Thermoelectric conversion module

By using thermally conductive interface members with specified thermal resistance ratios and shear stress conditions, the thermoelectric conversion module achieves enhanced thermoelectric performance and reliability.

JP2024146619APending Publication Date: 2024-10-15LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023059639
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing thermoelectric conversion modules lack improvements in thermoelectric performance, reliability, and mass productivity, with insufficient study on the relationship between resistance values, thermal resistance values, and the effects of insulating layers on interface shear stress and adhesive strength.

Method used

Incorporating thermally conductive interface members with adhesive properties on both surfaces of the thermoelectric conversion elements, with specific thermal resistance ratios and shear stress conditions to enhance heat conductivity at the interfaces.

Benefits of technology

The solution results in a thermoelectric conversion module with improved thermoelectric performance and heat conductivity, maintaining reliability and mass productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146619000001_ABST
    Figure 2024146619000001_ABST
Patent Text Reader

Abstract

To provide a thermoelectric conversion module having a high thermal electric performance in which a heat transmission effect of an interface between members is improved.SOLUTION: In a thermoelectric conversion module including a heat transfer conductive interface member B that includes a heat transfer conductive interface A having an adhesive property on one surface of a thermal conversion element, and a heat member in this order, and includes an adhesive property on the other surface. When a whole thermal resistance value that is a sum of a thermal resistance value of the heat transfer conductive interface A and a thermal resistance value of the heat transfer conductive interface member B is RAB, and a whole thermal resistance value of the thermoelectric conversion module is RM, RAB / RM is 1.40 or less, and a shearing stress τA applied to the heat transfer conductive interface A in the case where the heat transfer conductive interface A is adhered to one surface of the thermal conversion element, and a shearing stress τB applied to the heat transfer conductive interface member B in the case where the heat transfer conductive interface member B is adhered to the other surface is 0.001(N / mm2) or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric conversion module. [Background technology]

[0002] 2. Description of the Related Art Conventionally, as one of the means for effectively utilizing energy, there has been a device that directly converts thermal energy into electrical energy and vice versa using a thermoelectric conversion module having a thermoelectric effect such as the Seebeck effect or the Peltier effect. As a thermoelectric conversion module, a configuration of a so-called π-type thermoelectric conversion element is known. The π-type thermoelectric conversion element is configured by providing a pair of electrodes spaced apart from each other on a substrate, for example, providing a P-type thermoelectric element on one electrode and an N-type thermoelectric element on the other electrode, also spaced apart from each other, and connecting the upper surfaces of both thermoelectric elements to a common electrode on the opposing substrate. Also, a configuration of a so-called in-plane type thermoelectric conversion element is known. From the viewpoint of thermoelectric performance, the in-plane type thermoelectric conversion element is usually configured by alternately providing P-type thermoelectric elements and N-type thermoelectric elements in the in-plane direction of the substrate, and for example, by connecting the upper or lower parts of adjacent or abutting P-type thermoelectric elements and N-type thermoelectric elements in series via electrodes. In this situation, various demands remain for thermoelectric conversion modules, such as further improvement in thermoelectric performance, thinning, improved reliability, and improved mass productivity. In Patent Document 1, for example, in the configuration of an in-plane type thermoelectric conversion module, an insulating layer is provided between a thermoelectric element layer and a heat dissipation layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 179544 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in Patent Document 1, the insulating layer is used for the purpose of preventing short circuits between the heat source and the thermoelectric element layer, or between the heat dissipation layer and the thermoelectric element layer, etc., from the viewpoint of improving the reliability of the in-plane thermoelectric conversion module. Therefore, from the viewpoint of improving the thermoelectric performance, the arrangement of another specific insulating layer on the in-plane thermoelectric conversion module or the π-type thermoelectric conversion module, and the relationship between the thermal resistance value of the other specific insulating layer and the thermal resistance value of the members constituting the in-plane thermoelectric conversion module or the π-type thermoelectric conversion module are not considered. In addition, the effects and the like derived from the shear stress and adhesive strength of the other specific insulating layer are not considered.

[0005] In view of the above, an object of the present invention is to provide a thermoelectric conversion module having high thermoelectric performance with improved heat conductivity at the interfaces between members. [Means for solving the problem]

[0006] As a result of extensive research into solving the above-mentioned problems, the inventors have discovered that the thermal conductivity of the interfaces between the components constituting a thermoelectric conversion module can be further improved by providing an adhesive thermally conductive interface member (hereinafter sometimes simply referred to as "TIM") on the upper and lower surfaces of a thermoelectric conversion element, setting the ratio of the total thermal resistance value of the adhesive thermally conductive interface member to the total thermal resistance value of the thermoelectric conversion module within a specific value range, and setting the shear stress applied to the adhesive thermally conductive interface member within a specific value range, thereby completing the present invention. That is, the present invention provides the following [1]. [1] A thermoelectric conversion module including a thermally conductive interface member A having adhesive properties on one surface of a thermoelectric conversion element and a heat dissipation member, in that order, and a thermally conductive interface member B having adhesive properties on the other surface of the thermoelectric conversion element, The thermal resistance value of the thermally conductive interface member A is R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is RAB (mK / W), and the total thermal resistance of the thermoelectric conversion module is R M (mK / W), the above R M R AB Ratio (R AB / R M ) is less than or equal to 1.40, and The shear stress τ applied to the thermally conductive interface member A when the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element A (N / mm 2 ) and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B (N / mm 2 ) and 0.001 (N / mm 2 ) or more. Effect of the Invention

[0007] According to the present invention, it is possible to provide a thermoelectric conversion module having high thermoelectric performance with improved heat conductivity at the interface between members. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view showing an embodiment of a thermoelectric conversion module of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of an evaluation configuration of a thermoelectric conversion module used in an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Thermoelectric conversion module] The thermoelectric conversion module of the present invention includes a thermally conductive interface member A having adhesive properties on one surface of a thermoelectric conversion element, and a heat dissipation member, in this order, and also includes a thermally conductive interface member B having adhesive properties on the other surface of the thermoelectric conversion element, The thermal resistance value of the thermally conductive interface member A is RA (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the thermoelectric conversion module is R M (mK / W), the above R M R AB Ratio (R AB / R M ) is less than or equal to 1.40, and The shear stress τ applied to the thermally conductive interface member A when the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element A (N / mm 2 ) and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B (N / mm 2 ) and 0.001 (N / mm 2 ) or more. The thermoelectric conversion module of the present invention includes a thermally conductive interface member A (hereinafter, sometimes simply referred to as "TIMA") having adhesive properties on one side of a thermoelectric conversion element, a heat dissipation member, and further includes a thermally conductive interface member B (hereinafter, sometimes simply referred to as "TIMB") having adhesive properties on the other side of the thermoelectric conversion module. In this configuration, the shear stress τ A and TIMB shear stress τ B , respectively, 0.001 (N / mm 2 ) or more, and the total thermal resistance value R M Total thermal resistance value R of the thermally conductive interface material AB By setting the ratio to 1.40 or less, it is possible to improve the heat transfer at the interface between the members constituting the thermoelectric conversion module, resulting in higher thermoelectric performance.

[0010] In this specification, the components of a "thermoelectric conversion module" include a "thermoelectric conversion element", an "adhesive thermally conductive interface member A and an adhesive thermally conductive interface member B", and a "heat dissipation member".

[0011] In this specification, preferred definitions may be selected arbitrarily, and combinations of preferred definitions may be considered more preferred. In this specification, the expression "XX to YY" means "at least XX and at most YY." In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., the range of the content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."

[0012] Hereinafter, the thermoelectric conversion module of the present invention will be described with reference to the drawings.

[0013] 1 is a cross-sectional view showing an embodiment of a thermoelectric conversion module of the present invention. The thermoelectric conversion module 1 includes a thermally conductive interface member A10a having adhesiveness on one surface of a thermoelectric conversion element 9, a heat dissipation member 11, and further includes a thermally conductive interface member B10b having adhesiveness on the other surface of the thermoelectric conversion element 9. The thermoelectric conversion element 9 includes a chip 4 of a P-type thermoelectric conversion material and a chip 5 of an N-type thermoelectric conversion material, which are alternately arranged in series in the in-plane direction of the first substrate 2a and the second substrate 2b via a common first electrode 3a and a common second electrode 3b. The chip 4 of the P-type thermoelectric conversion material and the chip 5 of the N-type thermoelectric conversion material are joined to the common first electrode 3a and the common second electrode 3b via a solder receiving layer 7 and a solder material layer 6, and further includes a heat dissipation layer A8a and a heat dissipation layer B8b on the first substrate 2a and the second substrate 2b, respectively, in this order. By providing an adhesive thermally conductive interface member A10a between the heat dissipation layer A8a, the outermost layer on one surface side of the thermoelectric conversion element 9, and the heat dissipation member 11, it is possible to reduce the contact thermal resistance generated therebetween. Similarly, by providing an adhesive thermally conductive interface member B10b between the heat dissipation layer B8b, the outermost layer on the other surface side of the thermoelectric conversion element 9, and, for example, a heat source (not shown), it is possible to reduce the contact thermal resistance generated therebetween. Using a thermally conductive interface member A having such an effect and a thermally conductive interface member B having an adhesive property, the shear stress τ A and shear stress τ applied to adhesive thermally conductive interface member B B , respectively, 0.001 (N / mm 2 ) or more, and further, the total thermal resistance value R M The total thermal resistance R of the thermally conductive interface material that has adhesive properties to AB By setting the ratio to 1.40 or less, it is possible to improve the heat transfer at the interface between the members constituting the thermoelectric conversion module, resulting in higher thermoelectric performance.

[0014] The shear stress τ acting on the thermally conductive interface material A when the thermally conductive interface material A is bonded to one side of the thermoelectric conversion element. A and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B are each independently 0.001 (N / mm 2 )That's all. Shear stress τ on thermally conductive interface member A A and shear stress τ on thermally conductive interface member B B are preferably 0.001 (N / mm 2 )~5.00(N / mm 2 ), and more preferably 0.01 (N / mm 2 )~3.00(N / mm 2), and more preferably 0.02 (N / mm 2 )~1.00(N / mm 2 ) The shear stress τ A and shear stress τ B When the temperature is within this range, the adhesion between the components constituting the thermoelectric conversion module is improved, and the P-type thermoelectric conversion material chip and the N-type thermoelectric conversion material chip are not physically damaged, making it easier to improve the thermoelectric performance.

[0015] The total thermal resistance R is the sum of the thermal resistances of the individual components that make up the thermoelectric conversion module. M The thermal resistance value R of TIMA A and the thermal resistance value R of TIMB B The total thermal resistance R AB Ratio of (R AB / R M ) is less than or equal to 1.40. Ratio(R AB / R M ) is preferably 0.01 to 1.00, more preferably 0.05 to 0.80, and further preferably 0.10 to 0.40. Ratio(R AB / R M When the ratio (R) is within this range, the heat transfer at the interface between the members is more easily improved, and the thermoelectric performance is improved.

[0016] <Thermal conductive interface member A and thermal conductive interface member B> The thermoelectric conversion module of the present invention includes a thermally conductive interface member A having adhesive properties on one surface of a thermoelectric conversion element, and a heat dissipation member, and further includes a thermally conductive interface member B having adhesive properties on the other surface of the thermoelectric conversion element. By providing an adhesive thermally conductive interface member A between one surface of the thermoelectric conversion element and the heat dissipation member, the contact thermal resistance occurring therebetween can be reduced. Similarly, by providing an adhesive thermally conductive interface member B between the other surface of the thermoelectric conversion element and, for example, a heat source, the contact thermal resistance occurring therebetween can be reduced. In this way, by using the adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B, the thermal conduction in the thermoelectric conversion element is easily improved, which can lead to an improvement in the thermoelectric performance of the thermoelectric conversion module.

[0017] The adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B are preferably pressure-sensitive adhesive layers. Hereinafter, "the adhesive thermally conductive interface member A and the adhesive thermally conductive interface member B" may be collectively referred to simply as "thermally conductive interface members".

[0018] The adhesive used in the adhesive layer is not particularly limited, and may be any of an acrylic adhesive, a silicone adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, etc. The adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be any of a crosslinked type or a non-crosslinked type. Among them, an acrylic adhesive or a silicone adhesive is preferred.

[0019] From the viewpoint of improving the thermal conductivity, the adhesive layer may be filled with a thermally conductive filler. The thermally conductive filler is not particularly limited, and may be, for example, at least one selected from carbon fiber, graphite, silica, alumina, magnesium oxide, silicon nitride, aluminum nitride, magnesium nitride, boron nitride, copper, and aluminum. These thermally conductive fillers may be used alone or in combination of two or more. The thermally conductive filler preferably has an average particle size of 0.01 to 200 μm. The average particle size may be measured, for example, by a Coulter counter method. The content of the thermally conductive filler is appropriately adjusted according to the desired thermal conductivity, and is preferably 40 to 99 mass % in the composition. When the content of the thermally conductive filler is within this range, the thermally conductive interface member has excellent heat dissipation properties, folding resistance, and flex resistance, and maintains its strength.

[0020] The thickness of the thermally conductive interface member is preferably 0.05 to 1.50 mm, more preferably 0.08 to 1.20 mm, and further preferably 0.10 to 1.00 mm. When the thickness of the thermally conductive interface member is within this range, the thermal resistance of the thermally conductive interface member can be kept low, and the contact thermal resistance generated between the heat source and the heat dissipation member can be efficiently reduced.

[0021] Examples of commercially available thermally conductive interface members include the following: Highly thermally conductive heat dissipation sheet (manufactured by Sekisui Polymatech, product number: Manion50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m·K)), heat dissipation sheet TIMLIGHT (manufactured by Sekisui Polymatech, product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m·K)), heat dissipation sheet TIMLIGHT (manufactured by Sekisui Polymatech, product number: PT-UT, thickness: 0.50 mm, thermal conductivity: 6.0 W / (m·K)), thermally conductive double-sided tape (manufactured by 3M, product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m·K)), thermally conductive double-sided tape (manufactured by 3M, product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m·K)).

[0022] <Heat dissipation materials> The heat dissipation member may be any member capable of conducting generated heat and dissipating it to the outside, and is not particularly limited, but examples thereof include a heat sink, a heat spreader, etc. Examples of materials for the heat sink and the heat spreader include copper, aluminum, etc. In addition to the heat spreader and the heat sink, examples of the heat dissipation member include a radiator, a cooler, a cooling fan, a heat pipe, a vapor chamber, a metal cover, a housing, etc. The heat pipe is, for example, a hollow structure having a cylindrical, approximately cylindrical, or flattened tubular shape.

[0023] <Heat dissipation layer> In the thermoelectric conversion element, from the viewpoint of efficiently applying a temperature difference to the chip of the thermoelectric conversion material, it is preferable to further provide a heat dissipation layer on at least one surface of the above-mentioned substrate. The material used for the heat dissipation layer is not particularly limited, and any known material can be used, but is preferably selected from gold, silver, copper, nickel, tin, iron, chromium, platinum, palladium, rhodium, iridium, ruthenium, osmium, indium, zinc, molybdenum, manganese, titanium, aluminum, stainless steel, and brass.

[0024] The method for laminating the heat dissipation layer is not particularly limited, and examples thereof include dry processes such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, wet processes such as electrodeposition, silver halide methods, electrolytic plating, and electroless plating. The heat dissipation layer can be patterned by known physical or chemical treatments, mainly photolithography, or a combination of these. The thermal conductivity of each of the heat dissipation layers is independently preferably 5 to 500 W / (m·K), more preferably 8 to 500 W / (m·K), even more preferably 10 to 450 W / (m·K), particularly preferably 12 to 420 W / (m·K), and most preferably 15 to 400 W / (m·K).

[0025] The thickness of the heat dissipation layer is appropriately determined from the viewpoint of thermoelectric performance, but is preferably 1 to 550 μm, more preferably 10 to 400 μm, and further preferably 30 to 200 μm.

[0026] The adhesive strength of the thermally conductive interface member A to the heat dissipation layer and the adhesive strength of the thermally conductive interface member B to the heat dissipation layer are each independently preferably 0.01 (N / cm) to 50.0 (N / cm), more preferably 0.05 (N / cm) to 25.0 (N / cm), and further preferably 0.10 (N / cm) to 10.0 (N / cm). When the adhesive strength of the thermally conductive interface member A to the heat dissipation layer and the adhesive strength of the thermally conductive interface member B to the heat dissipation layer are within this range, the adhesion between the members constituting the thermoelectric conversion module is improved while maintaining a desired thermal conductivity, and the thermoelectric performance is easily improved without causing physical damage to the chips of P-type thermoelectric conversion material and N-type thermoelectric conversion material.

[0027] (Thermoelectric conversion material chip) The chip of the thermoelectric conversion material used in the present invention is preferably formed by dividing a thermoelectric conversion material layer made of a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (hereinafter sometimes referred to as "thermoelectric semiconductor particles"), a binder resin, and an ionic compound (ionic liquid, inorganic ionic compound).

[0028] (Thermoelectric semiconductor materials) The thermoelectric semiconductor material is preferably pulverized to a predetermined size using, for example, a fine grinding device, and then used as thermoelectric semiconductor particles. The particle size of the thermoelectric semiconductor particles is preferably 10 nm to 100 μm, more preferably 50 nm to 50 μm, and further preferably 1 μm to 30 μm. The average particle size of the thermoelectric semiconductor particles was obtained by measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000) and was taken as the median value of the particle size distribution.

[0029] The thermoelectric semiconductor material used in the present invention is not particularly limited, and examples thereof include bismuth-tellurium-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-tellurium-based thermoelectric semiconductor materials; ZnSb, Zn3Sb 2、Zinc-antimony-based thermoelectric semiconductor materials such as Zn4Sb3; silicon-germanium-based thermoelectric semiconductor materials such as SiGe; bismuth selenide-based thermoelectric semiconductor materials such as Bi2Se3; β-FeSi2, CrSi2, MnSi 1.73 , silicide-based thermoelectric semiconductor materials such as Mg2Si; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, FeVTiAl, and sulfide-based thermoelectric semiconductor materials such as TiS2 are used.

[0030] Among these, the thermoelectric semiconductor material used in the present invention is preferably a bismuth-tellurium-based thermoelectric semiconductor material such as P-type bismuth telluride or N-type bismuth telluride. The P-type bismuth telluride has holes as carriers and a positive Seebeck coefficient. For example, Bi X Te3Sb 2-X represented by is preferably used. In this case, X is preferably 0 < X ≤ 0.8, more preferably 0.4 ≤ X ≤ 0.6. When X is greater than 0 and less than or equal to 0.8, the Seebeck coefficient and electrical conductivity increase, and the characteristics as a P-type thermoelectric conversion material are maintained, which is preferable. In addition, the N-type bismuth telluride has electrons as carriers and a negative Seebeck coefficient. For example, Bi2Te 3-Y Se Y represented by is preferably used. In this case, Y is preferably 0 ≤ Y ≤ 3 (when Y = 0: Bi2Te3), more preferably 0.1 < Y ≤ 2.7. When Y is 0 to 3, the Seebeck coefficient and electrical conductivity increase, and the characteristics as an N-type thermoelectric conversion material are maintained, which is preferable.

[0031] The content of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass. More preferably, it is 50 to 96% by mass, and further preferably, it is 70 to 95% by mass. If the content of the thermoelectric semiconductor particles is within the above range, the Seebeck coefficient (absolute value of the Peltier coefficient) is large, and the decrease in electrical conductivity is suppressed, and only the thermal conductivity decreases, so that a film exhibiting high thermoelectric performance and having sufficient film strength and flexibility is preferably obtained. Note that, in calculating the content in the thermoelectric semiconductor composition, the value is calculated assuming that the solvent is not included (hereinafter, the same applies).

[0032] The thermoelectric semiconductor particles are preferably annealed. By performing annealing, the crystallinity of the thermoelectric semiconductor particles is improved and the surface oxide film of the thermoelectric semiconductor particles is removed, so that the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material is increased, and the thermoelectric figure of merit can be further improved.

[0033] (binder resin) The binder resin used in the present invention has the effect of physically binding the thermoelectric semiconductor material (thermoelectric semiconductor particles) together, and can increase the flexibility of the thermoelectric conversion module while facilitating the formation of a thin film by coating or the like.

[0034] The binder resin is appropriately selected depending on the temperature of the heat treatment of the thermoelectric semiconductor material and the baking (annealing) temperature. It is preferable to heat the material at a temperature higher than the decomposition temperature of the binder resin. Furthermore, it is more preferable to use a resin that maintains various physical properties such as mechanical strength and thermal conductivity without being impaired when the coating film made of the thermoelectric semiconductor composition is subjected to a heat treatment or the like to cause crystal growth of the thermoelectric semiconductor particles. In this specification, the term "decomposition temperature" refers to the temperature at which the mass reduction rate by thermogravimetry (TG) is 100% (the mass after decomposition is less than 1% of the mass before decomposition). The decomposition temperature of the binder resin is preferably 150 to 400° C., and it is preferable that 90% by mass or more of the binder resin is decomposed and vaporized.

[0035] As such a binder resin, a thermoplastic resin or a curable resin can be used. Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, polyisobutylene, and polymethylpentene; polycarbonate; thermoplastic polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyvinyl polymers such as polystyrene, acrylonitrile-styrene copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride, polyvinylpyridine, polyvinyl alcohol, and polyvinylpyrrolidone; polyurethane; and cellulose derivatives such as ethyl cellulose. Examples of the curable resin include thermosetting resins and photocurable resins. Examples of the thermosetting resin include epoxy resins and phenolic resins. Examples of the photocurable resin include photocurable acrylic resins, photocurable urethane resins, and photocurable epoxy resins. These may be used alone or in combination of two or more. Among these, thermoplastic resins are preferred, polycarbonate and cellulose derivatives such as ethyl cellulose are more preferred, and polycarbonate is particularly preferred.

[0036] The content of the binder resin in the thermoelectric semiconductor composition is preferably 0.1 to 20 mass %, more preferably 0.5 to 15 mass %, and further preferably 1.0 to 10 mass %.

[0037] <Ionic compounds> (Ionic Liquid) The ionic liquid that can be contained in the thermoelectric semiconductor composition is a molten salt formed by combining a cation and an anion, and refers to a salt that can exist in a liquid state in any temperature range of -50°C or more and less than 400°C. In other words, the ionic liquid is an ionic compound whose melting point is in the range of -50°C or more and less than 400°C. The melting point of the ionic liquid is preferably -25°C or more and 200°C or less, more preferably 0°C or more and 150°C or less. The ionic liquid has characteristics such as extremely low vapor pressure and non-volatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity, and therefore can effectively suppress the reduction in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary. In addition, the ionic liquid exhibits high polarity based on an aprotic ionic structure and has excellent compatibility with binder resins, so that the electrical conductivity of the thermoelectric element layer can be made uniform.

[0038] The ionic liquid may be a known or commercially available one. For example, a mixture of a cationic component such as a pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, imidazolium, etc., and a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as a phosphonium, trialkylsulfonium, tetraalkylphosphonium, etc., and a derivative thereof; a lithium cation and a derivative thereof; and a mixture of a Cl cation and ... - , Br - , I - , AlCl4 - , Al2Cl7 - , BF4 - , PF6 - , ClO4 - , NO3 - , CH3COO - , CF3COO - , CH3SO3 - , CF3SO3 - , (FSO2)2N - , (CF3SO2)2N - , (CF3SO2)3C - , AsF6 - , SbF6 - , NbF6 - , TaF6- , F(HF) n - , (CN)2N - , C4F9SO3 - , (C2F5SO2)2N - , C3F7COO - , (CF3SO2)(CF3CO)N - and an anion component such as the above.

[0039] Of the above ionic liquids, from the viewpoints of high-temperature stability, compatibility with thermoelectric semiconductor materials and resins, suppression of a decrease in the electrical conductivity in the gaps between thermoelectric semiconductor materials, and the like, it is preferable that the cationic component of the ionic liquid contains at least one selected from pyridinium cations and derivatives thereof, and imidazolium cations and derivatives thereof.

[0040] As the ionic liquid in which the cationic component contains a pyridinium cation or a derivative thereof, 1-butyl-4-methylpyridinium bromide, 1-butylpyridinium bromide, N-octylpyridinium bromide, and 1-butyl-4-methylpyridinium hexafluorophosphate are preferred.

[0041] As the ionic liquid in which the cationic component contains an imidazolium cation or a derivative thereof, [1-butyl-3-(2-hydroxyethyl)imidazolium bromide] or [1-butyl-3-(2-hydroxyethyl)imidazolium tetrafluoroborate] is preferred.

[0042] The content of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 20 mass%. When the content of the ionic liquid is within the above range, the decrease in electrical conductivity is effectively suppressed, and a film having high thermoelectric performance is obtained.

[0043] (Inorganic ionic compounds) The inorganic ionic compound that can be contained in the thermoelectric semiconductor composition is a compound composed of at least a cation and an anion. The inorganic ionic compound exists in a solid state in a wide temperature range of 400 to 900°C and has characteristics such as high ionic conductivity, so that it can suppress the decrease in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary.

[0044] The content of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 10 mass%. If the content of the inorganic ionic compound is within the above range, the decrease in electrical conductivity can be effectively suppressed, and as a result, a film with improved thermoelectric performance can be obtained. In addition, when an inorganic ionic compound and an ionic liquid are used in combination as the ionic compound, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.4 to 20 mass%, and even more preferably 0.8 to 10 mass%.

[0045] (Other additives) The thermoelectric semiconductor composition used in the present invention may further contain, as necessary, other additives other than those mentioned above, such as dispersants, film-forming assistants, light stabilizers, antioxidants, tackifiers, plasticizers, colorants, resin stabilizers, fillers, pigments, conductive fillers, conductive polymers, curing agents, etc. These additives may be used alone or in combination of two or more.

[0046] (Method for preparing thermoelectric semiconductor composition) The method for preparing the thermoelectric semiconductor composition is not particularly limited, and the thermoelectric semiconductor composition may be prepared by, for example, mixing and dispersing the thermoelectric semiconductor particles, the binder resin, and the ionic compound, as well as the other additives as necessary and a solvent, using a known method such as an ultrasonic homogenizer, a spiral mixer, a planetary mixer, a disperser, or a hybrid mixer. Examples of the solvent include toluene, ethyl acetate, methyl ethyl ketone, alcohol, tetrahydrofuran, methylpyrrolidone, ethyl cellosolve, and the like. These solvents may be used alone or in combination of two or more. The solid content concentration of the thermoelectric semiconductor composition is not particularly limited as long as the composition has a viscosity suitable for coating.

[0047] The coating film made of the thermoelectric semiconductor composition is not particularly limited, but can be formed, for example, by applying the thermoelectric semiconductor composition to a substrate such as at least glass, alumina, silicon, or resin to obtain a coating film, and drying the coating film. Methods for applying the thermoelectric semiconductor composition to obtain a coating film include known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, doctor blade, etc., and are not particularly limited. When forming a coating film in a pattern, a screen printing method, a slot die coating method, etc., which can easily form a pattern using a screen plate having a desired pattern, are preferably used. The coating film is then dried to form a coating film, and the drying method may be a conventionally known drying method such as hot air drying, hot roll drying, infrared irradiation, etc. The heating temperature is usually 80 to 150° C., and the heating time varies depending on the heating method, but is usually several seconds to several tens of minutes. When a solvent is used in the preparation of the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range in which the solvent used can be dried. Furthermore, the dried coating film may be subjected to a hot press (heating and pressing) treatment to form a thermoelectric conversion material layer precursor for the purpose of suppressing voids in the chip of the thermoelectric conversion material, improving electrical conductivity, etc. The hot press (heating and pressing) treatment can be performed, for example, by using a device such as a hydraulic press to apply pressure to the entire upper surface of the coating film at a predetermined temperature and in an atmospheric atmosphere at a predetermined pressure for a predetermined time. The temperature for the hot press (heating and pressing) treatment is not particularly limited, but is usually 100 to 300°C, and preferably 200 to 300°C. The pressure for the hot pressing (heating and pressing) treatment is not particularly limited, but is usually 20 to 200 MPa, and preferably 50 to 150 MPa. The time for the hot press (heating and pressing) treatment is not particularly limited, but is usually from several seconds to several tens of minutes, preferably from several tens of seconds to several tens of minutes.

[0048] The obtained thermoelectric conversion material layer precursor is preferably subjected to a firing (annealing) treatment for the purposes of stabilizing the thermoelectric performance and causing crystal growth of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition to form a thermoelectric conversion material layer. The firing (annealing) treatment is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon, under a reducing gas atmosphere, or under vacuum conditions with the gas flow rate controlled. The temperature of the firing (annealing) treatment depends on the thermoelectric semiconductor particles, binder resin, ionic liquid, inorganic ionic compound, etc. used in the thermoelectric semiconductor composition and is appropriately adjusted, but is usually 260 to 600°C, preferably 280 to 550°C. The time for the firing (annealing) treatment is not particularly limited, but is usually from several minutes to several tens of hours, and preferably from several minutes to several hours.

[0049] The thermoelectric conversion material chips used in the present invention can be obtained by dicing the thermoelectric conversion material layer. There are no particular limitations on the method of dicing, but from the viewpoints of processing accuracy and process stability, it is preferable to affix the thermoelectric conversion material layer to a dicing tape and use a dicing blade.

[0050] <Substrate> As the substrates of the thermoelectric conversion module of the present invention, for example, the first substrate 2a and the second substrate 2b are preferably made of plastic films that do not affect the decrease in electrical conductivity or the increase in thermal conductivity of the thermoelectric conversion material chip. Even when the thermoelectric conversion material layer is annealed, the substrate does not thermally deform, and the performance of the thermoelectric conversion module can be maintained. In view of high heat resistance and dimensional stability, the plastic films are preferably polyimide films, polyamide films, polyetherimide films, polyaramid films, polyamideimide films, and glass-epoxy sheets.

[0051] The thickness of the plastic film used for the substrate is preferably from 1 to 1000 μm, more preferably from 10 to 500 μm, and even more preferably from 20 to 100 μm, from the viewpoints of flexibility, heat resistance, and dimensional stability.

[0052] <Electrode> There are no particular limitations on the metal material used as the electrodes of the thermoelectric conversion module of the present invention. For example, the metal material of the first electrode 3a and the second electrode 3b may be gold, nickel, aluminum, rhodium, platinum, chromium, palladium, stainless steel, molybdenum, or an alloy containing any of these metals. In addition to the metal material, a paste material containing a solvent or a resin component may be used. When using a paste material, it is preferable to remove the solvent or the resin component by firing, etc. As the paste material, silver paste and aluminum paste are preferable. The thickness of the electrode layer is preferably 10 nm to 200 μm, more preferably 30 nm to 150 μm, and further preferably 50 nm to 120 μm. When the thickness of the electrode layer is within the above range, the electrical conductivity is high and the resistance is low, and sufficient strength as an electrode is obtained.

[0053] Examples of methods for forming the electrodes include a method of processing into a predetermined pattern shape by known physical or chemical treatments mainly based on photolithography, or a combination of these, and a method of forming an electrode pattern by screen printing, stencil printing, inkjet printing, or the like. Methods for forming electrodes without a pattern include vacuum deposition methods such as PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, or CVD (chemical vapor deposition) methods such as thermal CVD and atomic layer deposition (ALD), or various coating methods such as dip coating, spin coating, spray coating, gravure coating, die coating, and doctor blade methods, wet processes such as electrodeposition, silver halide methods, electrolytic plating, electroless plating, and lamination of metal foils, and are appropriately selected depending on the metal material. The electrodes used in the present invention are required to have high conductivity, and since electrodes formed by plating or vacuum film formation can easily achieve high conductivity, vacuum film formation methods such as vacuum deposition and sputtering, electrolytic plating, and electroless plating are preferred. Depending on the size and dimensional accuracy of the pattern to be formed, a pattern can also be easily formed through a hard mask such as a metal mask. In addition, when forming a film by the vacuum film formation method, the substrate to be used may be heated to a degree that does not impair the characteristics of the substrate in order to improve adhesion to the substrate to be used and remove moisture. When forming a film by the plating method, a film may be formed by electrolytic plating on a film formed by electroless plating.

[0054] <Solder material layer> The solder material layer is used to join the chip of thermoelectric conversion material and the electrodes. The solder material constituting the solder material layer may be appropriately selected taking into consideration the heat resistance temperature of the binder resin contained in the substrate and the thermoelectric conversion material chip, as well as the electrical conductivity and thermal conductivity, and examples of known materials include Sn, Sn / Pb alloy, Sn / Ag alloy, Sn / Cu alloy, Sn / Sb alloy, Sn / In alloy, Sn / Zn alloy, Sn / In / Bi alloy, Sn / In / Bi / Zn alloy, Sn / Bi / Pb / Cd alloy, Sn / Bi / Pb alloy, Sn / Bi / Cd alloy, Bi / Pb alloy, Sn / Bi / Zn alloy, Sn / Bi alloy, Sn / Bi / Pb alloy, Sn / Pb / Cd alloy, and Sn / Cd alloy. From the viewpoints of lead-free and / or cadmium-free, melting point, electrical conductivity, and thermal conductivity, alloys such as 43Sn / 57Bi alloy, 42Sn / 58Bi alloy, 40Sn / 56Bi / 4Zn alloy, 48Sn / 52In alloy, and 39.8Sn / 52In / 7Bi / 1.2Zn alloy are preferred. Commercially available solder materials include the following: 42Sn / 58Bi alloy (manufactured by Tamura Manufacturing Co., Ltd., product name: SAM10-401-27), 41Sn / 58Bi / Ag alloy (manufactured by Nihon Handa Co., Ltd., product name: PF141-LT7HO), 96.5Sn3Ag0.5Cu alloy (manufactured by Nihon Handa Co., Ltd., product name: PF305-207BTO), etc.

[0055] The thickness of the solder material layer (after heating and cooling) is preferably 10 to 200 μm, more preferably 20 to 150 μm, further preferably 30 to 130 μm, and particularly preferably 40 to 120 μm. When the thickness of the solder material layer is within this range, adhesion between the thermoelectric conversion material chip and the electrodes can be easily obtained.

[0056] Methods for applying solder material to a board include stencil printing, screen printing, and die printing. The heating temperature varies depending on the solder material, resin film, etc., used, but is usually performed at 150 to 280° C. for 3 to 20 minutes.

[0057] <Solder acceptance layer> The solder-receiving layer has the function of improving the bonding strength between the chip of thermoelectric conversion material containing resin and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly bonded to the chip of thermoelectric conversion material.

[0058] The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, nickel, aluminum, rhodium, platinum, chromium, palladium, tin, and an alloy containing any of these metal materials. Among these, a two-layer structure of gold, silver, nickel, aluminum, or tin and gold is preferable, and from the viewpoints of material cost, high thermal conductivity, and bonding stability, silver, nickel, and aluminum are more preferable.

[0059] The thickness of the solder-receiving layer is preferably 10 nm to 50 μm, more preferably 200 nm to 10 μm, and particularly preferably 500 nm to 5 μm. When the thickness of the solder-receiving layer is within this range, the adhesion to the surface of the thermoelectric conversion material chip and the adhesion to the surface of the solder material layer on the electrode side constituting the thermoelectric conversion module are excellent, and a highly reliable bond can be obtained. In addition, high thermal conductivity as well as electrical conductivity can be maintained, and as a result, the thermoelectric performance of the thermoelectric conversion module is maintained without deterioration. The solder-receiving layer may be a single layer formed by directly depositing a metal material, or may be a multilayer formed by laminating two or more metal materials.

[0060] The solder-receiving layer is preferably formed using the above-mentioned metal material. Since the solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, it is preferable to use a solder-receiving layer formed by electrolytic plating, electroless plating, or vacuum film formation.

[0061] The thermoelectric conversion module of the present invention has high thermoelectric performance with improved heat transfer effect at the interface between members. EXAMPLES

[0062] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0063] The adhesive strength of the TIM, the shear stress, the thermal resistance value of each member, and the electromotive force of the thermoelectric conversion modules produced in the examples and comparative examples were evaluated by the following methods.

[0064] (a) Shear stress evaluation The TIM (10 mm x 10 mm) used in the examples and comparative examples was attached to a copper plate (45 mm x 45 mm x 3 mm thick), and a gold-plated copper chip (5 mm x 5 mm x 200 μm thick) was attached to the side of the TIM opposite the copper plate. A bond tester Dage Series 4000 (manufactured by Nordson Dage) was used to measure the shear stress (N / mm 2 ) was measured.

[0065] (b) Adhesion strength evaluation The TIM (25 mm x 40 mm) used in the examples and comparative examples was attached to a copper plate (100 mm x 100 mm x 3.0 mm thick), and then bonded to the copper plate by rolling it back and forth once using a 2 kg roll (φ95 mm, material: rubber). After 24 hours, the 90 degree peel strength was measured at a peel speed of 300 mm / min using a universal tensile strength tester (manufactured by Shimadzu Corporation, model name: Autograph AG-X Plus) in an atmosphere of 23°C and 50% RH, and the adhesive strength (N / cm) was recorded.

[0066] (c) Electromotive force evaluation (output evaluation) FIG. 2 is a cross-sectional view showing an example of a configuration for evaluating the electromotive force of a thermoelectric conversion module of the present invention. In the thermoelectric conversion module electromotive force evaluation configuration 21, a heat dissipation member 24 [heat sink UB2040-25B, manufactured by Alpha Corporation] was placed on one surface of the adhesive thermally conductive interface member A 23a on the thermoelectric conversion module 22 obtained in the examples and comparative examples, and a temperature controller (heat source) 25 (product name: Peltier temperature controller set VTH1.8-70S, manufactured by VICS Corporation) was placed on the other surface of the adhesive thermally conductive interface member B 23b. The temperature controller (heat source) 25 was set to 60°C, and a temperature difference was applied from the outside. With the temperature difference applied, the electromotive force between the extraction electrodes was measured using a Digital HiTester (manufactured by Hioki E.E. Corporation, model number: 3801-50).

[0067] (d) Thermal resistance evaluation The thermal resistance (K / W) of the TIM used in the examples and comparative examples was calculated based on the thermal conductivity [W / (m K)], thickness (m), and effective area [0.006 (m) × 0.021 (m) = 1.26 × 10 -4 (m 2 )] was used to calculate the value from the following formula (1). Thermal resistance of TIM = thickness of TIM / (thermal conductivity of TIM x effective area) (1) Similarly, the thermal conductivity, thickness, and effective area of ​​each of the following layers constituting the thermoelectric conversion module were calculated. Glass-epoxy substrate: Thermal conductivity 3.0 [W / (m K)]; thickness 6.0×10 -5 (m); Effective area 1.26×10 -4 (m 2 ) Heat dissipation layer: Cu thermal conductivity 398 [W / (m K)] thickness 3.5×10 -5 (m) Ni 90.9 [W / (m K)] Thickness 3.0×10 -6 (m); Effective area 1.26×10 -4 (m 2 ) Electrode layer: Cu, thermal conductivity 398 [W / (m K)], thickness 3.5×10 -5 (m) Ni 90.9 [W / (m K)] Thickness 3.0×10 -6 (m); Effective area 1.02×10-4 (m 2 ) Solder material layer: Thermal conductivity 20 [W / (m K)] Thickness 5.0×10 -5 (m); Effective area 1.02×10 -4 (m 2 ) Chip: Thermal conductivity 0.5 [W / (m K)] Thickness 2.85×10 -4 (m); Effective area 1.02×10 -4 (m 2 ) From the above, the thermal resistance value R of the thermally conductive interface material A A (mK / W), thermal resistance value R of thermally conductive interface material B B (mK / W) AB (mK / W), and the total thermal resistance value R M (mK / W) and R M R AB Ratio (R AB / R M ) was calculated.

[0068] Example 1 <Fabrication of thermoelectric conversion module> (1) Preparation of thermoelectric semiconductor particles As a P-type thermoelectric semiconductor particle, P-type bismuth telluride Bi, a bismuth-tellurium-based thermoelectric semiconductor material, was used. 0.4 Te3Sb 1.6 (manufactured by Kojundo Chemical Laboratory, average particle size: 16 μm) was used. As the N-type thermoelectric semiconductor particles, N-type bismuth telluride Bi2Te3 (manufactured by Kojundo Chemical Laboratory, particle size: 90 μm), a bismuth-tellurium based thermoelectric semiconductor material, was used, and was pulverized in a nitrogen gas atmosphere using a planetary ball mill (Fritsch Japan, Premium line P-7) to prepare thermoelectric semiconductor particles with an average particle size of 2.8 μm. The particle size distribution of each thermoelectric semiconductor particle was measured using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000).

[0069] (2) Preparation of coating solution of thermoelectric semiconductor composition Coating liquid (P) The P-type bismuth telluride Bi 0.4 Te3Sb 1.6 A coating liquid (P) was prepared, which was a thermoelectric semiconductor composition obtained by mixing and dispersing 78.5 parts by mass of particles, 5.2 parts by mass of polyethylene carbonate as a binder resin, 0.8 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 15.5 parts by mass of N-methylpyrrolidone as a solvent. Coating fluid (N) A coating liquid (N) was prepared by mixing and dispersing 78.8 parts by mass of the obtained N-type bismuth telluride Bi2Te3 particles, 4.25 parts by mass of polyethylene carbonate as a binder resin, 4.2 parts by mass of N-octylpyridinium bromide as an ionic liquid, and 12.75 parts by mass of N-methylpyrrolidone as a solvent.

[0070] (3) Fabrication of thermoelectric conversion material chips The coating solution (P) prepared in (2) was applied onto a polyimide film (manufactured by Ube Industries, product name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (manufactured by Newlong, model name: LS-34TVA), and the film was dried by heating at 110 ° C for 20 minutes to form a coating film with a thickness of 600 μm. Next, the coating film was subjected to a heat press at 250 ° C and 50 MPa for 10 minutes to obtain a P-type thermoelectric conversion material layer precursor with a thickness of 285 μm. The obtained P-type thermoelectric conversion material layer precursor was subjected to a baking (annealing) treatment at 430° C. for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain a P-type thermoelectric conversion material layer. Next, a solder-receiving layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was formed on the entire surface of the P-type thermoelectric conversion material layer by electroless plating, and then the P-type thermoelectric conversion material layer was diced into chips using a dicing device (manufactured by DISCO, model name: DFD6362) to produce P-type thermoelectric conversion material chips measuring 0.9 mm x 0.9 mm. Similarly, the coating solution (N) prepared in (2) was applied onto a polyimide film (manufactured by Ube Industries, product name "Kapton 500H", 100 mm x 160 mm x thickness 125 μm) using a screen printer (manufactured by Newlong, product name: LS-34TVA), and the film was dried by heating at 110 ° C for 20 minutes to form a coating film with a thickness of 540 μm. Next, the coating film was subjected to a heat press at 250 ° C and 30 MPa for 20 minutes to obtain an N-type thermoelectric conversion material layer precursor with a thickness of 285 μm. The obtained N-type thermoelectric conversion material layer precursor was subjected to a baking (annealing) treatment at 370° C. for 30 minutes in an argon-hydrogen mixed gas atmosphere to obtain an N-type thermoelectric conversion material layer. Next, a solder-receiving layer [Ni (thickness: 4 μm) laminated with Au (thickness: 30 nm)] was formed on the entire surface of the N-type thermoelectric conversion material layer by electroless plating, and then the layer was attached to a dicing tape and diced into chips using a dicing device (manufactured by DISCO, model number: DFD6362), to produce N-type thermoelectric conversion material chips measuring 0.9 mm x 0.9 mm.

[0071] (4) Preparation of electrode substrate First, a substrate was prepared by attaching copper foil of 35 μm thickness to both sides of a 60 μm thick glass-epoxy sheet. A nickel layer (thickness: 3 μm) and a gold layer (thickness: 40 nm) were laminated in this order on the copper foil of the substrate by electroless plating, and then an electrode pattern (0.9 × 0.9 mm, 126 pieces, distance between adjacent electrodes: 0.1 mm, 6 columns, 21 rows) was formed only on one side to produce a substrate with an electrode on one side and a heat sink on the other side (first substrate with first electrode, hereinafter sometimes referred to as "first electrode substrate"). Similarly, a substrate with electrodes arranged in a pattern was produced so that a π-type thermoelectric conversion module would be obtained when it was bonded to the first electrode substrate (a second substrate having a second electrode, hereinafter sometimes referred to as the "second electrode substrate"). Note that the materials of the substrate and electrodes, and the dimensions including the thickness, were the same as those of the first electrode substrate.

[0072] (Fabrication of thermoelectric conversion module) Using the P-type thermoelectric material chips with solder acceptance layers only on the top and bottom surfaces and the N-type thermoelectric material chips produced in (3), a π-type Peltier-cooled thermoelectric conversion module consisting of 63 pairs of P-type and N-type thermoelectric material chips was produced as follows.

[0073] A solder material layer with a thickness of 50 μm was formed on the first electrode substrate prepared in (4) by screen printing using solder paste (manufactured by Kokisha, product name: T4AB58-M742) as the solder material. Next, one side of the solder acceptance layer of each of the P-type and N-type thermoelectric conversion material chips prepared in (3) was placed on the solder material layer, heated at 190°C for 1 minute, and then cooled, thereby placing the P-type and N-type thermoelectric conversion material chips on the first electrode substrate, respectively. Furthermore, a solder material layer with a thickness of 50 μm was formed on the other side of the solder acceptance layer of each of the P-type and N-type thermoelectric conversion material chips using the solder paste in the same manner as described above, and the second electrode substrate prepared in (4) was attached to the layer. The layer was then heated at 190°C for 2 minutes to produce a thermoelectric conversion module consisting of 63 pairs each of P-type and N-type thermoelectric conversion material chips.

[0074] (TIM placement) The thermoelectric conversion module was fabricated with R AB / R M A TIM [Sekisui Polymatech Co., Ltd., product number: PT-V, thickness: 0.50 mm, thermal conductivity: 12 W / (m K)] with a shear stress of 0.039 and a thermal conductivity of 0.12 was installed, and the electromotive force between the extraction electrodes of the obtained thermoelectric conversion module was measured based on the above-mentioned (c) electromotive force evaluation (output evaluation).

[0075] Example 2 In Example 1, R AB / R M A thermoelectric conversion module was prepared in the same manner as in Example 1, except that a TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: PT-UT, thickness: 0.50 mm, thermal conductivity: 6 W / (m K)] with a shear stress of 0.042 and a thermal conductivity of 0.23 was installed, and the electromotive force between the extraction electrodes was measured.

[0076] Example 3 In Example 1, R AB / R M A thermoelectric conversion module was prepared in the same manner as in Example 1, except that a TIM [manufactured by 3M, product number: 8926, thickness: 0.20 mm, thermal conductivity: 1.5 W / (m K)] with a shear stress of 0.38 and a thermal conductivity of 0.780 was installed, and the electromotive force between the extraction electrodes was measured.

[0077] Comparative Example 1 In Example 1, R AB / R M A thermoelectric conversion module was prepared in the same manner as in Example 1, except that a TIM [manufactured by 3M, product number: VHR0601, thickness: 0.30 mm, thermal conductivity: 0.6 W / (m K)] with a thermal conductivity of 1.41 and a shear stress of 1.210 was installed, and the electromotive force between the extraction electrodes was measured.

[0078] Comparative Example 2 In Example 1, R AB / R M A thermoelectric conversion module was prepared in the same manner as in Example 1, except that a TIM [manufactured by Sekisui Polymatech Co., Ltd., product number: Manion50α, thickness: 0.50 mm, thermal conductivity: 17 W / (m K)] with a shear stress of 0.083 was installed, and the electromotive force between the extraction electrodes was measured.

[0079] Comparative Example 3 A thermoelectric conversion module was produced in the same manner as in Example 1, except that no TIM was provided on the top and bottom surfaces of the thermoelectric conversion module, and the electromotive force between the extraction electrodes was measured.

[0080] The adhesive strength, shear stress, and total thermal resistance R of the TIM in the thermoelectric conversion modules obtained in Examples 1 to 4 and Comparative Examples 1 to 3. AB , the total thermal resistance value R of each component of the thermoelectric conversion module M , total thermal resistance R AB / Total thermal resistance value R M The evaluation results of the electromotive force of the thermoelectric conversion module are shown in Table 1.

[0081] [Table 1]

[0082] R M R AB Ratio (R AB / R M ), and the electromotive force obtained from the thermoelectric conversion modules of Examples 1 to 3 in which the specific shear stress applied to the thermally conductive interface member A and the thermally conductive interface member B satisfies the provisions of the present invention is higher than the electromotive force obtained from the thermoelectric conversion modules of Comparative Examples 1 to 3 which do not satisfy the provisions of the present invention, and it can be seen that the thermoelectric performance is improved. [Industrial Applicability]

[0083] According to the thermoelectric conversion module of the present invention, a thermoelectric conversion module with improved electromotive force can be obtained, and therefore it is possible to apply it to power generation applications such as converting exhaust heat from various combustion furnaces such as factories, waste combustion furnaces, and cement combustion furnaces, exhaust heat from automobile combustion gases, and exhaust heat from electronic devices into electricity. As cooling applications, in the field of electronic devices, it is possible to apply it to temperature control of various sensors such as CPUs (Central Processing Units) used in smartphones and various computers, image sensors such as CMOS (Complementary Metal Oxide Semiconductors) and CCD (Charge Coupled Devices), and further, MEMS (Micro Electro Mechanical Systems), light receiving elements, etc. [Explanation of symbols]

[0084] 1: Thermoelectric conversion module 2a: 1st board 2b: 2nd board 3a: 1st electrode 3b: 2nd electrode 4: P-type thermoelectric conversion material chip 5: N-type thermoelectric conversion material chip 6: Solder material layer 7: Solder acceptance layer 8a: Heat dissipation layer A 8b: Heat dissipation layer B 9: Thermoelectric conversion element 10a: Adhesive thermally conductive interface member A 10b: Adhesive thermally conductive interface member B 11: Heat dissipation material 21: Thermoelectric conversion module electromotive force evaluation configuration 22: Thermoelectric conversion element 23a: Adhesive thermally conductive interface member A 23b: Adhesive thermally conductive interface member B 24: Heat dissipation material 25: Temperature controller (heat source)

Claims

[Claim 1] A thermoelectric conversion module including a thermally conductive interface member A having adhesive properties on one surface of a thermoelectric conversion element and a heat dissipation member in this order, and a thermally conductive interface member B having adhesive properties on the other surface of the thermoelectric conversion element, The thermal resistance value of the thermally conductive interface member A is R A (mK / W), the thermal resistance value of the thermally conductive interface member B is R B (mK / W), and the sum of these, the total thermal resistance, is R AB (mK / W), and the total thermal resistance of the thermoelectric conversion module is R M (mK / W), the R M The R AB The ratio (R AB / R M ) is 1.40 or less, and The shear stress τ applied to the thermally conductive interface member A when the thermally conductive interface member A is bonded to one surface of the thermoelectric conversion element. A (N / mm 2 ) and the shear stress τ acting on the thermally conductive interface member B when the thermally conductive interface member B is bonded to the other surface of the thermoelectric conversion element. B (N / mm 2 ) and each independently 0.001 (N / mm 2 ) or more.

Citation Information

Patent Citations

  • Thermoelectric module, its manufacturing method and cooling device

    JP2006041243A

  • Thermoelectric conversion module and power generating system

    JP2019204926A

  • Joining material, joining method of thermoelectric element and metal electrode, and thermoelectric conversion module

    JP2020141093A

  • Thermally conductive pressure sensitive adhesive comprising anisotropic boron nitride agglomerates