sheet. The protective film 31 is located between the polarizer 32 and the first adhesive sheet 2 and is in contact with the first adhesive sheet 2. The polarizing plate 30 may be a laminate further including a second protective film on the side opposite the viewing side of the polarizer 32.

[0169] (Polarizer) Any appropriate polarizer may be adopted as the polarizer 32. For example, the resin film forming the polarizer 32 may be a single-layer resin film or a laminate of two or more layers.

[0170] A specific example of a polarizer composed of a single-layer resin film is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, not only can dirt and antiblocking agents on the surface of the PVA-based film be washed off, but also uneven dyeing can be prevented by swelling the PVA-based resin film.

[0171] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer a polarizer. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate preferably forms a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin on one side of the resin substrate. Stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include air-stretching the laminate at a high temperature (for example, 95°C or higher) before stretching in the boric acid aqueous solution, as necessary. In addition, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the method for producing a polarizer includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, it is possible to increase the crystallinity of PVA even when PVA is applied onto a thermoplastic resin, and it is possible to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, problems such as a decrease in the orientation of PVA or dissolution when immersed in water in the subsequent dyeing step or stretching step can be prevented, and it is possible to achieve high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in the orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment step in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment, etc. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction by a drying shrinkage treatment.The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.

[0172] The polarizer 32 is preferably made of a laminate of two or more layers, and more preferably made of a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate.

[0173] The thickness of the polarizer 32 is preferably 15 μm or less, more preferably 12 μm or less, further preferably 10 μm or less, particularly preferably 8 μm or less, and typically 1 μm or more, preferably 3 μm or more. When the thickness of the polarizer 32 is in this range, the occurrence of warping of the optical laminate in a high-humidity environment can be more stably suppressed.

[0174] The polarizer 32 preferably exhibits absorptive dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer 32 is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer 32 is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0175] (Protective film) The protective film 31 is formed of any suitable film that can be used as a protective layer for the polarizer 32. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0176] The protective film 31 contains, for example, a (meth)acrylic resin. For example, a (meth)acrylic resin having a glutarimide structure is used as the (meth)acrylic resin. The (meth)acrylic resin having a glutarimide structure is described, for example, in JP-A-2006-309033, JP-A-2006-317560, JP-A-2006-328329, JP-A-2006-328334, JP-A-2006-337491, JP-A-2006-337492, JP-A-2006-337493, JP-A-2006-337569, JP-A-2007-009182, JP-A-2009-161744, and JP-A-2010-284840. These descriptions are incorporated herein by reference.

[0177] The thickness of the protective film 31 is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm.

[0178] (First phase difference film) When the film B33 functions as a retardation film, the first retardation film 33 may be composed of a retardation film having any appropriate optical properties and / or mechanical properties depending on the purpose. The first retardation film 33 is composed of, for example, a single layer. The first retardation film 33 is located on the opposite side to the viewing side of the polarizing plate 30 described above. In detail, the first retardation film 33 is attached to the opposite side to the viewing side of the polarizer 32 via any appropriate adhesive sheet. In this case, the first retardation film 33 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, the first retardation film 33 is provided at a position closer to the second adhesive sheet 4 than the polarizer 32. The first retardation film 33 may also serve as a protective layer on the opposite side to the viewing side of the polarizer 32.

[0179] The thickness of the first retardation film 33 is preferably 10 μm to 60 μm, and more preferably 20 μm to 50 μm.

[0180] The in-plane retardation Re(550) of the first retardation film 33 is preferably 80 nm to 150 nm, more preferably 90 nm to 140 nm, and further preferably 100 nm to 130 nm.

[0181] The refractive index characteristics of the first retardation film 33 preferably satisfy the relationship nx>ny>nz. The Nz coefficient of the first retardation film 33 is preferably 1.1 to 3.0, and more preferably 1.3 to 2.7.

[0182] The first retardation film 33 can be preferably disposed so that its slow axis is substantially parallel to the absorption axis of the polarizer.

[0183] The photoelastic coefficient of the first phase difference film 33 is, for example, as described above. By appropriately adjusting the photoelastic coefficient of the first phase difference film 33, even if a small object collides with or presses the screen with a small contact area, an optical laminate 10A that is more suitable for suppressing display defects can be obtained. In addition, by appropriately adjusting the photoelastic coefficient of the first phase difference film 33, phase difference change is unlikely to occur when shrinkage stress occurs during heating. Therefore, by appropriately adjusting the photoelastic coefficient of the first phase difference film 33, heat unevenness can be effectively prevented when the optical laminate 10A is applied to an image display device.

[0184] The first retardation film 33 may exhibit a reverse wavelength dispersion characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes according to the wavelength of the measurement light. It is preferable that the first retardation film 33 exhibits a flat wavelength dispersion characteristic. Specifically, Re(450) / Re(550) of the first retardation film 33 is preferably 0.99 to 1.03, and Re(650) / Re(550) is preferably 0.98 to 1.02. By arranging a λ / 2 plate and a λ / 4 plate having flat wavelength dispersion characteristics at a predetermined axial angle, it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, and as a result, it is possible to realize very excellent antireflection characteristics.

[0185] The first retardation film 33 may be made of any suitable resin film that can satisfy the above-mentioned characteristics. Examples of such resins include cyclic olefin resins, polycarbonate resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, and acrylic resins. A cyclic olefin resin may be suitably used for the first retardation film 33. The first retardation film 33 may be obtained, for example, by appropriately stretching a film formed from the above-mentioned resin.

[0186] (Second phase difference film) When the film C34 functions as a retardation film, the second retardation film 34 may be composed of a retardation film having any suitable optical properties and / or mechanical properties depending on the purpose. The second retardation film 34 is composed of, for example, a single layer. The second retardation film 34 is located on the opposite side to the viewing side of the first retardation film 33. The second retardation film 34 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, the second retardation film 34 is provided at a position closer to the second adhesive sheet 4 than the polarizer 32. The second retardation film 34 is preferably disposed between the first retardation film 33 and the second adhesive sheet 4.

[0187] The thickness of the second retardation film 34 is preferably 5 μm to 50 μm, and more preferably 5 μm to 40 μm.

[0188] The in-plane retardation Re(550) of the second retardation film 34 is preferably 10 nm to 60 nm, more preferably 20 nm to 50 nm, and further preferably 30 nm to 40 nm.

[0189] The refractive index characteristics of the second retardation film 34 preferably exhibit the relationship nz>nx>ny. The Nz coefficient of the second retardation film 34 is preferably -10 to -0.1, and more preferably -5 to -1.

[0190] The second retardation film 34 can be preferably disposed so that its slow axis is substantially perpendicular to the absorption axis of the polarizer.

[0191] The second retardation film 34 may be composed of any appropriate resin film that can satisfy the above-mentioned characteristics. An example of such a resin may be a polymer having negative intrinsic birefringence. A polymer having negative intrinsic birefringence is a polymer in which the refractive index in the orientation direction becomes relatively small when the polymer is oriented by stretching or the like. Examples of polymers having negative intrinsic birefringence include those in which chemical bonds and functional groups with large polarization anisotropy, such as aromatic and carbonyl groups, are introduced into the side chains of the polymer. Specific examples of polymers having negative intrinsic birefringence include modified polyolefin resins (e.g., modified polyethylene resins), acrylic resins, styrene resins, maleimide resins, fumaric acid ester resins, and the like. The second retardation film may be obtained, for example, by appropriately stretching a film formed from the above-mentioned resin.

[0192] The optical laminate 10A may include at least one selected from the group consisting of a first retardation film and a second retardation film as the second optical film 3, and the optical laminate 10A may not include the first retardation film and / or the second retardation film.

[0193] FIG. 4B is a cross-sectional view showing a schematic diagram of another example of the second optical film. As shown in FIG. 4B, the second optical film 3B is formed by laminating a film A31, a polarizer 32, and a film D35 in this order. The film A31 may be a protective film for the polarizer. The film D35 may be a retardation film or a protective film for the polarizer. When the film D35 is a protective film for the polarizer, the films A31 and D35 may be the same type of protective film or different types of protective films. The film A may be a film having a function other than the above. For example, the film A may have a function as a retardation film.

[0194] The photoelastic coefficient of the film D35 disposed between the polarizer 32 and the second adhesive sheet 4 is 4×10 -11 m 2The photoelastic coefficient is preferably 2×10 -11 m 2 / N or less, more preferably 1×10 -11 m 2 / N or less, and more preferably 5×10 -12 m 2 / N or less. The lower limit of the photoelastic coefficient is not particularly limited, but is, for example, 2×10 -13 m 2 / N or more, preferably 5 × 10 -13 m 2 / N or more, more preferably 1×10 -12 m 2 / N or more. At least one retardation film may be disposed between the polarizer 32 and the second adhesive sheet 4.

[0195] The following describes an embodiment in which the film D35 functions as a protective film for a polarizer.

[0196] 4B, the second optical film 3B includes a polarizer 32. In addition, the second optical film 3B has a configuration in which a protective film 35 is disposed between the polarizer 32 and the second adhesive sheet 4. That is, in the second optical film 3B, the protective film 35 is provided at a position closer to the second adhesive sheet 4 than the polarizer 32 is.

[0197] The photoelastic coefficient of the protective film 35 is, for example, as described above. By appropriately adjusting the photoelastic coefficient of the protective film 35, it is possible to obtain the optical laminate 10A that is more suitable for suppressing display defects even when a small object collides with or presses the screen with a small contact area.

[0198] (optical laminate) The thickness T of the optical laminate 10A is, for example, 200 μm or more. The thickness of the optical laminate 10A is preferably 250 μm or more, more preferably 500 μm or more, even more preferably 1000 μm or more, and particularly preferably 1500 μm or more. The upper limit of the thickness of the optical laminate 10A is, for example, 5000 μm or less, preferably 3000 μm or less, more preferably 2000 μm or less, and even more preferably 1000 μm or less.

[0199] The optical laminate 10A may not include a cover glass on the surface opposite to the side on which the first adhesive sheet 2 is formed of the first optical film 1. Even in this configuration, since the optical laminate 10A includes the first adhesive sheet 2, in an image display device including the optical laminate 10A, even if a small object collides with or presses the screen with a small contact area, display defects of the image display device can be further suppressed.

[0200] Fig. 5 is a cross-sectional view showing a schematic diagram of another example of the optical laminate. As shown in Fig. 5, the optical laminate 10B is a laminate including the optical laminate 10A, a third optical film 5, and a third adhesive sheet 6. In detail, the optical laminate 10B has a laminated structure in which a first optical film 1, a first adhesive sheet 2, a second optical film 3, a second adhesive sheet 4, a third optical film 5, and a third adhesive sheet 6 are laminated in this order. The optical laminate 10B can be used by being attached to an image forming layer via the third adhesive sheet 6, for example.

[0201] The thickness of the optical laminate 10B is, for example, 200 μm or more. The thickness of the optical laminate 10B is preferably 250 μm or more, and more preferably 300 μm or more. The upper limit of the thickness of the optical laminate 10B is, for example, 6000 μm or less, preferably 5000 μm or less, more preferably 3000 μm or less, even more preferably 2000 μm or less, and particularly preferably 1000 μm or less.

[0202] (Third adhesive sheet) The third adhesive sheet 6 is formed on the third optical film 5. The third adhesive sheet 6 is formed on one main surface of the third optical film 5. In FIG. 5, the third adhesive sheet 6 is formed on the entire one main surface of the third optical film 5. However, the third adhesive sheet 6 may be formed on only a portion of the one main surface of the third optical film 5.

[0203] Thickness T of the third adhesive sheet 6 3 is, for example, 5 μm or more and 100 μm or less, preferably 8 μm or more and 80 μm or less, more preferably 10 μm or more and 50 μm or less, and further preferably 12 μm or more and 30 μm or less. By appropriately adjusting the thickness of the third pressure-sensitive adhesive sheet 6, the adhesion between the third optical film 5 and the third pressure-sensitive adhesive sheet 6 can be improved.

[0204] A known adhesive can be used for the third adhesive sheet 6. The third adhesive sheet 6 may be an adhesive sheet formed from a photocurable adhesive composition (I) or a solvent-based adhesive composition (II). The first adhesive sheet 2 or the second adhesive sheet 4 may be used for the third adhesive sheet 6.

[0205] (Third Optical Film) 5, the third optical film 5 has two main surfaces facing each other. One main surface faces the second adhesive sheet 4, and is the surface of the third optical film 5 on which the second adhesive sheet 4 is laminated. The other main surface of the third optical film 5 faces the third adhesive sheet 6, and is the surface of the third optical film 5 on which the third adhesive sheet 6 is laminated.

[0206] The third optical film 5 includes, for example, at least one selected from the group consisting of a polarizing film and a retardation film. The third optical film 5 may be a laminated film including a polarizing film and / or a retardation film.

[0207] [Embodiment of image display device] An example of the image display device of this embodiment is shown in Fig. 6. The image display device 11 of Fig. 6 has a laminated structure in which an optical laminate 10A, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 7, and a substrate 8 are laminated in this order. That is, the image display device 11 of Fig. 6 has a laminated structure in which a first optical film 1, a first adhesive sheet 2, a second optical film 3, a second adhesive sheet 4, an image forming layer 7, and a substrate 8 are laminated in this order. The image display device 11 may have the optical laminate 10B of Fig. 5 instead of the optical laminate 10A. The image forming layer 7 and the substrate 8 may have the same configurations as the image forming layer and the substrate provided in a known image display device, respectively.

[0208] The image display device 11 in Fig. 6 may be an organic EL display or a liquid crystal display. However, the image display device 11 is not limited to this example. The image display device 11 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 11 can be used for home appliances, in-vehicle applications, public information displays (PID), and the like.

[0209] The image display device of this embodiment may have any configuration as long as it includes the optical laminate of this embodiment. EXAMPLES

[0210] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0211] FIG. 7 is a cross-sectional view that shows a schematic diagram of the optical laminate according to Examples 1 to 4, 6, and Comparative Examples 1 to 4. As shown in FIG. 7, the optical laminate 40 according to Examples 1 to 4, 6, and Comparative Examples 1 to 4 is a laminate in which a first optical film 1, a first adhesive sheet 2, a second optical film 3A, and a second adhesive sheet 4 are laminated in this order. The second optical film 3A had a structure in which a protective film 31, a polarizer 32, a first retardation film 33, and a second retardation film 34 were laminated in this order. The first retardation film 33 and the second retardation film 34 were disposed between the polarizer 32 and the second adhesive sheet 4. That is, the first retardation film 33 and the second retardation film 34 were provided at a position closer to the second adhesive sheet 4 than the polarizer 32.

[0212] 8 is a cross-sectional view that shows a schematic diagram of an optical laminate according to Example 5. As shown in FIG. 8, an optical laminate 41 according to Example 5 is a laminate in which a first optical film 1, a first adhesive sheet 2, a second optical film 3B, and a second adhesive sheet 4 are laminated in this order. The second optical film 3B had a structure in which a protective film 31, a polarizer 32, and a protective film 35 were laminated in this order. The protective film 35 was disposed between the polarizer 32 and the second adhesive sheet 4. That is, the protective film 35 was provided at a position closer to the second adhesive sheet 4 than the polarizer 32.

[0213] For convenience, the following description will be given based on the reference symbols given in FIG. 7 and FIG.

[0214] [Evaluation method] <Breaking elongation> In Examples 1 to 5 and Comparative Examples 1 to 4, a laminate LX consisting of a release liner A, a first adhesive sheet 2 (thickness 20 μm), and a release liner B was prepared by the same preparation method as the laminate L1b described later, except that the thickness of the first adhesive sheet 2 was set to 20 μm. This laminate LX was cut into a size of 3 cm wide x 10 cm long, and the release liner B was peeled off to prepare a test sample. In Example 6, a laminate LY in which a first adhesive sheet 2 (thickness 20 μm) was formed on the surface of a PET film was prepared by the same preparation method as the laminate L6 described later, except that the thickness of the first adhesive sheet 2 was set to 20 μm. This laminate LY was cut into a size of 3 cm wide x 10 cm long to prepare a test sample. In each test sample, the first adhesive sheet 2 was rolled into a string-like shape in the length direction on the release liner to prepare a test piece. The release liner was peeled off from this test piece, and the string-like first adhesive sheet 2 was set in a tensile tester, and a tensile test was performed under conditions of an initial chuck distance of 10 mm and a tensile speed of 300 mm / min. The length of the test piece when it broke in the tensile test was measured and L 1 The breaking elongation was calculated by the following formula: Breaking elongation [%] = {(L 1 -L 0 ) / L 0}×100

[0215] In the above formula, L 0 [mm] indicates the initial length of the test piece in the longitudinal direction (before the tensile test). The tensile tester used was the Shimadzu Autograph AG-10G. The tensile test was performed by pulling the test piece in the longitudinal direction.

[0216] The breaking elongation of the second adhesive sheet 4 was calculated by the same method as above, except that the laminate L2a was used.

[0217] <Penetration test> The optical laminates 40 and 41 according to the examples and comparative examples were cut into a size of 5 cm x 5 cm to prepare test samples. Next, the test samples were attached to a glass plate having a thickness of 1.2 mm via a second adhesive sheet 4 to prepare measurement samples.

[0218] The measurement samples according to the examples and comparative examples were placed on the stage of an indenter CMS tester (manufactured by Instron, product name: 5581) equipped with a piercing jig. The piercing jig had a rounded and sharp tip. In addition, the radius of curvature R of the tip of the piercing jig was 550 μm. The piercing jig was pierced into the test sample on the stage with a load of 5 kg in a room temperature (23° C.±3° C.) environment. The optical laminates 40 and 41 after the piercing test were arranged so that the polarizers 32 of the optical laminates 40 and 41 and the polarizer attached to the microscope were in a crossed Nicol state. The light leakage at this time was observed with a microscope (magnification of the objective lens: 5 times). Evaluation was made according to the following criteria. A: No light leakage is observed. B: Light leakage is observed, but has no practical effect. C: Light leakage is significant and practically unacceptable.

[0219] <Photoelastic coefficient> In the second optical films 3A and 3B used in the examples and comparative examples, the film (layer) disposed between the polarizer 32 and the second adhesive sheet 4 was cut into a size of 20 mm × 100 mm to prepare a sample. The sample was measured with an ellipsometer (manufactured by JASCO Corporation, M-150) using light with a wavelength of 550 nm to measure the photoelastic coefficient.

[0220] <Smoothness> Evaluation samples were prepared by attaching the optical laminates 40 and 41 according to the examples and comparative examples to a black plate via a second adhesive sheet 4. The smoothness of the evaluation samples was visually confirmed from the first optical film 1 side of the evaluation samples, and evaluated according to the following criteria. A: There was an inconspicuous unevenness. B: The unevenness was extremely noticeable.

[0221] <Weight average molecular weight of (meth)acrylic polymer> The weight average molecular weight (Mw) of the (meth)acrylic polymer was measured by GPC (gel permeation chromatography). Analytical equipment: Tosoh HLC-8120GPC Column: Tosoh G7000H XL +GMH XL +GMH XL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene

[0222] [First Optical Film 1 (Polarizing Film)] As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment.

[0223] A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water.

[0224] The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate.

[0225] The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment).

[0226] Next, the laminate after the auxiliary air-stretching treatment was immersed for 30 seconds in an insolubilizing bath having a liquid temperature of 40° C. (insolubilizing treatment). The insolubilizing bath was an aqueous boric acid solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water.

[0227] Next, the film was immersed in a dye bath at a liquid temperature of 30° C. for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizer would be the desired value (dyeing treatment). The dye bath was an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water.

[0228] Next, the piece was immersed in a crosslinking bath at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). The crosslinking bath was an aqueous boric acid solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water.

[0229] Thereafter, the laminate was uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times while being immersed in an aqueous boric acid solution at a liquid temperature of 70° C. (underwater stretching treatment). The aqueous boric acid solution contained 4% by weight of boric acid and 5% by weight of potassium iodide.

[0230] Thereafter, the laminate was immersed in a cleaning bath at a liquid temperature of 20° C. (cleaning treatment) The cleaning bath was an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water.

[0231] Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment).

[0232] In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate.

[0233] An acrylic resin film (thickness: 40 μm) having a glutarimide structure as a protective layer was attached to the surface of the obtained polarizer (the surface opposite to the resin substrate) via an ultraviolet-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was about 2.0 μm, and the layers were attached using a rolling machine. Thereafter, the adhesive was cured by irradiating it with UV light from the acrylic resin film side. Next, the resin substrate was peeled off to obtain a polarizing film (first optical film 1) having a configuration of acrylic resin film (protective layer) / polarizer.

[0234] [Second optical film] In Examples 1 to 4 and 6 and Comparative Examples 1 to 4 (see FIG. 7), a laminate X having a configuration in which a protective film 31, a polarizer 32, a first retardation film 33, and a second retardation film 34 were laminated in this order was used as the second optical film 3A. The polarizer prepared above was used as the polarizer 32. The protective film 31 was an acrylic resin film having a glutarimide structure (manufactured by Kaneka Corporation, product name: HTX) (thickness: 40 μm). The protective film 31 and the polarizer 32 were bonded together via an ultraviolet-curing adhesive.

[0235] A cyclic olefin film (manufactured by Zeon Corporation, product name: Zeonorfilm ZT12-50135) was used as the first retardation film 33. The thickness of the first retardation film 33 was 18 μm.

[0236] The second retardation film 34 was prepared as follows.

[0237] [Synthesis of polymer and preparation of dope] In an autoclave equipped with a stirrer, a cooling tube, a nitrogen inlet tube and a thermometer, 48 parts by weight of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical, trade name Metolose 60SH-50), 15601 parts by weight of distilled water, 8161 parts by weight of diisopropyl fumarate, 240 parts by weight of 3-ethyl-3-oxetanylmethyl acrylate and 45 parts by weight of t-butyl peroxypivalate as a polymerization initiator were placed, and after nitrogen bubbling for 1 hour, the mixture was stirred and held at 49°C for 24 hours to carry out radical suspension polymerization. The mixture was then cooled to room temperature, and the suspension containing the produced polymer particles was centrifuged. The obtained polymer was washed twice with distilled water and twice with methanol, and then dried under reduced pressure to obtain a white fumarate ester resin.

[0238] The obtained fumaric acid ester-based resin was dissolved in methyl ethyl ketone to obtain a solution with a solid content concentration of 20% by weight. Furthermore, 5 parts by weight of tributyl trimellitate as a plasticizer was added to 100 parts by weight of the fumaric acid ester-based resin to prepare a dope.

[0239] A polyester film (polyethylene terephthalate / isophthalate copolymer biaxially stretched film) with a thickness of 75 μm was used as the support film. The above dope was applied to a film thickness of about 6 μm after drying and dried to obtain a laminate A in which a coating film of a fumaric acid ester resin was tightly laminated on the support.

[0240] The laminate A was uniaxially stretched at its free end to obtain a laminate B in which a second retardation film 34 (positive B plate) having a refractive index anisotropy of nz>nx>ny was laminated in close contact with the support. The support was peeled off from the laminate B to obtain a second retardation film 34 (positive B plate) having a refractive index anisotropy. The first retardation film 33 and the second retardation film 34 were bonded together via an ultraviolet-curing adhesive.

[0241] The photoelastic coefficient of the protective film 31 is 3×10 -12 m 2 The photoelastic coefficient of the first retardation film 33 was 1×10-12 m 2 The photoelastic coefficient of the second retardation film 34 was 5×10 -11 m 2 / N.

[0242] In Example 5 (see FIG. 8), a laminate Y having a configuration in which a protective film 31, a polarizer 32, and a protective film 35 were laminated in this order was used as the second optical film 3B. The polarizer 32 used was the polarizer 32 prepared above. The protective films 31 and 35 used were acrylic resin films having a glutarimide structure (manufactured by Kaneka Corporation, product name: HTX) (thickness: 40 μm).

[0243] [Release Liner A] Addition reaction curing type silicone (LTC761 containing hexenyl group-containing polyorganosiloxane, 30 wt% toluene solution, manufactured by Dow Corning Toray) 30 parts by weight, release control agent (BY24-850 containing unreactive silicone resin, manufactured by Dow Corning Toray) 0.9 parts by weight, and curing catalyst (SRX212 containing platinum catalyst, manufactured by Dow Corning Toray) 2 parts by weight, and toluene / hexane mixed solvent (volume ratio 1: 1) as a dilution solvent were mixed to obtain a silicone-based release agent composition. The concentration of silicone solids in the release agent composition was 1.0 wt%. Next, the release agent composition was applied to one side of a liner substrate (Lumirror XD500P, a polyester film, thickness 75 μm) with a wire bar and heated at 130 ° C for 1 minute to prepare a release liner A having a release layer (thickness 60 nm) on one side.

[0244] [Release Liner B] Release liner B having a release layer (thickness 120 nm) on one side was prepared in the same manner as release liner A, except that the thickness of the release agent composition applied to the liner substrate was changed.

[0245] [Monomer Syrup A1] 100 parts by weight of n-butyl acrylate (BA), 5 parts by weight of acrylic acid (AA), 0.16 parts by weight of 1-hydroxycyclohexyl-phenyl ketone (Omnirad184, manufactured by IGM Resins BV) as a photopolymerization initiator, and 0.04 parts by weight of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819, manufactured by IGM Resins BV) were placed in a four-bottom flask and irradiated with ultraviolet light under a nitrogen atmosphere to obtain a partially photopolymerized monomer syrup A1. The ultraviolet light irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa·s.

[0246] [Table 1]

[0247] The abbreviations in Table 1 are as follows. BA: n-butyl acrylate AA: Acrylic acid

[0248] [Photocurable adhesive compositions C1 to C6] Next, photocurable pressure-sensitive adhesive compositions C1 to C3 were obtained by mixing the monomer syrup and the crosslinking agent so as to obtain the compositions shown in the following Table 2. The abbreviation "NDDA" in Table 2 stands for 1,9-nonanediol diacrylate.

[0249] [Table 2]

[0250] Example 1 Please refer to FIG. 7. A photocurable pressure-sensitive adhesive composition C1 was applied to the release layer surface of release liner A with an applicator to form a coating layer (thickness: 50 μm). Next, the above-mentioned release liner B was placed on the formed coating layer to obtain laminate L1a. Release liner B was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 9 mW / cm was applied from the side of release liner A in laminate L1a.2 Conditions (accumulated light amount 868mJcm 2 ) was used. This caused the coating layer to photocure, forming a laminate L1b composed of release liner A, first adhesive sheet 2 (thickness 50 μm), and release liner B. The light source used was a combination of a black light source and an LED. The peak wavelength of the irradiated light from the LED was 340 nm. The accumulated light amount was the sum of the accumulated light amounts from both light sources.

[0251] Next, the release liner B was peeled off from the laminate L1b, and the above-mentioned polarizing film (first optical film 1) was placed on the exposed surface of the first adhesive sheet 2, thereby obtaining a laminate L1c in which the release liner A, the first adhesive sheet 2, and the polarizing film were laminated in this order. Note that the polarizing film was placed so that the surface on the transparent protective film side made of a modified acrylic polymer was in contact with the first adhesive sheet 2.

[0252] Separately, a photocurable pressure-sensitive adhesive composition C3 was applied to the surface of the release layer of the release liner A with an applicator to form a coating layer (thickness 15 μm). Next, the above-mentioned release liner B was placed on the formed coating layer to obtain a laminate L2a. The release liner B was placed so that the release layer was in contact with the coating layer. Next, light was irradiated from the release liner A side of the laminate L2a. As a result, the coating layer was photocured, and a laminate L2b composed of the release liner A, the second pressure-sensitive adhesive sheet 4 (thickness 15 μm), and the release liner B was formed. The light irradiation conditions were the same as those when the first pressure-sensitive adhesive sheet 2 was produced.

[0253] Next, the release liner B was peeled off from the laminate L2b, and the laminate X described above as the second optical film 3A was placed on the exposed surface of the second adhesive sheet 4 so that the second retardation film 34 was in contact with the second adhesive sheet 4, thereby obtaining a laminate L2c in which the release liner A, the second adhesive sheet 4, and the second optical film 3A were laminated in this order. Note that the laminate X was placed so that the second retardation film 34 was in contact with the second adhesive sheet 4.

[0254] The release liner A was peeled off from the laminate L1c to obtain a laminate L1d. The first adhesive sheet 2 of the laminate L1d was transferred to the protective film 31 of the laminate L2c to obtain a laminate L3 in which a polarizing film (first optical film 1), a first adhesive sheet 2, a second optical film 3A, a second adhesive sheet 4, and a release liner A were laminated in this order. The release liner A was peeled off from the laminate L3 to obtain the optical laminate 40 according to Example 1.

[0255] Example 2 An optical laminate 40 according to Example 2 was obtained in the same manner as in Example 1, except that the thickness of the first adhesive sheet 2 was changed to 100 μm.

[0256] Example 3 An optical laminate 40 according to Example 3 was obtained in the same manner as in Example 1, except that the photocurable pressure-sensitive adhesive composition C2 was used instead of the photocurable pressure-sensitive adhesive composition C1.

[0257] Example 4 An optical laminate 40 according to Example 4 was obtained in the same manner as in Example 3, except that the thickness of the first adhesive sheet 2 was changed to 100 μm.

[0258] Example 5 See Fig. 8. An optical laminate 41 according to Example 5 was obtained in the same manner as in Example 4, except that laminate Y was used instead of laminate X as the second optical film.

[0259] Example 6 [Preparation of (meth)acrylic polymer B1] A monomer mixture containing 79.9 parts by weight of n-butyl acrylate (BA), 5 parts by weight of acrylic acid (AA), 0.1 parts by weight of 4-hydroxybutyl acrylate (HBA), and 15 parts by weight of benzyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN; manufactured by Kishida Chemical Co., Ltd.) was charged as a polymerization initiator together with ethyl acetate with respect to 100 parts by weight of the monomer mixture to prepare a mixture. While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at about 55°C and a polymerization reaction was carried out for 7 hours. Thereafter, ethyl acetate was added to the obtained reaction liquid to adjust the solid concentration to 30%, and a solution of (meth)acrylic polymer B1 having a weight average molecular weight (Mw) of 2.2 million was prepared.

[0260] [Adhesive sheet] A solution of the (meth)acrylic adhesive composition D1 (solvent-based adhesive composition) of Example 6 was prepared by further blending 12 parts by weight of a crosslinker (manufactured by Mitsui Chemicals, Inc., product name: Takenate D-101E), 0.1 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403), and 1 part by weight of a polyether compound having an alkoxysilyl group (manufactured by Kaneka Corporation, product name: Silyl SAT10) with respect to 100 parts by weight of the solid content of the solution of the (meth)acrylic polymer B1. Takenate D-101E is a trimethylolpropane / tolylene diisocyanate trimer adduct. KBM-403 is 3-glycidoxypropyltrimethoxysilane.

[0261] A (meth)acrylic adhesive composition D1 was applied to the surface of a PET film, which was a base film (release liner), so that the adhesive sheet had a thickness of 100 μm after drying. A fountain coater was used to apply the (meth)acrylic adhesive composition D1. The coating film formed by application was dried in an air-circulating thermostatic oven at 90° C. for 1 minute to obtain a laminate L6 in which a first adhesive sheet 2 was formed on the surface of the PET film. The adhesive sheet had a thickness of 100 μm.

[0262] [Optical laminate] 7, the first adhesive sheet 2 of the obtained laminate L6 was transferred to the above-mentioned polarizing film (first optical film 1), thereby producing a laminate L7 in which the polarizing film (first optical film 1), the first adhesive sheet 2, and the base film were laminated in this order.

[0263] The base film was peeled off from the laminate L7 and the exposed surface of the first adhesive sheet 2 was transferred to the protective film 31 of the above-mentioned laminate L2c to obtain a laminate L8 in which a polarizing film (first optical film 1), a first adhesive sheet 2, a second optical film 3A, a second adhesive sheet 4, and a release liner A were laminated in this order.

[0264] The release liner A was peeled off from the laminate L8 to obtain the optical laminate 40 of Example 6.

[0265] Comparative Example 1 The optical laminate 40 of Comparative Example 1 was obtained by the same method as in Example 1, except that the photocurable adhesive composition C3 was used instead of the photocurable adhesive composition C1, and the thickness of the first adhesive sheet 2 was changed to 12 μm.

[0266] Comparative Example 2 An optical laminate 40 according to Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the thickness of the first adhesive sheet 2 was changed to 50 μm.

[0267] Comparative Example 3 An optical laminate 40 according to Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that the thickness of the first adhesive sheet 2 was changed to 100 μm.

[0268] Comparative Example 4 An optical laminate 40 according to Comparative Example 4 was obtained in the same manner as in Example 3, except that the thickness of the first adhesive sheet 2 was changed to 12 μm.

[0269] [Table 3]

[0270] [Table 4]

[0271] [Table 5]

[0272] As shown in Table 3, the results of the piercing test were good in each example. The optical layered bodies according to the examples are suitable for suppressing display defects. [Industrial Applicability]

[0273] The optical layered body of the present invention can be used, for example, in an image display device. [Explanation of symbols]

[0274] 1 Daiichi Optical Film 2 First adhesive sheet 3. Secondary Optical Film 4 Second adhesive sheet 5. Third Optical Film 6 Third adhesive sheet 7 Image forming layer 8 Substrate 10A, 10B Optical laminate 11 Image display devices 14 light 15 First laminate 16 Second laminate 21 Base sheet 22 Coating layer 23 Release Liner 30 Polarizing plate 31 Film A (protective film) 32 Polarizer 33 Film B (first phase difference film) 34 Film C (second phase difference film) 35 Film D (protective film) 40, 41 Optical multilayers

Claims

1. An optical laminate in which a first optical film, a first adhesive sheet, a second optical film, and a second adhesive sheet are laminated in this order, The thickness T of the first adhesive sheet 1 is 30 μm or more and 1000 μm or less, and the breaking elongation of the first adhesive sheet is 500% or less.

2. The optical laminate according to claim 1 , wherein the first pressure-sensitive adhesive sheet is formed from a photocurable pressure-sensitive adhesive composition (I) containing a monomer group and / or a partial polymer of the monomer group.

3. 3. The optical laminate according to claim 2, wherein the photocurable pressure-sensitive adhesive composition (I) contains a crosslinking agent, and a blending amount of the crosslinking agent in the photocurable pressure-sensitive adhesive composition (I) is 0.4 parts by weight or more and 20 parts by weight or less per 100 parts by weight of the total of the monomer group and the partially polymerized product.

4. The optical laminate according to claim 1 , wherein the optical laminate has a thickness T of 200 μm or more.

5. the second optical film comprises a plurality of layers; The plurality of layers includes a polarizer and at least one film disposed between the polarizer and the second adhesive sheet, The photoelastic coefficient of the at least one film is 4×10 -11 m 2 The optical laminate according to claim 1, wherein the optical density is 1 / N or less.

6. An image display device comprising the optical laminate according to claim 1.

Citation Information

Patent Citations

  • Roll of optical sheet material and continuous manufacturing method of liquid crystal display device

    WO2011001834A1

  • Layered body for flexible image display device, and flexible image display device

    WO2019026753A1

  • Adhesive sheet used for laminate within flexible image display device, laminate used for flexible image display device, and flexible image display device

    WO2021187278A1

  • Adhesive sheet used in layered product in flexible image display device, layered product used in flexible image display device, and flexible image display device

    WO2021256331A1

  • Adhesive composition, adhesive sheet, optical laminate, and image display device

    WO2022244557A1

Cited By

  • Adhesive sheet, optical laminate, and image display device

    WO2026004727A1