Decorative film
A decorative film with a (meth)acrylic resin base and tailored adhesive layer addresses adhesion and durability issues, allowing easy reapplication and preventing lifting on curved surfaces.
Patent Information
- Application Number
- JP2024049239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
AI Technical Summary
Decorative films using polyvinyl chloride or urethane resin face issues with adhesion and durability, leading to peeling, floating, and wrinkling on curved surfaces, and require improvements in reapplication and adhesion workability.
A decorative film comprising a base film made of (meth)acrylic resin with a specific adhesive layer containing (meth)acrylic copolymers and a crosslinking agent, where the copolymers have defined structural units and glass transition temperatures, enhancing adhesion and preventing lifting and wrinkling.
The film can be easily reapplied and prevents lifting, ensuring strong adhesion to curved surfaces without wrinkling or shock lines, even when using flexible materials.
Smart Images

Figure 2024146838000005 
Figure 2024146838000006 
Figure 2024146838000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative film. [Background technology]
[0002] In recent years, decorative films have been used instead of paint as a means of decorating the exterior of automobiles, in order to reduce the amount of solvent used and shorten construction times in line with the reduction of CO2 emissions in line with the SDGs. Polyvinyl chloride is often used as the resin material for decorative films for the exterior of automobiles due to its high formability, durability, and economical efficiency. However, polyvinyl chloride is prone to deterioration over time, and measures to improve weather resistance are required.
[0003] As one of such measures, a technique is known in which a surface protective layer of a fluororesin film is used in combination with a colored layer of polyvinyl chloride in order to suppress deterioration of polyvinyl chloride over time (see, for example, Patent Document 1). As another of the above measures, a decorative film for the exterior of an automobile is used that uses polyurethane, which is flexible and has excellent weather resistance, instead of polyvinyl chloride. As such a decorative film, for example, a decorative layer-forming film for the exterior of an automobile having a surface protective layer made of urethane resin is known (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-214434 A [Patent Document 2] JP 2021-143269 A Summary of the Invention [Problem to be solved by the invention]
[0005] A decorative film made by layering a polyvinyl chloride film and a fluororesin film has a significantly improved weather resistance of the polyvinyl chloride, but the fluororesin film is a hard film, so the entire decorative film is also a hard film. Therefore, if the decorative film is attached to a curved adherend surface such as an automobile, the decorative film may peel off and float over time.
[0006] A decorative film using urethane resin instead of polyvinyl chloride can conform to a curved or uneven surface because polyurethane is flexible, but the film is prone to excessive slack and wrinkles. In addition, shock lines may occur in the decorative film when the decorative film is reattached to the adherend in order to adjust the attachment position of the decorative film relative to the adherend. Therefore, decorative films using only urethane resin have room for improvement in terms of application.
[0007] For this reason, there is a demand for a decorative film that can be easily repositioned and that can be prevented from lifting off after application, even when a flexible base film is used.
[0008] Therefore, an object of the present invention is to provide a decorative film and related technologies that can prevent the film from lifting off after application and can be easily reapplied, even when a flexible base film is used. [Means for solving the problem]
[0009] The present invention provides the following aspects.
[0010] [1] A decorative film comprising a base film and a pressure-sensitive adhesive layer laminated on the base film, The base film contains a (meth)acrylic resin, the pressure-sensitive adhesive layer is a layer formed from a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (A), a (meth)acrylic copolymer (B), and a crosslinking agent, the (meth)acrylic copolymer (A) contains a structural unit (a1) derived from a monomer having an acidic functional group that undergoes a crosslinking reaction with the crosslinking agent, the content of the structural unit (a1) is 4.5% by mass or more and 15.0% by mass or less based on all structural units contained in the (meth)acrylic copolymer (A); The (meth)acrylic copolymer (A) has a glass transition temperature of −30° C. or higher and −15° C. or lower; the (meth)acrylic copolymer (B) contains a structural unit (b1) derived from a monomer having a polar group other than the acidic functional group, the content of the structural unit (b1) is 3.0% by mass or more and 15.0% by mass or less based on all structural units contained in the (meth)acrylic copolymer (B); The (meth)acrylic copolymer (B) has a glass transition temperature of 100° C. or higher; The content of the (meth)acrylic copolymer (B) is 3 parts by mass or more and 14 parts by mass or less based on 100 parts by mass of the (meth)acrylic copolymer (A), The decorative film, wherein the crosslinking agent is at least one of an epoxy-based crosslinking agent and a metal chelate-based crosslinking agent. [2] The decorative film according to [1], wherein the polar group is a hydroxyl group. [3] The decorative film according to [1] or [2], wherein the base film has a stress relaxation rate of 50% or more and 63% or less at 20°C. [4] The decorative film according to any one of [1] to [3], wherein the upper yield point load of the base film at 20° C. is 10.0 N / 10 mm or more and 45.0 N / 10 mm or less. [5] The decorative film according to any one of [1] to [4], wherein the (meth)acrylic copolymer (A) has a weight average molecular weight of 200,000 or more and 1,800,000 or less. [6] The decorative film according to any one of [1] to [5], wherein the (meth)acrylic copolymer (B) has a weight average molecular weight of 3,000 or more and 10,000 or less. Effect of the Invention
[0011] According to one aspect of the present invention, it is possible to provide a decorative film, and related techniques thereof, which can be easily repositioned even when a flexible base film is used, and which can prevent the film from lifting off after application. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing a layer structure of a decorative film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining an outline of a procedure for evaluating lifting of a decorative film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention. In addition, when multiple upper and lower limit values are described for a specific parameter, any of these upper and lower limit values can be combined to form a suitable numerical range.
[0014] [Decorative film] The decorative film of the present invention includes a substrate film containing a (meth)acrylic resin, and a pressure-sensitive adhesive layer laminated on the substrate film.
[0015] <Adhesive layer> The pressure-sensitive adhesive layer (hereinafter also referred to as "first pressure-sensitive adhesive layer") is a layer for attaching the decorative film of the present invention to an adherend that is the target of decoration. The pressure-sensitive adhesive layer is a layer formed from a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (A), a (meth)acrylic copolymer (B) and a crosslinking agent.
[0016] In this specification, the (meth)acrylic copolymer (A), the (meth)acrylic copolymer (B), and the (meth)acrylic resin refer to a resin (copolymer) in which (meth)acrylate is polymerized as the main monomer. Here, "(meth)acrylate" includes either one or both of "acrylate" and "methacrylate". In addition, (meth)acrylate refers to a (meth)acrylic acid ester.
[0017] (Adhesive composition) 1. (Meth)acrylic copolymer (A) The pressure-sensitive adhesive composition contains a (meth)acrylic copolymer (A). The (meth)acrylic copolymer (A) is a (meth)acrylic copolymer obtained by polymerizing a (meth)acrylate and a monomer having an acidic functional group (hereinafter, also simply referred to as an "acidic functional group") that undergoes a crosslinking reaction with a crosslinking agent. Thus, the (meth)acrylic copolymer (A) contains a structural unit (a2) derived from a (meth)acrylate and a structural unit (a1) derived from a monomer having an acidic functional group. In addition to these structural units, the (meth)acrylic copolymer (A) may contain a structural unit (a3) derived from another monomer.
[0018] Structural unit (a2) derived from (meth)acrylate The (meth)acrylic copolymer (A) contains a structural unit (a2) derived from a (meth)acrylate. A (meth)acrylate is an ester of an alcohol and (meth)acrylic acid. Examples of the alcohol include linear, branched, or cyclic alkyl alcohols, alkoxyalkyl alcohols, and alcohols having an aromatic ring. The number of carbon atoms in the alkyl alcohol is preferably 1 to 18, more preferably 1 to 12, and even more preferably 1 to 8.
[0019] Examples of the (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, i-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, i-nonyl (meth)acrylate, n-decyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; and (meth)acrylates having an aromatic ring such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate.
[0020] Of these (meth)acrylates, the (meth)acrylate constituting the structural unit (a2) is preferably an alkyl (meth)acrylate, more preferably at least one selected from the group consisting of methyl acrylate (MA), n-butyl acrylate (n-BA), and 2-ethylhexyl acrylate (2EHA), and even more preferably a combination of at least one of n-BA and 2EHA with MA.
[0021] The (meth)acrylic copolymer (A) may contain only one type of the structural unit (a2), or may contain two or more types. When the (meth)acrylic copolymer (A) contains, for example, two or more types of the structural unit (a2), the glass transition temperature of the (meth)acrylic copolymer (A) is easily adjusted to the range described below.
[0022] In the (meth)acrylic copolymer (A), the content of the structural unit (a2) may be, for example, 50.0 mass % or more and 95.5 mass % or less relative to all structural units (100.0 mass %) contained in the (meth)acrylic copolymer (A). The lower limit of the content of the structural unit (a2) is preferably 70.0% by mass or more, more preferably 80.0% by mass or more, and even more preferably 85.0% by mass or more. The upper limit of the content of the structural unit (a2) is preferably 95.0% by mass or less, more preferably 93.0% by mass or less, and even more preferably 92.0% by mass or less.
[0023] Structural unit (a1) derived from a monomer having an acidic functional group The (meth)acrylic copolymer (A) contains a structural unit (a1) derived from a monomer having an acidic functional group that undergoes a crosslinking reaction with a crosslinking agent. The acrylic copolymer (A) contains the structural unit (a1), so that the acidic functional group can undergo a crosslinking reaction with the crosslinking agent. This makes it possible to prevent the adhesive strength of the adhesive layer formed from the adhesive composition from increasing excessively when the decorative film is applied. In addition, since the initial adhesive strength of the adhesive layer does not increase excessively, it is possible to prevent the occurrence of shock lines in the decorative film during reapplication.
[0024] Examples of the acidic functional group include a carboxy group, a sulfonic acid group, a phosphoric acid group, etc. The monomer having an acidic functional group may be a monomer having an acidic functional group and an unsaturated double bond group. Examples of monomers having a carboxy group include acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, glutaconic acid, citraconic acid, ω-carboxy-polycaprolactone mono(meth)acrylate [e.g., ω-carboxy-polycaprolactone (n≒2) monoacrylate], and succinic acid esters [e.g., 2-acryloyloxyethyl-succinic acid]. Examples of monomers having a sulfonic acid group include (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, sodium vinylsulfonate, styrenesulfonic acid, allylsulfonic acid, and 2-(meth)acrylamido-2-methylpropanesulfonic acid. An example of a monomer having a phosphate group is 2-hydroxyethyl acryloyl phosphate. Among these, the monomer having an acidic functional group is preferably a monomer having a carboxy group, and more preferably at least one of acrylic acid (AA) and methacrylic acid (MAA).
[0025] The (meth)acrylic copolymer (A) may contain only one type of structural unit (a1), or may contain two or more types.
[0026] In the (meth)acrylic copolymer (A), the content of the structural unit (a1) is from 4.5% by mass to 15.0% by mass, based on all structural units (100.0% by mass) contained in the (meth)acrylic copolymer (A). The lower limit of the content of the structural unit (a1) is preferably 5.0% by mass or more, more preferably 5.5% by mass or more, even more preferably 6.0% by mass or more, and particularly preferably 6.5% by mass or more. The upper limit of the content of the structural unit (a1) is preferably 14.0% by mass or less, more preferably 13.0% by mass or less, and even more preferably 12.0% by mass or less. When the content of the structural unit (a1) is the lower limit or more, high adhesive strength can be exhibited to the adherend, and lifting after application can be prevented. In addition, when the content of the structural unit (a1) is the upper limit or less, the occurrence of zipping, shock lines, etc. can be suppressed during reapplication work. When the content of the structural unit (a1) is within the above range, in particular when the content of the structural unit (a2) is not less than the lower limit (e.g., not less than 85.0% by mass) and the content of the structural unit (a1) is within the above range (e.g., not less than 4.5% by mass and not more than 15.0% by mass), the glass transition temperature of the (meth)acrylic copolymer (A) can be suitably adjusted while the crosslinking reactivity with a crosslinking agent can be enhanced.
[0027] Structural units derived from other monomers (a3) The (meth)acrylic copolymer (A) may contain a structural unit (a3) derived from a monomer (other monomer) other than the (meth)acrylate and the monomer having an acidic functional group.
[0028] Other monomers include, for example, aromatic monovinyls such as styrene, α-methylstyrene, t-butylstyrene, p-chlorostyrene, chloromethylstyrene, and vinyltoluene; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate, and various derivatives of these monomers.
[0029] The content of the structural unit (a3) in the (meth)acrylic copolymer (A) is not particularly limited as long as it is within a range that does not impair the effects of the present invention. In one embodiment of the present invention, the (meth)acrylic copolymer (A) does not need to contain the structural unit (a3). When the (meth)acrylic copolymer (A) contains the structural unit (a3), the content of the structural unit (a3) may be, for example, 0.010 mass% or more and 10.0 mass% or less, preferably 0.010 mass% or more and 5.0 mass% or less, and more preferably 0.010 mass% or more and 3.0 mass% or less, relative to all structural units (100.0 mass%) contained in the (meth)acrylic copolymer (A).
[0030] Glass transition temperature (Tg) of (meth)acrylic copolymer (A) The glass transition temperature of the (meth)acrylic copolymer (A) is -30°C or higher and -15°C or lower. The lower limit of the glass transition temperature is preferably -28°C or higher, more preferably -26°C or higher, and even more preferably -25°C or higher. The upper limit of the glass transition temperature is preferably -17°C or lower, more preferably -18°C or lower, and even more preferably -20°C or lower. When the glass transition temperature of the (meth)acrylic copolymer (A) is at or above the lower limit, the initial adhesive strength of the pressure-sensitive adhesive layer can be prevented from increasing excessively during application of the decorative film, and the workability of reapplication can be improved while avoiding the occurrence of shock lines in the decorative film, particularly in the base film containing a (meth)acrylic resin. When the glass transition temperature of the (meth)acrylic copolymer (A) is at or below the upper limit, the decorative film can be prevented from lifting off the adherend.
[0031] The glass transition temperature (Tg) of the (meth)acrylic polymer (A) and the acrylic polymer such as the (meth)acrylic polymer (B) described later is a glass transition temperature calculated from the following formula 1, and is a value obtained by converting absolute temperature (unit: K; the same applies below) to Celsius temperature (unit: °C; the same applies below). 1 / Tg=m1 / Tg1+m2 / Tg2+ +m(k-1) / Tg(k-1)+mk / Tgk (Formula 1)
[0032] In formula 1, Tg1, Tg2, , Tg(k-1), and Tgk represent the glass transition temperatures expressed as absolute temperatures when each monomer constituting the (meth)acrylic copolymer is made into a homopolymer. m1, m2, , m(k-1), and mk represent the mole fractions of each monomer constituting the (meth)acrylic copolymer, and m1+m2+···+m(k-1)+mk=1.
[0033] For the glass transition temperature of homopolymers, values listed in the Polymer Handbook can be referred to, and for homopolymers not listed, measurements were performed using a differential scanning calorimeter (DSC) [model: EXSTAR6000, Seiko Instruments Inc.] under conditions of a nitrogen gas flow, 10 mg of a measurement sample, and a heating rate of 10°C / min, and the inflection point of the obtained DSC curve was taken as the glass transition temperature of the homopolymer. However, in this specification, the following values are referred to for the glass transition temperatures of the monomers shown below.
[0034] The glass transition temperatures of representative monomers for calculating the glass transition temperature of the (meth)acrylic copolymer by the above formula 1 are as follows: 2-ethylhexyl acrylate (2EHA) -70°C, 2-ethylhexyl methacrylate (2EHMA) -10°C, n-butyl acrylate (n-BA) -54°C, n-butyl methacrylate (n-BMA) 20°C, t-butyl acrylate (t-BA) 43°C, t-butyl methacrylate (t-BMA) 118°C, i-butyl methacrylate (i-BMA) 53°C, methyl acrylate (MA) 10°C, methyl methacrylate (MMA) 105°C, isobornyl methacrylate (IBXMA) 180°C, isobornyl methacrylate (IBXMA) 180°C, and isobornyl methacrylate (IBXMA) 180°C. The temperatures are: nyl acrylate (IBXA) at 94°C, ethyl acrylate (EA) at −22°C, methacrylic acid at 228°C, 4-hydroxybutyl acrylate (4HBA) at −80°C, 2-hydroxyethyl acrylate (2HEA) at −15°C, 2-hydroxyethyl methacrylate (2HEMA) at 85°C, 2-hydroxypropyl acrylate (2HPA) at −7°C, acrylic acid (AA) at 106°C, i-octyl acrylate (i-OA) at −65°C, dimethylaminoethyl methacrylate (DM) at 18°C, ω-carboxy-polycaprolactone (n≈2) monoacrylate at −30°C, and 2-acryloyloxyethyl-succinic acid at −40°C.
[0035] The glass transition temperature of the (meth)acrylic copolymer can be appropriately adjusted, for example, by using two or more monomers having different glass transition temperatures when made into a homopolymer. For example, by combining a monomer having a high glass transition temperature (high Tg monomer) with a monomer having a low glass transition temperature (low Tg monomer) to make a polymer, the glass transition temperature of the polymer can be adjusted to be between the glass transition temperature of the high Tg monomer used and the glass transition temperature of the low Tg monomer.
[0036] The weight average molecular weight (also referred to as "Mw") of the (meth)acrylic copolymer (A) may be, for example, 200,000 or more and 1,800,000 or less, preferably 300,000 or more and 1,000,000 or less, more preferably 350,000 or more and 800,000 or less, and even more preferably 400,000 or more and 600,000 or less. The weight average molecular weight of the (meth)acrylic copolymer is a value measured by gel permeation chromatography (GPC) using standard polystyrene standards, more specifically, a value measured by the method described in the examples.
[0037] Method for producing (meth)acrylic copolymer (A) The method for producing the (meth)acrylic copolymer (A) is not particularly limited, and for example, the (meth)acrylic copolymer (A) can be produced by polymerizing monomers corresponding to each structural unit of the copolymer (A) by a known polymerization method represented by solution polymerization method, emulsion polymerization method, suspension polymerization method, and bulk polymerization method. As the polymerization method, the solution polymerization method is preferable in that the processing step is relatively simple and can be carried out in a short time when preparing the pressure-sensitive adhesive composition after production.
[0038] 2. (Meth)acrylic copolymer (B) The pressure-sensitive adhesive composition includes a (meth)acrylic copolymer (B). The (meth)acrylic copolymer (B) is a (meth)acrylic copolymer in which a (meth)acrylate is polymerized, and includes a structural unit (b1) derived from a monomer having a polar group other than an acidic functional group (hereinafter, also simply referred to as a "polar group"). The (meth)acrylic copolymer (B) does not include a structural unit derived from a monomer having an acidic functional group. Therefore, by including the (meth)acrylic copolymer (B) in the pressure-sensitive adhesive composition that does not substantially undergo a crosslinking reaction with a crosslinking agent, the cohesive force of the pressure-sensitive adhesive layer is increased, and lifting of the decorative film can be prevented.
[0039] Structural unit (b1) having a polar group The (meth)acrylic copolymer (B) contains a structural unit (b1). The monomer having a polar group is not particularly limited, but from the viewpoint of compatibility, a (meth)acrylate having a polar group is preferred. The polar group is not particularly limited as long as it is a polar group other than an acidic functional group. Specific examples of the polar group include a hydroxyl group containing a methylol group, and an amide group. Among these, the polar group is preferably a hydroxyl group, and more preferably an alcoholic hydroxyl group. When the polar group is a hydroxyl group, the affinity of the pressure-sensitive adhesive layer to the adherend is further increased, and lifting of the decorative film can be further prevented.
[0040] Examples of monomers having a hydroxyl group include 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 3-methyl-3-hydroxybutyl (meth)acrylate, 1,1-dimethyl-3-hydroxybutyl (meth)acrylate, and 1,2-dimethyl-3-hydroxybutyl (meth)acrylate. Examples of such mono(meth)acrylates include butyl acrylate, 1,3-dimethyl-3-hydroxybutyl (meth)acrylate, 2,2,4-trimethyl-3-hydroxypentyl (meth)acrylate, 2-ethyl-3-hydroxyhexyl (meth)acrylate, N-hydroxyethyl (meth)acrylamide, glycerin mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and poly(ethylene glycol-propylene glycol) mono(meth)acrylate.
[0041] Among these monomers having a hydroxyl group, hydroxyalkyl (meth)acrylates are preferred, hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 1 to 4 carbon atoms are more preferred, at least one selected from the group consisting of 2-hydroxyethyl methacrylate (2HEMA), 2-hydroxyethyl acrylate (2HEA), and 4-hydroxybutyl acrylate (4HBA) is even more preferred, and 2-hydroxyethyl methacrylate (2HEMA) is particularly preferred.
[0042] The (meth)acrylic copolymer (B) may contain only one type of structural unit (b1), or may contain two or more types.
[0043] In the (meth)acrylic copolymer (B), the content of the structural unit (b1) is from 3.0 mass % to 15.0 mass % based on all structural units (100.0 mass %) contained in the (meth)acrylic copolymer (B). The lower limit of the content of the structural unit (b1) is preferably 4.0 mass% or more, more preferably 5.0 mass% or more, and even more preferably 6.0 mass% or more. The upper limit of the content of the structural unit (b1) is preferably 14.5 mass% or less, more preferably 14.0 mass% or less, and even more preferably 13.0 mass% or less. When the content of the structural unit (b1) is within the above range, the affinity of the pressure-sensitive adhesive layer to the adherend is increased, and lifting of the decorative film can be prevented.
[0044] Structural unit (b2) derived from a (meth)acrylate having no polar group The (meth)acrylic copolymer (B) preferably contains, in addition to the structural unit (b1), a structural unit (b2) derived from a (meth)acrylate having no polar group. By further containing the structural unit (b2) in the (meth)acrylic copolymer (B), when the pressure-sensitive adhesive layer is attached to an adherend having polarity, the increase in adhesive strength over time can be mitigated.
[0045] Examples of the (meth)acrylate having no polar group include the alkyl (meth)acrylates described in the section "1. (Meth)acrylic copolymer (A)". Among these, (meth)alkyl acrylates which are esters of alkyl alcohols and (meth)acrylic acid are preferred. The number of carbon atoms in the alkyl alcohol is preferably 1 to 18, more preferably 1 to 12, and even more preferably 1 to 8. The (meth)acrylate having no polar group is preferably at least one selected from the group consisting of MA, n-BA and t-butyl (meth)acrylate, among alkyl (meth)acrylates, and more preferably t-butyl (meth)acrylate.
[0046] The (meth)acrylic copolymer (B) may contain only one type of structural unit (b2), or may contain two or more types.
[0047] In the (meth)acrylic copolymer (B), the content of the structural unit (b2) may be, for example, 60.0 mass% or more and 97.0 mass% or less, preferably 70.0 mass% or more and 95.0 mass% or less, and more preferably 80.0 mass% or more and 94.0 mass% or less, relative to all structural units contained in the (meth)acrylic copolymer (B) (100.0 mass%).
[0048] Building blocks derived from other monomers (b3) The (meth)acrylic copolymer (B) may contain a structural unit (b3) derived from a monomer having a polar group and a monomer (other monomer) other than (meth)acrylate that does not have a polar group. Examples of the other monomer in the (meth)acrylic copolymer (B) include the same monomers as the other monomers in the (meth)acrylic copolymer (A).
[0049] The content of the structural unit (b3) in the (meth)acrylic copolymer (B) is not particularly limited as long as it is within a range that does not impair the effects of the present invention. In one embodiment of the present invention, the (meth)acrylic copolymer (B) does not need to contain the structural unit (b3). When the (meth)acrylic copolymer (B) contains the structural unit (b3), the content of the structural unit (b3) may be, for example, from 0.010 mass% to 10.0 mass% or less, preferably from 0.010 mass% to 5.0 mass% or less, and more preferably from 0.010 mass% to 3.0 mass% or less, relative to all structural units (100.0 mass%) contained in the (meth)acrylic copolymer (B).
[0050] The glass transition temperature of the (meth)acrylic copolymer (B) is 100°C or higher, and may be, for example, 100°C or higher and 150°C or lower. The lower limit of the glass transition temperature is preferably 105°C or higher, more preferably 108°C or higher, and even more preferably 110°C or higher. The upper limit of the glass transition temperature is preferably 140°C or lower, more preferably 130°C or lower, and even more preferably 120°C or lower. The glass transition temperature of the (meth)acrylic copolymer (B) is 100°C or higher, so that the adhesive layer can be prevented from lifting off an adherend having a curved portion. In addition, the (meth)acrylic copolymer (B), which has a higher glass transition temperature than the (meth)acrylic copolymer (A), does not substantially undergo a crosslinking reaction with the crosslinking agent, so that the adhesive layer formed from the adhesive composition can be prevented from excessively coagulating, and the decorative film can be suppressed from lifting off an adherend having a curved surface. Furthermore, the decorative film can be prevented from having a shock line during re-application.
[0051] The weight average molecular weight (also referred to as "Mw") of the (meth)acrylic copolymer (B) may be, for example, from 3,000 to 10,000, preferably from 3,000 to 9,000, more preferably from 3,000 to 8,000, even more preferably from 4,000 to 7,000, and particularly preferably from 4,000 to 6,000. The Mw of the (meth)acrylic copolymer (B) can be measured in the same manner as the Mw of the (meth)acrylic copolymer (A).
[0052] The content of the (meth)acrylic copolymer (B) in the pressure-sensitive adhesive composition is 3 parts by mass or more and 14 parts by mass or less based on 100 parts by mass of the (meth)acrylic copolymer (A). The lower limit of the content of the (meth)acrylic copolymer (B) is preferably 4 parts by mass or more, more preferably 5 parts by mass or more, and the upper limit of the content of the (meth)acrylic copolymer (B) is preferably 13 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 11 parts by mass or less. By including the (meth)acrylic copolymer (B) that contains the structural unit (b1) and does not substantially undergo a crosslinking reaction with a crosslinking agent within the above range, the cohesive strength of the pressure-sensitive adhesive layer is increased, and lifting of the decorative film can be prevented.
[0053] 3. Crosslinking Agent The adhesive composition includes a crosslinking agent. The crosslinking agent is a crosslinking agent that crosslinks the (meth)acrylic copolymer (A) by reacting with an acidic functional group. The crosslinking agent is not an isocyanate-based crosslinking agent, but at least one of an epoxy-based crosslinking agent and a metal chelate-based crosslinking agent, from the viewpoint of preferentially crosslinking with the acidic functional group. By using at least one of an epoxy-based crosslinking agent and a metal chelate-based crosslinking agent as the crosslinking agent, the (meth)acrylic copolymer (A) can be preferentially crosslinked. This prevents the adhesive strength of the decorative film having an adhesive layer formed from the adhesive composition from increasing excessively during application, while sufficiently increasing the adhesive strength of the adhesive layer after application. Therefore, it is possible to prevent the decorative film from lifting over time after application of the decorative film having an acrylic resin as a base film.
[0054] The epoxy crosslinking agent may be any compound having two or more epoxy groups. Examples of the epoxy crosslinking agent include ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polytetramethylene glycol diglycidyl ether, glycerol diglycidyl ether, resorcinol diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, adipic acid diglycidyl ester, fluoroglycidyl ether ... Epoxy compounds having two epoxy groups such as diglycidyl ester of tartaric acid; and epoxy compounds having three or more epoxy groups such as glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, tris(glycidyl)isocyanurate, tris(glycidoxyethyl)isocyanurate, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, sorbitol polyglycidyl ether, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine). Among these, epoxy compounds having three or more epoxy groups are preferred.
[0055] Examples of commercially available epoxy crosslinking agents include "TETRAD (registered trademark)-X" and "TETRAD (registered trademark)-C" (both manufactured by Mitsubishi Gas Chemical Company, Inc.), as well as "Denacol (registered trademark) EX-201" and "Denacol (registered trademark) EX-931" (both manufactured by Nagase ChemteX Corporation).
[0056] Examples of the metal chelate crosslinking agent include aluminum chelate compounds such as aluminum monoacetylacetonate bis(ethylacetoacetate), aluminum tris(ethylacetoacetate), and aluminum tris(acetylacetonate), titanium chelate compounds, zirconium chelate compounds, cobalt chelate compounds, etc. As the metal chelate crosslinking agent, for example, an aluminum chelate compound is preferred from the viewpoint of crosslinking speed.
[0057] Examples of commercially available metal chelate crosslinking agents include Aluminum Chelate A (trade name: aluminum tris(acetylacetonate), Kawaken Fine Chemicals Co., Ltd.), Aluminum Chelate D (trade name: aluminum monoacetylacetonate bis(ethylacetoacetate), Kawaken Fine Chemicals Co., Ltd.), and ALCH-TR (trade name: aluminum tris(ethylacetoacetate), Kawaken Fine Chemicals Co., Ltd.).
[0058] The content of the crosslinking agent may be designed according to the type of the crosslinking agent, and is not limited. The content of the crosslinking agent may be, for example, 0.01 to 4 parts by mass relative to 100 parts by mass of the (meth)acrylic copolymer (A), preferably 0.05 to 3 parts by mass, more preferably 0.1 to 3 parts by mass, even more preferably 0.1 to 2 parts by mass, and particularly preferably 0.1 to 1 part by mass. By making the content of the crosslinking agent equal to or more than the lower limit (for example, 0.01 parts by mass or more relative to 100 parts by mass of the (meth)acrylic copolymer (A)), the adhesive strength of the adhesive layer formed from the adhesive composition can be sufficiently increased. In addition, by making the content of the crosslinking agent equal to or less than the upper limit (for example, 4 parts by mass or less relative to 100 parts by mass of the (meth)acrylic copolymer (A)), the adhesive strength of the adhesive layer during application can be prevented from being excessively increased.
[0059] 4. Additives The pressure-sensitive adhesive composition may or may not contain additives such as an ultraviolet absorber, a light stabilizer, and an antioxidant, as long as the effects of the present invention are not impaired. When an additive is contained, the content of the additive may be, for example, 0.01 parts by mass or more and 5 parts by mass or less, preferably 0.01 parts by mass or more and 3 parts by mass or less, more preferably 0.01 parts by mass or more and 1 part by mass or less, and even more preferably 0.01 parts by mass or more and 0.1 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic copolymer (A).
[0060] (Adhesive layer) The pressure-sensitive adhesive layer is a layer formed from a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (A), a (meth)acrylic copolymer (B), and a crosslinking agent. That is, the pressure-sensitive adhesive layer is a layer derived from a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (A), a (meth)acrylic copolymer (B), and a crosslinking agent. The pressure-sensitive adhesive layer contains a component derived from the (meth)acrylic copolymer (A) and a component derived from the (meth)acrylic copolymer (B), and at least a part of the component derived from the (meth)acrylic copolymer (A) is linked by a partial structure derived from the crosslinking agent.
[0061] The thickness of the adhesive layer is preferably 20 μm or more and 60 μm or less, more preferably 22 μm or more and 55 μm or less, and even more preferably 25 μm or more and 50 μm or less. When the thickness of the adhesive layer is equal to or more than the lower limit (e.g., 25 μm or more), repositioning workability and adhesiveness are more likely to be improved. When the thickness of the adhesive layer is equal to or less than the upper limit (e.g., 60 μm or less), thermal shrinkage of the colored layer is easily suppressed. The thickness of the adhesive layer is measured with a micrometer and calculated as the average value of the measurements at five points. The thickness of the adhesive layer may be calculated by directly measuring the adhesive layer with a micrometer, or by subtracting the thickness of the two films from the total thickness when the adhesive layer is sandwiched between two films with specified thicknesses.
[0062] The adhesive strength of the decorative film to the adherend is affected by the rigidity of the base film. Therefore, if the rigidity of the base film is designed to be low in order to obtain a flexible decorative film, the rigidity of the entire decorative film also decreases, and the adhesive strength tends to decrease. However, even when a base film with low rigidity, i.e., a flexible base film, is used, by combining it with a pressure-sensitive adhesive layer with a certain degree of rigidity, the rigidity of the entire decorative film can be maintained, and a decorative film with sufficient adhesive strength can be obtained. Therefore, in one embodiment of the present invention, the storage modulus of the adhesive layer at 20°C is preferably 0.10 MPa or more and 0.60 MPa or less, more preferably 0.12 MPa or more and 0.55 MPa or less, and even more preferably 0.15 MPa or more and 0.50 MPa or less. When the storage modulus of the adhesive layer is equal to or less than the upper limit, the wettability of the adhesive layer to the adherend is improved, and lifting can be more effectively prevented. When the storage modulus of the adhesive layer is equal to or more than the lower limit, the rigidity of the entire decorative film including the adhesive layer can be maintained, and therefore a decorative film having sufficient adhesive strength can be obtained.
[0063] The loss tangent of the adhesive layer (loss modulus at 20°C / storage modulus at 20°C) is preferably 0.20 or more and 1.5 or less, more preferably 0.30 or more and 1.2 or less, and even more preferably 0.50 or more and 1.1 or less. When the loss tangent of the adhesive layer is equal to or less than the upper limit, the rigidity of the entire decorative film including the adhesive layer can be maintained, so that a decorative film having sufficient adhesive strength can be obtained. When the loss tangent of the adhesive layer is equal to or more than the lower limit, the wettability of the adhesive layer to the adherend is improved. Therefore, when the loss tangent of the adhesive layer is within the above-mentioned range, even a soft base film has sufficient adhesive strength and wettability, and lifting can be prevented.
[0064] The storage modulus and loss modulus of the pressure-sensitive adhesive layer at 20° C. can be measured using a dynamic viscoelasticity measuring device. More specifically, they can be measured by the method described in the Examples.
[0065] The method for forming the pressure-sensitive adhesive layer is not particularly limited, and any commonly used method can be used. In the decorative film of the present invention, the pressure-sensitive adhesive layer is laminated on the base film. One method for forming a pressure-sensitive adhesive layer on a substrate film includes the following method. The pressure-sensitive adhesive composition is applied onto a substrate film as is, or diluted with a solvent as necessary, to form a coating film. The formed coating film is then dried to form a pressure-sensitive adhesive film on the substrate film. The pressure-sensitive adhesive film formed on the substrate film is then cured to form a pressure-sensitive adhesive layer on the substrate film. In addition, the following method can be mentioned as another method for forming a pressure-sensitive adhesive layer on a substrate film. The pressure-sensitive adhesive composition is applied as it is or diluted with a solvent as necessary onto a release film such as paper or a resin film that has been surface-treated with a release agent, to form a coating film on the release film. Next, the formed coating film is dried to form a pressure-sensitive adhesive film on the release film. Thereafter, the exposed surface of the formed pressure-sensitive adhesive film is brought into contact with the substrate film and pressed, and the pressure-sensitive adhesive film is transferred to the substrate to form a pressure-sensitive adhesive film on the substrate film. Finally, the formed pressure-sensitive adhesive film is cured to form a pressure-sensitive adhesive layer on the substrate film.
[0066] Examples of the solvent for diluting the pressure-sensitive adhesive composition include aromatic hydrocarbon compounds such as benzene, toluene, ethylbenzene, n-propylbenzene, t-butylbenzene, o-xylene, m-xylene, p-xylene, tetralin, decalin, and aromatic naphtha; aliphatic or alicyclic hydrocarbon compounds such as n-hexane, n-heptane, n-octane, i-octane, n-decane, dipentene, petroleum spirit, petroleum naphtha, and turpentine oil; ester compounds such as ethyl acetate, n-butyl acetate, n-amyl acetate, 2-hydroxyethyl acetate, 2-butoxyethyl acetate, 3-methoxybutyl acetate, and methyl benzoate; acetone, methyl ethyl ketone, methyl Examples of the dilution solvent include ketone compounds such as ethyl-i-butyl ketone, isophorone, cyclohexanone, and methylcyclohexanone; glycol ether compounds such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether; and alcohol compounds such as methyl alcohol, ethyl alcohol, n-propyl alcohol, i-propyl alcohol, n-butyl alcohol, i-butyl alcohol, s-butyl alcohol, and t-butyl alcohol. The dilution solvent may be used alone or in combination of two or more.
[0067] Among these solvents, aromatic hydrocarbon compounds, ester compounds and ketone compounds are preferred, and from the viewpoint of the solubility of the (meth)acrylic copolymer, ethyl acetate is more preferred.
[0068] When the pressure-sensitive adhesive composition is diluted with a solvent, the solid content concentration of the diluted pressure-sensitive adhesive composition is, from the viewpoint of coatability, preferably 3% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 15% by mass or less, and even more preferably 8% by mass or more and 13% by mass or less, based on the total amount of the diluted pressure-sensitive adhesive composition. The solid content of the pressure-sensitive adhesive composition refers to all components of the diluted pressure-sensitive adhesive composition excluding the liquid medium such as the solvent.
[0069] The release film is not particularly limited as long as it can be easily peeled off from the pressure-sensitive adhesive layer, and examples include resin films that have been surface-treated with a release agent on one or both sides (so-called easy-peeling treatment). An example of the resin film is a polyester film, typically a polyethylene terephthalate (PET) film. Examples of the release agent include fluorine-based resins, paraffin wax, silicone, and long-chain alkyl group compounds. In the decorative film of the present invention, the exposed pressure-sensitive adhesive layer may be protected by a release film. When the pressure-sensitive adhesive layer is protected by a release film, the release film is peeled off during application of the decorative film.
[0070] The method for applying the pressure-sensitive adhesive composition onto the substrate or release film is not particularly limited, and examples thereof include known methods using a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a knife coater, a spray coater, a bar coater, an applicator, etc. The amount of the adhesive composition applied onto the substrate or release film is appropriately determined depending on the thickness of the adhesive layer to be formed.
[0071] The method for drying the coating film formed on the substrate or release film is not particularly limited, and examples thereof include natural drying, heat drying, hot air drying, and vacuum drying. The drying temperature and drying time of the coating film are not particularly limited and are appropriately set depending on the thickness of the coating film, the amount of organic solvent in the coating film, etc. An example of the drying conditions is drying at 70°C to 120°C for 1 minute to 3 minutes using a hot air dryer.
[0072] The curing may be carried out for 4 to 7 days in an environment of, for example, 20° C. to 35° C. By curing, the crosslinking reaction of the pressure-sensitive adhesive composition is completed, and a pressure-sensitive adhesive layer is formed.
[0073] <Base film> The base film contains a (meth)acrylic resin, which allows the base film to maintain its overall rigidity compared to a single urethane layer, and increases the stress relaxation rate, thereby preventing the film from sagging and causing wrinkles. When the base film includes a plurality of layers, it is sufficient that at least one layer included in the base film includes a (meth)acrylic resin. "(Meth)acrylic resin" is a general term for acrylic resin and methacrylic resin.
[0074] The substrate film may include two or more layers, and preferably includes a surface protective layer and a colored layer. When the substrate film includes a surface protective layer and a colored layer, the colored layer is protected by the surface protective layer, so that deterioration of the decorative film can be prevented, and color fading of the colored layer due to friction can be prevented. When the substrate film includes a surface protective layer and a colored layer, from the viewpoint of ensuring weather resistance and solvent resistance, it is preferable that the (meth)acrylic resin is included in the colored layer.
[0075] (colored layer) The colored layer preferably contains a (meth)acrylic resin. From the viewpoint of weather resistance, the (meth)acrylic resin may be a resin material that provides sufficient weather resistance to the decorative film by itself, or may be a resin material that provides sufficient weather resistance to the decorative film by using it in combination (laminate structure) with a resin other than the (meth)acrylic resin, such as a polyurethane resin. The (meth)acrylic resin contained in the colored layer may be one type of resin, or may be a combination of two or more types of resins with different hardness. Examples of hard resins with relatively high hardness in the combination include hard (meth)acrylic resins used in films, sheets, etc. formed by melt extrusion. Examples of soft (meth)acrylic resins with relatively low hardness in the combination include resins for adjusting flowability and resins for soft materials. From the viewpoint of adjusting the mechanical properties of the base film and the decorative film including the base film and realizing the physical properties described below, it is preferable that the (meth)acrylic resin includes a hard (meth)acrylic resin and a soft (meth)acrylic resin.
[0076] A hard (meth)acrylic resin is a (meth)acrylic resin that, when made into a sheet material of 100 μm in thickness and 10 mm in width, has an upper yield point load of 10.0 N / 10 mm or more at 20°C. A soft (meth)acrylic resin is a (meth)acrylic resin that, when made into a sheet material of 100 μm in thickness and 10 mm in width, has an upper yield point load of less than 10.0 N / 10 mm at 20°C.
[0077] The upper yield point load of the (meth)acrylic resin can be determined by measuring a 10 mm wide sample with a known measuring device such as a Tensilon universal testing machine. The upper yield point load is the load at the upper yield point of the sample observed in a tensile test, and since it is a load measured using a 10 mm wide sample, the unit is expressed as "N / 10 mm".
[0078] The upper yield point load of the rigid (meth)acrylic resin at 20° C. may be, for example, 10.0 N / 10 mm or more and 35 N / 10 mm or less, from the viewpoint of obtaining sufficient application properties of the decorative film (suppression of wrinkles during application) and curved surface conformability. The lower limit of the upper yield point load of the rigid (meth)acrylic resin at 20° C. is preferably 15.0 N / 10 mm or more, more preferably 20.0 N / 10 mm or more, from the viewpoint of improving the workability of the decorative film. The upper limit of the upper yield point load of the rigid (meth)acrylic resin at 20° C. is preferably 30.0 N / 10 mm or less, more preferably 28.0 N / 10 mm or less, from the viewpoint of improving the curved surface conformability of the decorative film.
[0079] The hard (meth)acrylic resin may be a (meth)acrylic resin having a Shore A hardness of more than 90. The Shore A hardness may be, for example, more than 90 and not more than 150, preferably not less than 95 and not more than 130, and more preferably not less than 98 and not more than 120. It should be noted that "Shore A hardness" can be measured, for example, using a durometer GS-706N manufactured by Techclock Corporation, and refers to the maximum value when a Type A sensor is pressed perpendicularly against the surface of the object to be measured with a load of 1 kg.
[0080] The hard (meth)acrylic resin can be prepared by radical polymerization of known monomers capable of constituting a (meth)acrylic resin. Examples of hard (meth)acrylic resins include polymethyl methacrylate and methyl methacrylate-styrene copolymers.
[0081] The rigid (meth)acrylic resin is preferably a resin having a Shore A hardness of more than 90 and a molded product thereof having an upper yield point load of 10.0 N / 10 mm or more at 20° C. The rigid (meth)acrylic resin may be a commercially available product, examples of which include Parapet (registered trademark) GR-F1000P (Kuraray Co., Ltd.), Kane Ace (registered trademark) MC-732 (Kaneka Co., Ltd.), Dianale LP-3202, 3207, 3130, and 3121 (all Mitsubishi Chemical Co., Ltd.), and Delpet (Asahi Kasei Co., Ltd.).
[0082] The upper yield point load of the soft (meth)acrylic resin at 20° C. may be, for example, 2.0 N / 10 mm or more and less than 10.0 N / 10 mm from the viewpoint of obtaining sufficient application properties of the decorative film (suppression of wrinkles during application) and curved surface conformability. The lower limit of the upper yield point load of the soft (meth)acrylic resin at 20° C. is preferably 3.0 N / 10 mm or more, more preferably 3.5 N / 10 mm or more, from the viewpoint of improving the workability of the decorative film. The upper limit of the upper yield point load of the soft (meth)acrylic resin at 20° C. is preferably 7.0 N / 10 mm or less, more preferably 5.0 N / 10 mm or less, from the viewpoint of improving the curved surface conformability of the decorative film.
[0083] The soft (meth)acrylic resin may be a resin having a Shore A hardness of 50 or more and 90 or less. The Shore A hardness is preferably 60 or more and 85 or less, more preferably 65 or more and 80 or less, and further preferably 70 or more and 75 or less.
[0084] The soft (meth)acrylic resin is preferably a resin having a Shore A hardness of 50 or more and 90 or less, and a molded product thereof has an upper yield point load of less than 10.0 N / 10 mm at 20° C. The soft (meth)acrylic resin may be a commercially available product, and an example thereof is Parapet (registered trademark) SA-F1000P (Kuraray Co., Ltd.).
[0085] At least one of the hard (meth)acrylic resin and the soft (meth)acrylic resin may be a resin composition containing core-shell particles in which core particles having rubber elasticity are covered with acrylic resin. Examples of commercially available resin compositions containing core-shell particles include Parapet (registered trademark) GR-F1000P and SA-F1000P (Kuraray Co., Ltd.). The resin composition containing core-shell particles may be formed by polymerization of a monomer mixture consisting of a (meth)acrylic acid ester, a multifunctional monomer copolymerizable therewith, and another monofunctional monomer. At least one of the hard (meth)acrylic resin and the soft (meth)acrylic resin may be a thermoplastic elastomer.
[0086] Among the (meth)acrylic acid esters, examples of the acrylic acid esters include esters of acrylic acid and saturated aliphatic alcohols having 1 to 18 carbon atoms, esters of acrylic acid and alicyclic alcohols having 5 or 6 carbon atoms, and esters of acrylic acid and phenols or aromatic alcohols. Specific examples of acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, octadecyl acrylate, cyclohexyl acrylate, phenyl acrylate, and benzyl acrylate.
[0087] Among the (meth)acrylic acid esters, examples of methacrylic acid esters include esters of methacrylic acid and saturated aliphatic alcohols having 1 to 22 carbon atoms, esters of methacrylic acid and alicyclic alcohols having 5 or 6 carbon atoms, and esters of methacrylic acid and phenols or aromatic alcohols. Specific examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, and benzyl methacrylate.
[0088] Examples of polyfunctional monomers include esters of unsaturated monocarboxylic acids and unsaturated alcohols, diesters of unsaturated monocarboxylic acids and glycols, esters of dicarboxylic acids and unsaturated alcohols, aromatic divinyl monomers, and conjugated diene monomers. Examples of unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and cinnamic acid. Examples of unsaturated alcohols include allyl alcohol and methallyl alcohol. Examples of glycols include ethylene glycol, butanediol, and hexanediol. Examples of dicarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, and maleic acid. Examples of conjugated diene monomers include butadiene, isoprene, 2,3-dimethylbutadiene, 2-methyl-3-ethylbutadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 2-ethyl-1,3-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 3,4-dimethyl-1,3-hexadiene, 1,3-heptadiene, 3-methyl-1,3-heptadiene, 1,3-octadiene, cyclopentadiene, chloroprene, and myrcene. Specific examples of polyfunctional monomers include allyl acrylate, methallyl acrylate, allyl methacrylate, methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate. Incidentally, "(meth)acrylate" is a general term for acrylate and methacrylate, and refers to either or both of them.
[0089] Examples of monofunctional monomers include aromatic vinyl monomers and vinyl cyanide monomers.
[0090] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrenes.
[0091] Examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile.
[0092] The upper yield point load of the colored layer at 20° C. is preferably, for example, 8.3 N / 10 mm or more and 13.2 N / 10 mm or less. The lower limit of the upper yield point load of the colored layer at 20 ° C. is preferably 8.3 N / 10 mm or more, more preferably 9.0 N / 10 mm or more, and even more preferably 10.0 N / 10 mm or more, from the viewpoint of improving the application property. The upper limit of the upper yield point load of the colored layer at 20 ° C. is preferably 13.2 N / 10 mm or less, more preferably 12.0 N / 10 mm or less, and even more preferably 11.0 N / 10 mm or less, from the viewpoint of improving the curved surface followability. If the upper yield point load of the colored layer at 20 ° C. is the lower limit or more, it tends to be easy to suppress the occurrence of wrinkles when attaching the decorative film. In addition, if the upper yield point load of the colored layer at 20 ° C. is the upper limit or less, it tends to be easy to suppress the occurrence of lifting after application. The upper yield point load of the colored layer can be adjusted by using (meth)acrylic resins with different upper yield point loads in an appropriate amount ratio.
[0093] The colored layer preferably contains a (meth)acrylic resin and a colorant. For example, the colored layer may be a layer in which the colorant is dispersed in a continuous phase of the (meth)acrylic resin.
[0094] The colorant that can be contained in the colored layer may be a known pigment or dye that is used in paint for printing on a resin film. The colorant may be one type or a combination of two or more types. The colorant is used in an amount according to the desired color to be expressed in the decorative film. Examples of white colorants include titanium oxide and barium sulfate. Examples of black colorants include iron black, carbon black, and aniline black. Examples of yellow colorants include cadmium yellow and oil yellow 2G. Examples of orange colorants include chrome vermilion and cadmium orange. Examples of red colorants include cadmium red, permanent red 4R, and oil red. Examples of purple colorants include cobalt violet and anthraquinone violet. Examples of blue colorants include ultramarine, Prussian blue, and cobalt blue. Examples of green colorants include phthalocyanine green and chrome green.
[0095] The thickness of the colored layer may be, for example, 60 μm or more and 150 μm or less. From the viewpoint of fully expressing the desired chromaticity, the lower limit of the thickness of the colored layer is preferably 60 μm or more, more preferably 80 μm or more, and even more preferably 100 μm or more. The upper limit of the thickness of the colored layer can be appropriately determined from the above viewpoint, and may be, for example, 150 μm or less, 130 μm or less, or 110 μm or less. The thickness of the colored layer is measured with a micrometer and calculated as the average value of the measurements at five points.
[0096] (Surface protective layer) The surface protective layer is a layer overlapping the colored layer. The upper yield point load of the surface protective layer at 20° C. is preferably, for example, 4.5 N / 10 mm or more and 6.0 N / 10 mm or less. The lower limit of the upper yield point load of the surface protective layer at 20°C is preferably 4.5N / 10mm or more, more preferably 5.0N / 10mm or more, and even more preferably 5.2N / 10mm or more, from the viewpoint of improving the ease of application. The upper limit of the upper yield point load of the surface protective layer at 20°C is preferably 6.0N / 10mm or less, more preferably 5.9N / 10mm or less, from the viewpoint of improving the curved surface conformability. If the upper yield point load is the lower limit or more, it tends to be easier to suppress the occurrence of wrinkles when applying the decorative film. If the upper yield point load is the upper limit or less, it tends to be easier to suppress the occurrence of lifting after application. The upper yield point load of the surface protective layer can be adjusted by using one type of relatively soft resin material alone or by using two or more types in combination.
[0097] The surface protective layer preferably contains a polyurethane resin. The polyurethane resin is preferably a resin that can be designed so that the upper yield point load of the surface protective layer at 20°C can be at least 4.5 N / 10 mm, more preferably a resin that can be designed so that the upper yield point load can be set to 4.5 N / 10 mm or more and 6.0 N / 10 mm or less, and even more preferably a resin that can be designed so that the upper yield point load of the surface protective layer can be set to 4.5 N / 10 mm or more and 5.9 N / 10 mm or less. The polyurethane resin is preferably a resin material capable of realizing the upper yield point load and stress relaxation rate of the decorative film described below. The polyurethane resin or its material is preferably selected from one-component thermoplastic resins used for film and sheet molding, or thermoplastic resins or thermoplastic elastomers for melt molding.
[0098] The polyurethane resin may be a resin material that imparts sufficient weather resistance to the decorative film by itself, or may be a resin material that imparts sufficient weather resistance to the decorative film by combining with a (meth)acrylic resin (laminate structure). The polyurethane resin may be one type, or two or more types may be combined. Examples of polyurethane resins include polycarbonate-based urethane resins and polycaprolactone-based urethane resins. These urethane resins have a main chain of polycaprolactone or polycarbonate, etc., and a urethane structure. The urethane structure is preferably a urethane structure derived from an aliphatic isocyanate or an alicyclic isocyanate. The urethane resin may be a commercially available product, and examples thereof include Resamine (registered trademark) NE (Dainichiseika Color & Chemicals Mfg. Co., Ltd.), Miractoran (registered trademark) E (Nihon Miractoran Co., Ltd.), and CRISBON (registered trademark) NY (DIC Corporation).
[0099] The thickness of the surface protection layer may be, for example, 15 μm or more and 60 μm or less. From the viewpoint of protecting the colored layer with a sufficient thickness, the lower limit of the thickness of the surface protective layer is preferably 15 μm or more, more preferably 20 μm or more, and further preferably 30 μm or more. The upper limit of the thickness of the surface protective layer can be appropriately determined from the above viewpoint, and may be, for example, 60 μm or less, 50 μm or less, or 40 μm or less. The thickness of the surface protective layer is measured by a macrometer and calculated as the average value of the measurements at five points.
[0100] The colored layer and the surface protective layer may further contain other components other than the resin and the colorant within a range in which the effects of the present invention can be obtained. Examples of such other components include ultraviolet absorbers, light stabilizers, plasticizers, and extender pigments. An example of an extender pigment is calcium carbonate. The content of the other components in each layer can be appropriately set within a range in which both the effects of the present invention and the effects of the other components can be obtained.
[0101] The colored layer and the surface protective layer preferably contain an ultraviolet absorbing agent and a light stabilizer from the viewpoint of improving weather resistance. Examples of the ultraviolet absorbing agent include benzotriazole-based compounds, benzophenone-based compounds, cyanoacrylate-based compounds, ultrafine particles of zinc oxide and titanium oxide, etc. Examples of the light stabilizer include hindered amine-based compounds.
[0102] The colored layer and the surface protective layer described above can achieve the effects of the present invention without containing other components. For example, in this embodiment, by using a soft polyurethane resin and two (meth)acrylic resins with different hardness, it is possible to achieve the upper yield point load and stress relaxation rate described below without containing a plasticizer. In this way, the embodiment in which the decorative film does not contain other components (such as plasticizers) for adjusting the upper yield point load and stress relaxation rate is a preferred embodiment.
[0103] The "other components for adjusting the upper yield point load and the stress relaxation rate" may be used in an amount that affects the upper yield point load and the stress relaxation rate. Components that exhibit the intended function but do not substantially affect the upper yield point load and the stress relaxation rate, such as ultraviolet absorbers and light stabilizers, are not included in the "other components for adjusting the upper yield point load and the stress relaxation rate." An embodiment in which the colored layer and the surface protective layer do not contain a plasticizer is a preferred embodiment from the viewpoint of suppressing bleeding out of the plasticizer.
[0104] (other layers) The base film may further have layers other than the colored layer and the surface protective layer. Examples of such layers include a second adhesive layer other than the above-mentioned first adhesive layer. When the base film has multiple layers (for example, a surface protective layer and a colored layer), the second adhesive layer bonds between the multiple layers.
[0105] For example, the base film may further have a second adhesive layer interposed between the colored layer and the surface protective layer to bond the two layers to each other. The thickness of the second adhesive layer may be appropriately set depending on the type of adhesive layer and the object to be adhered, for example, from within the range of 3 μm or more and 70 μm or less, preferably 10 μm or more and 50 μm or less, more preferably 15 μm or more and 45 μm or less, and even more preferably 20 μm or more and 40 μm or less. The thickness of the second pressure-sensitive adhesive layer is measured with a micrometer and calculated as the average value of measurements at five points.
[0106] The second adhesive layer can be made of various known adhesives such as rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, polyvinyl ether-based adhesives, etc. The second adhesive layer may be made of an adhesive composition for forming the adhesive layer constituting the decorative film of the present invention.
[0107] (Base film) The upper yield point load of the substrate film at 20° C. may be, for example, 10.0 N / 10 mm or more and 45.0 N / 10 mm or less. The lower limit of the upper yield point load of the substrate film at 20 ° C. is preferably 13.7 N / 10 mm or more, more preferably 15.0 N / 10 mm or more, and even more preferably 17.0 N / 10 mm or more, from the viewpoint of improving the pasting workability. The upper limit of the upper yield point load of the substrate film at 20 ° C. is preferably 30.0 N / 10 mm or less, more preferably 25.0 N / 10 mm or less, even more preferably 20.0 N / 10 mm or less, even more preferably 19.0 N / 10 mm or less, and particularly preferably 18.0 N / 10 mm or less, from the viewpoint of improving the curved surface followability. If the upper yield point load is the lower limit or more, it tends to be easier to suppress the occurrence of wrinkles during pasting work. Also, if the upper yield point load is the upper limit or less, it tends to be easier to suppress the occurrence of lifting after pasting work. The upper yield point load of the substrate film is the boundary load at which the deformation of the substrate film changes from elastic deformation to plastic deformation when a load is applied to the substrate film. The temperature of the substrate film when the upper yield point load is measured is 20°C. The upper yield point load of the substrate film can be adjusted by the upper yield point loads or material resins of the colored layer and the surface protective layer.
[0108] In this specification, unless otherwise specified, when the base film is a laminate having a laminate structure, the upper yield point load of the base film means the upper yield point load of the laminate.For example, when the base film is a laminate having a surface protective layer and a colored layer, the upper yield point load of the base film means the upper yield point load of the laminate of the surface protective layer and the colored layer.In addition, when the base film is a laminate further having a second adhesive layer, the upper yield point load of the base film means the upper yield point load of the laminate composed of the surface protective layer, the second adhesive layer, and the colored layer stacked in this order.
[0109] The stress relaxation rate of the base film at 20°C is preferably, for example, 50% or more and 63% or less. The stress relaxation rate of the base film is the rate of change in tensile load before and after stretching when a tensile load that stretches the base film by 5% (to 105% of its length) is applied for 5 minutes. The temperature of the base film when measuring the stress relaxation rate is 20°C. The stress relaxation rate of the base film is calculated from the following formula, where x is the tensile load immediately after 5% stretching and y is the tensile load 5 minutes after 5% stretching. Stress relaxation rate z[%]={(xy) / x}×100
[0110] The lower limit of the stress relaxation rate of the base film is preferably 51% or more, more preferably 53% or more, and even more preferably 55% or more, from the viewpoint of improving the ease of application. The upper limit of the stress relaxation rate of the base film is preferably 60% or less, more preferably 58% or less, and even more preferably 57% or less, from the viewpoint of improving the ability to follow curved surfaces. If the stress relaxation rate of the base film is the lower limit or more, it tends to be easier to suppress the occurrence of wrinkles when the decorative film is applied. If the stress relaxation rate of the base film is the upper limit or less, it tends to be easier to suppress the occurrence of lifting after application.
[0111] The stress relaxation rate of the base film can be determined by measuring the tensile load with a known measuring device such as a Tensilon universal testing machine. The stress relaxation rate of the base film can be adjusted by adjusting the material resins of the colored layer and the surface protective layer or the thicknesses of both layers.
[0112] In this specification, unless otherwise specified, when the base film is a laminate having a laminated structure, the stress relaxation rate of the base film means the stress relaxation rate of the laminate.For example, when the base film is a laminate having a surface protective layer and a colored layer, the stress relaxation rate of the base film means the stress relaxation rate of the laminate of the surface protective layer and the colored layer.In addition, when the base film is a laminate further having a second adhesive layer, the upper yield point load of the base film means the stress relaxation rate of the laminate composed of the surface protective layer, the second adhesive layer and the colored layer stacked in this order.
[0113] The thickness of the base film of this embodiment is represented by, for example, the total thickness of the surface protective layer, the colored layer, and the second adhesive layer. The thickness of the base film can be appropriately determined according to the application of the decorative film. The thickness of the base film may be, for example, 100 μm or more and 200 μm or less. The lower limit of the thickness of the base film is preferably 100 μm or more, more preferably 120 μm or more, even more preferably 140 μm or more, even more preferably 150 μm or more, and particularly preferably 160 μm or more, from the viewpoint of adjusting at least one of the application property and the curved surface conformability. The upper limit of the thickness of the base film is preferably 200 μm or less, more preferably 180 μm or less, and even more preferably 170 μm or less, from the viewpoint of fully expressing the curved surface conformability. When the thickness of the base film is the lower limit or more, sufficient application property and curved surface conformability can be obtained. Also, when the thickness of the base film is the upper limit or less, sufficient curved surface conformability can be obtained.
[0114] (Method of manufacturing base film) The substrate film can be produced by a method that enables the surface protective layer and the colored layer to be laminated in this order, for example.
[0115] For example, the base film can be produced by a method including the steps of preparing a colored layer, preparing a surface protective layer, and attaching the surface protective layer to the colored layer.
[0116] The step of preparing the colored layer may be a step of mixing a (meth)acrylic resin and a colorant and forming a film of the mixture obtained. The film formation of the colored layer may be performed, for example, by extrusion molding or calendar molding. The step of preparing the surface protective layer may be a step of producing a layer of a urethane resin, or a step of applying a material for the surface protective layer to one surface of the colored layer to form a coating film, and then solidifying or curing the coating film.
[0117] The step of attaching the surface protective layer to the colored layer may be, for example, a step of directly bonding the colored layer and the surface protective layer by heat fusion or the like. The step of attaching the surface protective layer to the colored layer may also be a step of supplying the material of the other layer in a layered form to one surface of a colored layer or a surface protective layer prepared in advance, and bonding the other layer onto the one layer to form the other layer. Furthermore, the step of attaching the surface protective layer to the colored layer may be a step of attaching the surface protective layer to the second adhesive layer obtained by applying a second adhesive layer to one surface of the colored layer. Attaching the colored layer and the surface protective layer via the second adhesive layer is advantageous from the viewpoint of increasing the degree of freedom in material design of both layers.
[0118] <Decorative film> The decorative film of the present invention includes a base film and an adhesive layer, and the base film and the adhesive layer are the specific base film and adhesive layer described above. Therefore, even when a flexible base film is used, the decorative film of the present invention can prevent lifting after application, and can also suppress the occurrence of shock lines and zipping during reapplication, making it easy to reapplication. The decorative film of one embodiment of the present invention is flexible and has high curved surface conformability, and can prevent lifting after application, and can also suppress the occurrence of shock lines and zipping during reapplication, making it easy to reapplication.
[0119] The decorative film preferably has an adhesive strength of 4.0 N / 10 mm or more and 6.0 N / 10 mm or less one hour after the adhesive layer of the decorative film is attached to the adherend. The lower limit of the adhesive strength after one hour is preferably 4.2 N / 10 mm or more, more preferably 4.4 N / 10 mm or more, from the viewpoint of preventing lifting after application. The upper limit of the adhesive strength after one hour is preferably 5.5 N / 10 mm or less, more preferably 5.0 N / 10 mm or less, from the viewpoint of suppressing the occurrence of shock lines and zipping. If the adhesive strength after one hour is equal to or less than the upper limit, the workability of reapplication of the decorative film is improved. The decorative film preferably has an adhesive strength of, for example, 5.0 N / 10 mm or more and 20.0 N / 10 mm or less 168 hours after the adhesive layer of the decorative film is attached to the adherend. The lower limit of the adhesive strength after 168 hours is preferably 5.5 N / 10 mm or more, more preferably 6.0 N / 10 mm or more, from the viewpoint of preventing lifting after application. The upper limit of the adhesive strength after 168 hours is preferably 15.0 N / 10 mm or less, more preferably 10.0 N / 10 mm or less, from the viewpoint of repositionability due to deterioration over time.
[0120] The adhesive strength of the decorative film to the adherend is affected by the rigidity of the base film and the rigidity of the adhesive layer. Therefore, when the rigidity of the base film is reduced to obtain a flexible decorative film, the rigidity of the adhesive layer is increased to obtain a decorative film that is flexible and has high adhesive strength to the adherend. Therefore, in one embodiment of the present invention, the decorative film preferably comprises a base film having an upper yield point load at 20°C of 10.0 N / 10 mm or more and 45.0 N / 10 mm or less and an adhesive layer having a storage modulus at 20°C of 0.10 MPa or more and 0.60 MPa or less, more preferably a base film having an upper yield point load at 20°C of 13.7 N / 10 mm or more and 30.0 N / 10 mm or less and an adhesive layer having a storage modulus at 20°C of 0.12 MPa or more and 0.55 MPa or less, and even more preferably a base film having an upper yield point load at 20°C of 15.0 N / 10 mm or more and 20.0 N / 10 mm or less and an adhesive layer having a storage modulus at 20°C of 0.15 MPa or more and 0.50 MPa or less. In one embodiment of the present invention, the decorative film preferably comprises a base film having an upper yield point load at 20°C of 10.0 N / 10 mm or more and 45.0 N / 10 mm or less and an adhesive layer having a loss tangent at 20°C of 0.20 or more and 1.5 or less, more preferably a base film having an upper yield point load at 20°C of 13.7 N / 10 mm or more and 30.0 N / 10 mm or less and an adhesive layer having a loss tangent at 20°C of 0.30 or more and 1.2 or less, and even more preferably a base film having an upper yield point load at 20°C of 15.0 N / 10 mm or more and 20.0 N / 10 mm or less and an adhesive layer having a loss tangent at 20°C of 0.50 or more and 1.1 or less.
[0121] The thickness of the decorative film is represented by the sum of the thickness of the base film and the thickness of the adhesive layer, and is preferably 100 μm or more and 300 μm or less, more preferably 150 μm or more and 250 μm or less, and even more preferably 180 μm or more and 220 μm or less.
[0122] [Method of manufacturing decorative film] The decorative film of the present invention can be produced by forming a pressure-sensitive adhesive layer on a substrate film by the above-mentioned method. When the substrate film includes a surface protective layer and a colored layer, the pressure-sensitive adhesive layer is formed on the substrate film on the colored layer side.
[0123] [Specific embodiment] The layer structure of a decorative film according to one embodiment of the present invention is shown in Fig. 1. The decorative film 10 is disposed on a releasable surface of a release sheet 20. The decorative film 10 is configured by stacking a surface protection layer 11, a second adhesive layer 12, a colored layer 13, and a first adhesive layer 14 in this order from the side opposite to the release sheet 20 (the top in the figure).
[0124] The surface protective layer 11 is made of, for example, a resin composition (urethane resin) containing both urethane resins, that is, a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin.
[0125] The second pressure-sensitive adhesive layer 12 is formed from, for example, an acrylic pressure-sensitive adhesive.
[0126] The first pressure-sensitive adhesive layer 14 is formed from a pressure-sensitive adhesive composition according to one embodiment of the present invention.
[0127] The colored layer 13 is, for example, a layer in which a pigment, which is a colorant, is dispersed in a resin. The resin is, for example, a resin composition containing both a hard (meth)acrylic resin and a soft (meth)acrylic resin.
[0128] The total thickness of the surface protective layer 11 and the colored layer 13 can be, for example, 100 μm or more. By adjusting the thickness of such layers and the materials and physical properties of the layers, the decorative film 10 can have, for example, an upper yield point load of 10.0 N / 10 mm or more and 45.0 N / 10 mm or less at 20° C. and a stress relaxation rate of 51% or more and 63% or less.
[0129] [Application] The decorative film of the present embodiment is preferably used for applications in which the film is attached to an object to be decorated to decorate the object to be decorated. The decorative film of the present embodiment has weather resistance and is excellent in curved surface conformability and application workability, and is therefore preferably used as a film for vehicle exterior that is adhered to an exterior part of a vehicle.
[0130] The adherend to which the decorative film of the present invention is applied may be a urethane-coated plate, a melamine-coated plate, an aluminum plate, a stainless steel plate, or the like. EXAMPLES
[0131] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0132] The properties of each material used in the examples and comparative examples, as well as the properties of the resulting base film and decorative film, were measured as follows.
[0133] [Glass transition temperature (Tg)] The glass transition temperature of the (meth)acrylic copolymer was calculated from (Equation 1). As the glass transition temperature of each monomer unit, the glass transition temperature value of the monomer described in the section "Glass transition temperature (Tg) of (meth)acrylic copolymer (A)" in this specification was used.
[0134] [Weight average molecular weight (Mw)] The weight average molecular weight of the (meth)acrylic copolymer was measured according to the following (1) to (3). (1) A solution of the (meth)acrylic copolymer was applied to a release paper and dried at 100° C. for 1 minute to obtain a film of the (meth)acrylic copolymer. (2) Using the film-like (meth)acrylic copolymer obtained in (1) above and tetrahydrofuran, a sample solution with a solid content concentration of 0.2% by mass was obtained. Note that the "solid content concentration" here refers to the mass ratio of the (meth)acrylic copolymer in the sample solution. (3) The weight average molecular weight of the (meth)acrylic copolymer was measured in terms of standard polystyrene using gel permeation chromatography (GPC) under the following conditions.
[0135] (Measurement conditions) Measurement equipment: High-speed GPC [Model: HLC-8220 GPC, Tosoh Corporation] Detector: Differential Refractometer (RI) [Installed in HLC-8220, Tosoh Corporation] Column: 4 TSK-GEL GMHXL (Tosoh Corporation) connected in series Column temperature: 40℃ Eluent: Tetrahydrofuran Sample solution injection volume: 100μL Flow rate: 0.8mL / min
[0136] [Upper yield point load] The upper yield point load of each of the surface protective film, the colored film, and the base film was measured as follows. A rectangular sample with a width of 10 mm and a length of 150 mm was prepared, and the distance between the chucks of a Tensilon (registered trademark, manufacturer: A&D Co., Ltd., model RTG-1310) was set to 100 mm, and the sample was clamped and fixed between the chucks. The sample was stretched at a constant tensile speed of 300 mm / min at 20°C, and the tensile load during stretching was measured. The load at which necking began (when an inflection point was observed in the tensile load graph) was taken as the upper yield load.
[0137] [Stress relaxation rate] The stress relaxation rate of the substrate film was measured as follows. A rectangular sample with a width of 10 mm and a length of 150 mm was prepared, and the distance between the chucks of a Tensilon (registered trademark, manufacturer: A&D Co., Ltd., model RTG-1310) was set to 100 mm, and the sample was clamped and fixed between the chucks. The tensile speed was set to 300 mm / min at 20°C, and the sample was stretched by 5%, and the tensile load x immediately after 5% stretching and the tensile load y 5 minutes after 5% stretching were measured. The stress relaxation rate z was then calculated from the following formula. z[%]={(xy) / x}×100
[0138] [Storage modulus, loss modulus, loss tangent] The storage modulus, loss modulus and loss tangent of the adhesive layer were determined by dynamic viscoelasticity measurement as follows. An adhesive layer having a thickness of 40 μm was laminated until it reached 300 μm to 600 μm, and cut into a circle having a diameter of 10 mm. The storage modulus, loss modulus and loss tangent were determined by measuring the dynamic viscoelasticity using a dynamic viscoelasticity device (registered trademark, manufacturer: Anton Paar Inc., model: MCR301) under the conditions of a measurement temperature of -15°C to +130°C, a frequency of 1 Hz and a heating rate of 2°C / min.
[0139] [Thickness] The thickness of each layer was measured with a micrometer and calculated as the average value of the measurements at five points. The thickness of the surface protection film, colored film, and base film were each measured, and the thickness of the adhesive layer was calculated by subtracting the thickness of the two films from the total thickness when sandwiched between two films with specified thicknesses.
[0140] [Preparation of Base Film] The materials used to prepare the base film are shown below. (urethane resin) Urethane resin 1: Rezamin (registered trademark) (manufactured by Dainichiseika Chemicals Co., Ltd.) Product number NE-8836 (Polycarbonate-based polyurethane resin) Urethane resin 2: NY585-N11A (manufactured by FCI Co., Ltd., polycaprolactone-based polyurethane resin, melting temperature 130°C) (Fluorine resin) Fluorine resin 1: Denka DX Film (manufactured by Denka Co., Ltd.) Product code 14S0230 ((Meth)acrylic resin) (Hard (meth)acrylic resin) Hard (meth)acrylic resin 1: Kaneace (registered trademark) MC-732 (manufactured by Kaneka Corporation, upper yield point load is 16.0 N / 10 mm when the film thickness is 100 μm) Hard (meth)acrylic resin 2: Parapet (registered trademark) GR-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load is 27.1 N / 10 mm when the film thickness is 100 μm, and Shore A hardness is 100) (Soft (meth)acrylic resin) Soft (meth)acrylic resin 1: Parapet (registered trademark) SA-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load at a film thickness of 100 μm is 3.9 N / 10 mm, Shore A hardness is 70) (Vinyl chloride resin) Polyvinyl chloride resin: Kanevinyl (registered trademark) S1001N (manufactured by Kaneka Corporation, average degree of polymerization 1050) (coloring agent) Carbon black: W8012-G5 (registered trademark) carbon black (manufactured by Nikko Bix Co., Ltd.) (Additives) Additive 1: Tinuvin (registered trademark) 213 (manufactured by BASF Japan Ltd.) Additive 2: Tinuvin (registered trademark) 243 (manufactured by BASF Japan Ltd.)
[0141] <Production of surface protective film (surface protective layer)> (Surface protection film 1) 100 parts by mass of urethane resin 1 was diluted to a solid content of 25% by mass with a dilution solvent obtained by mixing isopropanol (IPA) and toluene in a 1:1 mass ratio, and then 1.2 parts by mass of additive 1 was mixed to obtain a composition for surface protection layer 1. The composition 1 was cast onto a polyester release film having a thickness of 75 μm, and then dried at 80° C. for 3 minutes and then at 140° C. for 3 minutes to produce a surface protection film 1 having a thickness of 30 μm. The upper yield point load of the surface protection film 1 was 5.9 N / 10 mm.
[0142] (Surface protection film 2) The fluororesin 1 film having a thickness of 30 μm was used as it was to form a surface protective film 2. The upper yield point load of the surface protective film 2 was 13.1 N / 10 mm.
[0143] (Surface protection film 3) 100 parts by mass of urethane resin 2 was diluted with a dilution solvent in which isopropanol (IPA) and toluene were mixed in a mass ratio of 1:1 to a solid content of 25 mass%, and then 1.2 parts by mass of additive 1 were added to obtain a composition for surface protection layer 2. The composition 2 was cast onto a polyester release film having a thickness of 75 μm, and then dried at 80° C. for 3 minutes and then at 140° C. for 3 minutes to produce a surface protection film 3 having a thickness of 30 μm. The upper yield point load of the surface protection film 3 was 4.5 N / 10 mm.
[0144] <Production of colored film (colored layer)> (Colored film 1) 70 parts by mass of hard (meth)acrylic resin 1, 30 parts by mass of soft (meth)acrylic resin 1, 19 parts by mass of carbon black, and 0.3 parts by mass of additive 2 were melt-kneaded in a Henschel mixer, and molded into a 100 μm-thick colored film 1 using a calendar molding machine set at 180° C. The upper yield point load of the colored film 1 was 10.2 N / 10 mm.
[0145] (Colored film 2) A 100 μm thick colored film 2 was molded under the same conditions as for the colored film 1, except that 70 parts by mass of the hard (meth)acrylic resin 1 was changed to 48 parts by mass of the hard (meth)acrylic resin 2, and 52 parts by mass of the soft (meth)acrylic resin 1 was used. The upper yield point load of the colored film 2 was 8.3 N / 10 mm.
[0146] (Colored film 3) A 100 μm thick colored film 3 was molded under the same conditions as for the colored film 2, except that 59 parts by mass of the hard (meth)acrylic resin 2 and 41 parts by mass of the soft (meth)acrylic resin 1 were used. The upper yield point load of the colored film 3 was 13.2 N / 10 mm.
[0147] (Colored film 4) Pigmented film 4 was formed in the same manner as for pigmented film 1, except that 100 parts by mass of vinyl chloride resin was used instead of 70 parts by mass of hard (meth)acrylic resin 1 and 30 parts by mass of soft (meth)acrylic resin 1. The upper yield point load of pigmented film 4 was 10.6 N / 10 mm.
[0148] <Preparation of Adhesive Composition 0> Aluminum chelate A (Kawaken Fine Chemicals Co., Ltd.) was mixed into a solution of acrylic resin (Tg: -37.4°C, BA / AA=90 / 10) to prepare adhesive composition 0 for bonding the surface protection film and the colored film.
[0149] <Preparation of base film> Base films BF1 to 7 were prepared as follows.
[0150] (Base film BF1) The adhesive composition 0 was applied to the surface of the surface protection film 1 prepared on the release film so that the thickness after drying would be 30 μm, and after heating and drying for 1 minute in a 100° C. atmosphere, it was laminated with the colored film 1 to prepare the base film BF1 for the decorative film. The prepared base film BF1 is a laminate in which the surface protection layer 1, the adhesive layer 0, and the colored layer 1 are laminated in this order.
[0151] (Base film BF2) A base film BF2 for a decorative film was produced under the same conditions as the base film BF1, except that a colored film 2 was attached to the surface of a surface protection film 1 produced on a release film, instead of the colored film 1. The produced base film BF2 is a laminate in which a surface protection layer 1, a pressure-sensitive adhesive layer 0, and a colored layer 2 are laminated in this order.
[0152] (Base film BF3) A base film BF3 for a decorative film was produced under the same conditions as the base film BF1, except that a colored film 3 was attached to the surface of a surface protection film 1 produced on a release film, instead of the colored film 1. The produced base film BF3 is a laminate in which a surface protection layer 1, a pressure-sensitive adhesive layer 0, and a colored layer 3 are laminated in this order.
[0153] (Base film BF4) 100 parts by mass of urethane resin 1 was diluted to a solid content of 25% by mass with a dilution solvent obtained by mixing isopropanol (IPA) and toluene in a 1:1 mass ratio, and then 1.2 parts by mass of additive 1 was mixed to obtain a composition for base film 10. The composition 10 was cast onto a polyester release film having a thickness of 75 μm, and then dried at 80° C. for 3 minutes and then at 140° C. for 3 minutes to produce a base film BF4 having a thickness of 160 μm.
[0154] (Base film BF5) 100 parts by mass of urethane resin 2 and 1.2 parts by mass of additive 1 were blended to obtain a base film composition 11. Next, a base film BF5 having a thickness of 160 μm was produced from composition 11 using an extruder under conditions of 160° C., a rotation speed of 7 rpm, a load of 30 A, and a line speed of 1.0 m / min.
[0155] (Base film BF6) A base film BF6 for a decorative film was produced under the same conditions as the base film BF1, except that a colored film 4 was laminated to the surface of a surface protection film 2 produced on a release film, instead of the colored film 1. The produced base film BF6 is a laminate in which a surface protection layer 2, a pressure-sensitive adhesive layer 0, and a colored layer 4 are laminated in this order.
[0156] (Base film BF7) A base film BF7 for a decorative film was produced under the same conditions as the base film BF1, except that a colored film 2 was attached to the surface of a surface protection film 3 produced on a release film, instead of the colored film 1. The produced base film BF7 is a laminate in which a surface protection layer 3, a pressure-sensitive adhesive layer 0, and a colored layer 2 are laminated in this order.
[0157] Table 1 below shows the configuration of the base film, as well as the upper yield point load and stress relaxation rate of each film.
[0158] [Table 1]
[0159] [Preparation of Adhesive Layer] <Synthesis of (meth)acrylic copolymer> The (meth)acrylic copolymers (A1) to (A12) and the (meth)acrylic copolymers (B1) to (B11) were synthesized as follows.
[0160] The synthesis of each (meth)acrylic copolymer was carried out by solution polymerization. Ethyl acetate was used as a solvent, and 2,2'-azobisisobutyronitrile [AIBN; polymerization initiator] was added to 20 parts by mass of the monomer mixture at 0.026 parts by mass under reflux temperature conditions. The monomer mixture was then successively added dropwise to 80 parts by mass of the monomer mixture over 120 minutes, and after the dropwise addition was completed, the mixture was allowed to react for another 30 minutes. The mixture was then diluted with ethyl acetate to a solid content concentration of 35.0% by mass to obtain a solution of each (meth)acrylic copolymer.
[0161] The composition of each structural unit, the content of structural unit (a1), the content of structural unit (b1), Tg and Mw of the obtained (meth)acrylic copolymer (A) and (meth)acrylic copolymer (B) are shown in Table 2 below.
[0162] [Table 2]
[0163] In Table 2, BA stands for n-butyl acrylate, 2EHA stands for 2-ethylhexyl acrylate, MA stands for methyl acrylate, and AA stands for acrylic acid, while tBMA stands for tert-butyl methacrylate, 2EHMA stands for 2-ethylhexyl methacrylate, MMA stands for methyl methacrylate, 2HEMA stands for 2-hydroxyethyl methacrylate, EA stands for ethyl acrylate, DM stands for dimethylaminoethyl methacrylate, and silicone stands for polydimethylsiloxane.
[0164] <Preparation of Pressure-Sensitive Adhesive Composition> The crosslinking agents used in the pressure-sensitive adhesive compositions are as follows. (Crosslinking agent) EP: TETRAD-X (epoxy crosslinking agent, manufactured by Mitsubishi Gas Chemical Company, Inc.) MC: Aluminum Chelate A (metal chelate crosslinking agent, manufactured by Kawaken Fine Chemicals Co., Ltd.) ICN: Coronate (registered trademark) L45E (isocyanate-based crosslinking agent, manufactured by Tosoh Corporation)
[0165] (Adhesive composition AD1) To 100 parts by mass of the (meth)acrylic copolymer (A1) shown in Table 2, 10 parts by mass of the (meth)acrylic copolymer (B1) and 0.1 parts by mass of EP (crosslinking agent) were added, and ethyl acetate was used as a diluting solvent to prepare a pressure-sensitive adhesive composition AD1 with a solid content of 27% by mass. The (meth)acrylic copolymer (A1) contains 35 mass% of a (meth)acrylic copolymer having the composition shown in Table 2 as a solid content, and the (meth)acrylic copolymer (B1) was blended so that the solid content of the (meth)acrylic copolymer (B1) was 10 parts by mass per 100 parts by mass of the solid content.
[0166] (Adhesive compositions AD2 to AD33) According to the compositions shown in Tables 3 and 4, the (meth)acrylic copolymer (B) and the crosslinking agent were added to the (meth)acrylic copolymer (A) to prepare pressure-sensitive adhesive compositions AD2 to AD33 in the same manner as the pressure-sensitive adhesive composition AD1.
[0167] <Preparation of adhesive layer> (Adhesive layer AD1) The adhesive composition AD1 was cast onto a release-treated release film (release sheet) so that the thickness after drying would be 40 μm, and the dilution solvent was removed by heating and drying for 1 minute in an atmosphere of 100° C. The adhesive composition was then cured for 1 week in an environment of 40° C. to produce an adhesive layer AD1 made of the adhesive composition AD1.
[0168] (Adhesive layers AD2 to AD33) Similarly to the pressure-sensitive adhesive layer AD1, pressure-sensitive adhesive compositions AD2 to AD33 were cast onto a release sheet and dried by heating to produce each of the pressure-sensitive adhesive layers to have the thicknesses shown in Tables 3 and 4.
[0169] [Preparation of decorative film] <Example 1> A decorative film was produced by overlaying an adhesive layer AD1 made of an adhesive composition AD1 on the colored film 1 side of the base film BF1. In this way, a decorative film was obtained in which a surface protective layer 1, an adhesive layer 0, a colored layer 1, and an adhesive layer AD1 were overlaid in this order.
[0170] <Examples 2 to 18 and Comparative Examples 1 to 21> Decorative films were produced using the combinations of base film and pressure-sensitive adhesive layer and thicknesses shown in Tables 3 and 4.
[0171] The decorative films obtained in the examples and comparative examples were evaluated by the following methods.
[0172] [Adhesion Evaluation] The adhesiveness of the decorative films obtained in the Examples and Comparative Examples was evaluated by measuring the adhesive strength and by checking for the occurrence of zipping during the adhesive strength measurement. The occurrence of zipping was confirmed by visual inspection.
[0173] (Adhesion force measurement) The decorative films obtained in the examples and comparative examples were cut to prepare sample pieces with a width of 10 mm and a tensile length of 100 mm. The adhesive layer surface of the sample piece was then attached to a urethane-coated plate (a metal plate coated with urethane) prepared as an adherend, and the sample was attached to the urethane-coated plate by applying a load of 2 kg to the plate twice using a roller. The sample attached to the urethane-coated plate was stored in an environment of 23°C and 50% humidity for 1 hour and 168 hours after attachment. For the samples attached to the urethane-coated boards after storage for 1 hour and 168 hours, the adhesion strength of the samples to the urethane-coated boards was measured using Tensilon (registered trademark) (manufactured by A&D Corporation) at a peel speed of 200 mm / min, a peel angle of 180°, and a measurement temperature of 23°C.
[0174] The adhesiveness of the decorative film was evaluated according to the following criteria. (Adhesion Evaluation Criteria) A: There was no zipping, and the adhesive strength after 168 hours was 6.0 N / 10 mm or more. B: There was no zipping, and the adhesive strength after 168 hours was 5.0 N / 10 mm or more and less than 6.0 N / 10 mm, and the adhesive strength after 1 hour was 4.0 N / 10 mm or more. C: Zipping occurred or the adhesive strength after 168 hours was less than 5.0 N / 10 mm. The evaluation results of the adhesive strength, the presence or absence of zipping, and the adhesiveness of the decorative film are shown in Tables 3 and 4.
[0175] [Floating evaluation] The decorative films obtained in the examples and comparative examples were evaluated for lifting as follows. First, as shown in FIG. 2(I), a urethane-coated plate 100 with a convex shape of 6.5 mm in height and 20.6 mm in width was prepared as a tool for lifting evaluation. Next, a sample S of the decorative film was attached to the urethane-coated plate 100 according to the procedure shown in FIG. 2(II) to (III). Specifically, first, a sample S of the decorative film 10 (width 10 mm) was attached to the top of the convex shape of the urethane-coated plate 100 and a point 10 mm away from the bottom of the convex shape without sagging (FIG. 2(II)). Next, the sample S was attached from the inclined part of the convex shape toward the bottom of the convex shape (FIG. 2(III)). Then, the plate was stored in an environment of 23° C. and 10° C., and the occurrence of lifting as shown in FIG. 2(IV) was visually judged over time, and the lifting evaluation was performed. (Float evaluation criteria) A: No floating was observed after more than two weeks in the floating evaluation at 10°C and 23°C. B: Floating was observed within two weeks at 10°C. C: Floating was observed within 24 hours at 23°C. The evaluation results of the decorative film lifting are shown in Tables 3 and 4.
[0176] [Re-pasting workability evaluation] The re-application workability of the decorative films obtained in the Examples and Comparative Examples was evaluated as follows. A decorative film was attached to the exterior of an automobile (urethane-coated panel) using a squeegee, and then the decorative film was peeled off at a peeling angle of 120°. The presence or absence of shock lines on the surface of the decorative film was visually evaluated. The evaluation criteria are as follows: (Evaluation criteria for re-pasting workability) A: It was possible to reapply it without any shock lines. C: Shock lines appeared on the decorative film. The evaluation results of the sticking and peeling properties are shown in Tables 3 and 4.
[0177] 〔comprehensive evaluation〕 The results of the adhesion evaluation, lifting evaluation and re-application workability evaluation were converted into scores based on the following criteria. A 2 points B 1 point C 0 points
[0178] The scores for each decorative film were tallied, and the operation was evaluated according to the scores for each decorative film according to the following criteria. The overall evaluation is shown in Tables 3 and 4 above. A Total of 5 points or more B Total of 3 points or more and 4 points or less C Total of 2 points or less
[0179] [Table 3]
[0180] [Table 4]
[0181] As shown in Tables 3 and 4 above, it is believed that by using an adhesive layer made of a blend of (meth)acrylic copolymers (A) and (B) for a low-rigidity base film, the adhesive layer's holding power is increased, preventing the decorative film from lifting off the application surface when applied. In addition, it is believed that by blending different (meth)acrylic copolymers (A) and (B), the initial adhesive strength is suppressed, making it easier to reapply the film. [Industrial Applicability]
[0182] The present invention relates to a decorative film for decorating an object to be decorated, which may have a curved or uneven surface, and can be suitably used, for example, as a film for the exterior of a vehicle. [Explanation of symbols]
[0183] 10 Decorative film 11 Surface protective layer 12 Second adhesive layer 13 Colored layer 14 First adhesive layer 20 Release sheet
Claims
1. A decorative film comprising a base film and a pressure-sensitive adhesive layer laminated on the base film, The base film contains a (meth)acrylic resin, the pressure-sensitive adhesive layer is a layer formed from a pressure-sensitive adhesive composition containing a (meth)acrylic copolymer (A), a (meth)acrylic copolymer (B), and a crosslinking agent, The (meth)acrylic copolymer (A) contains a structural unit (a1) derived from a monomer having an acidic functional group that undergoes a crosslinking reaction with the crosslinking agent, the content of the structural unit (a1) is 4.5% by mass or more and 15.0% by mass or less, based on all structural units contained in the (meth)acrylic copolymer (A); The (meth)acrylic copolymer (A) has a glass transition temperature of −30° C. or higher and −15° C. or lower, The (meth)acrylic copolymer (B) contains a structural unit (b1) derived from a monomer having a polar group other than the acidic functional group, the content of the structural unit (b1) is 3.0% by mass or more and 15.0% by mass or less, based on all structural units contained in the (meth)acrylic copolymer (B); The (meth)acrylic copolymer (B) has a glass transition temperature of 100° C. or higher, The content of the (meth)acrylic copolymer (B) is 3 parts by mass or more and 14 parts by mass or less based on 100 parts by mass of the (meth)acrylic copolymer (A), The decorative film, wherein the crosslinking agent is at least one of an epoxy-based crosslinking agent and a metal chelate-based crosslinking agent.
2. The decorative film according to claim 1 , wherein the polar group is a hydroxyl group.
3. The decorative film according to claim 1 , wherein the base film has a stress relaxation rate of 50% or more and 63% or less at 20° C.
4. The decorative film according to claim 1, wherein the upper yield point load of the base film at 20°C is 10.0 N / 10 mm or more and 45.0 N / 10 mm or less.
5. The decorative film according to claim 1, wherein the (meth)acrylic copolymer (A) has a weight average molecular weight of 200,000 or more and 1,800,000 or less.
6. The decorative film according to claim 1, wherein the weight average molecular weight of the (meth)acrylic copolymer (B) is from 3,000 to 10,000.
Citation Information
Patent Citations
Marking sheet
JP2008214434A
Adhesive agent composition for vehicle protective film and vehicle protective film
JP2021143269A
Cited By
Decorative film, decorative laminated structure, and peeling method
JP2026165786A