Polarization film with pressure sensitive adhesive sheet, optical laminate and image display device

The optical film with a specific gel fraction and sol component composition addresses peeling issues in high-temperature environments, ensuring image quality in image display devices by enhancing adhesion.

JP2024146807AActive Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024039512
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-15
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Photocurable adhesive sheets used in image display devices experience image quality deterioration due to peeling at high temperatures, particularly when exposed to high-temperature environments.

Method used

An optical film with a photocurable adhesive sheet having a gel fraction of 55% to 94% and a sol component with a weight average molecular weight of 100,000 or less comprising less than 6.6% by weight, along with specific molecular weight ranges for the polymer and sol components, is developed to enhance adhesion and reduce peeling.

Benefits of technology

The solution provides an optical film with improved adhesion and reduced peeling in high-temperature environments, maintaining image quality in image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146807000001_ABST
    Figure 2024146807000001_ABST
Patent Text Reader

Abstract

To provide an optical film with a pressure sensitive adhesive sheet that is suitable for use in an image display device exposable to high temperature environments while having a photo-curable pressure sensitive adhesive sheet.SOLUTION: An optical film with a pressure sensitive adhesive sheet includes a photo-curable pressure sensitive adhesive sheet and an optical film. The gel fraction of the pressure sensitive adhesive sheet is 55% or more and less than 94%; the content of a sol part A having a weight average molecular weight of 100,000 or less in the pressure sensitive adhesive sheet is less than 6.6 wt.%; the content of the sol part A may be 5.8 wt.% or less and further 4.9 wt.% or less; and the pressure sensitive adhesive sheet may be acrylic.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing film with a pressure-sensitive adhesive sheet, an optical laminate, and an image display device. [Background technology]

[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is usually used for bonding between the optical films included in the optical laminate and bonding between the optical laminate and an image display panel. A typical adhesive sheet is a sheet obtained by curing a monomer group including an acrylic monomer, a silicone monomer, etc., by polymerization and crosslinking. Patent Document 1 discloses an adhesive sheet-attached polarizing film including an adhesive sheet (hereinafter, referred to as a photocurable adhesive sheet) formed from a photocurable composition and a polarizing film as an optical film. Note that, as a type of adhesive sheet different from the photocurable type, there is a thermosetting adhesive sheet formed by curing a layer including an adhesive composition and a solvent by heat. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-56510 Summary of the Invention [Problem to be solved by the invention]

[0004] When a photocurable pressure-sensitive adhesive sheet is used in an optical film with a pressure-sensitive adhesive sheet, problems tend to occur in the quality of images produced in image display devices that may be exposed to high-temperature environments.

[0005] An object of the present invention is to provide an optical film with a pressure-sensitive adhesive sheet, which is equipped with a photocurable pressure-sensitive adhesive sheet and is suitable for use in an image display device that may be exposed to a high-temperature environment. [Means for solving the problem]

[0006] The present invention relates to The optical film is a photocurable adhesive sheet. The pressure-sensitive adhesive sheet has a gel fraction of 55% or more and less than 94%, The content of sol component A having a weight average molecular weight of 100,000 or less in the pressure-sensitive adhesive sheet is less than 6.6% by weight. Optical film with adhesive sheet, to provide.

[0007] Further, the present invention relates to There is provided an optical laminate comprising the above-mentioned optical film with a pressure-sensitive adhesive sheet.

[0008] Further, the present invention relates to The present invention provides an image display device including the above-mentioned optical film with a pressure-sensitive adhesive sheet. Effect of the Invention

[0009] According to the present invention, it is possible to provide an optical film with a photocurable pressure-sensitive adhesive sheet, which is suitable for use in an image display device that may be exposed to a high-temperature environment. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of an optical film with a pressure-sensitive adhesive sheet of the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining one example of a method for forming a pressure-sensitive adhesive sheet that can be provided in the pressure-sensitive adhesive sheet-attached optical film of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 4] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 6] FIG. 1 is a cross-sectional view that illustrates an example of an image display device of the present invention. [Figure 7]1 is a graph showing the relationship between the gel fraction and the content of sol fraction A having a weight-average molecular weight of 100,000 or less in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The optical film with a pressure-sensitive adhesive sheet according to the first aspect of the present invention is The optical film is a photocurable adhesive sheet. The pressure-sensitive adhesive sheet has a gel fraction of 55% or more and less than 94%, The content of sol component A having a weight average molecular weight of 100,000 or less in the pressure-sensitive adhesive sheet is less than 6.6% by weight.

[0012] In a second aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the first aspect, the content of the sol component A is 5.8% by weight or less.

[0013] In a third aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the first aspect, the content of the sol component A is 4.9% by weight or less.

[0014] In a fourth aspect of the present invention, for example, in an optical film with an adhesive sheet according to any one of the first to third aspects, the weight average molecular weight of the polymer contained in the adhesive sheet is 700,000 or more and less than 800,000, and the weight average molecular weight of all sol components B contained in the adhesive sheet is 600,000 or more, or the weight average molecular weight of the polymer is 800,000 or more, and the weight average molecular weight of the sol components B is 450,000 or more.

[0015] In a fifth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to fourth aspects, the pressure-sensitive adhesive sheet contains a (meth)acrylic polymer.

[0016] In a sixth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the fifth aspect, the (meth)acrylic polymer has a constituent unit derived from a carboxyl group-containing monomer.

[0017] In a seventh aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to the fifth or sixth aspect, the (meth)acrylic polymer has a constitutional unit derived from a nitrogen atom-containing monomer.

[0018] In an eighth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to seventh aspects, the pressure-sensitive adhesive sheet contains a silane coupling agent.

[0019] In a ninth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to eighth aspects, the pressure-sensitive adhesive sheet has a thickness of 50 μm or less.

[0020] In a tenth aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to ninth aspects, the pressure-sensitive adhesive sheet has a solvent content of 5 wt % or less.

[0021] In an eleventh aspect of the present invention, for example, in the optical film with a pressure-sensitive adhesive sheet according to any one of the first to tenth aspects, the pressure-sensitive adhesive sheet and the optical film are in contact with each other.

[0022] In a twelfth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet-attached optical film according to any one of the first to eleventh aspects, the optical film is a polarizing film.

[0023] An optical laminate according to a thirteenth aspect of the present invention comprises an optical film with a pressure-sensitive adhesive sheet according to any one of the first to twelfth aspects.

[0024] An image display device according to a fourteenth aspect of the present invention includes the pressure-sensitive adhesive sheet-attached optical film according to any one of the first to twelfth aspects.

[0025] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention.

[0026] [Optical film with adhesive sheet] An example of an optical film with an adhesive sheet of this embodiment is shown in FIG. 1. The optical film with an adhesive sheet 11 in FIG. 1 includes an adhesive sheet 1 and an optical film 2. The adhesive sheet 1 and the optical film 2 are in contact with each other. The adhesive sheet 1 is a photocurable adhesive sheet formed from a photocurable composition. The gel fraction of the adhesive sheet 1 is 55% or more and 94% or less. The content of sol fraction (sol fraction A) having a weight average molecular weight (hereinafter referred to as Mw) of 100,000 or less in the adhesive sheet 1 is less than 6.6% by weight. The gel fraction is based on weight.

[0027] Through the study by the present inventors, it has been found that one of the factors that causes deterioration of image quality due to exposure to a high-temperature environment is that the adhesive sheet in the optical laminate and the adherend (object to be adhered) in contact therewith tend to peel off at high temperatures. For the adhesive sheet 1, it is estimated that satisfying both of the above-mentioned ranges of gel fraction and content of sol fraction A contributes to making the balance of the stress relaxation properties and cohesive force of the adhesive sheet 1 suitable for suppressing the above-mentioned peeling at high temperatures and to suppressing segregation of the sol fraction near the interface between the adhesive sheet 1 and the adherend. It is considered that the area where the sol fraction, especially the sol fraction A having an Mw of 100,000 or less, is segregated is relatively prone to destruction at high temperatures. An example of the adherend is a glass substrate.

[0028] The lower limit of the gel fraction of the pressure-sensitive adhesive sheet 1 may be 56% or more, 57% or more, 58% or more, 59% or more, or even 60% or more. The upper limit of the gel fraction may be 93.5% or less, 93% or less, 92.5% or less, 92% or less, 91.5% or less, 91% or less, 90.5% or less, or even 90% or less.

[0029] The gel fraction of the adhesive sheet 1 can be evaluated as follows. A test piece of about 0.1 g is taken from the adhesive sheet 1, wrapped in a polytetrafluoroethylene porous sheet (average pore size 0.2 μm, product name "NTF1122", manufactured by Nitto Denko Corporation), and then tied with a kite string to obtain a measurement sample. Next, the weight of the obtained measurement sample (weight C before immersion) is measured. The weight C before immersion is the total weight of the test piece, the polytetrafluoroethylene porous sheet, and the kite string. Separately from this, the bag weight B, which is the total weight of the polytetrafluoroethylene porous sheet and the kite string, is measured. Next, the measurement sample is placed in a container with a volume of 50 mL filled with ethyl acetate and left to stand at 23 ° C for 7 days. After standing, the measurement sample is taken out of the container and transferred to an aluminum cup, and the ethyl acetate is removed by drying at 130 ° C for 2 hours using a dryer. The weight of the measurement sample after drying (weight A after immersion) is measured. The value calculated from the following formula is specified as the gel fraction of the adhesive sheet 1. Gel fraction (%) = (AB) / (CB) x 100

[0030] The content of the sol component A in the pressure-sensitive adhesive sheet 1 may be 6.5% by weight or less, 6.3% by weight or less, 6.0% by weight or less, 5.8% by weight or less, 5.5% by weight or less, 5.3% by weight or less, 5.0% by weight or less, 4.9% by weight or less, 4.5% by weight or less, 4.3% by weight or less, 4.1% by weight or less, 4.0% by weight or less, 3.8% by weight or less, 3.7% by weight or less, 3.6% by weight or less, 3.5% by weight or less, 3.3% by weight or less, 3.0% by weight or less, 2.8% by weight or less, 2.5% by weight or less, 2.4% by weight or less, 2.3% by weight or less, 2.2% by weight or less, 2.1% by weight or less, or even 2.0% by weight or less. The lower limit of the content is not particularly limited, and may be, for example, 0.0% by weight or more, 0.05% by weight or more, 0.1% by weight or more, or even 0.2% by weight or more.

[0031] In this specification, the sol content refers to a component that can be extracted from the pressure-sensitive adhesive sheet 1 by ethyl acetate. The sol content A refers to a component having an Mw of 100,000 or less among all the sol contents (sol content B) contained in the pressure-sensitive adhesive sheet 1. The content (wt %) of sol content B in the pressure-sensitive adhesive sheet 1 can be specified as 100-gel fraction (%).

[0032] The content of sol content A in the pressure-sensitive adhesive sheet 1 can be evaluated by gel permeation chromatography (GPC) as follows. A portion of the pressure-sensitive adhesive sheet 1 is dissolved in a GPC eluent to prepare a solution with a sol content concentration of about 2.0 g / L. A GPC eluent that does not substantially dissolve the gel content in the pressure-sensitive adhesive sheet 1 but dissolves the sol content is selected. The prepared solution is left overnight and then filtered through a 0.45 μm membrane filter. GPC measurement is performed on the filtrate, and the ratio X of components with Mw of 100,000 or less is calculated. The value calculated from the following formula can be specified as the content of sol content A in the pressure-sensitive adhesive sheet 1. Content of sol A (wt%) = Content of sol B (wt%) × X / 100

[0033] The gel fraction and the content of sol fraction A in the pressure-sensitive adhesive sheet 1 can vary depending on, for example, the composition of the photocurable composition used to form the pressure-sensitive adhesive sheet 1 and the curing conditions of the photocurable composition. Examples of the composition are the type and content of each monomer constituting the monomer group contained in the photocurable composition, the type and content of the photopolymerization initiator, and the type and content of the crosslinking agent. Examples of the curing conditions are the integrated light amount of the irradiated light, the type of light source, the wavelength distribution, and the thickness of the coating film of the photocurable composition irradiated with light.

[0034] <Adhesive sheet> (Photocurable composition) The adhesive sheet 1 is formed from a photocurable composition. The photocurable composition usually contains a monomer group and / or a partial polymer of the monomer group. By irradiating the photocurable composition with light, a polymer is generated from the monomer group and / or the partial polymer, and the adhesive sheet 1 is formed. The generated polymer is usually the main component of the adhesive sheet 1. The monomer group may contain a (meth)acrylic monomer. The content of the (meth)acrylic component in the photocurable composition, i.e., the (meth)acrylic monomer and its partial polymer, may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic adhesive sheet containing a (meth)acrylic polymer can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic means acrylic and methacrylic. (Meth)acrylate means acrylate and methacrylate. In this specification, the main component means the component with the largest content. The content of the main component is, for example, 50% by weight or more, and may be 60% by weight or more, 70% by weight or more, or even 80% by weight or more.

[0035] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate and octadecyl (meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl (meth)acrylate.

[0036] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.

[0037] The monomer group may contain a carboxyl group-containing monomer. In this case, the (meth)acrylic polymer that the pressure-sensitive adhesive sheet 1 may contain has a constituent unit derived from the carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of the carboxyl group-containing monomer are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content is, for example, 0.1% by weight or more, and may be 0.5% by weight or more, 1% by weight or more, 1.5% by weight or more, 2% by weight or more, 2.5% by weight or more, 3% by weight or more, 3.5% by weight or more, 4% by weight or more, or even 4.5% by weight or more. The monomer group does not need to contain a carboxyl group-containing monomer.

[0038] The monomer group may contain a hydroxy group-containing monomer. In this case, the (meth)acrylic polymer that the pressure-sensitive adhesive sheet 1 may contain has a constituent unit derived from a hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxy group-containing monomer. Examples of the hydroxy group-containing monomer are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxyl group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxyl group-containing monomer.

[0039] The monomer group may contain a nitrogen atom-containing monomer. In this case, the (meth)acrylic polymer that the pressure-sensitive adhesive sheet 1 may contain has a constituent unit derived from the nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule). In this specification, a monomer having a hydroxyl group and a nitrogen atom in the molecule is classified as a nitrogen atom-containing monomer. A monomer having a carboxyl group and a nitrogen atom in the molecule is classified as a carboxyl group-containing monomer.

[0040] The nitrogen atom-containing monomer is preferably N-vinyl cyclic amide, (meth)acrylamide, etc. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.

[0041] The N-vinyl cyclic amide is preferably represented by the following formula (A). [ka]

[0042] In formula (A), R 1 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 1 are directly bonded via a single bond to form a ring structure.

[0043] As the N-vinyl cyclic amide represented by formula (A), N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, more preferably N-vinyl-2-pyrrolidone, N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.

[0044] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamide include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nn-butyl(meth)acrylamide, N-octylacrylamide, etc. Examples of N-alkyl(meth)acrylamides include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.

[0045] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.

[0046] (Meth)acrylamides also include, for example, various N-hydroxyalkyl (meth)acrylamides. Examples of N-hydroxyalkyl (meth)acrylamides include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, and N-methyl-N-2-hydroxyethyl (meth)acrylamide.

[0047] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.

[0048] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocyclic ring-containing monomers such as vinylpyrrolidone; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and other imide group-containing monomers; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.

[0049] The content of the nitrogen atom-containing monomer in the monomer group may be, for example, 40% by weight or less, 35% by weight or less, or even 30% by weight or less. The lower limit of the content may be, for example, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.

[0050] The monomer group preferably includes a carboxyl group-containing monomer and / or a nitrogen atom-containing monomer, and more preferably includes both a carboxyl group-containing monomer and a nitrogen atom-containing monomer. When a nitrogen atom-containing monomer, particularly both a nitrogen atom-containing monomer and a carboxyl group-containing monomer, are present in a photopolymerization system, the molecular weight of the polymer tends to increase. The above tendency may be due to the fact that the viscosity of the polymerization system increases due to the formation of hydrogen bonds, which suppresses the termination reaction between the growing ends of the polymer, making it easier for the monomer to remain at the end of the growing chain. The increase in the molecular weight of the polymer may contribute to an excellent balance between the stress relaxation property and the cohesive force in the adhesive sheet 1. In addition, in a thermosetting adhesive composition, since the monomer is dispersed in the solvent, hydrogen bonds are unlikely to occur, and chain transfer of radicals to the solvent also occurs frequently, so the above-mentioned action of the nitrogen atom-containing monomer is not observed.

[0051] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.

[0052] The photocurable composition usually contains a photopolymerization initiator. An example of the photopolymerization initiator is a photoradical generator that generates radicals by irradiation with light. The photopolymerization initiator has an absorption coefficient for light of 340 nm, for example, of 0.1 L / (g·cm) or more, and may be 0.5 L / (g·cm) or more, 1.0 L / (g·cm) or more, 3.0 L / (g·cm) or more, or even 5.0 L / (g·cm) or more. The upper limit of this absorption coefficient is not particularly limited, and is, for example, 50 L / (g·cm) or less. The absorption coefficient of the photopolymerization initiator is a calculated value from the absorbance of a 0.01 mg / mL methanol solution measured by a visible-ultraviolet spectrophotometer using a quartz cell with a path length of 1 cm.

[0053] Examples of photopolymerization initiators include benzoin ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; substituted benzoin ethers such as anisole methyl ether; substituted acetophenones such as 2,2-diethoxyacetophenone and 2,2-dimethoxy-2-phenylacetophenone; α-hydroxyalkylphenones such as 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, and 2,2'-dihydroxy-2,2'-dimethyl-1,1'-[methylenebis(4,1-phenylene)]bis(propan-1-one); and substituted alpha alkyl phenones such as 2-methyl-2-hydroxypropiophenone. -ketols; aromatic sulfonyl chlorides such as 2-naphthalenesulfonyl chloride; photoactive oximes such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and 2,4-diethylthioxanthone;2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, 2,4-trichloromethyl- triazine-based compounds such as (4'-methoxystyryl)-6-triazine; oxime ester-based compounds such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], O-(acetyl)-N-(1-phenyl-2-oxo-2-(4'-methoxy-naphthyl)ethylidene)hydroxylamine; phosphine-based compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; quinone-based compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate-based compounds; carbazole-based compounds; imidazole-based compounds; and titanocene-based compounds. The photocurable composition may contain one or more photopolymerization initiators. In addition, α-hydroxyalkylphenones tend to have high absorption of light with a wavelength of 340±10 nm.

[0054] Another example of the photopolymerization initiator is a compound having a chemical structure shown in the following formula (1) (hereinafter, referred to as chemical structure X) in the molecule. [ka]

[0055] R in the above formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR51 , -OOCR 52 , or -NR 53 R 54 an alkyl group having 1 to 4 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R; an alkenyl group having 3 to 6 carbon atoms, the hydrogen atom of which is replaced by -CH2-C6H4-R 55 R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group. 51 is an alkyl group having 1 to 8 carbon atoms. 52 is a C1 to C4 alkyl group. 53 and R 54 are each independently a hydrogen atom, a C1-C12 alkyl group; -OH, a C1-C4 alkoxy group, -CN and -COOR 59 R is a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 53 and R 54 are bonded to each other to form -O- or -N(R 60 R may be a C3 to C9 alkylene group optionally interrupted by -. 55 is a C1 to C4 alkyl group. 59 is a C1 to C4 alkyl group. 60 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 61 Or -CH2CH2CN. 61 is a C1 to C4 alkyl group.

[0056] X is -OR 56 , or -NR 57 R 58 R 56 is a hydrogen atom, -SiR 62 3. A C1 to C8 alkyl group or a C3 to C6 alkenyl group. R 57 and R 58 represents an alkyl group having 1 to 12 carbon atoms; -OH, an alkoxy group having 1 to 4 carbon atoms, -CN and -COOR63 R is a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 57 and R 58 are bonded to each other to form -O- or -N(R 64 R may be a C3 to C9 alkylene group optionally interrupted by -. 62 is a C1 to C6 alkyl group. 63 is a C1 to C4 alkyl group. 64 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 65 Or -CH2CH2CN. 65 is a C1 to C4 alkyl group.

[0057] The chemical structure X can be bonded to a hydrogen atom or a structure substituted with a hydrogen atom via the carbon atom indicated by * in formula (1).

[0058] The alkyl group, alkoxy group, alkenyl group, alkylene group, oxyalkylene group, azaalkylene group, and hydroxyalkyl group described in the explanation of formula (1) may be unbranched or branched. In addition, the description of "Cn1 to Cn2" (n1 and n2 are natural numbers) in this specification, including the explanation of formula (1), means that the number of carbon atoms is in the range of n1 to n2.

[0059] R 1 and R 2 may be, independently of each other, a C1 to C8 alkyl group, a C3 to C6 alkenyl group, or a C1 to C8 alkyl group. 1 and R 2 may be, independently of each other, a C1 to C4 alkyl group, a C1 to C3 alkyl group, or a C1 to C2 alkyl group. 1 and R 2 may be a methyl group.

[0060] R 1and R 2 may be identical.

[0061] X is -OR 56 R 56 may be a hydrogen atom or a C1 to C8 alkyl group, or may be a hydrogen atom In other words, X may be -OH.

[0062] R 1 , R 2 and X may be any combination of the preferred examples above.

[0063] The chemical structure X may be a structure shown in the following formula (2). In the chemical structure X of formula (2), when a hydrogen atom substitution structure is bonded to the carbon atom indicated by *, the substitution structure and -COCR in formula (2) may be bonded to each other. 1 XR 2 The group is in a para-position relationship with respect to the benzene ring of the chemical structure X. [ka]

[0064] The photopolymerization initiator may be a compound having two or more chemical structures X in one molecule.

[0065] The photopolymerization initiator may be a compound represented by the following formula (3). The compound of formula (3) has two chemical structures X in one molecule. The two chemical structures X are located at both ends of the molecule of the photopolymerization initiator, respectively. More specifically, the two chemical structures X are bonded to each other by -A- at the carbon atom of the phenylene group represented by * above. [ka]

[0066] R in Equation (3) 1 ' and R 2 ' are each other and R 1 and R 2 Independently of R 1 and R2 R is a possible group. 1 ' and / or R 2 ' is R 1 and / or R 2 It may be the same as R 1 , R 2 , R 1 ' and R 2 ' may all be the same.

[0067] X' in formula (3) is a possible group for X, independent of X in formula (1). X' and X may be the same.

[0068] A is -O-, -CYR 3 - or -C(CH3)R 4 It is.

[0069] Y is a hydrogen atom, -Cl, -Br, -OR 71 , -NR 72 R 73 , or -SR 74 R 3 is a hydrogen atom, an alkyl group having C1 to C8, an alkenyl group having C3 to C6, a benzyl group, -CH2-C6H4-R 75 or a phenyl group. 4 is a C1 to C6 alkyl or alkylene group, and this alkylene group is bonded to a carbon atom of the phenylene group that the compound of formula (3) has.

[0070] R 71 is a hydrogen atom, -Si(R 76 )3, C1-C12 alkyl groups, C2-C18 acyl groups, -CO-NH-R 77 , C2-C20 hydroxyalkyl group, C2-C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms. 72and R 73 are each independently a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, or -COOR 79 a C2-C4 alkyl group, in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group. R 72 and R 73 are bonded to each other to form -O- or -N(R 80 R may be a C3 to C9 alkylene group optionally interrupted by -. 74 is an alkyl group having C1 to C18, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, an alkylphenyl group having C1 to C12, -CH2-COOR 81 -CH2CH2-COOR 82 or -CH(CH3)-COOR 83 R 75 is a C1 to C4 alkyl group. 76 is a C1 to C6 alkyl group. 77 is a C1 to C12 alkyl group. 78 is a C1 to C18 alkoxy group. 79 is a C1 to C4 alkyl group. 80 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a benzyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 84 , or -CH2CH2CN. 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group. 84 is a C1 to C4 alkyl group.

[0071] The alkyl group, alkenyl group, acyl group, hydroxyalkyl group, methoxyalkyl group, alkoxy group, alkyl moiety in the phenylalkyl group, and alkylene group described in the explanation of formula (3) may be either unbranched or branched.

[0072] R in Equation (3) 1 , R 2 , R 1 ' and R 2 Preferred examples of R 1 and R 2 The preferred examples of X' in formula (3) are the same as the preferred examples of X described above in the explanation of formula (1). A is -CYR 3 Y may be a hydrogen atom. 3 may be a hydrogen atom. 3 - and Y and R 3 and may both be hydrogen atoms. In other words, A may be -CH2-.

[0073] R in Equation (3) 1 , R 2 , R 1 ', R 2 X′, X′, and A may take any combination of the preferred examples above.

[0074] The photopolymerization initiator may be a compound represented by the following formula (4): The compound of formula (4) is a type of compound of formula (3). [ka]

[0075] Specific examples of the photopolymerization initiator are shown in the following formulas (5) to (9). The photopolymerization initiator may be a compound represented by at least one formula selected from the group consisting of formulas (5) to (9), a compound represented by at least one formula selected from the group consisting of formulas (5) to (8), a compound represented by at least one formula selected from the group consisting of formulas (5) to (7), or a compound represented by formula (5). The compound represented by formula (8) is derived from a vinyl compound having a chemical structure X in its side chain. More specifically, it is an oligomer of the vinyl compound.

[0076] [ka]

[0077] [ka]

[0078] [ka]

[0079] [ka]

[0080] [ka]

[0081] The photopolymerization initiators represented by the formulas (5) to (9) are commercially available as Omnirad127, Esacure KIP160, Esacure one, Esacure KIP150, and Omnirad1173 (all manufactured by IGM Resins). The photopolymerization initiator may be at least one selected from these groups.

[0082] Specific examples of photopolymerization initiators include 1-hydroxycyclohexyl-phenyl ketone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one. Among these, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one is preferred. Each of the above photopolymerization initiators is commercially available as Omnirad184, Omnirad819, and Omnirad127 (all manufactured by IGM Resin).

[0083] The amount of the photopolymerization initiator in the photocurable composition is, for example, 20 parts by weight or less, and may be 10 parts by weight or less, 5.0 parts by weight or less, 3.0 parts by weight or less, 1.0 parts by weight or less, 0.5 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, 0.2 parts by weight or less, 0.15 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, based on 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount is, for example, 0.01 parts by weight or more, and may be 0.03 parts by weight or more, based on 100 parts by weight of the total of the monomer group and its partial polymer.

[0084] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. An example of the polyfunctional monomer is a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.

[0085] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N DDA), 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and other polyfunctional acrylates (such as ester compounds of polyhydric alcohols and (meth)acrylic acid); allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0086] The amount of the crosslinking agent to be blended varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.3 parts by weight or less, 0.2 parts by weight or less, 0.15 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the blending amount may be, for example, 0.01 parts by weight or more, 0.03 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.

[0087] The photocurable composition may contain additives other than those described above. Examples of additives include chain transfer agents, silane coupling agents, viscosity modifiers, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, antioxidants, surfactants, antistatic agents, and ultraviolet absorbing agents. The photocurable composition may not contain additives.

[0088] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.

[0089] The silane coupling agent may be an oligomeric silane coupling agent. The oligomeric silane coupling agent usually has a plurality of alkoxysilyl groups in one molecule. Specific examples of the oligomeric silane coupling agent are the trade names "X-41-1053", "X-41-1056", "X-41-1059A", "X-41-1805", "X-41-1810", "X-41-1818", "X-40-2651" and "X-24-9591F" manufactured by Shin-Etsu Silicone Co., Ltd. The oligomeric silane coupling agent may have a reactive functional group. Examples of the reactive functional group are an epoxy group, a mercapto group, an acid anhydride group and an amino group. Among them, those having an epoxy group are preferred, and those having a plurality of epoxy groups in one molecule are more preferred. Examples of oligomeric silane coupling agents having an epoxy group are the above-mentioned "X-41-1053", "X-41-1056" and "X-41-1059A". Examples of oligomeric silane coupling agents having a mercapto group are the above-mentioned "X-41-1805", "X-41-1810" and "X-41-1818". An example of an oligomeric silane coupling agent having an acid anhydride group is the above-mentioned "X-24-9591F". An example of an oligomeric silane coupling agent having an amino group is the above-mentioned "X-40-2651".

[0090] The silane coupling agent may be an acetoacetyl group-containing silane coupling agent (for example, product name "A-100" manufactured by Soken Chemical Industries, Ltd.).

[0091] When the photocurable composition contains a silane coupling agent, the amount of the silane coupling agent is, for example, 5 parts by weight or less, and may be 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or even 0.05 parts by weight or less, based on 100 parts by weight of the total of the monomer group and its partial polymer. The photocurable composition does not need to contain a silane coupling agent.

[0092] The viscosity of the photocurable composition is preferably 5 to 100 poise. A photocurable composition having a viscosity in the above range is particularly suitable for forming the pressure-sensitive adhesive sheet 1.

[0093] The content of the solvent in the photocurable composition is, for example, 5% by weight or less, and may be 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or even 0.5% by weight or less. The photocurable composition may be substantially free of a solvent. The meaning of "substantially free of a solvent" is that the solvent derived from additives and the like is allowed at a content of, for example, 0.1% by weight or less, preferably 0.05% by weight or less, more preferably 0.01% by weight or less. The content of the solvent in the pressure-sensitive adhesive sheet 1 may be within the above range. The pressure-sensitive adhesive sheet 1 may be substantially free of a solvent.

[0094] (Manufacturing method of adhesive sheets) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 24 onto a first laminate 20 including, in this order, a base sheet 21, a coating layer 22 containing a photocurable composition, and a release liner 23 (see FIG. 2). The coating layer 22 is cured by irradiation with light 24 to become the pressure-sensitive adhesive sheet 1. Irradiation with light 24 is typically performed from the side of the base sheet 21. At this time, the light 24 penetrates the base sheet 21 to reach the coating layer 22, and cures the coating layer 22. However, irradiation with light 24 may also be performed from the side of the release liner 23, or from both the side of the release liner 23 and the side of the base sheet 21.

[0095] The formed adhesive sheet 1 is sandwiched between the base sheet 21 and the release liner 23 until the release liner 23 is peeled off, and constitutes a part of the second laminate 27. By peeling the release liner 23 from the second laminate 27, a third laminate 25 including the base sheet 21 and the adhesive sheet 1 is obtained. In the third laminate 25, the surface of the adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the adhesive sheet 1 directly or via another layer.

[0096] The light 24 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may contain light having a wavelength in the same region as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light with a wavelength of 300 nm or less cut by a filter or the like may be irradiated, and cutting short wavelength light is suitable for suppressing deterioration of the base sheet 21 and / or the release liner 23 caused by the light 24. The light source 28 of the light 24 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of the ultraviolet irradiation lamp include an ultraviolet LED, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a xenon lamp, a microwave excited mercury lamp, a black light lamp, a chemical lamp, a germicidal lamp, a low pressure discharge mercury lamp, and an excimer laser. Two or more ultraviolet irradiation lamps may be combined. With the ultraviolet LED, the band of the irradiated ultraviolet light can be narrowed compared to the case of using other light sources.

[0097] The light source 28 may be an LED. Compared to a black light source, an LED not only has an easily adjustable illuminance, but also tends to have a longer light source life. Compared to a black light source using mercury, an LED is superior in terms of reducing environmental load. When an ultraviolet LED is used as the light source, an LED having a peak wavelength of 325 to 350 nm may be selected. According to the study by the present inventors, the use of an LED having a peak wavelength of 325 to 350 nm may contribute to at least one of the following: an improvement in the polymerization rate of the monomer group in the adhesive sheet 1, an improvement in the molecular weight of the polymer, and a reduction in the amount of remaining photopolymerization initiator, compared to, for example, the use of a black light source. Furthermore, an LED that emits light 14 with a peak wavelength of 325 nm to 350 nm tends to generate less heat and to control the temperature of the coating layer 22 more easily than an LED that emits light with a peak wavelength of about 365 nm. As far as the present inventors know, no examples of producing an adhesive sheet using an LED that emits light with a peak wavelength of 325 nm to 350 nm have been reported.

[0098] As an LED having a peak wavelength of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED340) may be selected.

[0099] Focusing on the peak wavelength of the light 24, the peak wavelength of the light 24 irradiated to the first laminate 20 (specifically, the coating layer 22) may be 325 nm to 350 nm. The peak wavelength of the light 24 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength means a wavelength at which the intensity is a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 24. The light 24 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but preferably does not have one.

[0100] The illuminance of the light 24 irradiated onto the first laminate 20 (specifically, the coating layer 22) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5mW / cm 2 More than 3.0mW / cm 2 More than 3.5mW / cm 2 More than 4.0mW / cm 2 More than 5.0mW / cm 2 More than 6.0mW / cm 2 More than 7.0mW / cm 2 More than 8.0mW / cm 2 More than 9.0mW / cm 2 or even 10mW / cm 2 The upper limit of the illuminance is, for example, 25 mW / cm 2 Less than 20mW / cm 2 Below 15mW / cm 2 It may be the following.

[0101] The time for irradiating the first laminate 20 (specifically, the coating layer 22) with the light 24 is, for example, 10 seconds to 1000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, 200 seconds or more, 250 seconds or more, or even 300 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 350 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 24 may be continuous or intermittent.

[0102] The integrated amount of light 24 applied to the first laminate 20 (specifically, the coating layer 22) is, for example, 25 mJ / cm 2 More than 100 mJ / cm 2 More than 250mJ / cm 2 More than 500mJ / cm 2 More than 750mJ / cm 2 More than 850mJ / cm 2 More than 1000mJ / cm 2 More than 1250mJ / cm 2 or even 1500mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 5000 mJ / cm 2 Less than 4000mJ / cm 2 Below, 3000mJ / cm 2 Below, 2500mJ / cm 2 Below, 2000mJ / cm 2 Below that, and even 1750mJ / cm 2 It may be the following.

[0103] An example of the substrate of the release liner 23 (hereinafter, "liner substrate") is a resin film. Examples of resins that may be included in the liner substrate are polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.

[0104] The release liner 23 may include a layer other than the liner substrate. The release liner 23 may include a release layer. The release liner 23 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 23 can be used such that the release layer is on the coating layer 22 side. The release layer is typically a cured layer of a release agent composition containing a release agent. As the release agent, various release agents such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder can be used.

[0105] The release liner 23 may be in the form of a sheet or a continuous piece.

[0106] An example of the base sheet 21 is a resin film. Examples of the resin contained in the base sheet 21 are the same as the examples of the resin that can be contained in the liner base material.

[0107] The thickness of the base sheet 21 is, for example, 10 to 200 μm, and may be 25 to 150 μm.

[0108] The base sheet 21 may have a release layer on the surface on the side of the coating layer 22. Examples of the release layer that may be provided on the base sheet 21 are the same as the examples of the release layer that may be provided on the release liner 23. Both the release liner 23 and the base sheet 21 may have a release layer.

[0109] For base sheet 21, a sheet having a greater peeling strength from adhesive sheet 1 than release liner 23 can usually be selected.

[0110] The base sheet 21 may be in the form of a sheet or a long piece.

[0111] The first laminate 20 can be formed, for example, by forming a coating layer 22 on a base sheet 21 (or a release liner 23) and then arranging the release liner 23 (or base sheet 21) on the formed coating layer 22. Alternatively, the first laminate 20 may be formed by applying the photocurable composition in a pouring manner into the space between the base sheet 21 and the release liner 23 that are held at a predetermined distance such that their main surfaces face each other.

[0112] The coating layer 22 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.

[0113] The thickness of coating layer 22 can be adjusted depending on the intended thickness of adhesive sheet 1, and may be, for example, 5 to 100 μm, 5 to 50 μm, 5 to 25 μm, or even 5 to 20 μm.

[0114] The first laminate 20 may include a long base sheet 21, a long coating layer 22, and a long release liner 23, in other words, may be long. The long first laminate 20 can be obtained, for example, by forming the coating layer 22 between the base sheet 21 and the release liner 23 while conveying them, the base sheet 21 and the release liner 23 being unwound from a roll.

[0115] The Mw of the polymer contained in the pressure-sensitive adhesive sheet 1 may be, for example, 500,000 or more, 550,000 or more, 600,000 or more, 650,000 or more, 700,000 or more, more than 700,000, 750,000 or more, 800,000 or more, 850,000 or more, 900,000 or more, 950,000 or more, 1 million or more, 1.1 million or more, 1.2 million or more, 1.3 million or more, or even 1.4 million or more. The upper limit of Mw is not particularly limited, and is, for example, 3 million or less. The Mw of the polymer and the Mw of the sol component B are determined from values ​​measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0116] The Mw of the sol fraction B contained in the pressure-sensitive adhesive sheet 1 is, for example, 300,000 or more, and may be 350,000 or more, 400,000 or more, 450,000 or more, 500,000 or more, 550,000 or more, 600,000 or more, 650,000 or more, 700,000 or more, 750,000 or more, 800,000 or more, 850,000 or more, 900,000 or more, 950,000 or more, or even 1 million or more. The upper limit of Mw is not particularly limited, and is, for example, 3 million or less.

[0117] In the pressure-sensitive adhesive sheet 1, (I) the polymer may have an Mw of 700,000 or more and less than 800,000, and the sol fraction B may have an Mw of 600,000 or more. In the pressure-sensitive adhesive sheet 1, (II) the polymer may have an Mw of 800,000 or more, and the sol fraction B may have an Mw of 450,000 or more. The pressure-sensitive adhesive sheet 1 that satisfies the condition (I) or (II) is particularly suitable for preventing the pressure-sensitive adhesive sheet 1 from peeling off from the adherend at high temperatures. The adherend is, for example, a glass substrate.

[0118] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 70 μm. The thickness may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more. Even when the thickness of the pressure-sensitive adhesive sheet 1 is, for example, 30 μm or less, it is suitable for suppressing foaming and peeling from an adherend in a high-temperature environment.

[0119] <Optical film> Examples of the optical film 2 include a polarizing film, a retardation film, and a laminated film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may include a glass film.

[0120] The optical film 2 may be a polarizing film, and the adhesive sheet 1 may be in contact with the polarizing film. Among optical films, polarizing films tend to have a large dimensional change due to heat. The dimensional change of the polarizing film may cause peeling from the adhesive film. For this reason, the present invention is particularly advantageous when the optical laminate further includes a polarizing film.

[0121] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with the main surface (surface having the widest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.

[0122] The polarizer is not particularly limited, and examples thereof include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine and dichroic dyes; polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride; etc. Polarizers are typically made of polyvinyl alcohol films (polyvinyl alcohol films include partially saponified ethylene-vinyl acetate copolymer films) and dichroic substances such as iodine.

[0123] The thickness of the polarizer is not particularly limited, and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness of the polarizer is not particularly limited, and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change, and can contribute to improving the durability of the optical laminate, particularly the durability at high temperatures.

[0124] As the material of the protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different from each other. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curing resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more types of optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.

[0125] The thickness of the protective film can be appropriately determined, but is generally about 5 to 200 μm in terms of strength, workability such as handleability, thinness, and the like.

[0126] The polarizer and the protective film are usually adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include an isocyanate-based adhesive, a polyvinyl alcohol-based adhesive, a gelatin-based adhesive, a vinyl-based latex, a water-based polyurethane, and a water-based polyester. Examples of adhesives other than the above-mentioned adhesives include an ultraviolet-curable adhesive and an electron beam-curable adhesive. The electron beam-curable polarizing film adhesive exhibits suitable adhesion to various protective films. The adhesive may contain a metal compound filler.

[0127] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.

[0128] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for the purposes of anti-reflection, anti-sticking, diffusion, anti-glare, etc.

[0129] The polarizing film may be a circular polarizing film.

[0130] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness is, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.

[0131] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.

[0132] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a retardation film for compensating for viewing angles (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or a tilted orientation retardation film for compensating for viewing angles (see, for example, paragraph 0227 of JP 2012-13303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, and the like, of the retardation film. A known film can be used for the retardation film.

[0133] The optical film 2 has a thickness of, for example, 1 to 200 μm.

[0134] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.

[0135] The adhesive sheet-attached optical film 11 may include layers other than the adhesive sheet 1 and the optical film 2. Other layers may be disposed between the adhesive sheet 1 and the optical film 2, but it is preferable that the adhesive sheet 1 and the optical film 2 are in contact with each other.

[0136] The optical film 11 with a pressure-sensitive adhesive sheet can be used, for example, in an optical laminate or an image display device. However, the uses of the optical film 11 with a pressure-sensitive adhesive sheet are not limited to the above examples.

[0137] [Optical laminate] An example of the optical laminate of this embodiment is shown in Fig. 3. The optical laminate 30A in Fig. 3 includes the optical film 11 with the adhesive sheet of this embodiment. The optical laminate 30A has a layered structure in which a release liner 3, an adhesive sheet 1, and an optical film 2 are layered in this order. The optical laminate 30A can be used as the optical film 11 with the adhesive sheet by peeling off the release liner 3.

[0138] The release liner 3 is typically a resin film. Examples of resins constituting the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that contacts the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment using a silicone compound. However, the release liner 3 is not limited to the above examples. The release liner 3 is peeled off when the optical laminate 30A is used, for example, when it is attached to an image forming layer.

[0139] Another example of the optical laminate of this embodiment is shown in Fig. 4. The optical laminate 30B in Fig. 4 includes an optical film 11 with a pressure-sensitive adhesive sheet of this embodiment. The optical laminate 30B has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are layered in this order. After the release liner 3 is peeled off, the optical laminate 30B can be used by being attached to, for example, an image forming layer.

[0140] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may be used as the adhesive sheet 4.

[0141] Another example of the optical laminate of this embodiment is shown in Fig. 5. Optical laminate 30C in Fig. 5 includes an optical film 11 with a pressure-sensitive adhesive sheet of this embodiment. Optical laminate 30C has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. After peeling off the release liner 3, optical laminate 30C can be used by being attached to, for example, an image forming layer.

[0142] The protective film 5 has a function of protecting the optical film 2 (polarizing film 2A) which is the outermost layer during distribution and storage of the optical laminate 30C and in a state where the optical laminate 30C is incorporated in an image display device. The protective film 5 may also function as a window to the external space in a state where it is incorporated in an image display device. The protective film 5 is typically a resin film. The resin constituting the protective film 5 is, for example, polyester such as PET, polyolefin such as polyethylene and polypropylene, acrylic, cycloolefin, polyimide, and polyamide, and polyester is preferable. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminated film including a glass film. The protective film 5 may be subjected to surface treatment such as anti-glare, anti-reflection, and anti-static.

[0143] The protective film 5 may be bonded to the optical film 2 by any pressure-sensitive adhesive. Bonding by a pressure-sensitive adhesive sheet 1 is also possible.

[0144] The optical laminate of the present embodiment may include any layer other than the layers described above. The optical laminate of the present embodiment may have any configuration as long as it includes the optical film 11 with a pressure-sensitive adhesive sheet.

[0145] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.

[0146] The optical laminate of the present embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.

[0147] [Image display device] An example of the image display device of this embodiment is shown in Fig. 6. The image display device 31 in Fig. 6 has a laminated structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, an adhesive sheet 4, a retardation film 2B, an adhesive sheet 1, a polarizing film 2A, and a protective film 5 are laminated in this order. The image display device 31 includes an optical film 11 with an adhesive sheet in Fig. 1, and optical laminates 30A, 30B, and 30C in Figs. 3 to 5 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of a known image display device.

[0148] The image display device 31 in Fig. 6 may be an organic EL display or a liquid crystal display. However, the image display device 31 is not limited to this example. The image display device 31 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED: Field Emission Display), or the like. The image display device 31 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.

[0149] The image display device 31 may have any configuration as long as it includes the pressure-sensitive adhesive sheet-attached optical film 11 and / or the optical laminate of this embodiment. EXAMPLES

[0150] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0151] [Preparation of photocurable composition] (Monomer Syrup A1) 95.1 parts by weight of n-butyl acrylate (BA), 0.1 parts by weight of 4-hydroxybutyl acrylate (HBA), 4.8 parts by weight of acrylic acid (AA), and 0.05 parts by weight of Omnirad184 (manufactured by IGM Resin) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain monomer syrup A1 in which the monomers were partially photopolymerized. The ultraviolet light irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached 20 Pa·s.

[0152] (Monomer syrup A2~A6) Monomer syrups A2 to A6 were prepared in the same manner as for the monomer syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.

[0153] [Table 1]

[0154] The abbreviations in Table 1 are as follows. BA: n-butyl acrylate HBA: 4-hydroxybutyl acrylate AA: Acrylic acid Omnirad184: 1-Hydroxycyclohexyl-phenyl ketone (Omnirad184, IGM Resin) Omnirad819: Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819, IGM Resins) Omnirad127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad127, IGM Resin)

[0155] (Photocurable compositions C1 to C29) Next, the monomer syrup, the monomer, the crosslinking agent, and the silane coupling agent were mixed so as to obtain the compositions shown in Table 2 below, thereby obtaining photocurable compositions C1 to C29.

[0156] [Table 2]

[0157] The abbreviations in Table 2 are as follows. AA: Acrylic acid NVP: N-vinyl-2-pyrrolidone NDDA: 1,9-nonanediol diacrylate KBM403: 3-Glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Silicones, product name "KBM-403") X-41-1056: Epoxy group-containing oligomer type silane coupling agent (manufactured by Shin-Etsu Silicones, product name "X-41-1056")

[0158] The final composition of the monomers contained in each photocurable composition is shown in Table 3 below.

[0159] [Table 3]

[0160] [Preparation of adhesive sheet] <Example 1> (Preparation of release liner) Addition reaction curing type silicone (LTC761 containing hexenyl group-containing polyorganosiloxane, 30 wt% toluene solution, manufactured by Dow Corning Toray) 30 parts by weight, release control agent (BY24-850 containing unreactive silicone resin, manufactured by Dow Corning Toray) 0.9 parts by weight, curing catalyst (SRX212 containing platinum catalyst, manufactured by Dow Corning Toray) 2 parts by weight, and toluene / hexane mixed solvent (volume ratio 1: 1) as a dilution solvent were mixed to obtain a silicone-based release agent composition. The concentration of silicone solids in the release agent composition was 1.0 wt%. Next, the release agent composition was applied to one side of a liner substrate (Lumirror XD500P, a polyester film, thickness 75 μm) with a wire bar and heated at 130 ° C for 1 minute to prepare a release liner having a release layer (thickness 60 nm) on one side.

[0161] (Preparation of adhesive sheet) Monomer syrup C1 was applied to one side of a substrate sheet (PET separator, manufactured by Mitsubishi Plastics, MRF38) using an applicator to form a coating layer (thickness 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, a light with an illuminance of 3.5 mW / cm was applied from the substrate sheet side of the first laminate. 2 and irradiation time 460 seconds (accumulated light intensity 1600 mJ / cm 2 ) was used as the light source. An LED was used as the light source, and the peak wavelength of the irradiated light was 340 nm. This caused the coating layer to photocure, and an adhesive sheet (thickness 20 μm) of Example 1 was obtained that was sandwiched between the base sheet and the release liner. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse) at a position near the ultraviolet ray incident surface of the base sheet.

[0162] <Examples 2 to 24 and Comparative Examples 1 to 6> Pressure-sensitive adhesive sheets of Examples 2 to 24 and Comparative Examples 1 to 6 were obtained by the same method as in Example 1, except that the photocurable composition and light irradiation conditions used were changed as shown in Table 4. Regarding the light source, "LED" refers to the LED used in Example 1, and "BL+LED" refers to a combination of a black light source and the LED used in Example 1. The integrated light amount in the case of "BL+LED" is the sum of the integrated light amounts from both light sources. The irradiation conditions for each light source in the case of "BL+LED" were as follows: BL: Illuminance 6.2mW / cm 2 and irradiation time 95 seconds (accumulated light intensity 589 mJ / cm 2 ) LED: Illuminance 3.1mW / cm 2 and irradiation time 90 seconds (accumulated light intensity 279 mJ / cm 2 )

[0163] [Evaluation method] <Polymer Mw> Samples were prepared that had the same composition as the photocurable compositions used in Examples 1 to 24 and Comparative Examples 1 to 6, except that they did not contain a crosslinking agent. The samples were irradiated with light under the conditions of the corresponding Examples and Comparative Examples. As a result, the monomer groups contained in the samples were polymerized to form a polymer. The Mw of this polymer was measured. The Mw was measured by GPC. The measuring device and measuring conditions were as follows. The measuring device and measuring conditions were different for the NVP-containing composition and the NVP-free composition.

[0164] (NVP-free composition) Analytical equipment: Tosoh HLC-8320GPC Column: Tosoh Corporation, TSKgel GMH-H(S) x 2 Column size: 7.8mmφ×30cm each, total 60cm Column temperature: 40℃ ·Flow rate: 0.5mL / min ·Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene

[0165] (NVP-containing composition) Analytical equipment: Agilent Technologies, Agilent 1200 Column: Tosoh Corporation, TSKgel SuperAWM-H+superAW4000+superAW2500 Column size: 6.0mmφ×15cm each, total 45cm Column temperature: 40℃ ·Flow rate: 0.4mL / min ·Injection volume: 40μL Eluent: N,N-dimethylformamide (DMF) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0166] <Content of sol A> The content of sol component A in each PSA sheet of the Examples and Comparative Examples was measured by the above-mentioned method using GPC. The GPC measuring device and measuring conditions were as follows. The measuring device and measuring conditions were different for the NVP-containing composition and the NVP-free composition.

[0167] (NVP-free composition) Analytical equipment: Tosoh HLC-8320GPC Column: Tosoh Corporation, TSKgel GMH-H(S) x 2 Column size: 7.8mmφ×30cm each, total 60cm Column temperature: 40℃ ·Flow rate: 0.5mL / min ·Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene

[0168] (NVP-containing composition) Analytical equipment: Agilent Technologies, Agilent 1200 Column: Tosoh Corporation, TSKgel SuperAWM-H+superAW4000+superAW2500 Column size: 6.0mmφ×15cm each, total 45cm Column temperature: 40℃ ·Flow rate: 0.4mL / min ·Injection volume: 40μL Eluent: N,N-dimethylformamide (DMF) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0169] <Mw of sol B> The Mw of sol fraction B in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was determined by the same GPC measurement as used to evaluate the content of sol fraction A.

[0170] [Gel fraction] The gel fraction of each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was measured by the method described above.

[0171] (Reliability test) <Preparation of polarizing film> A polyvinyl alcohol film having a thickness of 80 μm was stretched to 3 times while being dyed for 1 minute in an iodine solution having a concentration of 0.3% at a temperature of 30° C. between rolls having different speed ratios. Next, the film was stretched to a total stretching ratio of 6 times while being immersed for 0.5 minutes in an aqueous solution having a temperature of 60° C. and containing boric acid at a concentration of 4% and potassium iodide at a concentration of 10%. Next, the film was immersed for 10 seconds in an aqueous solution having a temperature of 30° C. and containing potassium iodide at a concentration of 1.5%, and then dried at 50° C. for 4 minutes to obtain a polarizer having a thickness of 28 μm. A transparent protective film having a thickness of 30 μm and made of a modified acrylic polymer having a lactone ring structure was attached to one side of the polarizer with a polyvinyl alcohol adhesive. Furthermore, a 47 μm-thick transparent protective film made of a triacetyl cellulose film (Konica Minolta, product name "KC4UY") with a hard coat layer (HC) was attached to the other surface of the polarizer using a polyvinyl alcohol adhesive. The polarizing film was produced by heating and drying for 5 minutes in an oven set at 70°C. Furthermore, a discharge amount of 63 W / m was applied to the surface of the polarizing film on the transparent protective film side made of modified acrylic polymer. 2 Corona treatment was performed for 1 min.

[0172] <Preparation of polarizing film with adhesive sheet> The above-mentioned polarizing film was placed on the exposed surface of each of the pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples to prepare a polarizing film with a pressure-sensitive adhesive sheet. The polarizing film was placed so that the surface of the transparent protective film made of a modified acrylic polymer was in contact with the pressure-sensitive adhesive sheet.

[0173] <Reliability test (85℃)> The prepared polarizing film with adhesive sheet was evaluated for reliability (85°C reliability) by the following method. First, the polarizing film with adhesive sheet was cut into a strip of 228mm length x 128mm width to prepare a test piece. Next, the test piece was attached to the surface of 0.7mm thick alkali-free glass (manufactured by Corning, product name "EG-XG") with an adhesive sheet. The test piece was attached to the alkali-free glass using a laminator. After the test piece was attached, it was placed in an autoclave at 50°C and 0.5MPa for 15 minutes to homogenize the bonding between the alkali-free glass and the adhesive sheet, and the adhesive sheet was adhered to the alkali-free glass. Next, the test piece was heat-treated at 85°C for 500 hours under atmospheric pressure. The vicinity of the end of the test piece was observed with an optical microscope to confirm the presence or absence of peeling from the end of the test piece and foaming near the end. A: No peeling or bubbling that affects image display was observed. B: There is a small amount of foaming at the edge, but it is not enough to affect the image display. C: There are several air bubbles on the edge, but they are not enough to affect the image display. D: Peeling and / or bubbling that affects image display E: Peeling and / or bubbling that significantly affects image display

[0174] <Reliability test (95℃)> The 95°C reliability was evaluated in the same manner as the 85°C reliability, except that the heat treatment temperature was changed from 85°C to 95°C. The evaluation items A to E were the same as those for the 85°C reliability.

[0175] The evaluation results are shown in the following Table 4. Moreover, the relationship between the gel fraction and the content of sol fraction A in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples is shown in FIG.

[0176] [Table 4]

[0177] As shown in Table 4, the pressure-sensitive adhesive sheets of the examples had improved reliability in high-temperature environments compared to the pressure-sensitive adhesive sheets of the comparative examples. [Industrial Applicability]

[0178] The optical film with a pressure-sensitive adhesive sheet of the present invention can be used in optical laminates and image display devices. [Explanation of symbols]

[0179] 1 Adhesive sheet 2. Optical Film 2A Polarizing Film 11 Optical film with adhesive sheet 30A, 30B, 30C Optical laminate 31 Image display devices

Claims

1. The optical film is a photocurable adhesive sheet. The pressure-sensitive adhesive sheet has a gel fraction of 55% or more and less than 94%, The content of the sol component A having a weight average molecular weight of 100,000 or less in the pressure-sensitive adhesive sheet is less than 6.6% by weight. Optical film with adhesive sheet.

2. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the content of the sol component A is 5.8% by weight or less.

3. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the content of the sol component A is 4.9% by weight or less.

4. The weight average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet is 700,000 or more and less than 800,000, and the weight average molecular weight of all the sol components B contained in the pressure-sensitive adhesive sheet is 600,000 or more, or The weight average molecular weight of the polymer is 800,000 or more, and the weight average molecular weight of the sol component B is 450,000 or more. The pressure-sensitive adhesive sheet-attached optical film according to claim 1 .

5. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive sheet contains a (meth)acrylic polymer.

6. The optical film with a pressure-sensitive adhesive sheet according to claim 5 , wherein the (meth)acrylic polymer has a structural unit derived from a carboxyl group-containing monomer.

7. The optical film with a pressure-sensitive adhesive sheet according to claim 5 , wherein the (meth)acrylic polymer has a structural unit derived from a nitrogen atom-containing monomer.

8. The optical film with the pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive sheet contains a silane coupling agent.

9. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive sheet has a thickness of 50 μm or less.

10. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive sheet has a solvent content of 5% by weight or less.

11. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive sheet and the optical film are in contact with each other.

12. The optical film with a pressure-sensitive adhesive sheet according to claim 1 , wherein the optical film is a polarizing film.

13. An optical laminate comprising the pressure-sensitive adhesive sheet-attached optical film according to any one of claims 1 to 12.

14. An image display device comprising the pressure-sensitive adhesive sheet-attached optical film according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Acrylic adhesive composition for polarizing plates containing a photoinitiator group

    JP2010508386A

  • Optical layered film having adhesive layer and image display device

    JP2020122141A

  • Adhesive sheet

    JP2022064782A

  • Optically clear adhesive sheet

    JP2023137397A

  • Transparent adhesive tape, film laminate with metal thin film, cover panel-touch panel module laminate, cover panel-display panel module laminate, touch panel module-display panel module laminate, and image display device

    WO2012173247A1