Powder including hollow particle and method for manufacturing the same

The production of hollow particles with controlled size and composition addresses the challenges of uniformity and performance in insulating materials, achieving reduced dielectric constant and loss tangent, and improved filling rates for semiconductor applications.

JP2024146810APending Publication Date: 2024-10-15JGC CATALYSTS & CHEMICALS LTD

Patent Information

Application Number
JP2024039651
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for producing hollow particles as fillers for insulating materials face challenges in achieving uniform particle size, high filling rates, and low dielectric constant and loss tangent, due to issues such as particle deformation, coalescence, and difficulty in removing large-diameter particles, which affect the performance of insulating layers in semiconductor devices.

Method used

A method involving the production of hollow particles with specific characteristics: average particle diameter of 0.1 to 5.0 μm, maximum particle diameter of 20.0 μm or less, broad particle size distribution, low crack particle rate, and a porosity of 10-50%, with an outer shell containing 70% silica, achieved through spray drying, neutralization, and firing processes to ensure high porosity and uniformity.

Benefits of technology

The solution results in a filler that significantly reduces the dielectric constant and dielectric loss tangent, allows for thinner insulating layers, and enhances filling rates, maintaining excellent dielectric properties even in thin films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146810000001
    Figure 2024146810000001
Patent Text Reader

Abstract

To provide a filler capable of reducing the dielectric constant and dielectric loss tangent of an insulation layer and capable of achieving the thin film of the insulating layer.SOLUTION: Powder including a hollow particle having a hollow in the inside of an outer shell has an average particle size (D50) of 0.1-5.0 μm and the maximum particle size (D100) of 20.0 μm or less. The total volume of particles having a particle size (Ps)×0.75 to (Ps)×1.25 μm of a peak in the particle size distribution of the powder is 50% or less of the total volume of all particles; the powder has a porosity of 10-50% and a crack particle rate of 10% or less; and the outer shell includes silica of 70 mass% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder suitable for use as a filler in an insulating material, and in particular to a powder containing hollow particles having a cavity inside an outer shell. [Background technology]

[0002] In recent years, the speed and capacity of information communication has increased. For this reason, materials used in communication devices are required to have a low dielectric constant (low Dk) and a low dielectric dissipation factor (low Df). For example, printed wiring boards on which semiconductor elements are mounted are required to have insulating materials with low dielectric constants and low dielectric dissipation factors. If the dielectric constant of an insulating material is high, dielectric loss occurs, and if the dielectric dissipation factor of an insulating material is high, not only dielectric loss but also the amount of heat generated may increase.

[0003] In order to realize low dielectric constant and low dielectric loss tangent of insulating materials, development of resin materials as the main insulating material is being carried out. As such resin materials, epoxy resins, polyphenylene ether resins, fluorine resins, etc. have been proposed.

[0004] Fillers are blended into such resin materials from the viewpoints of durability (rigidity), heat resistance, etc. It is known to use hollow silica particles as a filler in order to reduce the dielectric constant (see, for example, Patent Document 1).

[0005] Recently, semiconductor devices have become thinner, and there is a demand for thinner insulating layers. Therefore, the particle size (maximum particle size) of the filler to be mixed into the insulating layer (insulating material) must also be made smaller. Known methods for producing hollow particles with small particle sizes include the emulsion method (e.g., Patent Document 1), the core-shell method (e.g., Patent Documents 2 and 3), the pyrolysis method (e.g., Patent Documents 4 and 5), and the spray drying method (e.g., Patent Document 6).

[0006] The emulsion method and core-shell method can control the particle size to a uniform size, and can also prepare small particles with a size of 1 μm or less. However, during the drying process to obtain a powder from the liquid phase, deformation due to shrinkage forces and adhesion of particles occur, making it difficult to obtain monodispersed hollow particles. Even if monodispersed hollow particles are obtained, the particle size distribution is sharp, making it difficult to fill a large number of hollow particles into a resin material.

[0007] In addition, the thermal decomposition method, which utilizes the expansion of the raw material powder to form granules, requires the raw material powder to be extremely small (finely pulverized) in order to efficiently obtain small particles, making it an unrealistic method.

[0008] In the spray drying method, particles are formed in the gas phase of hot air, so a monodispersed powder can be obtained. In general, droplets are formed using a two-fluid nozzle that uses compressed air to atomize the liquid, so there is a distribution in the actual droplet size. That is, droplets ranging from small to large are mixed. Therefore, a powder containing a mixture of small particles formed from small droplets and large particles formed from large droplets is collected. In order to reduce the maximum particle size, it is necessary to remove large particles by classification, but large particles are prone to cracking during drying and granulation, and are also prone to cracking in the collection container. Broken particles reduce the porosity of the entire powder and do not contribute to low dielectric constant (low Dk) and low dielectric tangent (low Df). Broken particles are small, so it is difficult to remove them by classification.

[0009] In addition, generally, the smaller the particle diameter, the larger the specific surface area of ​​the particle, and the easier it is for the particles to adhere to each other. This reduces the dispersibility in the resin. This results in problems such as the particles not being able to be uniformly dispersed in the resin, forming aggregates that are removed by a filter, or clogging the filter. Furthermore, it is not possible to fill the amount of filler required to lower the dielectric constant and dielectric tangent (low filling rate). In addition, problems such as the inability to fill narrow gaps occur with underfill materials. Furthermore, if the shear force during kneading is increased or the kneading time is extended in order to uniformly disperse the filler, this can cause the hollow particles to crack. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2012-136363 A [Patent Document 2] Patent Publication No. 2022-19357 [Patent Document 3] JP 2022-172938 A [Patent Document 4] JP 2005-206436 A [Patent Document 5] JP 2020-45263 A [Patent Document 6] JP 2022-103683 A Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present invention is to provide a filler that enables an insulating layer to have a low dielectric constant and low dielectric loss tangent, as well as a thin insulating layer. [Means for solving the problem]

[0012] The present inventors have found that the above problems can be solved by a powder that satisfies the following characteristics: That is, the powder according to the present invention contains hollow particles having a cavity inside an outer shell, and satisfies the following requirements (a) to (f). (a) the average particle size (D50) of the powder is 0.1 to 5.0 μm; (b) The maximum particle size (D100) of the powder is 20.0 μm or less; (c) The sum of the volumes of particles in the peak particle size range (Ps) × 0.75 to (Ps) × 1.25 μm in the particle size distribution of the powder is 50% or less of the total volume of all particles, (d) the porosity of the powder is 10 to 50%; (e) The powder has a cracked particle rate of 10% or less; (f) The shell contains 70% or more by mass of silica.

[0013] Furthermore, the method for producing powder according to the present invention includes a first step of forming droplets having an average particle diameter of 10.0 μm or less from an alkali silicate aqueous solution, spraying the droplets into a hot air current, and drying to granulate hollow particles; a second step of neutralizing the alkali contained in the hollow particles with an acid solution and then washing the particles; and a third step of firing the neutralized and washed hollow particles. Effect of the Invention

[0014] The powder of the present invention enables the insulating layer to have a low dielectric constant and a low dielectric loss tangent, and is also suitable for making the insulating layer thinner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The powder of the present invention contains hollow particles having cavities inside the outer shell, has a small average particle size and a small maximum particle size, and has a relatively broad particle size distribution. Therefore, the filling rate in the insulating material (resin) is high, and excellent dielectric properties can be obtained even if the insulating layer is made thin. Furthermore, since the content of cracked particles is low, a high porosity can be obtained despite the small particle size, and the dielectric constant and dielectric loss tangent can be further reduced.

[0016] That is, the powder of the present invention has an average particle size (D50) of 0.1 to 5 μm, a maximum particle size (D100) of 20 μm or less, and when the peak particle size in the particle size distribution is defined as "Ps" μm, the sum of the volumes of particles having a particle size of (Ps)×0.75 to (Ps)×1.25 is 50% or less of the total volume of all particles, the cracked particle rate is 10 vol% or less, and the porosity is 10 to 50%. Also, the shell contains 70 mass% or more of silica.

[0017] Each requirement is explained below. a) Average particle size (D50) is 0.1 to 5.0 μm If the average particle size is less than 0.1 μm, many fine particles are contained, so that the specific surface area (SiOH group content) is large and excellent dielectric properties cannot be obtained. In addition, if the average particle size is more than 5.0 μm, it is difficult to highly fill the powder into a thin insulating material (resin). In consideration of use in a thin insulating material, the average particle size is preferably 0.3 to 4.5 μm, and more preferably 0.5 to 4.0 μm.

[0018] b) Maximum particle size (D100) is 20.0 μm or less If the maximum particle size (D100) exceeds 20.0 μm, it is difficult to highly fill a thin resin. The maximum particle size (D100) is preferably 15.0 μm or less, more preferably 10.0 μm or less, and even more preferably 8.0 μm or less.

[0019] c) Spread of particle size distribution When the peak particle diameter in the particle size distribution is "Ps" μm, the sum of the volumes of particles having a particle diameter of (Ps x 0.75) μm or more and (Ps x 1.25) μm or less is 50% or less of the total volume of all particles. If the volume ratio of particles in the range of (Ps x 0.75) to (Ps x 1.25) μm exceeds 50%, the particle diameters become uniform and the broadness of the particle size distribution is low. Therefore, it becomes difficult to highly fill a thin resin film, and excellent dielectric properties cannot be obtained. This volume ratio is preferably 45% or less, more preferably 40% or less.

[0020] Moreover, the broader the particle size distribution, the more preferable (the broader the particle size distribution, the more preferable). Therefore, the particle size distribution may have two or more peaks. That is, the particle size distribution may be bimodal (multimodal). This makes it possible to further increase the filling rate in the thin-film resin. In addition, when multiple peaks exist, the volume ratio of the above-mentioned particles is 50% or less for each peak.

[0021] d) Crack particle rate is 10% or less by volume Since cracked particles do not contribute to lowering the dielectric constant and dielectric tangent (they reduce the overall porosity), if the cracked particles exceed 10% by volume, excellent dielectric properties cannot be obtained and they also hinder a high packing rate. The cracked particle rate is preferably 8% by volume or less, and more preferably 6% by volume or less. Note that the cracked particles refer to hollow particles such as C-shaped particles that still retain their original shape, and do not include small pieces that have been broken into pieces.

[0022] e) Porosity is 10-50% If the porosity of the powder is less than 10%, the effect of lowering the dielectric constant and dielectric loss tangent is not sufficiently obtained, and the desired dielectric constant and dielectric loss tangent are not obtained. If the porosity exceeds 50%, the strength of the particles is reduced, and the particles are likely to crack. The porosity is preferably 15 to 45%, more preferably 20 to 40%.

[0023] f) The silica content of the outer shell is 70% by mass or more The shell contains 70% by mass or more of silica as a component. That is, the shell is formed of an inorganic oxide containing 70% by mass or more of silica. In addition to silica, the shell may contain inorganic oxides such as alumina, zirconia, and titania. The amount of silica contained in the shell is more preferably 90% by mass or more, and even more preferably 95% by mass or more, and it is particularly preferable that the shell is substantially formed only of silica.

[0024] Furthermore, the powder preferably satisfies any one of the following requirements. g) The alkali content of the powder is 100 ppm or less This allows the dielectric constant and dielectric loss tangent to be reduced. In addition, the particles are prevented from coalescing in the subsequent process, and the generation of sintered particles in the firing process is prevented. This is particularly suitable for semiconductor packaging. The alkali content is more preferably 90 ppm or less, and even more preferably 80 ppm or less.

[0025] h) The oil absorption per unit volume of the powder is 0.60 ml / cm 3 below The oil absorption per unit volume is 1 cm 3This indicates the amount of oil required to make particles of 1 cm into a flowable paste. Therefore, the smaller the value, the easier it is to fill the resin with high oil content. For example, 3 When it can be fluidized with 0.60 ml of oil, the particle packing ratio in the paste is 62.5 vol%. The oil absorption is 0.60 ml / cm 3 If the oil absorption is less than 0.50 ml / cm, it can be highly loaded when dispersed in resin. 3 Less than 0.40 ml / cm is preferred 3 The following is more preferred:

[0026] Furthermore, the powder preferably satisfies any one of the following requirements, and more preferably satisfies all of the requirements i) to m).

[0027] i) Sears number (ml / SiO21.5g) is less than 0.30 Generally, the Sears number is an index showing the amount of OH groups (silanol groups) in silica particles, and the larger the Sears number, the more OH groups there are in the particles. When the Sears number is 0.30 or more, the dielectric constant and dielectric loss tangent are high, and moisture absorption occurs over time, so that the dielectric constant and dielectric loss tangent tend to increase. Furthermore, the adhesion between particles is high, and there is a risk of particle aggregation. The Sears number is more preferably less than 0.29, and even more preferably less than 0.28.

[0028] The Sears number is measured by titration with sodium hydroxide according to the description by Sears in Analytical Chemistry 28 (1956), 12, 1981-1983. This method measures the amount of OH groups on the particle surface. The Sears number (ml / SiO21.5g) indicates the titration amount of 0.1N sodium hydroxide solution per 1.5g of silica.

[0029] j) The ratio of the BET specific surface area determined by the water vapor adsorption method and the nitrogen adsorption method is less than 0.30 The ratio of the BET specific surface area determined by the water vapor adsorption method to the BET specific surface area determined by the nitrogen adsorption method (water vapor specific surface area / nitrogen specific surface area) indicates the degree of hydrophilicity / hydrophobicity, with the larger the value being, the more hydrophilic the material is. Materials with this ratio of 0.30 or more are prone to hygroscopicity. This ratio is preferably less than 0.20, and more preferably less than 0.15.

[0030] k) Water vapor adsorption is less than 0.20% by mass The water vapor adsorption amount indicates stability over time with respect to moisture absorption. If the water vapor adsorption amount is 0.20 mass% or more, the material is prone to moisture absorption and has poor stability over time. The water vapor adsorption amount is more preferably less than 0.15, and even more preferably less than 0.10.

[0031] m) 29 In the structural analysis by Si-NMR, the peak area of ​​the Q4 structure is 90% or more of the total peak area of ​​the Q0 to Q4 structures. 29 In the structural analysis by Si-NMR, silicon atoms in the particles are divided into five types, Q0, Q1, Q2, Q3, and Q4, depending on the number of silicon atoms sharing oxygen around the silicon atom. Specifically, the chemical shift of the Q0 structure is -73.0 to -73.5 ppm, the chemical shift of the Q1 structure is -73.5 to -78.0 ppm, the chemical shift of the Q2 structure is -78.0 to -82.0 ppm, the chemical shift of the Q3 structure is -82.0 to -100.0 ppm, and the chemical shift of the Q4 structure is -100.0 to -120.0 ppm. Of these structures, the Q4 structure has fewer OH groups (more siloxane bonds) than the Q0 to Q3 structures. The greater the abundance ratio (area ratio) of the Q4 structure, the fewer unstable OH groups and the greater the bond ratio between silicon atoms. This results in a highly stable particle. When such particles are used as a filler, an insulating material that does not change much with time can be obtained. The peak area of ​​the Q4 structure is more preferably 93% or more, and even more preferably 95% or more, of the total peak area (area of ​​Q0 to Q4 structures). It is particularly preferable that only the Q3 structure and the Q4 structure are present.

[0032] The powder of the present invention is mostly spherical hollow particles, but may contain solid particles. The hollow particles preferably account for 80% or more of the total number, more preferably 90% or more of the total number. The proportion of hollow particles can be calculated, for example, from cross-sectional SEM images of any 100 particles.

[0033] The powder has a dielectric constant of preferably 2.8 or less, more preferably 2.5 or less, and a dielectric loss tangent of preferably less than 0.0010, more preferably less than 0.0005.

[0034] Furthermore, the specific surface area of ​​the powder is 1 to 50 m 2 / g is preferable. If the specific surface area is too large, the amount of SiOH groups is large, which may adversely affect the dielectric properties. In addition, the adhesion between particles increases, which may result in poor dispersibility in resin. The specific surface area is preferably 2 to 20 m 2 / g is more preferable, and 3 to 10m 2 / g is more preferred.

[0035] [Powder manufacturing method] The method for producing the powder of the present invention includes a first step of spraying droplets having an average particle size of 10.0 μm or less, formed from an aqueous alkali silicate solution, into a hot air stream, drying, and granulating hollow particles, a second step of neutralizing the alkali contained in the hollow particles in an acid solution, washing the particles, and a third step of firing the neutralized and washed hollow particles. The powder of the present invention can be obtained by such a production method. Note that other steps such as a classification step and a drying step may be provided before or after each step.

[0036] In the first step, the diameter of the sprayed droplets is adjusted to be smaller than that of the conventional method and to prevent the formation of large droplets. This can prevent the generation of large particles. Large particles have a small ratio of shell thickness to particle diameter (shell thickness / particle diameter) and are more likely to break than small particles. In other words, small hollow particles with high porosity can be obtained while suppressing the generation of broken particles. If it is only necessary to obtain small hollow particles, this can be achieved by classification, but in order to reduce the content of broken particles, it is necessary to reduce the droplet diameter so as not to granulate large particles that are easily broken. In general, the spray drying method can produce particles with a broad particle size distribution compared to the emulsion method and the like.

[0037] Each step will be described in detail below. (first step) In this process, droplets with an average particle size of 10.0 μm or less are formed from an alkali silicate aqueous solution, which are then sprayed into a hot air current and dried to granulate spherical hollow particles. That is, the diameter of the sprayed droplets is adjusted to be smaller than that of conventional methods and to exclude large droplets, thereby granulating the hollow particles.

[0038] The average particle size of the droplets is preferably 9.0 μm or less, more preferably 8.0 μm or less. The lower limit is 5.0 μm. Here, the average particle size of the droplets was measured by the liquid immersion method (Sauter average particle size).

[0039] Examples of spray drying methods for stably forming small-diameter droplets include a method using a collision type two-fluid nozzle having a structure for further homogenizing and finely dispersing droplets discharged from a two-fluid nozzle that atomizes liquid using compressed air, a nozzle that pulverizes liquid by the collision of two opposing air streams, a four-fluid nozzle, etc. Specifically, examples include a method using a collision type two-fluid nozzle manufactured by Kiri no Ikeuchi Co., Ltd., a nozzle (MicroFog) manufactured by Nozzle Network Co., Ltd., a four-fluid nozzle manufactured by GF Co., Ltd., etc. In addition, the droplets can be made smaller by increasing the volume ratio (gas / liquid volume ratio) of the gas supply amount to the raw material liquid supply amount in the nozzle injection. In order to make the average particle diameter of the droplets 10 μm or less, the gas / liquid volume ratio is preferably 6000 or more, more preferably 7000 or more, and particularly preferably 8000 or more.

[0040] In the spray drying, the inlet temperature of the spray dryer is preferably 300 to 600° C., more preferably 350 to 550° C., and the outlet temperature is preferably 120 to 350° C., more preferably 200 to 300° C. By increasing the inlet and outlet temperatures, the drying speed can be increased, and the porosity can be improved.

[0041] The concentration of the alkali silicate aqueous solution as SiO2 is preferably 1 to 30 mass%, more preferably 5 to 28 mass%, and even more preferably 10 to 25 mass%. The lower the concentration of the alkali silicate aqueous solution, the lower the viscosity becomes, and the smaller the droplets can be. Examples of the alkali silicate include sodium silicate and potassium silicate, which are soluble in water, and sodium silicate is preferred.

[0042] The molar ratio (SiO2 / M2O) of SiO2 to M2O (M is an alkali metal) in the alkali silicate is preferably 1 to 5, more preferably 2 to 4. If this molar ratio is less than 1, not only is it difficult to remove the alkali with an acid wash due to the excessive amount of alkali, but also the deliquescence of the particles obtained by spray drying becomes large, making it difficult to obtain the desired hollow particles. If this molar ratio exceeds 5, the solubility of the alkali silicate decreases, making it difficult to prepare an aqueous solution. Even if an aqueous solution can be prepared, there is a risk that the desired hollow particles cannot be formed by spray drying.

[0043] (Second process) In this process, the alkali contained in the granulated hollow particles is neutralized and removed in an acid solution under specified conditions (dealkalization). Specifically, the hollow particles are neutralized by immersing them in a large amount of acid solution to remove the alkali contained in the hollow particles. In other words, the neutralization is performed in a low pH state. The pH is preferably 2.0 or less.

[0044] Usually, pores are formed in the particles (shell) by removing the alkali from the particles. Rapid neutralization with a large amount of acid suppresses dissolution of silica in the shell, and prevents the formation of large pores. In other words, the pores can be made to a size (structure) that is easily blocked by the subsequent firing process. As a result, particles with a small amount of SiOH groups are obtained, and the insulating material has a low dielectric constant and low dielectric tangent. In addition, since the pores are blocked by the firing process, the change in the dielectric tangent caused by moisture absorption over time can be suppressed, and a low dielectric tangent can be maintained for a long time. In addition, adhesion between particles can be suppressed, improving the dispersibility of the particles. Furthermore, since almost no pores remain in the shell, the particle strength is also improved.

[0045] In this process, it is preferable to add the hollow particles to the acid solution, rather than adding the acid solution to the hollow particles. This prevents the pH from becoming such that the particles dissolve near the particles, and prevents the particles from dissolving. In the column flow method, the H + If the concentration of the surfactant decreases (pH increases) and the surfactant comes into contact with the particles at a pH that is not low enough, the particles may dissolve, and large pores may form and the desired effect may not be achieved.

[0046] In this process, the value obtained by multiplying the number of moles of alkali metal ions in the hollow particles by the valence (M SP ) to the number of moles of hydrogen ions in the acid (M H+ ) ratio (M H+ / M SPIt is preferable to use an acid solution with a ratio of H 2 exceeding 4.7. Conventionally, acid solutions with such high values ​​have not been used. For example, paragraph 0032 of JP 2013-103850 A describes that "even if this ratio exceeds 4.7, the skeletonization does not proceed further, and the acid is excessive, which is not economical." Also, in the examples of JP 04-104907 A, this ratio is 3.0 (200 L) and 4.4 (300 L). In the present invention, by deliberately carrying out neutralization treatment with such an acid solution, it is possible to remove alkali ions (H 2 ), while suppressing damage to the silica skeleton. + Therefore, large pores are not formed in the (outer) shell of the hollow particles. H+ / M SP ) is preferably 5.0 or more, more preferably 5.2 or more, and particularly preferably 5.5 or more. There is no upper limit, but it is, for example, 7.0 or less.

[0047] Although this process removes the alkali content from the particles (outer shell) and reduces the mass, the change in particle shape, hollow structure, etc. (volume) is extremely small. Therefore, when comparing before and after this process, the particle density decreases according to the amount of alkali removed. Particle density can be measured according to the gas pycnometer method (JIS Z 8837). Particles before this process (products after the first process) are measured as they are, and particles after this process are measured after drying at 120°C for 24 hours (after washing).

[0048] By removing the alkali in this process, pores are formed in the particles (outer shell). Therefore, the measurement result of particle density differs depending on whether the gas used for density measurement passes through the pores or not. When helium is used, helium penetrates the pores and fills the cavities inside the particles, so the measured particle density is almost the same as the density of silica (2.1 to 2.3 g / cm3). 3 )

[0049] On the other hand, when nitrogen is used, the nitrogen does not penetrate the pores of the outer shell, and the particle density reflecting the presence of internal cavities can be measured. In this process, if no pores into which nitrogen can penetrate are formed in the particles (outer shells) and all the alkali is removed, the particle density after this process (theoretical value: ρ 2T ) can be calculated using the following formula (X):

[0050] ρ 2T =ρ1×(1-W a )...Equation (X) ρ1: Particle density after the first process ρ 2T : Theoretical value of particle density after the second process W a : Mass ratio of alkali in raw material solids

[0051] The more pores that nitrogen can enter are formed in the second step, the greater the difference between the actual measured particle density (ρ2) and the theoretical value (ρ 2T ) becomes larger. The pores that are formed can be made smaller by a subsequent heat treatment or the like, but if the size is too large or the amount is too large, they cannot be fully blocked and ultimately remain in the particle (outer shell), causing increased hygroscopicity. For this reason, it is preferable for the pores to be small in size and small in amount. In other words, the particle density (ρ2) measured with nitrogen is smaller than the theoretical value (ρ 2T ) is preferably smaller. Specifically, this ratio ρ2 / ρ 2T is preferably 1.0 to 1.4, more preferably 1.0 to 1.3, and particularly preferably 1.0 to 1.2. The particle density (ρ2) after the second step was obtained by measuring the particles that were washed and then dried at 120° C. for 24 hours, as described above.

[0052] In addition, even if cracks occur in the hollow particles between the end of the first process and the end of the second process, the particle density (ρ2) will not exceed the theoretical value (ρ 2T In the present invention, small-diameter hollow particles that are less likely to break are granulated in the first step, so the deviation from the theoretical value is smaller than in the conventional method in which large-diameter hollow particles that are more likely to break are granulated.

[0053] Also, it is preferable to immerse the hollow particles in the acid solution so that the concentration of SiO2 becomes 1 to 30 mass%. If it is less than 1 mass%, there is no problem with alkali removal and cleaning, but the production efficiency decreases. If it exceeds 30 mass%, the concentration is too high and the alkali removal and cleaning efficiency may decrease. Also, problems such as particle cracking due to contact and friction between particles may occur. 5 to 25 mass% is more preferable. The immersion treatment may be performed in multiple steps.

[0054] The temperature condition for the immersion treatment is usually 5° C. or higher and the boiling point of the solution or lower. In order to form better pores and more reliably realize a low dielectric constant and a low dielectric loss tangent of the insulating material, the temperature is preferably 50° C. or higher, and more preferably 55° C. or higher. The treatment time is, for example, 0.5 to 24 hours.

[0055] After the immersion treatment, the hollow particles are thoroughly washed by a conventionally known method, for example, by filtration and washing with pure water.

[0056] The amount (mass ratio) of the alkali (M) remaining after alkali removal is preferably 100 ppm or less, more preferably 90 ppm or less, and even more preferably 80 ppm or less. By sufficiently removing the alkali in this step, the particles are prevented from coalescing in the subsequent step, and the generation of sintered particles in the firing step can be prevented.

[0057] The residual alkali amount is measured by dissolving the particles in acid and measuring the alkalinity using an atomic absorption spectrophotometer. When sodium silicate is used, Na is measured, and when potassium silicate is used, K is measured.

[0058] The amount of alkali in the final product (powder) is also preferably in the above-mentioned range, and is usually the same as the amount of alkali after the alkali removal step.

[0059] Examples of the acid used in this step include mineral acids such as hydrochloric acid, nitric acid, and sulfuric acid, and organic acids such as acetic acid, tartaric acid, and malic acid. Mineral acids are preferred, and sulfuric acid is particularly preferred in terms of valence. The acid solution is usually an aqueous solution, but may be mixed with alcohol or the like.

[0060] (Third step) In this step, the hollow particles that have been neutralized and washed are fired. The firing temperature is preferably 900°C or higher, more preferably 1000°C or higher. There is no upper limit, but it is, for example, 1200°C. Since the alkali is sufficiently removed by the second step, the particles are prevented from bonding together, and the generation of sintered particles can be prevented even when fired at a high temperature. Since the pores formed during alkali removal can be blocked by high-temperature firing, the outer shell becomes non-porous. This makes it possible to reduce the SiOH group, and particles with low dielectric constant and dielectric loss tangent can be obtained. For example, in the invention of JP 2013-103850 A, particles with a dielectric loss tangent of less than 0.0010 cannot be obtained, but in the present invention, particles with a dielectric loss tangent of less than 0.0010 can be obtained. In addition, particles with high strength can be obtained.

[0061] (Classification process) Furthermore, it is preferable to provide a classification step between the second step and the third step. The hollow particles obtained in the second step are classified. It is preferable to remove coarse particles by classification. The size of the particles to be removed as coarse particles may be appropriately determined depending on the purpose and application of the powder. For example, there can be mentioned an embodiment in which coarse particles exceeding 20.0 μm are removed, an embodiment in which coarse particles exceeding 15.0 μm are removed, and an embodiment in which coarse particles exceeding 10.0 μm are removed. That is, in this step, it is preferable that coarse particles exceeding 20.0 μm are substantially not contained, that coarse particles exceeding 15.0 μm are substantially not contained, and that coarse particles exceeding 10.0 μm are substantially not contained. Note that the content of coarse particles in the final product is usually not significantly different from the content after the classification step.

[0062] It is generally considered preferable to carry out classification treatment after firing in order to make the particle diameter uniform, but in the present invention, classification treatment is carried out before the firing step (third step). If firing is carried out without classification treatment, coarse particles with high porosity that should be removed will also be present. Such coarse particles are prone to cracking and may crack due to the stress of shrinkage caused by heating. Since the fragments generated by cracking have a small particle diameter, they cannot be removed even if classification treatment is carried out thereafter. In addition, since these fragments are dense silica without voids, they hinder the achievement of low dielectric constant and low dielectric loss tangent. By carrying out classification treatment before firing, such inconveniences can be avoided. Note that classification treatment may be further carried out after firing.

[0063] The classification in this process refers to particle size classification in which powder is divided according to particle size in order to make the particle size of the powder uniform. An example of this particle size classification operation is fluid classification, which can be divided into dry classification and wet classification.

[0064] In principle, classifiers used in dry classification can be broadly divided into gravity classifiers, inertial classifiers, and centrifugal classifiers. More precise classification is possible by using an inertial classifier that classifies particles by utilizing the inertial force of the particles, or a centrifugal classifier. Classifiers that can exhibit their characteristics even with light particles that are not easily subjected to centrifugal force include Elbow Jet manufactured by Nittetsu Mining Co., Ltd., SG Separator manufactured by Japan 3M Co., Ltd., Aero Fine Classifier manufactured by Nisshin Engineering Co., Ltd., and Microspin manufactured by Nippon Pneumatic Mfg. Co., Ltd. Among these, Elbow Jet and Aero Fine Classifier, which can precisely classify even light particles, are preferred.

[0065] In principle, classifiers used in wet classification can be broadly divided into gravity classifiers and centrifugal classifiers. By using a centrifugal classifier, more precise classification is possible. Classifiers that can exhibit their characteristics even with light particles that are not easily subjected to centrifugal force include the Hydrocyclone manufactured by Nippon Chemical Machinery Co., Ltd., the Superclone manufactured by Murata Kogyo Co., Ltd., and the Eye Classifier manufactured by Satake Multimix Co., Ltd. Among these, the Eye Classifier, which can precisely classify even light particles, is preferred.

[0066] Although it is not prohibited to remove fine particles of less than 0.1 μm in the classification step, it is preferable not to remove the fine particles, since this operation tends to sharpen the particle size distribution.

[0067] In order to suppress the generation of cracked particles, classification may be performed at an early stage between the first and second steps. However, since the hollow particles obtained in the first step are deliquescent, it is preferable to classify them in dry air rather than by wet classification.

[0068] (drying process) A drying step may be provided before or after the third step. Examples of the drying method include heat drying. The drying temperature is preferably 50 to 400°C, more preferably 50 to 200°C. Specifically, examples include a method of drying at a low temperature of about 50 to 200°C for a long time, a method of drying by gradually increasing the temperature, and a method of drying by changing the temperature in several stages. The drying step may be provided between the second and third steps, after the third step, or both. If necessary, the drying process may be repeated.

[0069] (Sieving process) Furthermore, it is preferable to carry out a sieving process to sieve out the particle agglomerates at least one of after the drying process and after the third process (firing). Note that the particle agglomerates refer to foreign matter having a particle size of, for example, more than 150 μm. The sieving process is carried out using a sieve with an opening (mesh number) that can remove such particle agglomerates.

[0070] [Resin composition] The resin composition of the present invention has the above-mentioned hollow particle-containing powder dispersed therein. Such a resin composition can be produced by mixing the hollow particle-containing powder with a resin. Specifically, for example, the hollow particle-containing powder, a thermosetting resin, etc. are mixed and kneaded with a roll mill or the like to prepare a resin composition (coating liquid). This is coated on a substrate and cured by heat, ultraviolet light, or the like.

[0071] Such a resin composition can be used as an insulating material for electronic materials such as semiconductors. Specifically, it can be used for copper-clad laminates, prepregs, build-up films, etc. for forming printed wiring boards (including rigid boards and flexible boards). In addition, this resin composition is useful as an insulating material for thin films, for example, insulating materials having a thickness of 50 μm or less, preferably 25 μm or less. It can also be used as a semiconductor package-related material such as mold resin, mold underfill, underfill, etc., and an adhesive for flexible boards.

[0072] As the resin to be mixed with the powder, a curable resin generally used in electronic materials such as semiconductors can be used. A photocurable resin may be used, but a thermosetting resin is preferred. Examples of such curable resins include epoxy resins, polyphenylene ether resins, fluorine resins, polyimide resins, bismaleimide resins, acrylic resins, methacrylic resins, silicone resins, BT resins, cyanate resins, and the like. Examples of epoxy resins include bisphenol-type epoxy resins, novolac-type epoxy resins, triphenol alkane-type epoxy resins, epoxy resins having a biphenyl skeleton, epoxy resins having a naphthalene skeleton, dicyclopentadiene phenol novolac resins, phenol aralkyl-type epoxy resins, glycidyl ester-type epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, halogenated epoxy resins, and the like. These resins may be used alone or in combination of two or more.

[0073] The resin composition contains the powder A of the present invention and the curable resin B in a mass ratio (A / B) of preferably 10 / 100 to 95 / 100, more preferably 30 / 100 to 80 / 100. This mass ratio allows the powder A to fully function as a filler while maintaining properties such as fluidity.

[0074] The resin composition preferably contains a curing agent such as a phenol compound, an amine compound, an acid anhydride, etc. When an epoxy resin is used as the curable resin, examples of the curing agent include phenol resins having two or more phenolic hydroxyl groups in one molecule, such as bisphenol type resins, novolac resins, triphenol alkane type resins, resol type phenol resins, phenol aralkyl resins, biphenyl type phenol resins, naphthalene type phenol resins, and cyclopentadiene type phenol resins, and acid anhydrides such as methylhexahydrophthalic acid, methyltetrahydrophthalic acid, and methylnadic anhydride.

[0075] Various additives such as colorants, stress relaxation agents, antifoaming agents, leveling agents, coupling agents, flame retardants, and curing accelerators may be added to the resin composition as required.

[0076] Examples of the present invention will now be described in detail. [Example 1] First, 30,000 g of a water glass aqueous solution (SiO2 / Na2O molar ratio 3.2, SiO2 concentration 20% by mass) was prepared, and the water glass aqueous solution was sprayed from two nozzles of the four-fluid nozzle, and air was sprayed from the other two nozzles to granulate hollow particles (first step). In this example, the inlet temperature was set to 450°C. The total flow rate of the water glass aqueous solution (i.e., the total flow rate of the liquid sprayed from the two nozzles) was set to 0.29 L / hr, and the total flow rate of the air (i.e., the total flow rate of the air sprayed from the two nozzles) was set to 2040 L / hr. In other words, the air / liquid volume ratio was 7034. At this time, the outlet temperature was 250°C.

[0077] Next, 5000 g of the obtained hollow particles were added to 40000 g of an aqueous sulfuric acid solution with a concentration of 25% by mass while stirring. The mixture was stirred for 15 hours while adjusting the liquid temperature to maintain it at 35°C, and then cooled to room temperature. At this time, the solid content (SiO2) concentration was 8.4% by mass, and the pH of the dispersion after cooling was less than 1.0. In addition, the value (M SP ) to the number of moles of hydrogen ions in the acid (M H+ ) ratio (MH+ / M SP ) was set to 5.2. After cooling, solid-liquid separation was performed, and further washing with pure water was performed (second step). Next, drying treatment was performed in a dryer at 120 ° C for 24 hours (drying step). The obtained dried material was crushed and further sieved with a 75 μm mesh to remove particle agglomerates (foreign matter). Then, dry inertial classification was performed using an elbow jet (EJ-15) manufactured by Nittetsu Mining Co., Ltd. With this device, powder can be classified into three types, F powder (fine powder), M powder (fine powder), and G fraction (coarse powder), by classification. The F edge distance was adjusted so that particles exceeding 10 μm contained in the F powder (fine powder) were 5 vol % or less, and it was collected using a bag filter (classification step). Then, a powder containing hollow particles was obtained by heat treatment at 1000 ° C for 10 hours (third step). It is to be noted that a 150 μm mesh sieve may be used to remove particle agglomerates (foreign matter) after firing in the third step.

[0078] <Manufacturing of resin molded products> The obtained powder was mixed with liquid epoxy resin "ZX-1059 manufactured by Nippon Steel Chemical & Material Co., Ltd." together with liquid acid anhydride "Rikacid MH700 manufactured by New Japan Chemical Co., Ltd." and imidazole-based epoxy resin curing agent "2PHZ-PW manufactured by Shikoku Kasei Co., Ltd." Here, "ZX-1059" was mixed at a ratio of 100 parts by mass, "Rikacid MH700" at 86 parts by mass, and "2PHZ-PW" at 1 part by mass, and the ratio of powder in this mixture was 65% by volume. This mixture was pre-mixed with a planetary mill, and then mixed with a three-roll mill to prepare a paste (resin composition). This paste was heated at 170°C for 2 hours to harden, and a plate-shaped resin molded body of 50 mm x 50 mm x 1 mm was obtained.

[0079] The physical properties of the powder and resin molded product obtained as described above were measured and evaluated as follows. The results, together with the preparation conditions, are shown in Table 1. The other examples and comparative examples were basically carried out in the same manner. 1) Particle size distribution, cracked particle rate 20g of a solution of a dispersant (Kao Corp. Rheodol TW-0120V) diluted to 0.5% with pure water and 0.125g of powder were placed in a 30ml glass screw tube and irradiated with ultrasonic waves for 10 minutes using an ultrasonic cleaner (Shinsan Denshi Co., Ltd. SC-20A). 0.2g of this solution was placed in a 6ml glass screw tube, 1.8g of pure water was added, and ultrasonic waves were irradiated again for 10 minutes using an ultrasonic cleaner. The resulting powder dispersion was observed under a microscope. From the observation of approximately 50,000 particles, the particle size distribution of the powder was obtained by image analysis. From this particle size distribution, the average particle size (D50), maximum particle size (D100), and peak particle size (Ps) were obtained. Furthermore, the volume of particles with particle sizes within the range of ±25% of the peak particle size (Ps) was calculated. In addition, the percentage of cracked particles (volume %) was calculated from the observation results of approximately 50,000 particles by image analysis. Particles with an area solidity of less than 0.75 were considered to be cracked particles.

[0080] 2) Porosity The particle density of the powder was measured by the gas pycnometer method using an Ultrapyc5000 manufactured by Quantachrome Instruments. From this particle density, the porosity (%) was calculated using the formula "[2.2 - (particle density)] / 2.2 x 100". In this formula, the density of silica is 2.2 g / cm 3 It was decided.

[0081] 3) Alkali content After the powder was pretreated (by adding sulfuric acid and hydrofluoric acid), it was dissolved in hydrochloric acid, and the alkali content was measured by atomic absorption spectrometry using an atomic absorption spectrometer (Hitachi Z-2310). In this example, the Na content was measured.

[0082] 4) Oil absorption amount The mass of the sample (powder) was weighed, and the oil absorption was measured using boiled linseed oil based on JIS K 5421. The above-mentioned particle density was used to convert it into the oil absorption per unit volume.

[0083] 5) Sears Number The Sears number was determined by titration with sodium hydroxide as described by Sears, Analytical Chemistry 28(1956), 12, 1981-1983. Specifically, 30 g of sodium chloride was added to 150 g of a solution in which the powder was diluted with pure water to a particle concentration of 1 mass%, and the pH was adjusted to 4.0 with hydrochloric acid. This solution was titrated with 0.01 N aqueous sodium hydroxide solution at a fixed rate of 0.1 ml / sec using an automatic titrator. The amount of aqueous sodium hydroxide solution required to reach pH 9.0 was reduced to one tenth and converted to the titration amount using 0.1 N aqueous sodium hydroxide solution (i.e., the titration amount of 0.1 N aqueous sodium hydroxide solution for 1.5 g of silica).

[0084] 6) Water vapor specific surface area / nitrogen specific surface area The BET specific surface area of ​​the powder was measured by nitrogen adsorption and water vapor adsorption using a Microtrack-Bell BELSORP-max. The ratio of the BET specific surface area measured by the nitrogen adsorption method to the BET specific surface area measured by the water vapor adsorption method (water vapor specific surface area / nitrogen specific surface area) was calculated.

[0085] 7) Water vapor adsorption amount Measurements were performed using the water vapor adsorption method with a Microtrack-Bell BELSORP-max, and the amount of water vapor adsorbed was calculated at a partial pressure of 0.9 relative to the powder mass (p / p0 = 0.9).

[0086] 8) 29 Si-NMR Silica particles 29 Structural analysis by Si-NMR was carried out as follows. The powder was dried at 110°C for 1 hour, and then conditioned at a relative humidity of 60% for 24 hours. The obtained powder (sample) was uniformly packed into a 5 mm diameter NMR solid sample tube, and measured by the single pulse non-decoupling method using a 14.1 T NMR device (Agilent VNMRS-600, 1H resonance frequency 600 MHz). Polydimethylsiloxane (-34.44 ppm) was used as the reference material. The obtained spectrum was subjected to waveform analysis, and the area of ​​each peak was calculated. The ratio of each structure was calculated by the peak area ratio of each structure (Si / ST) × 100 [%] (where i is an integer from 0 to 4. ST is the sum of the peak areas of each structure expressed as ST = S0 + S1 + S2 + S3 + S4).

[0087] 9) Dielectric constant (Dk) and dielectric tangent (Df) The dielectric constant (Dk) and dielectric loss tangent (Df) of the powder were measured by the cavity resonator perturbation method using a network analyzer (Anritsu, MS46122B) and a cavity resonator (1 GHz) in accordance with ASTM D2520 (JIS C2565). The dielectric constant (Dk) and dielectric loss tangent (Df) of the plate-shaped resin molded body were measured at 9.4 GHz using a network analyzer (MS46122B, manufactured by Anritsu Corporation) and a coaxial resonator. They were compared with a resin molded body that did not contain powder (filler) and evaluated according to the following evaluation criteria.

[0088] Reduction rate (%) of dielectric constant (Dk) = (Dielectric constant without filler added - Dielectric constant with filler added) / Dielectric constant without filler added) x 100 ○: Reduction rate > 0 △: Reduction rate = 0 ×: Reduction rate <0

[0089] Reduction rate (%) of dielectric loss tangent (Df) = (Dielectric loss tangent without added filler - Dielectric loss tangent with added filler) / Dielectric loss tangent without added filler) x 100 ○: Reduction rate 30% or more △: Reduction rate is 20% or more but less than 30% ×: Reduction rate less than 20%

[0090] In addition, the resin composition was stored for 1000 hours under conditions of a temperature of 80° C. and a humidity of 80%, and the dielectric constant (Dk) and dielectric loss tangent (Df) were evaluated according to the following criteria (high temperature and high humidity test).

[0091] Relative ratio of dielectric constant (Dk) between front and rear = Dk(rear) / Dk(front) ○: 1.1 or less △: greater than 1.1 and less than 1.2 ×: Greater than 1.2

[0092] Relative ratio of front and rear dielectric tangents (Df) = Df(rear) / Df(front) ○: 2.0 or less △: greater than 2.0 and less than 3.0 ×: Greater than 3.0

[0093] The average particle size of the sprayed droplets in the first step was determined by the immersion method. Specifically, the sprayed droplets were received on a plate glass with a thick layer of silicone oil applied, and an enlarged photograph was quickly taken. The particle size was measured using the photograph, and the average particle size (Sauter mean particle size) was determined.

[0094] [Example 2] In the first step, a spray dryer with a two-fluid nozzle was used, and a water glass aqueous solution was sprayed from one nozzle at a flow rate of 0.29 L / hr, and air was sprayed from the other nozzle at a flow rate of 2040 L / hr to granulate hollow particles (air / liquid volume ratio was 7034). In the second step, 45000 g of a sulfuric acid aqueous solution with a concentration of 25% by mass was used. Except for these, the same procedure as in Example 1 was used to obtain a powder containing hollow particles.

[0095] [Example 3] In the second step, the liquid temperature was adjusted to be maintained at 60° C. Other than this, the same procedure as in Example 1 was carried out to obtain a powder containing hollow particles.

[0096] [Example 4] In the second step, 5000 g of hollow particles were added while stirring 80000 g of a 10% by mass aqueous hydrochloric acid solution. Except for this, a powder containing hollow particles was obtained in the same manner as in Example 1. In this example, the F edge distance was adjusted in the classification step so that particles exceeding 24 μm contained in the F powder (fine powder) were 5% by volume or less. In the second step, the solid content (SiO2) concentration was 4.4% by mass, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / Msp) was 5.6.

[0097] [Example 5] In the first step, the flow rate of the water glass aqueous solution was set to 0.25 L / hr (air / liquid volume ratio 8160). Furthermore, in the second step, the liquid was stirred for 15 hours while maintaining the liquid temperature at 60° C. Except for this, a powder containing hollow particles was obtained in the same manner as in Example 1.

[0098] [Comparative Example 1] In the first step, the SiO2 concentration of the water glass aqueous solution was set to 24 mass%, and the flow rate of this water glass aqueous solution was set to 0.40 L / hr (air / liquid volume ratio 5100). Furthermore, in the second step, 32,000 g of an aqueous sulfuric acid solution with a concentration of 25 mass% was used. Except for this, a powder containing hollow particles was obtained in the same manner as in Example 1. Note that in the second step, the solid content (SiO2) concentration was 10.2 mass%, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / M SP ) was 4.1.

[0099] [Comparative Example 2] In the first step, the SiO2 concentration of the water glass aqueous solution was set to 24 mass%, and the flow rate of this water glass aqueous solution was set to 0.48 L / hr (air / liquid volume ratio 4250). Furthermore, in the second step, 32,000 g of an aqueous sulfuric acid solution with a concentration of 25 mass% was used. Except for these, a powder containing hollow particles was obtained in the same manner as in Example 1. Note that in the second step, the solid content (SiO2) concentration was 10.2 mass%, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / M SP ) was 4.1.

[0100] In Comparative Examples 1 and 2, since a resin composition could not be obtained when the hollow particles were mixed at a ratio of 65% by volume, the ratio was adjusted to 60% by volume.

[0101] [Table 1]

Claims

1. A powder containing hollow particles having a cavity inside an outer shell, The shell contains 70% by mass or more of silica, The average particle size (D50) of the powder is 0.1 to 5.0 μm, The maximum particle size (D100) of the powder is 20.0 μm or less, When the peak particle diameter in the particle size distribution of the powder is represented by Ps, the volume ratio of particles in the range of (Ps) x 0.75 to (Ps) x 1.25 μm is 50% or less of the total particles; The porosity of the powder is 10 to 50%, The powder has a cracked particle rate of 10 volume % or less.

2. 2. The powder according to claim 1, having an alkali content of 100 ppm or less.

3. Oil absorption per unit volume is 0.60 ml / cm 3 The powder according to claim 1 or 2, wherein:

4. Sears number (ml / SiO 2 1.5g) is less than 0.30; The BET specific surface area measured by the water vapor adsorption method / the BET specific surface area measured by the nitrogen adsorption method is less than 0.30; The water vapor adsorption amount is less than 0.20% by mass, 29 3. The powder according to claim 1, wherein the peak area of ​​the Q4 structure is 90% or more of the total peak area in Si-NMR structural analysis.

5. 3. The powder according to claim 1, having a dielectric constant of 2.8 or less and a dielectric loss tangent of less than 0.0010.

6. A method for producing a resin composition, comprising the step of blending the powder according to claim 1 with a resin material.

7. a first step of forming droplets having an average particle diameter of 10.0 μm or less using an alkali silicate aqueous solution, spraying the droplets into a hot air current, and drying the droplets to form hollow particles; a second step of neutralizing the alkali contained in the hollow particles in an acid solution and then washing the particles; a third step of calcining the neutralized and washed hollow particles; A method for producing a powder containing hollow particles, comprising:

8. The method for producing powder according to claim 7, characterized in that the acid solution used in the second step satisfies the following formula: (M H+ / M SP )>4.7 ・・・Formula Here, (M H+ ) is the number of moles of hydrogen ions in the acid solution, (M SP ) is the value obtained by multiplying the number of moles of alkali metal ions contained in the hollow particles by the valence.

Citation Information

Patent Citations

  • Spherical inorganic hollow powder and its manufacturing process and resin composition

    JP2005206436A

  • Hollow silica particle

    JP2012136363A

  • Inorganic oxide hollow particles and production method thereof

    JP2020045263A

  • Hollow inorganic particles and method for producing the same

    JP2022019357A

  • Silica-based hollow particle, method for producing the same, and resin composition

    JP2022103683A

Cited By

  • Method for manufacturing hollow silica particles

    JP7943062B1