Separation method and separation device
The use of an amorphous silica molecular sieve film formed by chemical vapor deposition addresses the challenge of separating fluorocarbon gases with high selectivity, enhancing separation efficiency and reducing energy costs.
Patent Information
- Application Number
- JP2023112649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-07-07
- Publication Date
- 2024-10-15
AI Technical Summary
Fluorocarbons in mixed refrigerant gases are difficult to separate due to azeotropy and small molecular size differences, leading to inefficient separation and regeneration, and existing membrane separation techniques lack sufficient selectivity.
A method using a molecular sieve film containing amorphous silica formed by chemical vapor deposition is employed to separate fluorocarbon gases, utilizing differences in molecular diameter to achieve high selectivity, with a gas separation step conducted at specific temperature and pressure ranges.
The method achieves efficient separation of fluorocarbon gases with high selectivity and transmittance ratios, particularly suitable for difluoromethane and pentafluoroethane, reducing energy consumption and costs compared to distillation.
Smart Images

Figure 2024146684000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method and apparatus for separating fluorocarbon gas mixtures. [Background technology]
[0002] Distillation is a technique for separating a specific refrigerant gas from a mixed refrigerant gas consisting of multiple types of refrigerant gas. However, the evaporation method requires a large amount of energy consumption and a large investment cost for equipment. Therefore, a technique for separating and recovering the mixed refrigerant gas into various refrigerant gases at low cost is desired.
[0003] For example, Patent Document 1 discloses a method for separating and recovering fluorocarbons from a gas mixture containing fluorocarbons, which comprises contacting the gas mixture containing fluorocarbons with a selectively permeable composite membrane having an active thin film formed by crosslinking a crosslinkable silicone resin on a porous support membrane made of polyimide or polysulfone, thereby allowing the fluorocarbons to selectively permeate through the membrane and separating them.
[0004] Furthermore, Non-Patent Document 1 reports that when a mixture of R410A consisting of 50% difluoromethane (HFC-32, CH2F2) and 50% pentafluoroethane (HFC-125, CHF2CF3) was separated using a fluorine-based amorphous polymer membrane consisting of polydimethylsiloxane and 5 mol % perfluoro(butenyl vinyl ether) and 95 mol % perfluoro(2,2-dimethyl-1,3-dioxole), the permeability of HFC-32 was higher than that of HFC-125. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 1-42444 [Non-patent literature]
[0006] [Non-Patent Document 1] Abby N. Harders et al.,J.Membr.Sci.,652,120467(2022) Summary of the Invention [Problem to be solved by the invention]
[0007] Fluorocarbons are used as mixed gases in refrigerants, but separation is difficult due to azeotropy and other factors. In addition, the difference in molecular diameter is small, so it is not easy to efficiently separate and regenerate them even with membrane separation. In the fluorocarbon gas separation techniques disclosed in Patent Document 1 and Non-Patent Document 1, the ratio of the permeability of each fluorocarbon gas is about several times to 20 times, and a separation technique with higher selectivity is desired.
[0008] An object of the present disclosure is to provide a new method and apparatus for separating fluorocarbons. [Means for solving the problem]
[0009] Means for solving the above problems include the following aspects. <1> A method for separating a fluorocarbon mixed gas, comprising a gas separation step of contacting a mixed gas containing two or more fluorocarbon gases having different molecular diameters with a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method, thereby separating the mixed gas into gases having different mixture ratios from the mixed gas. <2> The molecular sieve membrane is an amorphous silicon having a structure including a -Si-O-Si- bond. Lyca membrane <1> 2. The method for separating a fluorocarbon mixed gas according to claim 1 . <3> The gas separation process is carried out in an environment of 20°C to 300°C. <1> or <2> 2. The method for separating a fluorocarbon mixed gas according to claim 1 . <4> The gas separation step is carried out under an environment of 0.1 MPa or more. <1> ~ <3> 2. A method for separating a fluorocarbon mixed gas according to claim 1 . <5> The molecular sieve membrane is a molecular sieve membrane formed by using dimethoxydiphenylsilane as a chemical vapor deposition material in the chemical vapor deposition method. <1> ~ <4> 2. A method for separating a fluorocarbon mixed gas according to claim 1 . <6> The chemical vapor deposition method is a counter diffusion method. <1> ~ <5> 2. A method for separating a fluorocarbon mixed gas according to claim 1 . <7> The molecular sieve membrane is formed on a ceramic porous support. <1> ~ <6> 2. A method for separating a fluorocarbon mixed gas according to claim 1 . <8> The fluorocarbon gas mixture is a mixture of difluoromethane and pentafluoroethane. <1> ~ <7> 2. A method for separating a fluorocarbon mixed gas according to claim 1 . <9> A separation device equipped with a porous membrane containing amorphous silica formed by a chemical vapor deposition method, which separates a gas composition in which the mixture ratio of one fluorocarbon gas is increased from a mixed gas containing two or more fluorocarbon gases having different molecular diameters, or a single gas. Effect of the Invention
[0010] According to the present disclosure, a new method and apparatus for separating fluorocarbons is provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a molecular sieve membrane used in the fluorocarbon mixed gas separation method and separation device of the present disclosure. [Diagram 2] FIG. 1 is a schematic diagram showing a gas separator, which is a main part of one embodiment of an apparatus for carrying out the fluorocarbon mixed gas separation method of the present disclosure. [Diagram 3] 3 is a schematic cross-sectional view showing a cross section of the molecular sieve membrane and the housing taken along line CC in FIG. 2. [Figure 4] FIG. 1 is a schematic diagram showing the configuration of a film-forming apparatus and gas permeation test apparatus used in the examples. [Diagram 5] FIG. 2 is a diagram showing Arrhenius plots of each single component gas in the examples. [Figure 6] FIG. 2 is a graph showing the temperature dependence of ideal selectivity in an example. [Figure 7] FIG. 1 is a graph showing the pressure dependence of the transmittance of each single component gas of HFC-32 and HFC-125 at 200° C. [Figure 8] FIG. 1 is a graph showing the pressure dependence of the transmittance of each single component gas of HFC-32 and HFC-125 at 100° C. [Figure 9] FIG. 1 is a graph showing the pressure dependence of the transmittance at 25° C. of each of the single component gases HFC-32 and HFC-125. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In addition, the term "process" in this specification includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In addition, components indicated by the same reference numerals in each drawing are the same components. Reference numerals may be omitted for components having the same functions in the drawings. Reference numerals may be omitted in the following description. In addition, the dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.
[0013] The inventors of the present disclosure have repeatedly studied and experimented on a method for separating a refrigerant gas containing a mixture of two or more fluorocarbon gases having different molecular sizes (sometimes referred to as a "fluorocarbon mixed gas" in this disclosure) with high selectivity, and have found that by utilizing the differences in the physical properties (size, etc.) of the various gases, a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method (also called a chemical vapor deposition method; hereinafter, sometimes referred to as a CVD method) (sometimes referred to as a "CVD amorphous silica membrane," "amorphous silica membrane," or simply a "silica membrane" in this disclosure) can be formed. It was found that by using a fluorine-containing fluorine-containing solvent, separation with high selectivity was possible. For example, the activated thin film formed by crosslinking a crosslinkable silicone resin disclosed in Patent Document 1 and the fluorine-based amorphous polymer membrane disclosed in Non-Patent Document 1 are not porous membranes, but separate gases by a dissolution-diffusion effect that utilizes the difference in solubility and diffusivity of gases in the membrane. On the other hand, the CVD amorphous silica membrane used in the present disclosure mainly utilizes the difference in size of each gas molecule and separates gases by a molecular sieve effect due to pore size control.
[0014] For example, the mixed refrigerant R410A of difluoromethane (sometimes written as HFC-32 or R32) and pentafluoroethane (sometimes written as HFC-125 or R125) is used as a refrigerant in the fields of air conditioners and refrigeration and freezing, but there is a shift to R32, which has a smaller global warming potential. The CVD amorphous silica film used in the present disclosure has a transmittance of difluoromethane (R32, molecular diameter: 0.363 nm) that is more than 100 times higher than that of pentafluoroethane (R125, molecular diameter: 0.447 nm), and the transmittance ratio is temperature dependent in the range of room temperature (e.g., 25°C) to 200°C, and it has been revealed that the transmittance ratio is larger at higher temperatures and is more suitable for separation. In addition, almost no pressure dependency of the transmittance was observed. That is, the method for separating a fluorocarbon mixed gas (sometimes simply referred to as a "mixed gas" in this disclosure) of the present disclosure includes a gas separation step of separating a mixed gas containing two or more fluorocarbon gases having different molecular diameters into gases having different mixing ratios from the mixed gas by contacting the mixed gas with a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method.
[0015] <Molecular sieve membrane> First, the molecular sieve membrane used in the method for separating fluorocarbon mixed gases of the present disclosure will be described. FIG. 1 is a cross-sectional view that shows a schematic diagram of one embodiment of a gas separation member equipped with a molecular sieve membrane used in the method for separating fluorocarbon mixed gases of the present disclosure. The gas separation member 30 shown in FIG. 1 includes a porous support 10 and an amorphous silica layer (amorphous silica membrane) 20 formed as a molecular sieve membrane on one surface of the porous support 10. The amorphous silica layer 20 has a function of selectively or preferentially allowing a fluorocarbon gas having a relatively small molecular diameter to permeate by the molecular sieve among two or more fluorocarbon gases contained in the fluorocarbon gas mixture.
[0016] The molecular sieve membrane in the present disclosure may be composed of a CVD amorphous silica layer alone, but from the viewpoints of strength as a molecular sieve membrane, ease of membrane formation, etc., it is preferable that the molecular sieve membrane is in the form of a gas separation member 30 having a structure in which an amorphous silica layer 20 as a molecular sieve membrane is supported by a porous support 10 as shown in Fig. 1. Note that the amorphous silica layer 20 may be formed not only on the surface of the porous support 10 but also within the pores of the porous support 10, as described later.
[0017] (Porous support) As the porous support 10 supporting the amorphous silica layer 20, a porous support having pores that are permeable to the fluorocarbon gas to be separated can be used. In the embodiment shown in FIG. 1, the porous support 10 has a two-layer structure of a support layer 12 and an intermediate layer 14, each of which is a porous body. From the viewpoint of being able to more stably fix the amorphous silica layer 20 and making the amorphous silica layer 20 stable for a longer period of time, it is preferable to use a porous support 10 having a two-layer structure as shown in FIG. 1, which includes a support layer 12 that has good strength and gas permeability and is also advantageous in terms of cost, and an intermediate layer 14 that has better retention of the amorphous silica layer 20 and has smaller pores than the support layer 12. In the present disclosure, when the surface of the intermediate layer 14 opposite to the surface that contacts the support layer 12 is referred to as the "surface of the intermediate layer", There is.
[0018] In the two-layered porous support 10, at least the surface of the intermediate layer 14 has an amorphous silica layer 20. The amorphous silica layer 20 may be formed only on the surface of the intermediate layer 14, or the amorphous silica layer 20 may be formed not only on the surface of the intermediate layer 14 but also inside the pores of the intermediate layer 14. In particular, in the two-layered porous support 10, it is preferable to have the amorphous silica layer 20 inside the pores of the intermediate layer 14 and on the surface of the intermediate layer 14. By having the amorphous silica layer 20 inside the pores of the intermediate layer 14, the amorphous silica layer 20 exists more densely and more stably in a state where it is filled in the pores. Therefore, the function of the amorphous silica layer 20 as a molecular sieve is further improved, and it is considered that the amorphous silica layer 20 functions as a separation active region with good separation function for fluorocarbon mixed gas. The separation active region will be described later.
[0019] Here, "having an amorphous silica layer inside the pores" refers to both a state in which an amorphous silica layer is formed on the inner wall surface of the pores, and a state in which the pores are filled with amorphous silica so that a part of the fluorocarbon mixed gas can be permeated. When forming an amorphous silica layer by a chemical vapor deposition method described later, a silica precursor in a gas phase penetrates into the inside of the pores of the porous support and is converted to amorphous silica on the inner wall surface of the pores. If the chemical vapor deposition is continued, the thickness of the amorphous silica layer formed on the inner wall surface of the pores increases, and the pores of the porous support may be filled with an amorphous silica layer. Either of these is referred to as having an amorphous silica layer inside the pores. A preferred embodiment of the molecular sieve membrane used in the method for separating fluorocarbon mixed gases of the present disclosure is one having an amorphous silica layer inside the pores of the intermediate layer and on the surface of the intermediate layer, the thickness of the fluorocarbon gas separation active region in the amorphous silica layer being 5 nm to 15 nm, and the membrane length (length in the longitudinal direction) of the amorphous silica layer being 6 cm or more.
[0020] Examples of materials for the porous support include porous ceramics from the viewpoints of pore size, availability, and the like. From the viewpoint of heat resistance, metal oxides, metal nitrides, and metal nitrides are preferred. More specifically, porous supports such as alumina, silica, titania, zirconia, and magnesia are more preferred, and α-alumina supports are particularly preferred. In the case of a tubular porous support, the size is not particularly limited, but examples include porous tubular supports having an outer diameter of about 3 mm to 20 mm, an inner diameter of about 1 mm to 15 mm, and a wall thickness of about 1 mm to 3 mm. The average pore diameter of the porous support is preferably in the range of 30 nm to 1000 nm, more preferably in the range of 50 nm to 500 nm, and further preferably in the range of 80 nm to 180 nm.
[0021] A preferred porous support having a two-layer structure is one in which a tubular α-alumina layer having an average pore diameter of 20 nm to 1000 nm, preferably 80 nm to 180 nm is used as support layer 12, and a γ-alumina layer having an average pore diameter of 1 nm to 20 nm, preferably 3 nm to 5 nm is used as intermediate layer 14 on the outer surface of tubular support layer 12.
[0022] The average pore size of the porous support can be determined by measuring the pore size distribution using a through-pore size evaluation device based on the ASTM F316-86 (JIS K 3832) bubble point method. Examples of devices used for the measurement include a Perm Porometer manufactured by Seika Digital Image Co., Ltd.
[0023] The thickness of the support layer 12 can be selected arbitrarily depending on the purpose. From the viewpoint of the balance between strength and gas permeability, the thickness of the support layer 12 can be, for example, 0.5 mm to 3 mm, and is preferably in the range of 1 mm to 2 mm. The thickness of the intermediate layer 14 can be, for example, 0.5 μm to 10 μm, and is preferably in the range of 1 μm to 5 μm.
[0024] The thicknesses of the support layer 12 and the intermediate layer 14 in the porous support 10 can be measured by platinum sputtering a cross section and observing it with a field emission scanning electron microscope (FE-SEM). An example of an FE-SEM device is JSM-6701F (manufactured by JEOL Ltd.). The acceleration voltage of the FE-SEM can be, for example, 10.0 kV.
[0025] There is no particular limitation on the method for providing the intermediate layer 14 on the support layer 12 as the porous support, and any known method for producing a porous layer can be appropriately applied. Among these, when the support layer 12 is made of a material with good heat resistance such as alumina, a method of coating an intermediate layer forming material containing boehmite sol described below on the support layer 12 and firing the material is preferred. According to the method of forming the intermediate layer 14 using the intermediate layer forming material containing boehmite sol, the intermediate layer 14 can be formed to any thickness by adjusting the coating amount of the intermediate layer forming material, the firing temperature, and further by performing coating and firing multiple times.
[0026] An example of a method for producing a porous support having a two-layer structure is to dip coat the outer surface of a tubular porous support layer made of α-alumina with boehmite sol, which is an intermediate layer forming material, two to three times, and then sinter the layer to form a γ-alumina intermediate layer having an average pore size of 3 nm to 5 nm. When coating the intermediate layer forming material onto the tubular support layer, it is preferable to perform a process such as sealing the ends of the tubular body so that the intermediate layer forming material does not penetrate into the inside of the tubular body, which is the support layer 12. Boehmite sol can be prepared, for example, by using aluminum s-butoxide (sometimes abbreviated as ALSB), 2-propanol, and gallium (III) nitrate octahydrate, or It can be produced by a conventional method using aluminum s-butoxide (ALSB), 2-propanol, and nitric acid.
[0027] (amorphous silica layer) The amorphous silica layer 20 has a function of selectively separating the fluorocarbon gas contained in the fluorocarbon mixed gas by molecular sieving, that is, according to the molecular diameter (molecular size). The amorphous silica layer 20 preferably has an amorphous structure in which siloxane bonds represented by -Si-O-Si- form a three-dimensional network. It is believed that the three-dimensionally formed network structure of silicon dioxide plays the role of a molecular sieve.
[0028] There is no particular limit to the thickness of the amorphous silica layer 20. If the amorphous silica layer as a molecular sieve membrane is thick, the fluorocarbon gas separation efficiency is good, but the gas permeability tends to be low. From this viewpoint, the thickness of the separation active region in the amorphous silica layer is, for example, 5 nm to 100 nm, and preferably in the range of 5 nm to 15 nm. Here, the separation active region in the amorphous silica layer refers to a region in the amorphous silica layer that is dense and contributes to the separation of fluorocarbon gas. It is presumed that the region of the amorphous silica layer formed inside the pores of the intermediate layer, which has a denser structure than the silica film formed on the surface of the intermediate layer, functions as a separation active region with higher separation activity for fluorocarbon gas, and this region is referred to as the separation active region in the amorphous silica layer. The separation active region in the amorphous silica layer can be confirmed as a region where Al2p increases and Si2p decreases from the elemental composition in the depth direction of the formed amorphous silica layer as a result of analysis by X-ray photoelectron spectroscopy (XPS) described later.
[0029] The thickness of the amorphous silica layer and the thickness of the separation active region in the amorphous silica layer are The amorphous silica layer in the gas separation member can be measured by performing elemental composition analysis by X-ray photoelectron spectroscopy (hereinafter, referred to as XPS) in the depth direction of the membrane from the surface opposite to the porous support side. In this disclosure, the elemental composition of the amorphous silica layer in the gas separation member can be measured by X-ray photoelectron spectroscopy (hereinafter, referred to as XPS) using an XPS VG ESCALAB 250 spe equipped with an Al Kα radiation source. The chamber pressure was 10 -8 The values measured at less than Pa and an etching rate of 0.05 nm / s can be used. The elements and electron orbitals analyzed by XPS are Si: 2p, Al: 2p, O: 1s, and C: 1s.
[0030] When the fluorocarbon mixed gas to be separated contains two types of fluorocarbon gases with different molecular diameters, the amorphous silica layer 20 preferably has an average pore diameter that is larger than that of the fluorocarbon gas with a relatively smaller molecular diameter and smaller than that of the fluorocarbon gas with a relatively larger molecular diameter. For example, when separating a mixed gas of R32 (molecular diameter: 0.363 nm) and R125 (molecular size 0.447 nm), if the average pore diameter of the pores formed by the network structure of silicon dioxide in the amorphous silica layer 20 is set to about 0.38 to 0.42 nm, R32 is likely to permeate, R125 is less likely to permeate, and the fluorocarbon mixed gas can be efficiently separated with a high gas selectivity. Even if the average pore diameter of the amorphous silica layer 20 is larger than the molecular diameter of R125, since R32 is more likely to permeate than R125, the average pore diameter of the amorphous silica layer 20 may be larger than the molecular diameter of R125.
[0031] Note that the pore diameter of the amorphous silica membrane used in the present disclosure has a distribution, and since the pore diameter is 1 nm or less, there is no quantitative pore diameter distribution measurement method. However, the pore diameter can be analytically estimated by the Normalized Knudsen-based permeance (NKP) method using the permeation data of single-component gas permeation. In the present disclosure, specifically, an amorphous silica membrane with an average pore diameter estimated to be 0.3 to 0.6 nm using the NKP method (200 °C) described in the following literature can be used. <Literature on the NKP method> Evaluation and fabrication of pore-size-tuned silica membranes with tetraethoxydimethyl disiloxane for gas separation Hye Ryeon Lee,Masakoto Kanezashi,Yoshihiro Shimomura,Tomohisa Yoshioka,Toshinori Tsuru AIChE Journal,57(10) 2755-2765(2011)
[0032] <Method of manufacturing molecular sieve membrane> The molecular sieve membrane used in the method for separating a fluorocarbon mixed gas of the present disclosure can be produced by a chemical vapor deposition (CVD) method. By using the CVD method, an amorphous silica layer 20 having high durability can be formed on a porous support 10.
[0033] The CVD method used to form the amorphous silica layer 20 includes, for example, a one-way diffusion CVD method in which a silica precursor derived from a silica source and an oxidizing agent, preferably oxygen, are supplied to one side of a porous support to form an amorphous silica layer, and a counter diffusion CVD method in which a silica precursor derived from a silica source is supplied to one side of a porous support and an oxidizing agent is supplied to the other side of the porous support. According to the counter diffusion CVD method, by maintaining equal pressure on both sides of the porous support, the silica precursor diffused in the pores of the porous support comes into contact with the oxidizing agent in the pores to generate amorphous silica, an amorphous silica layer is formed on the pore walls in the pores of the porous support, and the reaction automatically terminates when the pores are filled with the silica layer. In the pores that are not filled with the silica layer, the reaction between the silica precursor and oxygen continues. Therefore, the reaction continues until the pores are filled with the amorphous silica layer, and it becomes easy to obtain a high-performance amorphous silica layer with good reproducibility. That is, by the counter diffusion CVD method, an amorphous silica layer can be easily produced not only on the surface of the intermediate layer of the porous support having a double structure, which is the above-mentioned preferred embodiment, but also inside the pores of the intermediate layer.
[0034] For example, the amorphous silica layer 20 is formed by counter diffusion CVD, in which the porous support 10 is placed in a housing. Meanwhile, a silicon compound, which is a silica source, is placed in a bubbler and heated while supplying nitrogen gas, and the vapor of the silicon compound is supplied into the housing. The temperature inside the housing is set to 300°C to 650°C. The vapor of the silicon compound, which is a silica source inside the housing, is supplied to one side (e.g., the outer peripheral surface side) of the porous support, and oxygen is circulated to the other side (e.g., the inner peripheral surface side) to react the two inside the porous support. For example, when an amorphous silica layer is formed on the outer surface of a tubular porous support having a length of 10 mm to 100 mm, the concentration of the silicon compound vapor is set to about 0.93 mol / m 3 If the flow rate of oxygen is about 200 mL / min, a sufficient amount of amorphous silica layer is formed in about 60 minutes. Thereafter, the supply of the silicon compound vapor is stopped, the inside of the housing is purged with oxygen, the supply of oxygen is stopped, and nitrogen is supplied to the inside of the porous support for purging, thereby obtaining an amorphous silica layer.
[0035] Examples of chemical vapor deposition materials (silica sources) that can be used to manufacture the amorphous silica layer 20 include dimethoxydimethylsilane (DMDMS), tetraethylorthosilicate (TEOS), hexamethyldisiloxane (HMDS), tetramethylorthosilicate (TMOS), trimethyloxy(methyl)silicate (TMMS), methoxytrimethylsilicate (MTMS), phenyltrimethoxysilane (PTMS), dimethoxydiphenylsilane (DMDPS), triethoxyethylsilane, diethoxydiethylsilane, ethoxytriethylsilane, methoxytriphenylsilane, etc. Note that the abbreviation for the compound is written in parentheses following the compound name, and hereinafter each compound may be described by the abbreviation in parentheses.
[0036] The silica source is preferably DMDMS, TMOS, HMDS, TEOS, TMMS, MTMS, DMDPS, etc., and more preferably DMDPS. That is, the amorphous silica layer is more preferably an amorphous silica layer derived from a silica source containing DMDPS.
[0037] A method for producing a molecular sieve membrane for use in the method for separating a fluorocarbon mixed gas of the present disclosure preferably includes, for example, a step of forming an amorphous silica layer having an average pore diameter of, for example, 0.3 nm to 0.6 nm by a CVD method using a silica source containing dimethoxydiphenylsilane (DMDPS) on an aluminum oxide porous support having an average pore diameter of 30 nm to 1000 nm by an NKP method (200° C.). As described above, the porous support has a two-layer structure including at least a support layer 12 and an intermediate layer 14. Preferably, the support layer 12 is a porous body having an average pore diameter of 50 nm to 200 nm, and the intermediate layer 14 is a porous body having an average pore diameter of 3 nm to 5 nm. It is more preferable to form an amorphous silica layer 20 not only on the surface of the intermediate layer 14 but also within the pores of the intermediate layer 14 of the two-layer porous support 10 by a counter diffusion CVD method.
[0038] <Method for separating fluorocarbon mixed gases> Next, a method for separating a fluorocarbon mixed gas by the method for separating a fluorocarbon mixed gas according to the present disclosure will be described with reference to the drawings. Fig. 2 is a schematic diagram showing a gas separator, which is a main part of one embodiment of an apparatus for carrying out the fluorocarbon mixed gas separation method of the present disclosure. Fig. 3 is a schematic cross-sectional view taken along the line CC in Fig. 2. The gas separator 50 shown in FIG. 2 has a tubular gas separation member 30 disposed inside a tubular housing 32, and both ends of the gas separation member 30 are sealed by sealing members 33A and 33B. A pipe 28 is connected to the center of the sealing member 33B, which leads to the inside A of the gas separation member 30 and introduces the mixed gas x. Meanwhile, a pipe 28A is connected to the center of the sealing member 33B, which leads to the inside A of the gas separation member 30 and discharges gas that has passed through the gas separation member 30 without permeating it, and a pipe 28B is connected to the outer periphery of the sealing member 33B, which leads to the space B between the gas separation member 30 and the housing 32 and discharges gas that has permeated the gas separation member 30. The gas separation member 30 has the layer structure shown in FIG. 1, and a CVD amorphous silica layer (silica membrane) 20 is formed as a molecular sieve membrane in the outermost layer.
[0039] A vacuum pump (not shown) can be connected to pipe 28B for suction to promote gas permeation from molecular sieve membrane 20. In addition, the gas flow rate and pressure can be adjusted by providing valves (not shown) in each of pipes 28, 28A, and 28B. The diameter of pipe 28A exhausting from gas separation member 30 may be made smaller than that of pipe 28 for introducing the mixed gas, thereby increasing the pressure inside gas separation member 30 and promoting gas permeation from molecular sieve membrane 20.
[0040] When a gas separation device including a gas separator 50 having such a configuration is used to separate a fluorocarbon mixed gas, for example, a mixture of R125 and R32, the mixed gas x is supplied to the inside (inside A) of the gas separation member 30 through the pipe 28. While the mixed gas x passes through the gas separation member 30, it comes into contact with the amorphous silica layer 20 via the porous support 10, and at least a part of the R32, which has a relatively small molecular diameter, permeates the amorphous silica layer 20 and moves to the space B between the gas separation member 30 and the housing 32. As a result, a gas having a lower concentration of R32 than the mixed gas x before being introduced is discharged from the pipe 28A, and a gas having a higher concentration of R32 than the mixed gas x before being introduced is discharged from the pipe 28B. For example, a gas separation apparatus equipped with a plurality of gas separators 50 can be used, and the mixed gas x can be passed through the gas separators 50 a plurality of times to increase the separation efficiency. The gas separation apparatus according to the present disclosure can also perform multi-stage separation of the mixed gas x. By using the gas separation apparatus according to the present disclosure, a gas composition having an improved mixture ratio of one type of fluorocarbon gas or a single gas can be separated from a mixed gas containing two or more types of fluorocarbon gases having different molecular diameters. Alternatively, the mixed gas x may be supplied to the outside (space B) of the gas separation member 30, and at least a portion of the R32 having a relatively small molecular diameter may be permeated to the inside (inside A) of the gas separation member 30, so that a gas having a higher concentration of R32 than the mixed gas x before introduction is discharged from pipe 28A, and a gas having a lower concentration of R32 is discharged from pipe 28B.
[0041] Although the environment in which gas separation is performed by the fluorocarbon mixed gas separation method of the present disclosure is not particularly limited, the gas separation member 30 used in the present disclosure is made of an inorganic material and therefore has high heat resistance, and further, according to a fluorocarbon gas permeation experiment in the present disclosure described below, it was found that a higher gas selectivity was exhibited at 100°C to 200°C than at room temperature (e.g., 25°C). Therefore, it is preferable to perform gas separation in an environment of, for example, 20°C to 300°C. On the other hand, according to the fluorocarbon gas permeation experiment described later, the permeability hardly depends on the pressure. Therefore, it is preferable to perform gas separation under an environment with a pressure of 0.1 MPa or more.
[0042] In addition, the permeation amount of the gas to be separated is not particularly limited and may be set according to the type of gas, etc. For example, the permeation amount of R32 ([mol / (m 2 sPa)] is preferably 1.0×10 -4 ~1.0×10 -10 and more preferably 1.0×10 -5 ~1.0×10 -9 and more preferably 1.0×10 -6 ~1.0×10 -8 It is. EXAMPLES
[0043] The method for separating fluorocarbon mixed gases according to the present disclosure will be described in more detail below with reference to examples. However, the following examples do not limit the method for separating fluorocarbon mixed gases according to the present disclosure.
[0044] [Deposition of amorphous silica film] The amorphous silica film was formed by the following procedure. A Ga-doped γ-alumina intermediate layer was formed on the outer surface of a tubular α-alumina substrate by the sol-gel method. Then, amorphous silica was deposited inside the pores of the Ga-doped γ-alumina intermediate layer by counter diffusion CVD to form an amorphous silica film (hereinafter, sometimes referred to as a “silica film”). The following is a detailed description of the method.
[0045] (1) Preparation of porous support (base material) A tubular α-alumina substrate (manufactured by Noritake Co., Ltd.) was used as the substrate for the support layer. The specifications of the α-alumina substrate are shown in Table 1. Note that the "pore diameter" refers to the average pore diameter.
[0046] [Table 1]
[0047] The α-alumina substrate was cut to a total length of 120 mm using a diamond cutter, and both ends of 20 mm were glass sealed. The length of the amorphous film formed on the substrate was 80 mm, which was not glass sealed.
[0048] (γ-alumina coating) The γ-alumina coating was applied only to the outer surface of the substrate. The procedure was as follows: preparation of Ga-doped boehmite sol (hereinafter sometimes referred to as "boehmite sol"), preparation of the coating solution, dip coating, and calcination.
[0049] (Preparation of Ga-doped boehmite sol) The following reagents were prepared: Aluminum s-butoxide (ALSB) 500g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. 2-Propanol 500mL, Fujifilm Wako Pure Chemical Corporation Gallium(III) nitrate octahydrate 25g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0050] <Production procedure> A glove box (manufactured by AS ONE Corporation) was placed with ALSB, 2-propanol, a 50 mL beaker, a stirring bar, a pass pipette, a 100 mL dropping bottle, a nitrogen balloon, an electronic balance, and a stirrer, and then closed. The nitrogen balloon was prepared before closing the glove box.
[0051] The atmosphere in the glove box was replaced with nitrogen for 15 minutes. After replacing the atmosphere with nitrogen, 3.60 g (0.06 mol) of 2-propanol was added to the beaker to wet the inner wall of the beaker. 24.6 g (0.10 mol) of ALSB was added directly from the reagent bottle to a beaker whose walls were wetted with 2-propanol, and the mixture was stirred for 1 hour. 360 mL of pure water was placed in a 500 mL beaker and heated to 90°C on a hot stirrer. Pure water at 90°C was prepared next to the beaker to adjust the liquid level, and the 500 mL beaker was replenished with pure water as necessary. The mouths of each beaker were covered with aluminum foil when not in use. In a glove box, a mixture of ALSB and 2-propanol was placed in a 100 mL dropping bottle, and a nitrogen balloon was attached to the upper opening of the dropping bottle.
[0052] A dropping bottle with a nitrogen balloon attached was taken out of the glove box, and the pure water at 90°C that had been prepared on a hot stirrer was vigorously stirred, to which the mixture of ALSB and 2-propanol was added dropwise. The beaker was not covered with aluminum foil and the mixture was stirred at 90°C until the 2-propanol evaporated (until the smell of alcohol disappeared). The liquid volume was maintained at 340 mL. Add 17.14 g (0.04 mol) of gallium(III) nitrate octahydrate to 108 g (6 mol), the mouth of the beaker was covered with parafilm and stirred for at least 1 hour to prepare an aqueous gallium nitrate solution. After the 2-propanol had evaporated, the mixture was transferred to a 500 mL Erlenmeyer flask. If there was any white precipitate, this was also transferred as much as possible. The mouth of the Erlenmeyer flask was covered with aluminum foil and left to cool. After cooling, the gallium nitrate aqueous solution was slowly dripped into the mixture while stirring vigorously. After stirring for 12 hours or more, a boehmite sol was obtained, which was then stored in a plastic bottle.
[0053] (Preparation of coating solution) In addition to the boehmite sol prepared above, the following chemicals were prepared. 1mol / L nitric acid, 500mL, Fujifilm Wako Pure Chemical Corporation Polyvinyl alcohol 500, fully saponified, 500g, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0054] <Production procedure> 1) 47.5 mL of pure water and 2.5 mL of 1M-HNO3 were placed in a 50 mL measuring cylinder. This solution was transferred to a 100 mL Erlenmeyer flask and a stir bar was also placed in it. 2) 1.75 g of polyvinyl alcohol 500, fully saponified (PVA) was added to a 100 L Erlenmeyer flask while gently stirring to avoid foaming. 3) Because PVA is difficult to dissolve, the 100 mL Erlenmeyer flask was moved to a hot plate stirrer, the mouth of the Erlenmeyer flask was sealed with aluminum foil, and the flask was heated to 90°C while stirring. After 40 minutes, the mixture was left to cool while still stirring, completing the PVA solution. 4) 20 mL of the prepared PVA solution and 30 mL of boehmite sol were placed in a 50 mL beaker, a stirrer was placed inside, the mouth of the beaker was covered with parafilm, and the mixture was stirred for 15 minutes to complete the coating solution.
[0055] (Dip coating / baking) <Operation Procedure> 1) In order to coat only the outer surface of the substrate, the opening at one end of the substrate (the lower side when dipping) was sealed with sealing tape to prevent the coating solution from entering the inside of the substrate. 2) The coating solution was placed in a test tube, taking care not to introduce air bubbles, and the remaining coating solution was stored while stirring. A substrate with a total length of 120 mm was placed in the coating solution from the side sealed with sealing tape and dipped for 5 seconds. Care was taken not to touch the wall of the test tube when inserting or removing the substrate. 3) The dipped substrate was placed in an electric muffle furnace KM-600 (Advantec Co., Ltd.) and dried and fired using a specified temperature program (hold at 60°C for 3 hours, then heat to 600°C over 6 hours, hold for another 6 hours, then cool to room temperature over 6 hours). When placing the substrate in the electric muffle furnace, the glass seal part of the substrate was placed on the base so that it did not come into contact with the part to be coated. 4) Dip coating and firing (the above steps 2) to 3) were repeated three times to produce a porous support (hereinafter sometimes referred to as "γ / α-alumina substrate" or simply "substrate") in which a Ga-doped γ-alumina layer (intermediate layer) was formed on the outer peripheral surface of a tubular α-alumina substrate (substrate layer).
[0056] (2) Formation of an amorphous silica layer (silica film) An amorphous silica layer (silica film) was formed on the outer peripheral surface of the double-structure porous support (γ / α-alumina substrate) produced as described above by a counter diffusion CVD method. The schematic configuration of the apparatus 100 used for forming the silica membrane is shown in Fig. 4. The apparatus 100 shown in Fig. 4 includes gas tank 24 containing oxygen used for membrane formation, as well as gas tanks 13, 16, 18, and 22 containing R125, R32, H2, and N2 gases, and is configured so that each gas permeation test can be performed by adjusting valves 38 and the like provided on each pipe 28. MFC stands for mass flow controller. SUS pipes are used for the pipes 28. 3, gas separator 40 has a glass tube housing 32 disposed outside gas separation member 30, with space B provided for the passage of gas that has permeated gas separation member 30. An electric furnace 34 provided with a thermocouple 36 is disposed outside housing 32.
[0057] The glass seal portions of the substrate 10 at both ends exposed from the housing 32 were joined to SUS pipe joints using graphite ferrules (manufactured by GL Sciences Inc.) and unions (manufactured by Swagelok) 31A and 31B. Additionally, pressure gauges 44 and 48, a soap film flow meter 52, a pressure transducer 54, and a vacuum pump 58 are connected to each pipe 28.
[0058] When an amorphous silica layer was formed on a porous support (γ / α-alumina substrate) 10 using the apparatus 100 configured as described above, a silica precursor was placed in a bubbler 26, and nitrogen was supplied to the bubbler 26 at a flow rate of 200 mL / min to supply silica precursor vapor to the housing 32 by bubbling. A ribbon heater 42 was wrapped around the pipe 28 to prevent condensation of the precursor, and the pipe temperature was kept at 180° C. An ice-water cold trap 46 was used to collect unreacted precursor. The temperature of the bubbler 26 was controlled by wrapping it in a mantle heater (not shown).
[0059] The silica precursor vapor concentration before film formation was measured by trapping the silica precursor in the nitrogen carrier gas for a certain period of time in an ice water cold trap 46 using a gas line that does not pass through the housing 32, and measuring the silica precursor vapor concentration (mol / m 3 ) was calculated.
[0060] (Silica film formation by counter diffusion CVD method) As a precursor, DMDPS (dimethoxydiphenylsilane, manufactured by Tokyo Chemical Industry Co., Ltd.) represented by the following structural formula was used.
[0061] [ka]
[0062] The physical properties of DMDPS are shown in Table 2.
[0063] [Table 2]
[0064] <Film production procedure> The temperature controls of the electric furnace 34, ribbon heater 42, and bubbler 26, which are located outside the housing, were turned on. The furnace 34 was heated from room temperature to 600°C over 1.5 hours, and the ribbon heater 42 was set to 180°C. After all temperatures were stabilized, an ice-water cold trap 46 was prepared. The DMDPS vapor concentration was measured using a gas line that did not pass through the housing 32, and the DMDPS vapor concentration was found to be about 0.08 mol / m 3 The bubbler temperature was adjusted so that it was around this temperature. After adjusting the bubbler temperature, DMDPS vapor was supplied to the housing 32 (outer side B of the substrate), and after 2 minutes, oxygen was circulated at 200 mL / min to the inner side A of the substrate to start film formation. After 60 minutes, the supply of DMDPS vapor was stopped, and nitrogen was circulated at full flow rate to the outside B of the substrate, and oxygen was circulated at 200 mL / min to the inside A of the substrate, to purge the inside of the housing 32. After one hour, the supply of oxygen was stopped, and nitrogen was purged into the inside A of the substrate at full flow rate for several minutes to complete the deposition.
[0065] <Gas permeability evaluation> (Single component gas permeation test 1) After the silica membrane was formed, a gas permeation test was carried out using an apparatus 100 shown in FIG. Gas was supplied to the supply side (outside the substrate), and pressure was applied to the supply side by closing the valve 38B at the membrane outlet. The supply side pressure at this time was set to 0.20 to 0.40 MPa, and the gas was permeated by a dead-end method in which the transmembrane pressure difference was 0.20 to 0.40 MPa, and the flow rate of the permeated gas obtained from the permeation side was measured using a bubble flowmeter (BFM) 52 (manufactured by HORIBA). Normally, when the permeation side gas flow rate was large, it was measured using the BMF 52. When the permeation side gas flow rate was small and could not be measured using the BMF, the permeation side gas flow rate was measured using the pressure change method. In the pressure change method, the supply side pressure was set to 0.20 MPa, and the permeation side was evacuated for 2 hours using an oil rotary vacuum pump 58 (manufactured by ULVAC, Inc.), giving a transmembrane pressure difference of about 0.35 MPa. When gas was supplied to the supply side, permeation occurred, and the pressure on the permeation side began to rise. By measuring the pressure over time, the pressure rise rate was measured, and the permeation gas flow rate was calculated from the permeation side volume.
[0066] (temperature dependence) The temperature dependence of the permeability of H2, N2, HFC-32, and HFC-125 for a silica membrane with a membrane length of 80 mm formed on a Ga-doped gamma / alpha-alumina substrate is shown in Figure 5. In Figure 5, "E" on the vertical axis means a power of 10. For example, "E-10" means "10 -10 The temperature dependence of the ideal selectivity is shown in Figure 6. According to the above-mentioned NKP method (200°C), the average pore size of the silica membrane is considered to be about 0.40 to 0.55 nm, which is suitable for separating HFC-32 and HFC-125. The transmittance and transmittance ratio of HFC-32 and HFC-125 at 200°C, 100°C, and 25°C are shown in Table 3 below.
[0067] [Table 3]
[0068] The ideal selectivity calculated as the HFC-32 permeability / HFC-125 permeability was 1026 at 200°C, 1623 at 100°C, and 617 at 25°C. For reference, the ideal selectivity calculated by the ratio of H2 permeability to N2 permeability was about 10 at all temperatures. This also shows that this method is particularly suitable for separating HFC-32 and HFC-125.
[0069] (Single component gas permeation test 2) After forming the silica membrane, a gas permeation test was performed using the apparatus 100 shown in FIG. 4. Gas was supplied to the supply side (outside the substrate) and pressure was applied to the supply side by closing the valve 38B at the membrane outlet. The supply side pressure was set to 0.20 to 0.60 MPa, and the gas was permeated by a dead-end method with a transmembrane pressure difference of 0.10 to 0.50 MPa, and the flow rate of the permeated gas obtained from the permeation side was measured using a bubble flowmeter (BFM) 52 (manufactured by HORIBA). Normally, when the permeation side gas flow rate is large, it is measured using the BMF 52. When the permeation side gas flow rate is small and cannot be measured using the BMF, the permeation side gas flow rate was measured using the pressure change method. In the pressure change method, the supply side pressure was set to 0.20 to 0.60 MPa, and the permeation side was evacuated for 2 hours using an oil rotary vacuum pump 58 (manufactured by ULVAC, Inc.), giving a transmembrane pressure difference of about 0.20 to 0.60 MPa. When gas is supplied to the supply side, permeation occurs and the pressure on the permeation side begins to rise. The pressure was measured over time to determine the rate of pressure rise, and the permeation gas flow rate was calculated from the volume of the permeation side. The relationship between the feed pressure and the permeability for HFC-32 and HFC-125 at 200℃, 100℃, and 25℃ are shown in Figures 7, 8, and 9, respectively. At any of the temperatures tested, no significant difference due to pressure differences (pressure dependency) was observed in the permeability of HFC-32 and HFC-125. [Industrial Applicability]
[0070] The method for separating fluorocarbon mixed gases according to the present disclosure can achieve energy-saving separation compared to separation by distillation, and is expected to have a large economic effect. It can also contribute to regulations on refrigerant gases, which have been pointed out to have a greenhouse effect 100 times greater than that of carbon dioxide. [Explanation of symbols]
[0071] 10 Porous support 13,16,18,22 Gas tank 12 Support layer 14 Middle Class 20 Amorphous silica layer (molecular sieve membrane) 24 Gas Tank 26 Bubbler 28, 28A, 28B Piping 30 Gas separation material 32 Case 33A,33B Sealing member 34 Electric furnace 36 Thermocouple 38,38B Valve 40 Gas separator 42 Ribbon heater 44 Pressure Gauge 46 Ice water cold trap 50 Gas separator 52 Soap film flowmeter 54 Pressure Transducer 58 Vacuum Pump 100 Film-forming equipment and gas permeation test equipment
Claims
1. A method for separating a fluorocarbon mixed gas, comprising a gas separation step of contacting a mixed gas containing two or more fluorocarbon gases having different molecular diameters with a molecular sieve membrane containing amorphous silica formed by a chemical vapor deposition method, thereby separating the mixed gas into gases having different mixing ratios from the mixed gas.
2. 2. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the molecular sieve membrane is an amorphous silica membrane having a structure containing --Si--O--Si-- bonds.
3. 2. The method for separating fluorocarbon mixed gases according to claim 1, wherein the gas separation step is carried out in an environment of 20°C to 300°C.
4. 2. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the gas separation step is carried out in an environment of 0.1 MPa or more.
5. 2. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the molecular sieve membrane is a molecular sieve membrane formed by using dimethoxydiphenylsilane as a chemical vapor deposition material in the chemical vapor deposition method.
6. 2. The method for separating fluorocarbon mixed gases according to claim 1, wherein the chemical vapor deposition method is a counter diffusion method.
7. 2. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the molecular sieve membrane is formed on a porous support made of ceramics.
8. 8. The method for separating a fluorocarbon mixed gas according to claim 1, wherein the fluorocarbon mixed gas is a mixed gas of difluoromethane and pentafluoroethane.
9. A separation device equipped with a porous membrane containing amorphous silica formed by a chemical vapor deposition method, which separates a gas composition in which a mixture ratio of one fluorocarbon gas is increased from a mixed gas containing two or more fluorocarbon gases having different molecular diameters, or a single gas.
Citation Information
Patent Citations
Method for separating and recovering flon
JP1989042444A