Decorative film
The decorative film with a polyurethane protective layer and acrylic colored layer addresses the issues of weather resistance and adhesion by maintaining flexibility and adhesion, ensuring durability and compatibility with curved surfaces.
Patent Information
- Application Number
- JP2024049248
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional decorative films for automobile exteriors face challenges in achieving simultaneous weather resistance, adhesion workability, and curved surface followability, with polyvinyl chloride films becoming brittle and polyurethane films prone to wrinkling and peeling.
A decorative film comprising a surface protective layer made of polyurethane resin and a colored layer made of acrylic resin, with specific upper yield point loads and stress relaxation rates to ensure adhesion and flexibility, enhancing weather resistance and curved surface compatibility.
The film provides sufficient weather resistance, adhesion workability, and curved surface followability, preventing peeling and wrinkling, and is suitable for automotive applications.
Smart Images

Figure 2024146839000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative film. [Background technology]
[0002] In recent years, decorative films have been used instead of paint as a means of decorating the exterior of automobiles, in order to reduce the amount of solvent used and shorten construction times in line with the reduction of CO2 emissions in line with the SDGs. Polyvinyl chloride is often used as the resin material for decorative films for the exterior of automobiles due to its high formability, durability, and economical efficiency. However, polyvinyl chloride is prone to deterioration over time, and measures to improve weather resistance are required.
[0003] As one of such measures, a technique is known in which a surface protective layer of a fluororesin film is used in combination with a colored layer of polyvinyl chloride in order to suppress deterioration of polyvinyl chloride over time (see, for example, Patent Document 1). As another of the above measures, a decorative film for the exterior of an automobile is used that uses polyurethane, which is flexible and has excellent weather resistance, instead of polyvinyl chloride. As such a decorative film, for example, a decorative layer-forming film for the exterior of an automobile having a surface protective layer made of urethane resin is known (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-214434 A [Patent Document 2] JP 2007-297569 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in a decorative film made by layering a polyvinyl chloride film and a fluororesin film, the weather resistance of the polyvinyl chloride is greatly improved, but the fluororesin film is a hard film, so the entire decorative film is also a hard film. Therefore, if the decorative film is attached to a curved adherend surface such as an automobile, the decorative film may peel off and float over time.
[0006] In addition, in a decorative film having a surface protective layer made of polyurethane, the polyurethane is flexible, so the film is likely to become loose and wrinkle when applied to the outer surface of an automobile. Thus, there is room for improvement in the ease of application of the decorative film.
[0007] As described above, it is difficult for conventional decorative films for the exterior of automobiles to simultaneously satisfy the requirements of weather resistance, resistance to lifting around curved sections, and ease of application.
[0008] In view of the above circumstances, one aspect of the present invention aims to provide a decorative film that fully exhibits weather resistance, ease of application, and curved surface conformability. In this specification, the term "curved surface conformability" refers to the property of a decorative film that is difficult to lift off when applied to a curved portion such as an uneven portion. [Means for solving the problem]
[0009] In order to solve the above problems, a decorative film according to one embodiment of the present invention is a decorative film formed by laminating a surface protective layer and a colored layer, wherein the surface protective layer contains a polyurethane resin, and the colored layer contains an acrylic resin and a colorant, and the upper yield point load of the decorative film at 20°C is 13.5 N / 10 mm or more and 25.0 N / 10 mm or less, and the stress relaxation rate at 20°C is 53% or more and 58% or less. Effect of the Invention
[0010] According to one aspect of the present invention, it is possible to provide a decorative film that satisfactorily exhibits weather resistance, ease of application, and ability to conform to curved surfaces. [Brief description of the drawings]
[0011] [Figure 1] 1 is a diagram showing a layer structure of a decorative film according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present inventors have found that the above-mentioned problems can be solved by providing a weather-resistant decorative film having a specific upper yield point load and stress relaxation rate. The decorative film according to one embodiment of the present invention has a colored layer and a surface protective layer overlapping the colored layer. The colored layer and the surface protective layer will be described in detail later.
[0013] [Upper yield point load] The upper yield point load of the decorative film of this embodiment at 20° C. is 13.5 N / 10 mm or more and 25.0 N / 10 mm or less.
[0014] The upper yield point load of the decorative film is the boundary load at which the deformation of the decorative film changes from elastic deformation to plastic deformation when a load is applied to the decorative film. The temperature of the decorative film when measuring the upper yield point load is 20°C.
[0015] In this specification, unless otherwise specified, the upper yield point load of the decorative film means the upper yield point load of the laminated structure of the surface protective layer and the colored layer (hereinafter also referred to as the base film). For example, when the decorative film further has an adhesive layer described later, the upper yield point load of the decorative film is the upper yield point load of the laminate (also referred to as the base film) in which the surface protective layer, the adhesive layer, and the colored layer are laminated in this order. In addition, when the decorative film further has an adhesive layer described later, the upper yield point load of the decorative film is the upper yield point load of the laminate not including the adhesive layer.
[0016] When the upper yield point load of the decorative film is equal to or greater than a specified value, the occurrence of wrinkles during application tends to be more easily prevented, and when it is equal to or less than the specified value, the occurrence of lifting after application tends to be more easily prevented. The lower limit of the upper yield point load of the decorative film is 13.5N / 10mm or more, preferably 13.7N / 10mm or more, more preferably 14.1N / 10mm or more, even more preferably 14.5N / 10mm or more, and even more preferably 15.0N / 10mm or more, 16.0N / 10mm or more, or 17.0N / 10mm or more. In addition, the upper limit of the upper yield point load of the decorative film is 25.0N / 10mm or less, preferably 20.9N / 10mm or less, more preferably 20.5N / 10mm or less, even more preferably 20.0N / 10mm or less, 19.0N / 10mm or less, or 18.0N / 10mm or less, from the viewpoint of improving the curved surface conformability.
[0017] The upper yield point load can be determined by measuring a 10 mm wide sample made from a substrate film with a known measuring device such as a Tensilon universal testing machine. The upper yield point load is the load at the upper yield point of the sample observed in a tensile test, and since it is a load measured using a 10 mm wide sample, its unit is expressed as "N / 10 mm". The upper yield point load of the decorative film can be adjusted by the upper yield point load or material resin and thickness of each of the colored layer and the surface protective layer.
[0018] When the upper yield point load of the surface protective layer at 20°C is a specified value or more, the occurrence of wrinkles when the decorative film is applied tends to be more easily prevented, and when it is below the specified value, the occurrence of lifting after application tends to be more easily prevented. The lower limit of the upper yield point load of the surface protective layer is preferably 3.5N / 10mm or more, more preferably 4.0N / 10mm or more, and even more preferably 4.5N / 10mm or more or 5.0N / 10mm or more, from the viewpoint of improving application workability. The upper limit of the upper yield point load of the surface protective layer is preferably 9.0N / 10mm or less, more preferably 7.5N / 10mm or less, and even more preferably 6.5N / 10mm or less, 6.0N / 10mm or less, or 5.9N / 10mm or less, from the viewpoint of improving curved surface conformability. The upper yield point load of the surface protective layer may be adjusted by using a relatively soft polyurethane resin material alone or by using two or more of them in combination.
[0019] When the upper yield point load of the colored layer at 20°C is a specified value or more, the occurrence of wrinkles when the decorative film is applied tends to be more easily prevented, and when it is below the specified value, the occurrence of lifting after application tends to be more easily prevented. The lower limit of the upper yield point load of the colored layer is preferably 7.1 N / 10 mm or more, more preferably 7.7 N / 10 mm or more, and even more preferably 8.0 N / 10 mm or more, 8.3 N / 10 mm or more, or 9.5 N / 10 mm or more, from the viewpoint of improving application workability. The upper limit of the upper yield point load of the colored layer is preferably 14.1 N / 10 mm or less, more preferably 13.7 N / 10 mm or less, and even more preferably 13.2 N / 10 mm or less, or 12.0 N / 10 mm or less, from the viewpoint of improving curved surface conformability. The upper yield point load of the colored layer can be adjusted, for example, by using two or more kinds of acrylic resins having different upper yield point loads in combination in an appropriate ratio.
[0020] In the decorative film, the ratio of the upper yield point load of the colored layer to the upper yield point load of the surface protective layer may be, for example, 1 or more and 3 or less. The lower limit of the ratio may be preferably 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, or 1.6 or more. The upper limit of the ratio may be preferably 2.8 or less, 2.6 or less, 2.4 or less, 2.3 or less, 2.2 or less, 2 or less, or 1.8 or less.
[0021] [Stress relaxation rate] The decorative film of this embodiment has a stress relaxation rate of 53% or more and 58% or less at 20°C. The stress relaxation rate of the decorative film is the rate of change in tensile load before and after stretching when a tensile load that stretches the decorative film by 5% (to 105% of its length) is applied for 5 minutes. The temperature of the decorative film when measuring the stress relaxation rate is 20°C. The stress relaxation rate of the decorative film is calculated from the following formula, where x is the tensile load immediately after 5% stretching and y is the tensile load 5 minutes after 5% stretching. Stress relaxation rate z[%]={(xy) / x}×100
[0022] In this specification, unless otherwise specified, the stress relaxation rate of the decorative film means the stress relaxation rate of the laminated structure (base film) of the surface protective layer and the colored layer. For example, when the decorative film further has an adhesive layer described later, the stress relaxation rate of the decorative film is the stress relaxation rate of the laminate (base film) in which the surface protective layer, the adhesive layer, and the colored layer are laminated in this order. In addition, when the decorative film further has an adhesive layer described later, the stress relaxation rate of the decorative film is the stress relaxation rate of the laminate not including the adhesive layer.
[0023] If the stress relaxation rate of the decorative film is a specified value or higher, it tends to be easier to prevent wrinkles from occurring when the decorative film is applied, and if it is a specified value or lower, it tends to be easier to prevent lifting after application. The lower limit of the stress relaxation rate of the decorative film is 53% or more, preferably 55% or more, and more preferably 56% or more, from the viewpoint of improving application workability. The upper limit of the stress relaxation rate of the decorative film is 58% or less, preferably 57% or less, from the viewpoint of improving curved surface conformability.
[0024] The stress relaxation rate of the decorative film can be determined by measuring the tensile load with a known measuring device such as a Tensilon universal testing machine. The stress relaxation rate of the decorative film can be adjusted by adjusting the material resins of the colored layer and the surface protective layer or the thicknesses of both layers.
[0025] [Weather resistance] The decorative film of the present embodiment has weather resistance. The weather resistance can be expressed in various forms, and in this specification, it is referred to as color (L * a * b * L in color space * Value, a * value and b * It is evaluated by the stability of the color (color specified by the value). In the decorative film of this embodiment, the cumulative light amount is 1200 MJ / m 2 The color difference before and after irradiation with light of 1350 MJ / m may be 3.0 or less, preferably 1.5 or less, and more preferably 1.2 or less. Alternatively, in the decorative film of this embodiment, the color difference before and after irradiation with light of 1350 MJ / m may be 3.0 or less, more preferably 1.5 or less, and more preferably 1.2 or less. 2 The color difference before and after irradiation with light is preferably 4.0 or less, more preferably 1.5 or less, and even more preferably 1.4 or less. These color differences indicate the same degree of weather resistance. The color difference ΔE of the decorative film is L * a * b * In the color system, lightness is L * , L * a * b * The position between magenta and green in the color space is a * (negative values are greener, positive values are magenta), L * a * b * The position between yellow and blue in the color space is b * When the difference in brightness before and after irradiation is ΔL * , a before and after irradiation * Difference Δa * and b before and after irradiation. * Difference Δb * It can be calculated using the following formula: Color difference ΔE={(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2} 1 / 2
[0026] The color difference of the decorative film can be measured using a known measuring device such as a colorimeter. The color difference of the decorative film can be adjusted by using a resin material having sufficient weather resistance, in other words, by using a resin material having sufficient weather resistance for at least one of an acrylic resin and a urethane resin. In addition, the weather resistance test may be accompanied by an accelerated test according to the use environment of the decorative film.
[0027] [Thickness] In the decorative film of this embodiment, the total thickness of the surface protective layer and the colored layer can be appropriately determined according to the application of the decorative film. For example, when the total thickness of the surface protective layer and the colored layer is a predetermined value or more, application workability and curved surface conformability tend to be sufficiently achieved, and when it is a predetermined value or less, curved surface conformability tends to be sufficiently achieved. The lower limit of the total thickness of the surface protective layer and the colored layer is preferably 80 μm or more, more preferably 90 μm or more, even more preferably 100 μm or more, and even more preferably 120 μm or more, from the viewpoint of adjusting at least one of application property and curved surface conformability. The upper limit of the total thickness of the surface protective layer and the colored layer is preferably 200 μm or less, more preferably 180 μm or less, even more preferably 170 μm or less, or even more preferably 140 μm or less, from the viewpoint of fully expressing curved surface conformability.
[0028] When the decorative film has an adhesive layer between the surface protection layer and the colored layer, the lower limit of the thickness of the base film, which is the sum of their thicknesses, may be, for example, 100 μm or more, preferably 120 μm or more, more preferably 140 μm or more, even more preferably 150 μm or more, or even more preferably 160 μm or more, from the viewpoint of adjusting at least one of the application ease and curved surface conformability.
[0029] On the other hand, the upper limit of the thickness of the base film may be 220 μm or less, preferably 200 μm or less, more preferably 180 μm or less, and even more preferably 170 μm or less, from the viewpoint of fully exhibiting curved surface conformability.
[0030] From the viewpoint of protecting the colored layer with a sufficient thickness, the lower limit of the thickness of the surface protective layer may be, for example, 15 μm or more, preferably 20 μm or more, more preferably 25 μm or more, and even more preferably 30 μm or more. The upper limit of the thickness of the surface protective layer can be appropriately determined from the above viewpoint, and may be, for example, 60 μm or less, preferably 50 μm or less, more preferably 40 μm or less, or more preferably 35 μm or less.
[0031] The lower limit of the thickness of the colored layer may be, for example, 60 μm or more, preferably 70 μm or more, and more preferably 90 μm or more. The upper limit of the thickness of the colored layer may be, for example, 150 μm or less, preferably 130 μm or less, more preferably 120 μm or less, and even more preferably 110 μm or less.
[0032] The decorative film may have a ratio of the thickness of the surface protective layer to the thickness of the colored layer of, for example, 0.10 or more and 1.00 or less. The lower limit of the ratio may be preferably 0.15 or more, 0.20 or more, or 0.25 or more. The upper limit of the ratio may be preferably 0.80 or less, 0.60 or less, 0.50 or less, or 0.40 or less.
[0033] [Colored layer] The colored layer is made of an acrylic resin and contains a colorant. For example, the colored layer may be a layer in which a colorant is dispersed in an acrylic resin matrix resin.
[0034] [Acrylic resin] The acrylic resin may be appropriately selected from known resins within a range that satisfies the physical properties described below as a decorative film or a colored layer. The acrylic resin may be a resin material that imparts sufficient weather resistance to the decorative film by itself, or may be a resin material that imparts sufficient weather resistance to the decorative film by using it in combination with a polyurethane resin (laminate structure). The acrylic resin may be used alone or in combination of two or more types. The acrylic resin is also preferable from the viewpoint of achieving the mechanical strength required for the decorative film. The term "acrylic resin" refers collectively to acrylic resin and methacrylic resin.
[0035] The acrylic resin is preferably a resin that can design the upper yield point load of the colored layer at 20°C to be at least 7.1 N / 10 mm or more and 14.1 N / 10 mm or less. The acrylic resin is one of the resin materials that affect the upper yield point load and stress relaxation rate of the decorative film. The acrylic resin may be one type of resin whose upper yield point load meets a predetermined requirement, or two or more types of resins with different hardness may be used in combination. When two or more types of resins with different hardness are used in combination, examples of the resin with relatively high hardness include acrylic resins used for films, sheets, etc. formed by melt extrusion. When two or more types of resins with different hardness are used in combination, examples of the resin with relatively low hardness include acrylic resins for adjusting flowability and acrylic resins for soft materials.
[0036] From the viewpoint of achieving the mechanical strength required for the decorative film while realizing the above-mentioned physical properties, it is preferable that the acrylic resin contains a hard acrylic resin and a soft acrylic resin.
[0037] In this specification, the term "rigid acrylic resin" refers to an acrylic resin that, when made into a sheet material having a thickness of 100 μm and a width of 10 mm, has an upper yield point load of 10.0 N / 10 mm or more at 20° C. The upper yield point load can be measured by a known measuring device such as a Tensilon universal testing machine.
[0038] When the upper yield point load of the hard acrylic resin is a specified value or more, the application property of the decorative film (reduction of the occurrence of wrinkles during application) may be further improved, and when it is less than the specified value, the curved surface conformability of the decorative film may be further improved. In this specification, the lower limit of the upper yield point load of the hard acrylic resin may be 10.0N / 10mm or more, preferably 15.0N / 10mm or more, more preferably 16.0N / 10mm or more, or more preferably 25.0N / 10mm or more, from the viewpoint of further improving the workability of the decorative film. In addition, in this specification, the upper limit of the upper yield point load of the hard acrylic resin may be 35.0N / 10mm or less, preferably 30.0N / 10mm or less, more preferably 28.0N / 10mm or less, from the viewpoint of further improving the curved surface conformability of the decorative film.
[0039] The hard acrylic resin can be prepared by radical polymerization of known monomers capable of constituting an acrylic resin. Examples of hard acrylic resins include polymethyl methacrylate and methyl methacrylate-styrene copolymers.
[0040] Furthermore, the hard acrylic resin may be an acrylic resin having a Shore A hardness of more than 90. The "Shore A hardness" is, for example, the maximum value measured using a durometer GS-706N manufactured by Techlock Corporation when a Type A sensor is pressed perpendicularly against the surface of the measurement target with a load of 1 kg.
[0041] As the hard acrylic resin, for example, it is preferable to first select an acrylic resin having a Shore A hardness of more than 90 as a standard, and then select from the selected acrylic resins a resin that provides an upper yield point load of 10.0 N / 10 mm or more for the molded body that is the sheet material. The hard acrylic resin may be a commercially available product, examples of which include Parapet (registered trademark) GR-F1000P (Kuraray Co., Ltd.), Kane Ace (registered trademark) MC-732 (Kaneka Co., Ltd.), Dianale LP-3202, 3207, 3130, and 3121 (all Mitsubishi Chemical Co., Ltd.), and Delpet (Asahi Kasei Co., Ltd.).
[0042] In this specification, the soft acrylic resin refers to an acrylic resin that, when made into a sheet material of the above size, has an upper yield point load of less than 10.0 N / 10 mm at 20° C. When the upper yield point load of the soft acrylic resin is a predetermined value or more, the application property of the decorative film (suppression of wrinkles during application) tends to be improved, and when it is the predetermined value or less, the curved surface conformability of the decorative film tends to be improved. The lower limit of the upper yield point load of the soft acrylic resin may be 2.0N / 10mm or more, preferably 3.0N / 10mm or more, and more preferably 3.5N / 10mm or more, from the viewpoint of further improving the workability of the decorative film. The upper limit of the upper yield point load of the soft acrylic resin may be less than 10.0N / 10mm, preferably 7.0N / 10mm or less, more preferably 5.0N / 10mm or less, or more preferably 4.5N / 10mm or less, from the viewpoint of further improving the curved surface conformability of the decorative film.
[0043] The soft acrylic resin may be an acrylic resin having a Shore A hardness of 70 or more and 90 or less. As the soft acrylic resin, for example, it is preferable to select an acrylic resin having a Shore A hardness of 70 or more and 90 or less as a first standard, and from the selected acrylic resins, select a resin that provides an upper yield point load of less than 10.0 N / 10 mm for the molded body that is the specified sheet material. The soft acrylic resin may be a commercially available product, and an example thereof is Parapet (registered trademark) SA-F1000P (Kuraray Co., Ltd.).
[0044] When a mixture of hard acrylic resin and soft acrylic resin is used as the acrylic resin, the mass-based mixing ratio of the soft acrylic resin to the hard acrylic resin may be, for example, 0.4 or more and 1.4 or less. The lower limit of the mixing ratio may be preferably 0.6 or more, or 0.9 or more. The upper limit of the mixing ratio may be preferably 1.2 or less, or 1.1 or less.
[0045] At least one of the hard acrylic resin and the soft acrylic resin may be formed from a resin composition containing core-shell particles in which a core particle having rubber elasticity is coated with an acrylic resin. The core-shell particles in which a core particle having rubber elasticity is coated with an acrylic resin may be formed by polymerization of a monomer mixture containing a core particle, an acrylic acid ester, and a multifunctional monomer and another monofunctional monomer copolymerizable therewith, which are included as necessary. At least one of the hard acrylic resin and the soft acrylic resin may be a thermoplastic elastomer.
[0046] Examples of acrylic acid esters include esters of acrylic acid and saturated aliphatic alcohols having 1 to 18 carbon atoms; esters of acrylic acid and alicyclic alcohols having 5 or 6 carbon atoms; and esters of acrylic acid and phenols or aromatic alcohols. More specifically, examples of acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, octadecyl acrylate, cyclohexyl acrylate, phenyl acrylate, and benzyl acrylate.
[0047] Examples of polyfunctional monomers include esters of unsaturated monocarboxylic acids and unsaturated alcohols; diesters of unsaturated monocarboxylic acids and glycols; aromatic divinyl monomers; diesters of dicarboxylic acids and unsaturated alcohols; and conjugated diene monomers. Examples of unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and cinnamic acid. Examples of unsaturated alcohols include allyl alcohol and methallyl alcohol. Examples of glycols include ethylene glycol, propanediol, butanediol, and hexanediol. Examples of dicarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, and maleic acid. Examples of conjugated diene monomers include butadiene, isoprene, 2,3-dimethylbutadiene, 2-methyl-3-ethylbutadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 2-ethyl-1,3-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 3,4-dimethyl-1,3-hexadiene, 1,3-heptadiene, 3-methyl-1,3-heptadiene, 1,3-octadiene, cyclopentadiene, chloroprene, and myrcene. More specifically, examples of the polyfunctional monomer include allyl acrylate, methallyl acrylate, allyl methacrylate, methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate. Note that "(meth)acrylate" is a general term for acrylate and methacrylate, and refers to either or both of them.
[0048] Examples of other monofunctional monomers include methacrylate esters, aromatic vinyl monomers, and vinyl cyanide monomers.
[0049] Examples of methacrylic acid esters include esters of methacrylic acid and saturated aliphatic alcohols having 1 to 22 carbon atoms; esters of methacrylic acid and alicyclic alcohols having 5 or 6 carbon atoms; and esters of methacrylic acid and phenols or aromatic alcohols. More specifically, examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, and benzyl methacrylate.
[0050] Examples of aromatic vinyl monomers include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrenes.
[0051] Examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile.
[0052] [Coloring agent] The colorant may be a known pigment or dye used in paints for printing on resin films. The colorant may be used alone or in combination of two or more. The colorant is used in an amount according to the desired color to be expressed in the decorative film. Examples of white colorants include titanium oxide and barium sulfate. Examples of black colorants include iron black, carbon black, and aniline black. Examples of yellow colorants include cadmium yellow and oil yellow 2G. Examples of orange colorants include chrome vermilion and cadmium orange. Examples of red colorants include cadmium red, permanent red 4R, and oil red. Examples of purple colorants include cobalt violet and anthraquinone violet. Examples of blue colorants include ultramarine, Prussian blue, and cobalt blue. Examples of green colorants include phthalocyanine green and chrome green.
[0053] The content of the colorant in the colored layer may be, for example, 10 parts by mass or more and 30 parts by mass or less, and preferably 15 parts by mass or more or 25 parts by mass or less, relative to 100 parts by mass of the acrylic resin.
[0054] [Surface protective layer] The surface protective layer is a layer overlapping the colored layer, and is composed of a polyurethane resin. The polyurethane resin is preferably a resin that can design the upper yield point load of the surface protective layer at 20°C to be 3.5 N / 10 mm or more and 9.0 N / 10 mm or less. The polyurethane resin is one of the resin materials that affect the upper yield point load and stress relaxation rate of the decorative film. The polyurethane resin or the material thereof can be preferably selected from one-component thermoplastic resins used for film and sheet molding, or thermoplastic resins or thermoplastic elastomers for melt molding.
[0055] The polyurethane resin may be a resin material that imparts sufficient weather resistance to the decorative film by itself, or may be a resin material that imparts sufficient weather resistance to the decorative film by combining with an acrylic resin (laminate structure). The polyurethane resin may be used alone or in combination of two or more kinds. Examples of such polyurethane resins include polycarbonate-based urethane resins and polycaprolactone-based urethane resins. These polyurethane resins have a main chain of polycaprolactone or polycarbonate, etc., and a urethane structure. Here, the urethane structure is preferably a urethane structure derived from an aliphatic isocyanate or an alicyclic isocyanate. The polyurethane resin may be a commercially available product, and examples thereof include Resamine (registered trademark) NE-8836, NE-8850, and NE-8811 (all from Dainichi Seikagaku Kogyo Co., Ltd.), Miractoran (registered trademark) E580, E585, E590, E595, E598, E980, E985, E990, E995, and E998 (all from Nippon Miractoran Co., Ltd.), NY88A10F, NY993-10HB4, and NY585N11A (all from F.C.I. Co., Ltd.), and CRISBON (registered trademark) NY-393, NY-331, and NY-328FTR (all from DIC Corporation).
[0056] [Other ingredients] The colored layer and the surface protective layer may further contain other components other than the resin and the colorant as described above, within a range in which the effects of the present invention can be obtained. The content of the other components in each layer can be appropriately set within a range in which both the effects of the present invention and the effects of the other components can be obtained. Examples of the other components include ultraviolet absorbers, light stabilizers, plasticizers, and extender pigments. An example of the extender pigment is calcium carbonate.
[0057] The ultraviolet absorbing agent and the light stabilizer are preferable from the viewpoint of improving weather resistance. Examples of the ultraviolet absorbing agent include benzotriazole-based compounds, benzophenone-based compounds, cyanoacrylate-based compounds, ultrafine zinc oxide particles, ultrafine titanium oxide particles, etc. Examples of the light stabilizer include hindered amine-based compounds.
[0058] The colored layer and the surface protective layer described above can achieve the effects of the present invention without containing other components. For example, in this embodiment, by using a soft polyurethane resin and two kinds of acrylic resins with different hardness, it is possible to achieve the desired upper yield point load and stress relaxation rate described above without containing a plasticizer. In this way, the embodiment in which the decorative film does not contain other components (such as plasticizers) for adjusting the upper yield point load and stress relaxation rate is a preferred embodiment.
[0059] The "other components for adjusting the upper yield point load and the stress relaxation rate" may be used in an amount that affects the upper yield point load and the stress relaxation rate within the range that satisfies the constitution of the present invention. Components that exhibit the intended function but do not substantially affect the upper yield point load and the stress relaxation rate, such as ultraviolet absorbers and light stabilizers, are not included in the "other components for adjusting the upper yield point load and the stress relaxation rate." An embodiment in which the colored layer and the surface protective layer do not contain a plasticizer is a preferred embodiment from the viewpoint of suppressing bleeding out of the plasticizer.
[0060] [Other layers] The decorative film of the present embodiment may further have layers other than the above-mentioned colored layer and surface protective layer, as long as the effects of the present invention can be obtained. Examples of such layers include an adhesive layer and a pressure-sensitive adhesive layer.
[0061] The decorative film of this embodiment may further have an adhesive layer interposed between the colored layer and the surface protective layer to bond the two layers to each other. That is, the adhesive layer is disposed between the surface protective layer and the colored layer. The decorative film of this embodiment may further have a pressure-sensitive adhesive layer on the opposite side of the colored layer to the surface protective layer. The thicknesses of the adhesive layer and the pressure-sensitive adhesive layer may be appropriately set, for example, in the range of 3 μm to 70 μm, preferably in the range of 10 μm to 50 μm, more preferably in the range of 20 μm to 45 μm, and even more preferably in the range of 25 μm to 40 μm, depending on the type of pressure-sensitive adhesive and the object to be adhered.
[0062] The adhesive layer is, for example, composed of a first adhesive. The adhesive layer is an adhesive layer for attaching the decorative film to an object to be decorated, and is, for example, composed of a second adhesive. For both the first adhesive and the second adhesive, various known adhesives such as rubber-based, acrylic-based, silicone-based, and polyvinyl ether-based adhesives can be applied. The first adhesive and the second adhesive may be the same or different. The first adhesive and the second adhesive may be, for example, an acrylic adhesive.
[0063] The acrylic pressure sensitive adhesive may be composed of a homopolymer of a (meth)acrylic acid ester or a copolymer with a copolymerizable comonomer.
[0064] Examples of the (meth)acrylic acid ester include alkyl esters of (meth)acrylic acid; hydroxyalkyl esters of (meth)acrylic acid; alkylaminoalkyl esters of (meth)acrylic acid; and glycidyl esters of (meth)acrylic acid. Examples of "alkyl esters" of (meth)acrylic acid include methyl ester, ethyl ester, butyl ester, 2-ethylhexyl ester, octyl ester, and isononyl ester. Examples of "hydroxyalkyl esters" of (meth)acrylic acid include hydroxyethyl esters, hydroxybutyl esters, and hydroxyhexyl esters. Examples of (meth)acrylic acid alkylaminoalkyl esters include dimethylaminoethyl methacrylate, and t-butylaminoethyl methacrylate.
[0065] Examples of copolymerizable comonomers include (meth)acrylic acid, itaconic acid, maleic anhydride, (meth)acrylic acid amide, (meth)acrylic acid N-hydroxymethylamide, vinyl acetate, styrene, and acrylonitrile.
[0066] The above pressure-sensitive adhesive may further contain additives such as a crosslinking agent, a tackifier, a filler, an antioxidant, and a colorant, as required.
[0067] Examples of the crosslinking agent include an isocyanate compound, a polyisocyanate compound, a melamine resin, a urea resin, a polyamine, an epoxy compound, and a metal chelate compound.
[0068] The pressure-sensitive adhesive may be an ultraviolet-curable pressure-sensitive adhesive composition further containing a polymerization initiator. The ultraviolet-curable pressure-sensitive adhesive composition may further contain an ultraviolet-curable component as required.
[0069] The polymerization initiator may be, for example, a material that is cleaved by ultraviolet light of an appropriate wavelength to produce radicals that can trigger a polymerization reaction. Examples of polymerization initiators include benzoin alkyl ethers, aromatic ketones, aromatic ketals, and thioxanthones. Examples of benzoin alkyl ethers include benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Examples of aromatic ketones include benzil, benzophenone, and α-hydroxycyclohexyl phenyl ketone. An example of an aromatic ketal is benzyl dimethyl ketal. Examples of thioxanthones include chlorothioxanthone, dodecylthioxanthone, dimethylthioxanthone, and diethylthioxanthone.
[0070] The ultraviolet curing component is a component that adds a carbon-carbon double bond to the side chain of the acrylic polymer. When the polymer is an ultraviolet curing polymer having a carbon-carbon double bond in the side chain, the adhesive does not need to contain the ultraviolet curing component. Examples of the ultraviolet-curable component include esters of (meth)acrylic acid and polyhydric alcohols, and isocyanurate compounds.
[0071] Examples of esters of (meth)acrylic acid and polyhydric alcohols include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol (meth)acrylate, neopentyl glycol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0072] Examples of isocyanurate compounds include 2-hydroxyethylbis(2-acryloxyethyl)isocyanurate, tris(2-methacryloxyethyl)isocyanurate, and tris(2-methacryloxyethyl)isocyanurate.
[0073] [Specific Example] The layer structure of a decorative film according to one embodiment of the present invention is shown in Fig. 1. The decorative film 10 is disposed on the release surface of a release sheet 20. More specifically, the decorative film 10 is configured such that a surface protection layer 11, an adhesive layer 12, a colored layer 13, and a pressure-sensitive adhesive layer 14 are stacked on the release surface of the release sheet 20 in this order, starting from the pressure-sensitive adhesive layer 14.
[0074] The surface protective layer 11 may be made of a resin composition (polyurethane resin) containing, for example, at least one of a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin, and an ultraviolet absorbing agent.
[0075] Both the adhesive layer 12 and the pressure-sensitive adhesive layer 14 may be layers of an acrylic pressure-sensitive adhesive.
[0076] The colored layer 13 may be a layer in which a colorant such as a pigment is dispersed in a matrix resin. The matrix resin may be, for example, a resin composition (acrylic resin) containing at least one of a hard acrylic resin and a soft acrylic resin.
[0077] The decorative film 10 has sufficient weather resistance and can withstand, for example, an irradiation intensity of 75 mW / cm 2The total light output is 1200MJ / m 2 It is preferable that the color difference before and after irradiation with an integrated light quantity of 1350 MJ / m be 3.0 or less. 2 It is more preferable that the color difference before and after irradiation with light is 4.0 or less.
[0078] The total thickness of the surface protective layer 11 and the colored layer 13 is preferably 80 μm or more. By appropriately setting the total thickness of the surface protective layer 11 and the colored layer 13 and the materials and physical properties of each layer, the upper yield point load of the decorative film 10 at 20° C. can be set to 13.5 N / 10 mm or more and 25.0 N / 10 mm or less, and the stress relaxation rate at 20° C. can be set to 53% or more and 58% or less.
[0079] [Manufacturing method] The decorative film of the present embodiment can be produced by a method that enables the surface protective layer and the colored layer to be overlaid in this order.
[0080] For example, the decorative film of this embodiment can be manufactured by a method including the steps of preparing a colored layer, preparing a surface protective layer, and attaching the surface protective layer to the colored layer.
[0081] The step of preparing the colored layer may be a step of mixing an acrylic resin and a colorant and forming a film of the mixture obtained. The step of preparing the surface protective layer may be a step of producing a polyurethane resin layer, or a step of applying a material for the surface protective layer to one surface of the colored layer to form a coating film, and then solidifying or curing the coating film.
[0082] The step of attaching the surface protective layer to the colored layer may be, for example, a step of directly bonding the colored layer and the surface protective layer by heat fusion or the like. The step of attaching the surface protective layer to the colored layer may also be a step of supplying the material of the other layer in a layer form to one surface of a colored layer or a surface protective layer prepared in advance, and bonding the other layer onto the one layer to form the other layer. Furthermore, the step of attaching the surface protective layer to the colored layer may be a step of attaching the surface protective layer to an adhesive layer obtained by applying a first adhesive to one surface of the colored layer. Attaching the colored layer and the surface protective layer via an adhesive layer is advantageous from the viewpoint of increasing the degree of freedom in material design of both layers.
[0083] In addition, the production of the decorative film may further include other steps other than the steps described above. Such other steps may be, for example, a step of laminating a colored layer to a coating film obtained by applying a second adhesive to a release sheet. The decorative film having an adhesive layer is advantageous from the viewpoint of increasing the convenience of the decorative film, since the decorative film can be attached to an object to be decorated by peeling off the release sheet.
[0084] [Application] The decorative film of the present embodiment is preferably used for applications in which the film is attached to an object to be decorated to decorate the object to be decorated. The decorative film of the present embodiment has weather resistance and is excellent in curved surface conformability and application workability, and is therefore preferably used as a film for vehicle exterior that is adhered to an exterior part of a vehicle.
[0085] 〔summary〕 As is clear from the above description, the decorative film (10) of the first embodiment of the present invention is a weather-resistant decorative film having a colored layer (13) made of an acrylic resin and containing a colorant, and a surface protective layer (11) made of a polyurethane resin and overlapping the colored layer. The decorative film of the first embodiment of the present invention has an upper yield point load of 13.5 N / 10 mm or more and 25.0 N / 10 mm or less at 20° C., and a stress relaxation rate of 53% or more and 58% or less at 20° C. According to the first embodiment, a decorative film can be provided that fully exhibits weather resistance, application workability (for example, application workability when applied to a curved surface), and curved surface conformability.
[0086] The decorative film of the second embodiment of the present invention is the decorative film of the first embodiment, in which the upper yield point load of the surface protective layer at 20° C. is 3.5 N / 10 mm or more and 9.0 N / 10 mm or less, and the upper yield point load of the colored layer at 20° C. is 7.1 N / 10 mm or more and 14.1 N / 10 mm or less. The second embodiment is even more effective in terms of improving the attachment workability and curved surface conformability of the decorative film.
[0087] The decorative film of the third embodiment of the present invention is a decorative film having an integrated light quantity of 1200 MJ / m in the first or second embodiment. 2 The color difference before and after irradiation with light of 3.0 or less, or the accumulated light amount is 1300MJ / m 2 The color difference before and after irradiation with the light is 4.0 or less. The third aspect is even more effective in terms of increasing the color stability of the decorative film.
[0088] The decorative film of the fourth aspect of the present invention is any one of the first to third aspects, in which the total thickness of the surface protective layer and the colored layer is 80 μm or more. The fourth aspect is more effective from the viewpoint of appropriately adjusting at least one of the application property and the curved surface conformability of the decorative film.
[0089] The decorative film of the fifth aspect of the present invention is any one of the first to fourth aspects, in which the colored layer contains an acrylic resin including a hard acrylic resin and a soft acrylic resin. The fifth aspect is preferable from the viewpoint of realizing the desired properties of the colored layer and the decorative film, and from the viewpoint of fully exhibiting the weather resistance, the upper yield point load, and the stress relaxation rate of the decorative film.
[0090] The decorative film of the sixth aspect of the present invention is any one of the first to fifth aspects, in which the surface protective layer contains a polyurethane resin containing one or both of a polycarbonate-based urethane resin and a polycaprolactone-based urethane resin. The sixth aspect is preferable from the viewpoint of fully exhibiting the weather resistance, upper yield point load, and stress relaxation rate of the decorative film.
[0091] The decorative film of the seventh aspect of the present invention is any one of the first to sixth aspects, and further includes an adhesive layer (12) that is made of a first pressure-sensitive adhesive and is interposed between the colored layer and the surface protective layer to bond the two layers together. That is, the adhesive layer is disposed between the surface protective layer and the colored layer. The seventh aspect is even more effective from the viewpoint of increasing the degree of freedom in designing the resin materials of the colored layer and the surface protective layer.
[0092] The decorative film of the eighth aspect of the present invention is any one of the first to seventh aspects, and further includes an adhesive layer (14) made of a second adhesive and laminated on the colored layer on the side opposite to the surface protective layer. That is, the decorative film is formed by laminating the surface protective layer, the colored layer, and the adhesive layer in this order. The eighth aspect is even more effective from the viewpoint of improving the convenience of the decorative film.
[0093] The decorative film of the ninth aspect of the present invention is a film for vehicle exterior use that is adhered to an exterior part of a vehicle in any one of the first to eighth aspects. Since a film for vehicle exterior use requires all of weather resistance, curved surface conformability, and application workability, the ninth aspect is suitable for use of such a film for vehicle exterior use.
[0094] According to the above-mentioned configuration, it is possible to realize exterior decoration more easily than painting, and it is expected to contribute to reducing CO2 emissions in the decoration. The present invention, which has such an effect, is expected to contribute to the achievement of Goal 13 "Take urgent action to combat climate change" of the Sustainable Development Goals (SDGs) proposed by the United Nations, for example.
[0095] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0096] An embodiment of the present invention will now be described.
[0097] [Material preparation] The following materials were prepared. In the following, acrylic resin 1 and acrylic resin 3 correspond to hard acrylic resins, and acrylic resin 2 corresponds to soft acrylic resin. [Polyurethane resin] Polyurethane resin 1: Lezamin (registered trademark) NE-8836 (manufactured by Dainichiseika Chemicals Mfg. Co., Ltd., polycarbonate type) Polyurethane resin 2 NY88A10F (manufactured by FCI Co., Ltd., polyether type, melting temperature 150°C) Polyurethane resin 3 NY993-10HB4 (manufactured by FCI Co., Ltd., polycaprolactone type, melting temperature 160°C) Polyurethane resin 4 NY585N11A (manufactured by FCI Co., Ltd., polyester type, melting temperature 130℃) [Fluororesin] Fluorine resin Denka DX Film (manufactured by Denka Co., Ltd., product number 14S0230) [Acrylic resin] Acrylic resin 1: Parapet (registered trademark) GR-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load at a film thickness of 100 μm is 27.1 N / 10 mm, Shore A hardness 100) Acrylic resin 2: Parapet (registered trademark) SA-F1000P (manufactured by Kuraray Co., Ltd., upper yield point load at a film thickness of 100 μm is 3.9 N / 10 mm, Shore A hardness 70) Acrylic resin 3 Kaneace (registered trademark) MC-732 (manufactured by Kaneka Corporation, upper yield point load is 16.0 N / 10 mm when the film thickness is 100 μm) [Vinyl chloride resin] Polyvinyl chloride resin Kanevinyl (registered trademark) S1001N (manufactured by Kaneka Corporation, average degree of polymerization 1050) [Adhesive] Adhesive: Tg=-37.4℃, adhesive made by cross-linking acrylic resin with a BA / AA composition ratio of 90:10 with Aluminum Chelate A (Kawaken Fine Chemicals Co., Ltd.) [Additives (UV absorbers)] Additive 1 Tinuvin (registered trademark) 234 (manufactured by BASF Japan Ltd., UVA) Additive 2 Tinuvin® 213 (manufactured by BASF Japan Ltd., UVA)
[0098] [Measurement method] The measurement methods used in the following Examples and Comparative Examples will be described.
[0099] [Upper yield point load] A rectangular sample with a width of 10 mm and a length of 150 mm was prepared and subjected to a tensile test using a TENSILON (registered trademark, manufacturer: A&D, model number RTG-1310). Specifically, the distance between the chucks of the TENSILON was set to 100 mm, and the sample was clamped and fixed between the chucks. The sample was stretched at a constant tensile speed of 300 mm / min at 20°C, and the tensile load during stretching was measured. When the elastic limit of the hook is exceeded, the sample increases nonlinearly and reaches the upper yield point, at which point necking occurs. The load at the upper yield point was taken as the upper yield point load.
[0100] [Stress relaxation rate] A rectangular sample with a width of 10 mm and a length of 150 mm was prepared, and a tensile test was performed using TENSILON (registered trademark, manufacturer: A&D, model number RTG-1310). More specifically, the distance between the chucks of the TENSILON was set to 100 mm, and the sample was clamped and fixed between the chucks. The sample was stretched by 5% at a tensile speed of 300 mm / min at 20°C, and the tensile load x immediately after 5% stretching and the tensile load y 5 minutes after 5% stretching were measured. The stress relaxation rate z was then calculated from the following formula. z[%]={(xy) / x}×100
[0101] [Weather resistance] Weather resistance test A of the decorative film was carried out using a Daipla Metal Weather (model KW-R7TP-A) manufactured by Daipla Wintes Co., Ltd. The sample stage on which the decorative film was placed was set at an inclination angle of 15°, the black panel temperature (BPT) was 63°C, and the light irradiation intensity was 75mW / cm. 2 The surface of the decorative film was wetted with water by showering for 2 minutes every 120 minutes, and this cycle was repeated for 445 hours. The cumulative light intensity under the above test A conditions was 1200MJ / m 2 and the conditions of Test A correspond to a 3.0 year service life on an automotive surface.
[0102] In addition, a weather resistance test B of the decorative film was conducted using a Daipla Metal Weather (model KW-R7TP-A) manufactured by Daipla Wintes Co., Ltd. The sample stage on which the decorative film was placed was set at an inclination angle of 15°, the black panel temperature (BPT) was 63°C, and the light irradiation intensity was 75mW / cm. 2 The surface of the decorative film was wetted with water by showering for 2 minutes out of every 120 minutes, and this cycle was repeated for 500 hours. The cumulative light intensity in the above test B was 1350 MJ / m 2 The conditions of test B correspond to a 4.5-year service life on an automotive surface.
[0103] (1) Color difference Using the KONICA MINOLTA SPECTRO PHOTO METER CM-3600A, the L of the decorative film before the weather resistance test was measured.* , a * , b * value, and L' of the decorative film after weather resistance test * , a' * , and b' * The value was measured, and the color difference ΔE was calculated from the following formula. * is the brightness, a * is the position between red / magenta and green (negative values are toward green, positive values are toward magenta), b * represents a position between yellow and blue (negative values are toward bluer, positive values are toward yellower). ΔE = {(L' * -L * ) 2 +(a' * -a * ) 2 +(b' * -b * ) 2} 1 / 2
[0104] (2) Gloss A digital variable angle gloss meter (type UGV-5) manufactured by Suga Test Instruments Co., Ltd. was used to measure the change in gloss value at 60° of the decorative film before and after the weather resistance test.
[0105] (3) Appearance The decorative film was visually observed before and after the weather resistance test to see whether there were any changes in appearance, such as scratches or discoloration.
[0106] [Workability] A decorative film was applied to a portion of the outer surface of a car that included an uneven line, and the state of the decorative film applied to that portion was observed. (4) Floating (ability to follow curved surfaces) The decorative film attached to the above portion was left in an environment at 10° C. Separately, another decorative film attached to the above portion was left in an environment at 23° C. Then, the presence or absence of lifting during the time was visually observed. (5) Wrinkles during application (appliance) When the decorative film was attached to the above-mentioned portion, the occurrence of wrinkles in the decorative film was visually observed.
[0107] [Example 1] <Production of colored film (colored layer)> The following components were dry blended in the amounts shown below, then kneaded in a Henschel mixer, and formed into a film with a thickness of 100 μm in a calendar molding machine set at 180° C. to produce colored film 1. The carbon black shown below is a carbon black pigment (product name "W-8012-G5") manufactured by Nikko Vicks Co., Ltd., and is coated with an acrylic resin. The upper yield point load of the obtained colored film 1 was measured, and the upper yield point load of colored film 1 was 10.6 N / 10 mm. Acrylic resin 1 50 parts by weight Acrylic resin 2 50 parts by weight Carbon black 19 parts by weight Additive 1 0.3 parts by weight
[0108] <Manufacture of surface protective film (surface protective layer)> A dispersion liquid containing 100 parts by mass of polyurethane resin 1 in a 1:1 IPA:toluene solution so as to have a solid content of 25% by mass was mixed with 1.2 parts by mass of additive 2 and then cast. Next, the mixture was dried at 80°C for 3 minutes, and then dried at 140°C for 3 minutes to form a film with a thickness of 30 μm. In this way, surface protection film 1 was produced. The upper yield point load of surface protection film 1 was 5.9 N / 10 mm.
[0109] <Adhesion of both films> An adhesive was applied to one surface of the colored film 1, and the surface protective film 1 was placed on the adhesive coating to adhere the surface protective film 1 to the colored film 1. In this way, a base film 1 was produced in which a colored layer, an adhesive layer made of an adhesive, and a surface protective layer were layered in this order. The adhesive layer had a thickness of 30 μm. The upper yield point load of the obtained base film 1 was 17.4 N / 10 mm, and the stress relaxation rate of the base film 1 was 56%.
[0110] <Adhesion to release sheet> The colored film 1 of the base film 1 was laminated on the coating of the adhesive formed by applying the adhesive onto the release film. In this way, a decorative film 1 was produced in which the release film, the adhesive layer made of the adhesive, the colored film 1, the adhesive layer, and the surface protection film 1 were laminated in this order. The thickness of the adhesive layer was 40 μm.
[0111] [Example 2] A colored film 2 was produced in the same manner as in Example 1, except that the amount of acrylic resin 1 in the production of the colored film was 59 parts by mass and the amount of acrylic resin 2 was 41 parts by mass. The upper yield point load of the colored film 2 was 13.2 N / 10 mm. A base film 2 and a decorative film 2 were produced in the same manner as in Example 1, except that the colored film 2 was used instead of the colored film 1. The upper yield point load of the base film 2 was 20.0 N / 10 mm, and the stress relaxation rate was 57%.
[0112] [Example 3] A colored film 3 was produced in the same manner as in Example 1, except that the amount of acrylic resin 1 in the production of the colored film was 55 parts by mass and the amount of acrylic resin 2 was 45 parts by mass. The upper yield point load of the colored film 3 was 11.8 N / 10 mm. A base film 3 and a decorative film 3 were produced in the same manner as in Example 1, except that the colored film 3 was used instead of the colored film 1. The upper yield point load of the base film 3 was 18.6 N / 10 mm, and the stress relaxation rate was 56%.
[0113] [Example 4] A colored film 4 was produced in the same manner as in Example 1, except that the amount of acrylic resin 1 in the production of the colored film was 48 parts by mass and the amount of acrylic resin 2 was 52 parts by mass. The upper yield point load of the colored film 4 was 8.3 N / 10 mm. A base film 4 and a decorative film 4 were produced in the same manner as in Example 1, except that the colored film 4 was used instead of the colored film 1. The upper yield point load of the base film 4 was 15.1 N / 10 mm, and the stress relaxation rate was 56%.
[0114] [Example 5] Surface protection film 5 was produced in the same manner as in Example 1, except that 50 parts by mass of polyurethane resin 1 and 50 parts by mass of polyurethane resin 3 were used instead of 100 parts by mass of polyurethane resin 1 in the production of the surface protection film. The upper yield point load of surface protection film 5 was 5.2 N / 10 mm. Substrate film 5 and decorative film 5 were produced in the same manner as in Example 1, except that surface protection film 5 was used instead of surface protection film 1. The upper yield point load of substrate film 5 was 16.7 N / 10 mm, and the stress relaxation rate was 56%.
[0115] [Example 6] In the manufacture of the surface protection film, a surface protection film 6 was produced in the same manner as in Example 1, except that polyurethane resin 3 was used instead of polyurethane resin 1. The upper yield point load of the surface protection film 6 was 4.5 N / 10 mm. A base film 6 and a decorative film 6 were produced in the same manner as in Example 1, except that surface protection film 6 was used instead of surface protection film 1. The upper yield point load of the base film 6 was 16.0 N / 10 mm, and the stress relaxation rate was 56%.
[0116] [Example 7] In the production of the colored film, a colored film 7 was produced in the same manner as in Example 1, except that 30 parts by mass of acrylic resin 2 and 70 parts by mass of acrylic resin 3 were used. The upper yield point load of the colored film 7 was 10.2 N / 10 mm. A base film 7 and a decorative film 7 were produced in the same manner as in Example 1, except that the colored film 7 was used instead of the colored film 1. The upper yield point load of the base film 7 was 16.6 N / 10 mm, and the stress relaxation rate was 56%.
[0117] [Example 8] In the production of the colored film, a colored film 8 was produced in the same manner as in Example 2, except that the thickness of the colored film was 70 μm. The upper yield point load of the colored film 8 was 9.8 N / 10 mm. A base film 8 and a decorative film 8 were produced in the same manner as in Example 2, except that the colored film 8 was used instead of the colored film 2. The upper yield point load of the base film 8 was 17.4 N / 10 mm, and the stress relaxation rate was 56%.
[0118] [Examples 9 to 11] In the production of the colored film, a titanium oxide pigment manufactured by Nikko Bix Co., Ltd. (product name: "W-0612-G5"), which is a white colorant, was used instead of carbon black. In addition, in the production of the colored film, a blue pigment manufactured by Nikko Bix Co., Ltd. (product name: "W-6122-G5"), which is a blue colorant, was used instead of 19 parts by mass of carbon black. In the production of the colored film, a blue film 10 was produced in the same manner as in Example 1. In addition, in the production of the colored film, a diketopyrrolopyrrole pigment manufactured by Nikko Bix Co., Ltd. (product name: W-1572-G5), which is a red colorant, was used instead of carbon black. In the production of the colored film, a diketopyrrolopyrrole pigment manufactured by Nikko Bix Co., Ltd. (product name: W-1572-G5) was used instead of carbon black. In ... each case, the upper yield point load of the colored films 9 to 11 was 10.6 N / 10 mm.
[0119] Substrate films 9 to 11 and decorative films 9 to 11 were obtained in the same manner as in Example 1, except that colored films 9 to 11 were used instead of colored film 1. The upper yield point loads of the substrate films 9 to 10 were all 17.4 N / 10 mm, the upper yield point load of the substrate film 11 was 16.6 N / 10 mm, and the stress relaxation rates of all were 56%.
[0120] [Comparative Example 1] In the production of the colored film, a colored film C1 was produced in the same manner as in Example 1, except that 60 parts by mass of acrylic resin 1 and 40 parts by mass of acrylic resin 2 were used. The upper yield point load of the colored film C1 was 14.2 N / 10 mm. The base film C1 and the decorative film C1 were produced in the same manner as in Example 1, except that the colored film C1 was used instead of the colored film 1. The upper yield point load of the base film C1 was 21.0 N / 10 mm, and the stress relaxation rate was 59%.
[0121] [Comparative Example 2] In the production of the colored film, a colored film C2 was produced in the same manner as in Example 1, except that 40 parts by mass of acrylic resin 1 and 60 parts by mass of acrylic resin 2 were used. The upper yield point load of the colored film C2 was 6.5 N / 10 mm. The base film C2 and the decorative film C2 were produced in the same manner as in Example 1, except that the colored film C2 was used instead of the colored film 1. The upper yield point load of the base film C2 was 13.2 N / 10 mm, and the stress relaxation rate was 54%.
[0122] [Comparative Examples 3 to 6] In the production of the colored film, 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2 were replaced with 100 parts by mass of acrylic resin 1 to acrylic resin 3 and vinyl chloride resin, respectively, in the same manner as in Example 1 to produce the colored films C3 to C6. The upper yield point load of the colored film C3 was 27.1 N / 10 mm, the upper yield point load of the colored film C4 was 3.9 N / 10 mm, the upper yield point load of the colored film C5 was 16.0 N / 10 mm, and the upper yield point load of the colored film C6 was 18.3 N / 10 mm. And, the base film C3 to C6 and the decorative film C3 to C6 were each produced in the same manner as in Example 1, except that the colored film 1 was replaced with the colored film C3 to C6. The upper yield point load of the base film C3 was 33.9 N / 10 mm, and the stress relaxation rate was 62%. The upper yield point load of the base film C4 was 10.7 N / 10 mm, and the stress relaxation rate was 51%. The upper yield point load of the base film C5 was 22.8 N / 10 mm, and the stress relaxation rate was 60%. The upper yield point load of the base film C6 was 23.9 N / 10 mm, and the stress relaxation rate was 68%.
[0123] [Comparative Examples 7 to 9] 100 parts by mass of each of polyurethane resins 4 to 2 was mixed with 1.2 parts by mass of additive 2 and 19 parts by mass of carbon black, and then the composition was formed into a film having a thickness of 160 μm using an extruder under the conditions of a rotation speed of 7 rpm, a load of 30 A, and a line speed of 1.0 m / min at 160 ° C. Thus, each of surface protection films C7 to C9 was produced. The upper yield point load of surface protection film C7 was 9.1 N / 10 mm, the upper yield point load of surface protection film C8 was 10.6 N / 10 mm, and the upper yield point load of surface protection film C9 was 9.9 N / 10 mm.
[0124] Then, the base film C7 to C9 and the decorative film C7 to C9 were produced in the same manner as in Example 1, except that the adhesive layer and the colored film were not used. The upper yield point load of the base film C7 was 9.1 N / 10 mm, and the stress relaxation rate was 49%. The upper yield point load of the base film C8 was 10.6 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C9 was 9.9 N / 10 mm, and the stress relaxation rate was 50%.
[0125] [Comparative Example 10] A dispersion containing 100 parts by mass of polyurethane resin 1 in a 1:1 IPA:toluene solution so that the solid content was 25% by mass was mixed with 1.2 parts by mass of additive 2 and 19 parts by mass of carbon black, and then cast. Next, the mixture was dried at 80°C for 3 minutes, and then dried at 140°C for 3 minutes to form a film with a thickness of 160 μm. In this way, a surface protective film C10 was produced. The upper yield point load of the surface protective film C10 was 14.0 N / 10 mm. Then, a base film C10 and a decorative film C10 were obtained in the same manner as in Example 1, except that an adhesive layer and a colored film were not used. The upper yield point load of the base film C10 was 14.0 N / 10 mm, and the stress relaxation rate was 50%.
[0126] [Comparative Examples 11 to 14] In the production of the colored films, the same procedure as in Example 1 was repeated except that 100 parts by mass of each of polyurethane resins 1 to 4 was used instead of 50 parts by mass of acrylic resin 1 and 50 parts by mass of acrylic resin 2. The upper yield point load of colored film C11 was 7.0 N / 10 mm, the upper yield point load of colored film C12 was 5.2 N / 10 mm, the upper yield point load of colored film C13 was 5.3 N / 10 mm, and the upper yield point load of colored film C14 was 5.0 N / 10 mm.
[0127] Then, the base film C11 to C14 and the decorative film C11 to C14 were produced in the same manner as in Example 1, except that the colored film 1 was replaced with the colored film C11 to C14. The upper yield point load of the base film C11 was 13.8 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C12 was 12.0 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C13 was 12.1 N / 10 mm, and the stress relaxation rate was 50%. The upper yield point load of the base film C14 was 11.8 N / 10 mm, and the stress relaxation rate was 50%.
[0128] [Comparative Examples 15 and 16] In the production of the surface protection film, a fluororesin was used instead of the polyurethane resin 1, and the thickness was 50 μm. The surface protection film C15 was produced in the same manner as in Example 1 except that the upper yield point load was 19.3 N / 10 mm. In addition, in the production of the colored film, a colored film C15 was produced in the same manner as in Example 1 except that 100 parts by mass of polyvinyl chloride was used instead of 50 parts by mass of the acrylic resin 1 and 50 parts by mass of the acrylic resin 2. The upper yield point load of the colored film C15 was 22.3 N / 10 mm. And, the surface protection film C15 was used instead of the surface protection film 1, and the colored film C15 was used instead of the colored film 1. The upper yield point load of the base film C15 was 48.5 N / 10 mm, and the stress relaxation rate was 64%.
[0129] In addition, in the manufacture of the surface protection film, a fluororesin was used instead of the polyurethane resin 1, and a thickness of 30 μm was used, but the same procedure as in Example 1 was used to produce a surface protection film C16. The upper yield point load of the surface protection film C16 was 13.1 N / 10 mm. The same procedure as in Example 1 was used to obtain a base film C16 and a decorative film C16, but the upper yield point load of the base film C16 was 23.4 N / 10 mm, and the stress relaxation rate was 63%.
[0130] [Comparative Example 17] A base film C17 and a decorative film C17 were obtained in the same manner as in Example 1, except that the thickness of the colored film 1 was 50 μm. The upper yield point load of the base film C17 was 12.4 N / 10 mm, and the stress relaxation rate was 50%.
[0131] The compositions, layer structures, upper yield point loads, and stress relaxation rates of the base films 1 to 11 and the decorative films 1 to 11 are shown in Tables 1 and 2. The compositions, layer structures, upper yield point loads, and stress relaxation rates of the base films C1 to C17 and the decorative films C1 to C17 are shown in Tables 3 and 4. In Tables 1 to 4, the upper yield point loads and stress relaxation rates of the decorative films correspond to the upper yield point loads and stress relaxation rates of the base films, respectively.
[0132] [Table 1]
[0133] [Table 2]
[0134] [Table 3]
[0135] [Table 4]
[0136] [evaluation] The weather resistance and workability evaluations described above were carried out for each of the decorative films 1 to 11 and C1 to C17, and the results were evaluated based on the following criteria. The upper yield point load and stress relaxation rate were evaluated using the measurement results of a tensile test on the state (laminate consisting of the combination of the surface protection layer, adhesive layer, and colored layer, i.e., the base film) before bonding with the release film coated with adhesive. <Upper yield point load> A: 13.5N / 10mm or more and 20.0N / 10mm or less. B: Greater than 20.0N / 10mm and less than 25.0N / 10mm. It was outside the range of CA and B (less than 13.5N / 10mm or greater than 25.0N / 10mm). <Stress relaxation rate> S: 55% or more and 58% or less. A: 53% or more but less than 55%. B: 48% or more but less than 53%. They were outside the CS, A, and B ranges (<48% or >58%). <Color difference ΔE (Test A, cumulative light amount 1200MJ / m 2 )> S ΔE≦1.0 A 1.0<ΔE≦1.5 B 1.5<ΔE≦3.0 C ΔE>3.0 <Color difference ΔE (Test B, accumulated light amount 1350MJ / m 2 )> S ΔE≦1.0 A 1.0<ΔE≦1.5 B 1.5<ΔE≦4.0 C ΔE>4.0 <Gloss change> A The change in gloss value before and after the weather resistance test was within ±5. C The change in gloss value before and after the weather resistance test was greater than ±5. <Abnormal appearance> A No abnormalities in appearance were observed. B: Minor abnormalities in appearance such as small scratches were observed. C: Visible scratches or yellowing or other obvious abnormalities in appearance were observed. <Float> S: No floating was observed even after more than two weeks in both floating evaluations at 10℃ and 23℃. A: When evaluated for floating at 10°C, floating occurred within 1 week or more and up to 2 weeks. B Floating occurred within 3 days at 10°C. C Floating occurred within 24 hours in both the 10℃ and 23℃ floatation evaluations. <Wrinkles during application> No (A) No wrinkles were generated when applied to the uneven lines of a car. Yes (C) Wrinkles occurred during application.
[0137] <Overall rating> The above evaluation results were converted into scores based on the following criteria. S 2 points A 1 point B 0 points C -1 point
[0138] The scores for each decorative film were then totaled, and the decorative films were evaluated according to the scores according to the following criteria. A Total of 8 points or more B Total of 3 points or more and 7 points or less C Total of 2 points or less
[0139] The weather resistance, workability and overall evaluation of decorative films 1 to 11 are shown in Tables 5 and 6. The weather resistance, workability and overall evaluation of decorative films C1 to C17 are shown in Tables 7 to 9. Yellowing was confirmed when the appearance of decorative film C7 was observed. Yellowing and cracks were confirmed when the appearance of decorative film C9 was observed.
[0140] [Table 5]
[0141] [Table 6]
[0142] [Table 7]
[0143] [Table 8]
[0144] [Table 9]
[0145] [Consideration] All of the decorative films 1 to 11 have sufficient weather resistance, curved surface conformability, and application workability. This is believed to be because the surface protective layer uses a urethane resin with excellent weather resistance, and the decorative film has an appropriate upper yield point load and stress relaxation rate. More specifically, if the stress relaxation rate is within the range of the embodiment, the decorative film will not float when attached to a curved surface, and if the upper yield point load is within the range of the embodiment, it is believed that wrinkles in the decorative film during application can be suppressed. And, since the decorative films 1 to 11 are laminated with a layer containing a polyurethane resin and a layer containing an acrylic resin, it is believed that it is possible to adjust the physical properties to have excellent weather resistance, as well as suppression of lifting of the decorative film and suppression of wrinkles during application.
[0146] In all of the decorative films C1 to C17, at least one of the upper yield point load and the stress relaxation rate of the decorative film was outside the specific range, and at least one of the evaluations of lifting and wrinkles during application was lower than the evaluations of the examples.
[0147] In addition, decorative films C6, C7, C9, C12, and C14 tended to have a higher ΔE, and at least one of the changes in gloss over time and abnormalities in appearance was insufficient. From these results, it is considered that the lamination of a layer containing polyurethane resin and a layer containing acrylic resin sufficiently improves weather resistance. [Industrial Applicability]
[0148] The present invention can be suitably used as a decorative film for decorating an object to be decorated, which may have a curved or uneven surface, and which requires weather resistance, such as a film for the exterior of a vehicle. [Explanation of symbols]
[0149] 10 Decorative film 11 Surface protective layer 12 Adhesive layer 13 Colored layer 14 Adhesive layer 20 Release sheet
Claims
1. A decorative film including a surface protective layer and a coloring layer, The surface protective layer contains a polyurethane resin, The colored layer contains an acrylic resin and a colorant, The upper yield point load of the decorative film at 20° C. is 13.5 N / 10 mm or more and 25.0 N / 10 mm or less, A decorative film having a stress relaxation rate of 53% or more and 58% or less at 20°C.
2. The decorative film according to claim 1 , wherein the acrylic resin comprises a hard acrylic resin and a soft acrylic resin.
3. The decorative film according to claim 1 , wherein the polyurethane resin comprises at least one selected from the group consisting of polycarbonate-based urethane resins and polycaprolactone-based urethane resins.
4. The upper yield point load of the surface protective layer at 20° C. is 3.5 N / 10 mm or more and 9.0 N / 10 mm or less, The decorative film according to claim 1, wherein the colored layer has an upper yield point load of 7.1 N / 10 mm or more and 14.1 N / 10 mm or less at 20°C.
5. Accumulated light intensity: 1200 MJ / m 2 2. The decorative film according to claim 1, wherein the color difference before and after irradiation with light is 3.0 or less.
6. Accumulated light quantity: 1350 MJ / m 2 2. The decorative film according to claim 1, wherein the color difference before and after irradiation with light is 4.0 or less.
7. The decorative film according to claim 1 , further comprising an adhesive layer, the adhesive layer being disposed between the surface protective layer and the coloring layer.
8. The decorative film according to claim 1 , further comprising an adhesive layer, the adhesive layer being disposed on a surface of the colored layer opposite to the surface protective layer.
Citation Information
Patent Citations
Film for forming ornamental layer, ornamental article and production process for ornamental article
JP2007297569A
Marking sheet
JP2008214434A
Cited By
Electroabsorption modulator and optical semiconductor device
CN121634574A