Decorative sheet, resin-impregnated decorative panel, and method for manufacturing resin-impregnated decorative panel
The decorative sheet with a controlled release layer configuration addresses the balance of peeling and gloss matte design issues, achieving stable peeling and matte finish in resin-impregnated boards.
Patent Information
- Application Number
- JP2024053792
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-15
AI Technical Summary
Existing decorative sheets for resin-impregnated boards struggle to balance the functions of selectively peeling off the cured resin layer and expressing a gloss matte design due to trade-offs in composition and structure, leading to instability in achieving both properties.
A decorative sheet with a specific configuration of a porous base material, design layer, and release layer, where the release layer has a 60° gloss value of 10 or less, a pure water contact angle of 85° or more, and an Spc (arithmetic mean curvature of peaks) of 80 mm⁻¹ or more, allowing for controlled peeling and gloss difference.
The solution enables stable peeling of the cured resin layer and expression of a gloss matte design by optimizing the release layer's properties, ensuring good releasability and matte finish.
Smart Images

Figure 2024146885000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a decorative sheet used in the manufacture of a resin-impregnated decorative board, a resin-impregnated decorative board, and a method for manufacturing a resin-impregnated decorative board. [Background technology]
[0002] Conventionally, resin-impregnated decorative boards are known which are obtained by impregnating a porous substrate with a precursor such as a melamine resin and then curing the resin precursor. Resin-impregnated decorative boards are used for walls, furniture, floors, etc. of residences, stores, public facilities, etc.
[0003] Melamine decorative boards that express a glossy matte design are known. For example, Patent Document 1 discloses a decorative board having a release layer in harmony with a pattern on a part of the surface of a porous substrate, and a thermosetting resin layer containing a melamine resin on the remaining surface area that does not have the release layer, and the thermosetting resin is impregnated and cured in the porous substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6716877 Summary of the Invention [Problem to be solved by the invention]
[0005] The release layer of the decorative sheet used in the manufacture of resin-impregnated decorative boards is required to have two functions simultaneously: 1) the function of selectively releasing the cured resin layer cured by the heating and pressurizing process, and 2) the function of expressing a good gloss matte design by the gloss difference with the cured resin layer. However, there is still room for further study in designing a decorative sheet that has a stable balance between the two functions.
[0006] The present disclosure has been made in consideration of the above-mentioned situation, and has as its main object to provide a decorative sheet used in the manufacture of resin-impregnated decorative boards, in which the cured resin layer cured by a heating and pressurizing process can be selectively peeled off, and which can express a gloss matte design due to the difference in gloss between the release layer and the cured resin layer. [Means for solving the problem]
[0007] In the present disclosure, there is provided a decorative sheet used in the manufacture of a resin-impregnated decorative board, the decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in this order in a thickness direction, the release layer having a 60° gloss value of 10 or less, a pure water contact angle of 85° or more, and an Spc (arithmetic mean curvature of peaks) of the release layer of 80 mm -1 As described above, a decorative sheet is provided.
[0008] In the present disclosure, there is provided a resin-impregnated decorative board, comprising: a decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in that order in the thickness direction; a core substrate arranged to face the porous substrate in the decorative sheet; and a cured resin layer arranged between the patterns of the release layer, thicker than the release layer, and containing a cured product of curable resin Y. The core substrate and the porous substrate contain the cured product of the curable resin Y, and the pure water contact angle of the release layer is 85° or more, and the Spc (arithmetic mean curvature of the peaks) of the release layer is 10 mm or less. -1 As described above, a resin-impregnated decorative board is provided.
[0009] The present disclosure also provides a method for producing a resin-impregnated decorative board, the method comprising: a preparation step for preparing the decorative sheet; a laminate formation step for forming a laminate having, in the thickness direction, a core substrate, the decorative sheet, a curable resin layer containing a curable resin Y, and a release film, in that order; (ii) a surface of the decorative sheet facing the porous substrate is arranged to face the core substrate; and (iii) the decorative sheet is impregnated with the curable resin Y; a heating and pressurizing step for heating and pressurizing the laminate to form a cured resin layer from the curable resin layer while curing the curable resin Y, thereby obtaining a cured laminate; and a peeling step for peeling the release film from the cured laminate, thereby removing the cured resin layer arranged in a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between the patterns of the release layer. Effect of the Invention
[0010] The present disclosure has the effect of providing a decorative sheet in which the cured resin layer cured by the heating and pressurizing process can be selectively peeled off, and which can express a gloss matte design due to the difference in gloss between the release layer and the cured resin layer. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. [Diagram 3] 1 is a schematic cross-sectional view illustrating a resin-impregnated decorative board according to the present disclosure. [Figure 4] 1 is a schematic cross-sectional view illustrating a method for producing a resin-impregnated decorative board using a decorative sheet according to the present disclosure. [Diagram 5] 1 is a schematic cross-sectional view illustrating a method for producing a resin-impregnated decorative board using a decorative sheet according to the present disclosure. [Figure 6] FIG. 2 is a diagram illustrating a method for producing a backing plate used when measuring the 60° gloss value of a release layer in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes the embodiments with reference to the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the description of the embodiments exemplified below. In addition, in order to clarify the description, the drawings may show the width, thickness, and shape of each part in a schematic manner compared to the actual form, but this is merely an example and should not be interpreted as being limiting.
[0013] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.
[0014] A. Decorative sheet The decorative sheet in the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view illustrating a decorative sheet in the present disclosure. The decorative sheet 10 shown in Fig. 1 is a decorative sheet used in the manufacture of a resin-impregnated decorative board, and comprises a porous substrate 1, a design layer 2, a release layer 3 having a pattern shape, and a thickness direction D T In the present disclosure, the 60° gloss value of the release layer 3 is 10 or less, the pure water contact angle of the release layer 3 is 85° or more, and the Spc (arithmetic mean curvature of the peaks) of the release layer 3 is 80 mm -1 That's all.
[0015] The release layer contains, for example, a matting agent and a release agent. Here, in order to improve the releasability of the release layer to the cured resin layer, methods such as increasing the content of the release agent, decreasing the content of the matting agent, decreasing the particle diameter of the matting agent, and increasing the film thickness of the release layer can be considered. However, these methods reduce the matte feeling and reduce the gloss matte design. On the other hand, methods such as decreasing the content of the release agent, increasing the content of the matting agent, increasing the particle diameter of the matting agent, and decreasing the film thickness of the release layer improve the gloss matte design while reducing the releasability. As such, since the releasability of the release layer to the cured resin layer and the gloss matte design are in a trade-off relationship, it is difficult to fully control the above two functions only by the composition and configuration. Furthermore, since there is a pressurizing process in the process of manufacturing the resin-impregnated decorative board, even if the release layer has a sufficient matte feeling in the state of the decorative sheet, the matte feeling may be lost after the pressurizing process. Therefore, there is still room for consideration in designing a decorative sheet that has a stable balance between the two functions.
[0016] The inventors of the present application have discovered that by controlling each of the parameters of the release layer, namely the 60° gloss value, pure water contact angle, and Spc (arithmetic mean curvature of the peaks) within a predetermined range, it is possible for the release layer to achieve both releasability from the cured resin layer and a gloss matte design with the cured resin layer.
[0017] 1.Release layer The release layer in the present disclosure is disposed on the surface of the design layer opposite the porous substrate, and has a pattern shape. In the area having the design layer on the porous substrate, at least a part of the release layer is disposed on the surface of the design layer opposite the porous substrate, and in the area not having the design layer on the porous substrate, the porous substrate and the release layer may be in contact with each other.
[0018] I. Characteristics In the present disclosure, the release layer has a 60° gloss value of 10 or less, a pure water contact angle of 85° or more, and an Spc (arithmetic mean curvature of peaks) of 80 mm -1As long as the 60° gloss value, the pure water contact angle, and the Spc are adjusted to fall within the above-mentioned ranges, the release layer can selectively peel off the cured resin layer, and a gloss matte design can be achieved due to the difference in gloss from the cured resin layer.
[0019] (1) 60° gloss value The release layer in the present disclosure usually has a 60° gloss value of 10 or less, preferably 6.5 or less, more preferably 5.5 or less, and even more preferably 4.0 or less. When the 60° gloss value is within the above range, the release layer imparts a matte design feel, thereby enabling a glossy matte design feel to be expressed. On the other hand, the 60° gloss value is, for example, 0.5 or more, preferably 1.0 or more, more preferably 1.2 or more, and even more preferably 2.0 or more.
[0020] In the present disclosure, the 60° gloss value of the release layer refers to the 60° specular gloss measured in accordance with Method 3 of JIS Z 8741:1997, and is a value measured by the following method. The decorative sheet is placed with the release layer side facing up, and the 60° specular gloss is measured from the release layer side using a gloss meter in accordance with method 3 of JIS Z 8741:1997. The 60° gloss value of the release layer is the average value of the measured values at any 10 points. At each measurement point, the release layer is located at the center of the measurement area of the gloss meter, and the measurement is performed after confirming that the area ratio of the release layer is 30% or more, preferably 50% or more, of the area of the measurement area. As a specific method, the method described in the examples can be adopted.
[0021] The 60° gloss value of the release layer can be adjusted by the average particle size of the matting agent, the content of the matting agent, and the thickness of the release layer. For example, the 60° gloss value can be lowered by reducing the thickness of the release layer. For example, the 60° gloss value can be lowered by increasing the content of the matting agent. For example, the 60° gloss value can be lowered by increasing the average particle size of the matting agent.
[0022] (2) Pure water contact angle The pure water contact angle of the release layer in the present disclosure is usually 85° or more, preferably 90° or more, more preferably 100° or more, and even more preferably 110° or more. When the pure water contact angle of the release layer is in the above range, the releasability of the cured resin layer is good. In addition, the contamination resistance is improved. On the other hand, the pure water contact angle of the release layer is, for example, 130° or less, and preferably 125° or less.
[0023] In the present disclosure, the pure water contact angle of the release layer is a value obtained by measuring by the following method. That is, the decorative sheet is placed on a horizontal surface with the release layer facing up. Next, a water droplet (pure water, 2.0 μL) is dropped onto the release layer from a direction perpendicular to the horizontal surface. At this time, the water droplet is not dropped on the boundary between the design layer and the release layer, but is dropped so that the entire water droplet is in contact with the release layer. After dropping the water droplet, wait for 1 second, and use a contact angle meter to measure the contact angle between the release layer and pure water. The above measurement is performed at any 10 points, and the average value is taken as the pure water contact angle.
[0024] The pure water contact angle can be adjusted by adjusting the content of the release agent and the thickness of the release layer. For example, the pure water contact angle can be increased by increasing the content of the release agent. For example, the pure water contact angle can be increased by increasing the thickness of the release layer.
[0025] (3) Spc (arithmetic mean curvature of the peak) The release layer in the present disclosure has an Spc (arithmetic mean peak curvature) of typically 80 mm -1 Above 100mm -1 It is preferable that the length is 120 mm or more. -1 More preferably, it is 150 mm or more. -1 It is more preferable that the Spc of the release layer is in the above range. Even after the heating and pressing process, the matte surface feeling is not lost, and a glossy matte design feeling can be expressed. On the other hand, the Spc (arithmetic mean curvature of the peaks) is 300 mm -1It is preferable that the length is less than 200 mm. -1 It is more preferable that:
[0026] Spc (arithmetic mean curvature of mountain peaks) is one of the three-dimensional surface texture parameters defined in ISO25178, and is the average curvature (average sharpness) of the tip of the mountain peak, calculated from the arithmetic mean value of the curvature radius of the mountain peaks (peaks) of the parts classified as mountains (convex parts) in the feature image included in the reference area. For this reason, Spc (arithmetic mean curvature of mountain peaks) is the reciprocal (mm -1 )
[0027] The larger the value of Spc (arithmetic mean curvature of the apex), the greater the curvature of the tip of the apex (convex part) (the reciprocal of the curvature radius is smaller, and the tip shape is sharper). On the other hand, the smaller the value of Spc (arithmetic mean curvature of the apex), the smaller the curvature of the apex (protrusion apex) (the reciprocal of the curvature radius is larger, and the tip shape is blunter).
[0028] In the present disclosure, the Spc (arithmetic mean curvature of the peaks) of the release layer is the average value of measurements taken on the surface of the release layer of a decorative sheet using a laser microscope manufactured by Keyence Corporation, with measurement points selected so that all of the measurement points are within the release layer, at any 10 points measured under the following conditions: (Measurement conditions) Objective lens: 5x Laser wavelength: 661nm Measurement area for each point: 500μm×500μm
[0029] Spc can be adjusted, for example, by the average particle size of the matting agent. Specifically, Spc can be increased by increasing the average particle size of the matting agent. In addition, Spc can be increased by increasing the content of the matting agent.
[0030] II. Composition (1) Resin component The release layer contains a resin component. The resin component is typically a cured product (crosslinked structure) of a curable resin X. Alternatively, the resin component may be a thermoplastic resin. In particular, the release layer preferably contains a cured product of a curable resin X. This is because a release layer having good abrasion resistance can be obtained. Furthermore, when the release layer contains a cured product of a curable resin X, the release layer has good releasability with respect to the cured resin layer.
[0031] Examples of the curable resin X include ionizing radiation curable resins and thermosetting resins. Examples of the ionizing radiation curable resin include electron beam curable resins and ultraviolet ray curable resins.
[0032] The ionizing radiation curable resin (ionizing radiation curable compound) is not limited as long as it undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes into a three-dimensional polymer structure. Examples of the ionizing radiation curable resin include prepolymers, oligomers, and monomers having polymerizable unsaturated bonds or epoxy groups in the molecule that can be crosslinked upon irradiation with ionizing radiation. In the present disclosure, only one type of ionizing radiation curable resin may be used, or two or more types may be used. Among them, it is preferable to use at least one of a polyfunctional monomer and an oligomer as the ionizing radiation curable resin.
[0033] Examples of ionizing radiation curable resins include (meth)acrylate-based resins such as urethane (meth)acrylate, ester (meth)acrylate, and epoxy (meth)acrylate; silicon-based resins such as siloxane; ester-based resins; and epoxy-based resins. (Meth)acrylate-based resins refer to acrylate-based resins or methacrylate-based resins.
[0034] The weight average molecular weight of the ionizing radiation curable resin is, for example, from 500 to 80,000, and may be from 1,000 to 50,000. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0035] The ionizing radiation curable resin preferably contains at least a polyfunctional monomer or oligomer having a weight average molecular weight of at least 500. Examples of such polyfunctional monomers or oligomers include (meth)acrylate-based resins such as dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, urethane (meth)acrylate, ester (meth)acrylate, and epoxy (meth)acrylate.
[0036] On the other hand, examples of thermosetting resins include unsaturated ester resins, urethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine urea co-condensation resins, silicon resins, and siloxane resins.
[0037] (2) Mattifying agent The release layer preferably contains a matting agent. Examples of the matting agent include inorganic particles and synthetic resin particles. Examples of the inorganic particles include silica, alumina, calcium carbonate, magnesium carbonate, calcium sulfate, barium sulfate, and kaolin. Examples of the synthetic resin particles include acrylic beads, urethane beads, nylon beads, silicone beads, silicone rubber beads, polycarbonate beads, and polyolefin wax (e.g., polypropylene wax, polyethylene wax).
[0038] The average particle size of the matting agent is, for example, 0.3 μm or more and 10 μm or less, or may be 0.5 μm or more and 7 μm or less, or may be 1 μm or more and 5 μm or less. The average particle size is D50 according to the volume-based particle size distribution measured by a laser diffraction scattering method.
[0039] The content of the matting agent is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and particularly preferably 10 parts by mass or more, relative to 100 parts by mass of the release layer. 100 parts by mass of the release layer means that the total solid content of the release layer is 100 parts by mass. On the other hand, the content of the matting agent is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and particularly preferably 15 parts by mass or less, relative to 100 parts by mass of the release layer.
[0040] (3) Release agent The release layer may contain a release agent. By adding a release agent, the releasability is improved. Examples of the release agent include silicone-based release agents such as silicone oil, wax-based release agents such as polyolefin wax, and fluorine-based release agents. Among them, silicone oil is preferred. This is because it has excellent heat resistance in the heating and pressurizing process. The silicone oil may be reactive silicone oil or non-reactive silicone oil, but reactive silicone oil is preferred. This is because it has even better heat resistance.
[0041] Reactive silicone oil refers to modified silicone oils that have an organic group introduced into the side chain or end, and have reactivity due to the nature of the organic group introduced.Specific examples of reactive silicone oils include modified silicone oil side chain type, modified silicone oil both ends type, modified silicone oil one end type, modified silicone oil side chain both ends type, etc., in which the organic group introduced is amino-modified, epoxy-modified, mercapto-modified, carboxyl-modified, carbinol-modified, phenol-modified, methacryl-modified, heterogeneous functional group-modified, etc.These reactive silicone oils can be used alone or in combination of two or more.
[0042] The non-reactive silicone oil is not particularly limited as long as it is a silicone oil that does not have a reactive functional group such as an amino group, an epoxy group, a mercapto group, a carboxy group, a hydroxy group, a (meth)acryloyl group, or an allyl group. Examples of the non-reactive silicone oil include silicone oils made of polysiloxane, polyether-modified silicone oils, aralkyl-modified silicone oils, fluoroalkyl-modified silicone oils, long-chain alkyl-modified silicone oils, higher fatty acid ester-modified silicone oils, higher fatty acid amide-modified silicone oils, and phenyl-modified silicone oils. These non-reactive silicone oils can be used alone or in combination of two or more kinds.
[0043] The content of the release agent is, for example, 1 part by mass or more and 10 parts by mass or less, preferably 2 parts by mass or more and 9 parts by mass or less, and more preferably 3 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the release layer.
[0044] The release layer may be colorless or colored. In the latter case, the release layer preferably contains a colorant. The colorant may be the same as the colorant used in the design layer described later.
[0045] The release layer may contain additives such as ultraviolet absorbers, infrared absorbers, light stabilizers, polymerization inhibitors, crosslinking agents, antistatic agents, antioxidants, leveling agents, coupling agents, plasticizers, defoamers, fillers, thermal radical generators, aluminum chelating agents, etc. The weather resistance of the release layer can be improved by adding ultraviolet absorbers and light stabilizers.
[0046] III. Thickness and Proportions The thickness of the release layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less, preferably 0.3 μm or more and 10 μm or less, and more preferably 0.5 μm or more and 8 μm or less. The thickness of the release layer refers to the thickness of the part that does not penetrate into the design layer 2 side and protrudes from the surface of the design layer 2 opposite to the substrate 1, as shown in the thickness T3 of the release layer 3 in FIG. 3. In addition, when the release layer is viewed from the pattern thickness direction of the decorative sheet, the ratio of S1 to S2 (S1 / S2) is, for example, 5% or more, and may be 10% or more. On the other hand, S1 / S2 is, for example, 80% or less, may be 70% or less, or may be 60% or less.
[0047] IV. Formation method The release layer is obtained, for example, by applying an ink for forming a release layer containing a curable resin X to the surface of the design layer opposite to the porous substrate and curing it. Since a part of the ink for forming a release layer penetrates the porous substrate, the porosity of the porous substrate affects the pure water contact angle, 60° gloss value, and Spc, as shown in the examples described later. In addition, the composition of the ink for forming a release layer (for example, the ratio of weathering agents such as light stabilizers and ultraviolet absorbers) mainly affects the 60° gloss value and Spc, as shown in the examples described later. In the present disclosure, good releasability and good gloss matte design can be obtained by adjusting the pure water contact angle, 60° gloss value, and Spc to a predetermined range while taking these influences into consideration.
[0048] When the ink for forming the release layer contains an electron beam curable resin as the curable resin X, the cured product of the electron beam curable resin is usually obtained by irradiating it with an electron beam. Examples of the electron beam source include various electron beam accelerators such as Cockcroft-Walt type, Van de Graff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is, for example, 100 kV or more and 1000 kV or less, or may be 100 kV or more and 300 kV or less. The irradiation dose of the electron beam is, for example, 2 Mrad or more and 15 Mrad or less.
[0049] When the ink for forming the release layer contains an ultraviolet-curable resin as the curable resin X, the ultraviolet-curable resin is usually cured by irradiating it with ultraviolet light. Examples of ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of the ultraviolet light is, for example, 190 nm or more and 380 nm or less.
[0050] When the ink for forming the release layer contains a thermosetting resin as the curable resin X, the ink is usually heated to obtain a cured product of the thermosetting resin. The heating temperature is appropriately set according to the type of the thermosetting resin. The ink for forming the release layer may contain a curing agent such as a crosslinking agent and a polymerization initiator, and a polymerization accelerator, in addition to the thermosetting resin. Examples of the curing agent include isocyanates, organic sulfonates, organic amines, peroxides (e.g., methyl ethyl ketone peroxide), and radical initiators (azoisobutylnitrile).
[0051] The ink for forming the release layer may contain a solvent as necessary. Examples of the solvent include water, hydrocarbon compounds such as toluene and xylene, alcohol compounds such as methanol, ethanol and methyl glycol, ketone compounds such as acetone and methyl ethyl ketone, ester compounds such as methyl formate and ethyl acetate, nitrogen-containing compounds such as N-methylpyrrolidone and N,N-dimethylformamide, ether compounds such as tetrahydrofuran and dioxane, halogenated hydrocarbon compounds such as methylene chloride and chloroform, and dimethyl sulfoxide.
[0052] V.Other The release layer has releasability with respect to the cured resin layer located between the release layer and the release film in the manufacturing process of the resin-impregnated decorative board described below. By having such releasability, in the resin-impregnated decorative board 100 shown in Fig. 3 manufactured using the decorative sheet of the present disclosure, the release layer 3 gives a matte design feel, and the cured resin layer 32 gives a glossy design feel, thereby expressing a glossy matte design feel.
[0053] Also, as shown in FIG. 2, it is preferable that the release layer 3 is arranged so as to be in harmony with the pattern of the design layer 2. "In harmony" means that the shapes and positions of the two target patterns are roughly the same. Specifically, it means that the shapes and positions of the release layer pattern and at least a part of the pattern constituting the design layer pattern are in harmony to an extent that does not impair the realism and luxury. In FIG. 2, the design layer 2 has a design layer y1 and a design layer y2, and the release layer 3 is in harmony with the design layer y1. By arranging the pattern of the release layer so as to be in harmony with the design layer pattern, a high quality texture can be obtained. On the other hand, the release layer does not have to be arranged so as to be in harmony with the design layer pattern.
[0054] 2. Design layer The design layer in the present disclosure is disposed on one surface of the porous substrate. The design layer preferably has a pattern.
[0055] Examples of patterns of the design layer include organic patterns, inorganic patterns, and abstract patterns. Organic patterns are patterns derived from the life activities of living organisms such as animals and plants. Inorganic patterns are patterns that do not fall under the category of organic patterns. Abstract patterns are patterns that interpret objects (e.g., images that exist in nature) abstractly and do not express a clear shape. Examples of organic patterns include wood grain patterns, leather patterns, floral patterns, and botanical patterns. Examples of inorganic patterns include stone patterns, concrete patterns, sand patterns, cloth patterns, metal patterns, tile patterns, and brick masonry patterns. Examples of abstract patterns include flickering patterns (e.g., ink flickering patterns), smoke patterns, and marble patterns.
[0056] The design layer has, for example, a pattern layer. The design layer may have a solid layer on the porous substrate side of the pattern layer. In the present disclosure, the pattern layer means a layer formed partially (particularly in a pattern) on one side of the porous substrate. The solid layer means a layer formed on the entire surface of one side of the porous substrate.
[0057] The design layer contains, for example, a colorant and a resin component. Examples of the colorant include inorganic pigments such as carbon black, titanium white, zinc oxide, red iron oxide, Prussian blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. Dyes may also be used as the colorant.
[0058] Examples of the resin component include (meth)acrylic resins, ester urethane resins, acrylamide resins, ethylene oxide resins, N-vinylpyrrolidone resins, ester resins, amide resins, vinyl acetate resins, vinyl chloride resins, urethane (meth)acrylic resins, natural rubber, and synthetic rubber. Among these, (meth)acrylic resins and urethane (meth)acrylic resins are preferred.
[0059] It is preferable that the resin component contains a resin having at least one polar group selected from the group consisting of a hydroxyl group, an amino group, and a carboxyl group. By containing the resin having the polar group, the impregnation of the curable resin Y into the porous substrate is improved.
[0060] A resin having a polar group contains at least one of the following polar groups: a hydroxy group (-OH), an amino group (-NH2), and a carboxy group (-COOH). The polar group may be ionized and stabilized, for example, by the influence of a solvent or other functional groups. Therefore, the "hydroxy group (-OH)" is in the ionized state, "-O - " and the above "amino group (-NH2)" is in the ionized state "-NH3 + " is a concept that includes "carboxyl group (-COOH)" in its ionized state, "-COO - " is a concept that includes
[0061] Examples of resins having one or more polar groups, such as a hydroxy group (-OH), an amino group (-NH2), or a carboxy group (-COOH), include aqueous proteins such as casein, cellulose derivatives such as cellulose, acetyl cellulose, cellulose nitrate, hydroxypropyl cellulose, and carboxymethyl cellulose, polyvinyl alcohol derivatives such as polyvinyl butyral resin, amino resins such as melamine resin, (meth)acrylic acid resins, phenolic resins, acrylic polyols, and natural polymers (for example, polynucleotides, polypeptides, and polysaccharides).
[0062] The design layer in the present disclosure preferably contains one or more of casein, melamine-based resin, polyvinyl alcohol, polyvinyl alcohol derivative, cellulose, and cellulose derivative as a resin having a polar group, and more preferably contains casein. As casein, α-casein, β-casein, γ-casein, or a mixture thereof can be used. As casein, derivatives such as sodium caseinate and ammonium caseinate can be used alone or in combination.
[0063] The ratio of the resin having the polar group to the resin components contained in the design layer is, for example, 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more. On the other hand, the ratio of the resin having the polar group is, for example, 100% by mass or less, or 90% by mass or less. If the content of the resin having the polar group is within the above range, the penetration of the ink of the release layer into the porous substrate can be further suppressed without inhibiting the penetration of the curable resin Y into the porous substrate.
[0064] The design layer may contain additives such as fillers (e.g., silica), extender pigments (e.g., organic beads), neutralizers, surfactants, etc., as necessary. The thickness of the design layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less.
[0065] The method for forming the design layer includes, for example, a coating method using an ink for forming the design layer containing a colorant, a binder resin, and a solvent (or a dispersion medium). For example, the ink for forming the design layer is applied to one side of the porous substrate and dried to obtain the design layer.
[0066] Examples of the solvent (or dispersion medium) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water.
[0067] Examples of the coating method include printing. Examples of the printing method include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. Examples of the coating method for forming a solid layer include various coating methods such as roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating.
[0068] 3. Porous base material The porous substrate in the present disclosure is a substrate impregnated with the curable resin Y during the manufacture of the resin-impregnated decorative board. Examples of the porous substrate include permeable fibrous substrates. Examples of the permeable fibrous substrate include paper, synthetic paper, nonwoven fabric, and woven fabric. Examples of the paper include titanium paper, tissue paper, craft paper, linter paper, paperboard, gypsum board paper, fine paper, coated paper, parchment paper, and Japanese paper. In addition, vinyl wallpaper rolls (paper dry-laminated with polyvinyl chloride resin) can also be used as the fibrous substrate. Other examples of the fibrous substrate include nonwoven fabrics or woven fabrics containing inorganic fibers such as glass fiber, asbestos, potassium titanate fiber, alumina fiber, silica fiber, and carbon fiber. Other examples of the fibrous substrate include nonwoven fabrics or woven fabrics containing synthetic resin fibers such as polyester, vinylon, polyethylene, and polypropylene. Among these porous substrates, titanium paper, thin paper, kraft paper, coated paper, art paper, parchment paper, paraffin paper, and Japanese paper are preferred in terms of impregnation with the curable resin Y. In particular, titanium paper is preferred as a porous substrate because it has excellent impregnation with the curable resin Y and also has excellent hiding power.
[0069] The porous substrate may be colored. For example, a colorant is added at the manufacturing stage of the porous substrate to obtain a colored porous substrate. For example, when the porous substrate is paper, a colorant is added at the papermaking stage to obtain colored paper. Examples of the colorant include inorganic pigments such as titanium dioxide, carbon black, and iron oxide, organic pigments such as phthalocyanine blue, and various dyes. The amount of the colorant is appropriately set according to the desired color tone. The porous substrate may also contain various additives such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, ultraviolet absorbers, and light stabilizers, as necessary.
[0070] The basis weight of the porous substrate is not particularly limited, but is, for example, 40 g / m 2 More than 150g / m 2The thickness of the porous substrate is not particularly limited, but is, for example, 50 μm or more and 170 μm or less. For example, in order to improve the adhesion of the ink that forms the design layer, the surface of the porous substrate on the design layer side may be subjected to a corona discharge treatment.
[0071] 4. Decorative sheets The decorative sheet of the present disclosure is used for producing a resin-impregnated decorative board. A method for producing a resin-impregnated decorative board using the decorative sheet of the present disclosure will be described later.
[0072] B. Resin-impregnated decorative board The resin-impregnated decorative board in the present disclosure will be described in detail below. Figure 3 is a schematic cross-sectional view illustrating the resin-impregnated decorative board in the present disclosure. The resin-impregnated decorative board 100 shown in Figure 3 includes a decorative sheet 10 having a porous substrate 1, a design layer 2, and a release layer 3 having a pattern shape in this order in the thickness direction, a core substrate 20 arranged to face the porous substrate 1 in the decorative sheet 10, and a cured resin layer 32 arranged between the patterns of the release layer 3, thicker than the release layer 3, and containing a cured product of a curable resin Y, the porous substrate containing the cured product of the curable resin Y, the pure water contact angle of the release layer 3 is within a predetermined range, and the Spc (arithmetic mean curvature of the peak) of the release layer 3 is within a predetermined range.
[0073] According to the resin-impregnated decorative board of the present disclosure, the pure water contact angle of the release layer is equal to or greater than a predetermined value, and the Spc (arithmetic mean curvature of the peaks) of the release layer is equal to or greater than a predetermined value, so that the cured resin layer arranged in a position overlapping the release layer is peeled off well, and a resin-impregnated decorative board having a good gloss matte design between the release layer and the cured resin layer is obtained.
[0074] 1. Decorative sheet The decorative sheet of the present disclosure has, in this order in the thickness direction, a porous substrate, a design layer, and a release layer having a pattern shape.
[0075] (1) Release layer In the resin-impregnated decorative board of the present disclosure, the pure water contact angle of the release layer is usually 85° or more, preferably 90° or more, more preferably 100° or more, and even more preferably 110° or more. When the pure water contact angle of the release layer in the resin-impregnated decorative board is in the above range, the peelability of the cured resin layer is good. In addition, the contamination resistance is improved. On the other hand, the pure water contact angle of the release layer in the resin-impregnated decorative board is, for example, 130° or less, and preferably 125° or less.
[0076] The pure water contact angle of the release layer in the resin-impregnated decorative plate is a value measured by completely removing the cured resin layer remaining on the release layer to expose the release layer, and then measuring the pure water contact angle of the release layer in the same manner as described in detail in "A. Decorative sheet" above. The method of removing the cured resin layer remaining on the release layer can be, for example, the same method as the cellophane tape resistance test in the examples.
[0077] The method for adjusting the pure water contact angle of the release layer is the same as that described in detail above in "A. Decorative sheet".
[0078] The Spc (arithmetic mean curvature of the peaks) of the release layer in the resin-impregnated decorative board is 10 mm -1 Above 15mm -1 More than 20mm is preferable. -1 More preferably, 40 mm or more -1 More preferably, 60 mm or more -1 The above is particularly preferable. If the Spc of the release layer is within the above range, the release layer imparts a matte design to the resin-impregnated decorative board, thereby allowing a glossy matte design to be expressed. On the other hand, the Spc (arithmetic mean curvature of the peaks) of the release layer in the resin-impregnated decorative board is, for example, 140 mm -1 Less than or equal to 120mm -1 Less than 100mm is preferable -1 The following is more preferred:
[0079] In the resin-impregnated decorative board, the method of measuring and adjusting the Spc of the release layer is the same as that described in detail above in "A. Decorative sheet."
[0080] The 60° gloss value of the release layer of the resin-impregnated decorative board is preferably 10 or less, more preferably 8 or less, and particularly preferably 7.5 or less. When the 60° gloss value of the release layer is within the above range, the release layer imparts a matte design feel, thereby making it possible to express a gloss matte design feel. On the other hand, the 60° gloss value of the release layer of the resin-impregnated decorative board is, for example, 2.0 or more, and preferably 3.0 or more.
[0081] The method of measuring and adjusting the 60° gloss of the release layer in the resin-impregnated decorative board is the same as that described in detail above in "A. Decorative sheet."
[0082] (2) Porous substrate and design layer The porous substrate and the design layer in this disclosure are the same as those described in detail in "A. Decorative sheet" above. In addition, in the resin-impregnated decorative board, the porous substrate contains a cured product of the curable resin Y.
[0083] 2. Cured resin layer The resin-impregnated decorative board of the present disclosure has a cured resin layer disposed between the patterns of the release layer and thicker than the release layer. The 60° gloss value of the cured resin layer is preferably greater than the 60° gloss value of the release layer. This is because a gloss matte design can be expressed. The 60° gloss value of the cured resin layer is, for example, 11 or more, may be 15 or more, or may be 20 or more. On the other hand, the 60° gloss value of the cured resin layer is, for example, 60 or less, may be 55 or less, or may be 50 or less.
[0084] In the resin-impregnated decorative board, the difference between the 60° gloss value of the release layer and the 60° gloss value of the cured resin layer is preferably 1.0 or more, and more preferably 3.0 or more, because this provides a more distinct gloss matte effect.
[0085] In the resin-impregnated decorative board, the ratio (G32 / G3) of the 60° gloss value G32 of the cured resin layer 32 to the 60° gloss value G3 of the release layer 3 is preferably 1.2 or more, and more preferably 1.5 or more, because this provides a more distinct gloss matte effect.
[0086] The cured resin layer includes a cured product of the curable resin Y. Among them, the curable resin Y is preferably a thermosetting resin. As the thermosetting resin, a wide variety of thermosetting resins can be used. Examples of the thermosetting resin include melamine-based resins (melamine-based resin precursors), melamine-urea co-condensation resins, unsaturated polyester-based resins, polyurethane-based resins (including two-component curing polyurethanes), epoxy-based resins, aminoalkyd-based resins, phenol-based resins, urea-based resins, diallyl phthalate-based resins, guanamine-based resins, silicon-based resins, and polysiloxane-based resins. Examples of methods for impregnating the thermosetting resin include a method of immersing the decorative sheet in a bath containing the thermosetting resin; a method of applying the thermosetting resin to the decorative sheet using a coater such as a kiss coater or a comma coater; and a method of spraying the thermosetting resin onto the decorative sheet using a spray device or a shower device.
[0087] In the present disclosure, the thickness T of the cured resin layer 32 32 is thicker than the thickness T3 of the release layer 3. The unevenness of the surface makes it easier to improve the design of the surface. 32 is not particularly limited, but may be, for example, 1 μm or more, and may be 10 μm or more. On the other hand, the thickness T 32 is, for example, 500 μm or less, and may be 300 μm or less. 32 The thickness T may be less than 30 μm. 32 By reducing the thickness T of the cured resin layer, the workability when peeling the release film from the cured resin layer is improved. 32 may be 28 μm or less, may be 25 μm or less, or may be 20 μm or less.
[0088] In this embodiment, the difference between the top position of the release layer and the top position of the cured resin layer (surface height difference of the resin-impregnated decorative sheet) is, for example, preferably 0.5 μm or more and 45.0 μm or less, more preferably 2.0 μm or more and 35.0 μm or less, and even more preferably 3.0 μm or more and 30.0 μm or less. The difference may be 0.5 μm or more and 25 μm or less, 2.0 μm or more and 25 μm or less, or 3.0 μm or more and 20 μm or less.
[0089] 3. Core substrate The resin-impregnated decorative board of the present disclosure has a porous core substrate 20 on the surface of the decorative sheet 10 facing the porous substrate 1 (the surface of the decorative sheet 10 that faces the porous substrate 1 with respect to the design layer 2). By having a core substrate, the mechanical strength of the resin-impregnated decorative board can be increased. An example of the core substrate 20 is phenolic resin-impregnated paper. The phenolic resin-impregnated paper is paper obtained by, for example, impregnating kraft paper, which is a core paper, with phenolic resin and drying it. The core substrate may contain a cured product of the curable resin Y.
[0090] 4. Hardened resin The porous substrate in the present disclosure contains a cured product of a curable resin Y. As described below, the cured product of the curable resin Y filled in the porous substrate and the cured product of the curable resin Y contained in the cured resin layer are formed of the same curable resin Y. These cured products are, for example, cured products of a thermosetting resin.
[0091] The resin-impregnated decorative board of the present disclosure preferably has a total light transmittance as defined in JIS K7361-1:1997 of 10% or less, more preferably 5% or less, and even more preferably 1% or less.
[0092] 5. Resin-impregnated decorative panels The resin-impregnated decorative board in the present disclosure is used, for example, by being disposed on the surface of a substrate. Examples of substrates include wood members, resin members, metal members, and ceramic members. Examples of wood members include wood veneer, wood plywood, particle board, and wood fiberboard. Examples of wood used for wood members include cedar, cypress, pine, and lauan. Examples of resins used for resin members include vinyl chloride resins, (meth)acrylic resins, ester resins, styrene resins, olefin resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), phenolic resins, cellulose resins, carbonate resins, melamine resins, and rubber. Examples of metals used for metal members include iron and aluminum. The material of the ceramic members may be ceramics such as glass and porcelain, non-cement ceramic materials such as gypsum, and non-ceramic ceramic materials such as ALC (lightweight aerated concrete).
[0093] The resin-impregnated decorative board of the present disclosure can be used, for example, as a building material or furniture. The building material can be an interior material or an exterior material. The building material can be, for example, a wall, a floor, a ceiling, a door, or a shelf. The furniture can be, for example, a table, a desk, or a cabinet.
[0094] C. Manufacturing method of resin-impregnated decorative board 4(a)-(d) and 5(a) and (b) are schematic cross-sectional views illustrating a method for manufacturing a resin-impregnated decorative board according to the present disclosure. The method for manufacturing a resin-impregnated decorative board according to the present disclosure includes a preparation step (FIG. 4(a)) of preparing the decorative sheet 10 described above, and a laminate shape forming step of forming a laminate 52 having (i) a core substrate 20, a decorative sheet 10, a curable resin layer 30 containing a curable resin Y, and a release film 40, in that order in the thickness direction, (ii) the surface of the decorative sheet 10 on the porous substrate 1 side is disposed opposite the core substrate 20, and (iii) the decorative sheet 10 is impregnated with the curable resin Y. The method includes a forming step (FIGS. 4(b) to 4(d)), a heating and pressurizing step (FIG. 5(a)) of heating and pressurizing the laminate 52 to harden the curable resin Y while forming a cured resin layer 31 from the curable resin layer 30, thereby obtaining a cured laminate 53, and a peeling step (FIG. 5(b)) of peeling the release film 40 from the cured laminate 53, thereby removing the cured resin layer 31 arranged at a position overlapping with the release layer 3 in the thickness direction, while leaving the cured resin layer 31 arranged between the patterns of the release layer 3.
[0095] 1.Preparation process This step is a step of preparing a decorative sheet. Details of the decorative sheet are as described above.
[0096] 2.Laminate formation process As shown in FIG. 4(d), this process is a process for forming a laminate 52 having (i) a core substrate 20, a decorative sheet 10, a curable resin layer 30 containing curable resin Y, and a release film 40, in that order in the thickness direction, (ii) the surface of the decorative sheet 10 facing the porous substrate 1 faces the core substrate 20, and (iii) the decorative sheet 10 is impregnated with the curable resin Y.
[0097] The method of forming such a laminate is not particularly limited. For example, as shown in FIG. 4(b), the decorative sheet 10 is impregnated with the curable resin Y, and the curable resin layer 30 that covers the design layer 2 and the release layer 3 and contains the curable resin Y is formed to obtain a precursor laminate 51 (FIG. 4(c)). Next, the release film 40 is placed on the surface of the precursor laminate on the side of the curable resin layer 30, and the core substrate 20 is placed on the side of the precursor laminate 51 opposite to the side having the release layer. This allows the laminate 52 to be obtained.
[0098] Details of the core substrate and the curable resin Y are as described above.
[0099] In this step, for example, the decorative sheet is immersed in a curable resin composition containing the curable resin Y. After immersion, it is preferable to dry the sheet. At this time, a part of the curable resin may be cured to give a semi-cured state.
[0100] The curable resin composition is a curable resin composition containing a curable resin Y. The ratio of the curable resin Y in the curable resin composition is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. The curable resin composition may contain water, alcohol, organic solvent, etc. as a solvent.
[0101] The release film is, for example, a film containing a polyester resin such as polyethylene terephthalate or polybutylene terephthalate, a polyolefin resin such as polyethylene or polypropylene, an acrylic resin, etc. The release film may have a release layer containing a cured product of the ionizing radiation curable resin composition on the surface facing the curable resin layer.
[0102] Another method for forming the laminate in this step is, for example, to arrange a core substrate so as to face the porous substrate in the decorative sheet, and while impregnating the core substrate and the porous substrate with the curable resin Y, to form a curable resin layer that covers the design layer and the release layer and contains the curable resin Y. Then, a release film 40 is arranged on the surface on the curable resin layer side. This also allows the laminate to be obtained.
[0103] 3. Heat and pressure process In this step, the laminate 52 is heated and pressurized to cure the curable resin Y, thereby forming the cured resin layer 31 from the curable resin layer 30, thereby obtaining the cured laminate 53.
[0104] The heating temperature is, for example, 90° C. or more and 160° C. or less, and the heating time is, for example, 30 seconds or more and 30 minutes or less.
[0105] 4. Peeling process In this process, the release film is peeled off from the cured laminate 53 to remove the cured resin layer 31 arranged at a position overlapping with the release layer 3 in the thickness direction, while leaving the cured resin layer 31 arranged between the patterns of the release layer 3. This results in a resin-impregnated decorative board 100 having the porous substrate 1, the design layer 2 arranged on one side of the porous substrate 1, the release layer 3 arranged on the side of the design layer 2 opposite the porous substrate 1 and having a pattern shape, and the cured resin layer 32 arranged between the patterns of the release layer 3 of the decorative sheet.
[0106] The resin-impregnated decorative board obtained by such a method for producing a resin-impregnated decorative board can have the Spc and pure water contact angle of the release layer within the ranges described above in "B. Resin-impregnated decorative board." Therefore, the cured resin layer arranged at a position overlapping the release layer can be peeled off well, and a resin-impregnated decorative board with a good gloss matte design between the release layer and the cured resin layer can be produced.
[0107] The present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0108] [Example 1] (Making decorative sheets) As a porous substrate, a paper substrate (basis weight 80 g / m 2 Titanium base paper for building materials (PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured in accordance with JIS-P8252 and found to be 26%. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain design by a gravure printing method using the following printing ink. Furthermore, the following ink 1 for forming a release layer was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0109] <Printing ink> Pigments (azo, quinacridone, carbon black, etc.) 10 parts by weight Casein / acrylic resin 10 parts by weight ·Water 70 parts by mass Dipropyl glycol 5 parts by weight Isopropyl alcohol 5 parts by weight
[0110] <Release layer forming ink 1> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0111] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0112] The impregnated decorative sheet is made by impregnating craft paper with phenolic resin liquid, with a basis weight of 245g / m 2 The sheet was laminated on top of a core substrate consisting of three sheets of phenolic resin-impregnated core paper (obtained by impregnating a core craft paper with a liquid uncured resin composition made of phenolic resin), and the release film described below was further laminated on top of the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, thereby obtaining a laminate.
[0113] (Preparation of release film) A coating solution containing 100 parts by mass of an ionizing radiation curable monomer (Aronix M-350, manufactured by Toagosei Co., Ltd.), 2 parts by mass of a reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.), 8 parts by mass of silica particles (product name "Silisia 450", average particle size: 8.0 μm, manufactured by Fuji Silysia Chemical Ltd.), and 50 parts by mass of ethyl acetate was applied at a rate of 5 g / m to the adhesive surface of a 50 μm-thick PET film (Cosmoshine (registered trademark) A4160, manufactured by Toyobo Co., Ltd.). 2 The coating was applied in an amount of (when dry) and cured by irradiation with an electron beam of 5 Mrad at an acceleration voltage of 165 kV to produce a release film having a peelable layer.
[0114] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This formed a cured laminate. Then, the cured laminate was taken out from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 1. When the release film was peeled off and removed from the cured laminate, the cured resin layer on the release layer of the cured resin layer was removed together with the release film, and the cured resin layer formed in the area without the release layer was left.
[0115] [Example 2] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 2 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0116] <Release layer forming ink 2> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 5.4 parts by weight (9.0 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0117] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0118] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0119] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 2.
[0120] [Example 3] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern. Furthermore, the following release layer forming ink 3 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0121] <Release layer forming ink 3> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 10.6 parts by weight (17.7 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0122] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0123] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0124] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 3.
[0125] [Example 4] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 4 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous base material, a design layer, and a release layer were laminated in this order.
[0126] <Release layer forming ink 4> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 1.4 parts by mass (2.3 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0127] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0128] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0129] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 4.
[0130] [Example 5] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 5 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous base material, a design layer, and a release layer were laminated in this order.
[0131] <Release layer forming ink 5> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 46.6 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 5.4 parts by mass (9.0 parts by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0132] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0133] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0134] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 5.
[0135] [Example 6] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 6 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0136] <Release layer forming ink 6> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 50.6 parts by mass Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 5 μm) 5.4 parts by weight (9.0 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0137] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0138] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0139] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 6.
[0140] [Example 7] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 7 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous base material, a design layer, and a release layer were laminated in this order.
[0141] <Release layer forming ink 7> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 1 μm) 10.6 parts by weight (17.7 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0142] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0143] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0144] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 7.
[0145] [Example 8] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 8 was laminated on the picture layer in a manner to be in sync with the previously formed picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 6 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0146] <Release layer forming ink 8> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45.4 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 10.6 parts by weight (17.7 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0147] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0148] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0149] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 8.
[0150] [Comparative Example 1] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 9 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous base material, a design layer, and a release layer were laminated in this order.
[0151] <Release layer forming ink 9> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 53.4 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 2.6 parts by weight (4.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0152] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0153] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0154] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 1.
[0155] [Comparative Example 2] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone pattern design. Furthermore, the following release layer forming ink 10 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which the paper base material, the design layer, and the release layer were laminated in this order.
[0156] <Release layer forming ink 10> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 51.4 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 0.6 parts by mass (1.0 part by mass per 100 parts by mass of total solids) Silane coupling treated silica (particle size 2 μm) 8.0 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0157] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0158] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0159] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain a melamine decorative board of Comparative Example 2.
[0160] [Comparative Example 3] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 11 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which the paper base material, the design layer, and the release layer were laminated in this order.
[0161] <Release layer forming ink 11> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 5 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0162] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2The composition was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet.
[0163] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0164] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 3.
[0165] [Comparative Example 4] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern. Furthermore, the following release layer forming ink 12 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0166] <Release layer forming ink 12> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 48 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 1 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Methyl ethyl ketone 40 parts by weight
[0167] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The composition was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet.
[0168] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0169] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 4.
[0170] [Comparative Example 5] (Making decorative sheets) A paper base material (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous base material. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper base material by a gravure printing method using the above printing ink so as to form a stone grain pattern design. In addition, the ink 1 for forming a release layer was laminated on the picture layer in a manner to be in sync with the previously formed picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 6 μm. This produced a decorative sheet in which the paper base material, the design layer, and the release layer were laminated in this order.
[0171] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The composition was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet.
[0172] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0173] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 5.
[0174] [Pure water contact angle of release layer of decorative sheet] The pure water contact angle of the release layer in the decorative sheets obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The decorative sheet was placed on a horizontal surface with the release layer facing up. Next, a water droplet (pure water, 2.0 μL) was dropped on the release layer from a direction perpendicular to the horizontal surface. At this time, the water droplet was not dropped on the boundary between the design layer and the release layer, but was dropped so that the entire water droplet was in contact with the release layer. After dropping the water droplet, a wait of 1 second was held, and the contact angle between the release layer and pure water was measured using a contact angle meter (fully automatic contact angle meter DMo-702, manufactured by Kyowa Interface Science Co., Ltd.). The above measurement was performed at any 10 points, and the average value was taken as the pure water contact angle. The results are shown in Tables 1 and 2. The pure water contact angle of the release layer of the resin-impregnated decorative board can basically be measured by the same method as described above, except that when water droplets are dropped onto the release layer, the water droplets are not dropped at the boundary between the cured resin layer and the release layer, but are dropped so that the entire water droplet comes into contact with the release layer.
[0175] [60° gloss value of release layer of decorative sheet] The 60° gloss value of the release layer in the decorative sheets obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The decorative sheet was placed with the release layer side facing up, and the 60° specular gloss was measured from the release layer side using a gloss meter ("Micro Trigloss (Cat. No. 4563)", manufactured by BYK Gardner) in accordance with Method 3 of JIS Z 8741:1997 by the following method. 1) Paper (Oji F-Tex Tencolor) <400> A sheet of paper (A4 black) was prepared and cut into a size of 180 mm x 60 mm as shown in Figure 6(a). 2) The gloss meter was placed on the cut-out paper and an impression of the gloss meter was made with a pencil (dotted frame in Figure 6(b)). 3) As shown in FIG. 6(c), a hole C of 15 mm×9 mm was cut in the center to prepare a backing plate 61. 4) The prepared backing plate was placed on the measurement sample, and the cut-out part (hole C) was visually inspected to confirm that the release layer was in the center and that the ratio of the area of the release layer to the area of the cut-out part (hole C) was 50% or more. 5) Taking care not to move the position of the backing plate set in 4), the gloss meter was placed in line with the molded part and the 60° gloss was measured. 6) The operations 4) and 5) were repeated to increase the number of points, and the average value of the measurements at 10 points was taken as the 60° gloss value of the release layer. The results are shown in Tables 1 and 2.
[0176] [Spc of release layer for decorative sheet and melamine laminate] The Spc (arithmetic mean curvature of peaks) of the release layer in the decorative sheets and melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was measured by the following method. The value was measured on the surface of the release layer of the decorative sheet using a laser microscope (VK-X3000, manufactured by Keyence Corporation) under the following conditions. Note that Spc is the average value of measurements taken at 10 arbitrary points, with the measurement points selected so that all of the measurement points are within the release layer. The results are shown in Tables 1 and 2. (Measurement conditions) Objective lens: 5x Laser wavelength: 661nm Measurement area for each point: 500μm×500μm
[0177] [Melamine peelability evaluation] Using the melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5, a cellophane tape resistance test was performed in the area including the release layer, and the melamine peelability was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2. (Scotch tape resistance test method) 1) Pull out 15 to 30 cm of Nichiban Cellotape (registered trademark) (No. 405 (industrial use) width 24 mm), and except for the last 5 cm at the end, stick the sticky surfaces of the remaining parts together (this part will be the grip for when peeling it off). 2) Attach the sticky side of the edge to the test area and rub it from above with a cloth or similar to ensure a strong adhesion. 3) Grab the part where the adhesive cotton is stuck together in 1) and pull it forcefully in a 45-degree direction. 4) Visually inspect the melamine layer on the adhesive surface and the surface of the test area and rate it using the A, B, or C criteria. 5) 1) to 4) are carried out at any 10 points on the release layer, and the most common evaluation is judged as the melamine release property (in the case of the same number of evaluations, the worse result is used).
[0178] (Evaluation Criteria) A: Almost no peeling of the melamine was observed, and no melamine remained on the release layer. B: Significant peeling of melamine is observed, but peeling is possible through testing. C: No peeling of the melamine was observed, and most of the melamine remained on the release layer after the test. (Tests have shown that most of the melamine on the release layer (more than 90% of the area of the release layer) cannot be peeled off.)
[0179] [Gloss Matte Design Evaluation] The gloss matte design of the melamine decorative boards obtained in Examples 1 to 8 and Comparative Examples 1 to 5 was visually evaluated. Specifically, under a light source of a natural color fluorescent lamp with color rendering AA (manufactured by Panasonic Corporation, model number: FLR40S·D-SDL / M), the obtained decorative boards were visually observed from a position 50 cm away, and the gloss matte design and the state of the matte part (release layer) were confirmed.
[0180] The observers scored the gloss matte design on a 5-point scale from 1 to 5 (1 being the worst and 5 being the best). The scale was based on a score of 1 when most of the melamine remained peeled off or significant whitening was observed in the matte area or nearby areas, and sufficient gloss matte design could not be confirmed, and a score of 5 when no peeled off melamine was found in the matte area and sufficient gloss matte design could be confirmed. Ten observers each conducted the test, and the average score of all observers was calculated to evaluate the gloss matte design according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation Criteria) A: The average score for the evaluation of gloss matte design is 3 points or more. B: The average score for the evaluation of gloss matte design is 2 points or more but less than 3 points. C: The average score for the evaluation of gloss matte design is less than 2 points.
[0181] [Table 1]
[0182] [Table 2]
[0183] As shown in Table 1, when the decorative sheets obtained in Examples 1 to 8 were used, the results showed that both melamine releasability and gloss matte design were excellent. On the other hand, as shown in Table 2, the decorative sheet obtained in Comparative Example 1 had a high 60° gloss value and a low Spc value, and was therefore confirmed to have poor gloss matte design. In addition, the decorative sheets obtained in Comparative Examples 2 and 3 had low pure water contact angles and were confirmed to have poor melamine releasability. The decorative sheets obtained in Comparative Examples 4 and 5 had low Spc, and were therefore confirmed to have poor gloss matte design.
[0184] [Example 9] (Making decorative sheets) As a porous substrate, a paper substrate (basis weight 80 g / m 2 Titanium base paper for building materials (PM-83P manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured in accordance with JIS-P8252 and found to be 18%. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain pattern design by a gravure printing method using the above printing ink. Furthermore, the ink 1 for forming a release layer was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0185] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0186] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0187] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 9.
[0188] [Example 10] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-83P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. In addition, the ink 3 for forming a release layer was laminated on the picture layer in synchronization with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0189] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0190] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0191] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 10.
[0192] [Example 11] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 13 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0193] <Release layer forming ink 13> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 46.8 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Hindered amine light stabilizer (BASF Ltd., Tinuvin 123) 1.2 parts by mass (2.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by weight
[0194] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0195] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0196] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Example 11.
[0197] [Example 12] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 14 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0198] <Release layer forming ink 14> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 45 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Hindered amine light stabilizer (BASF Ltd., Tinuvin 123) 3 parts by mass (5.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by weight
[0199] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0200] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0201] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 12.
[0202] [Example 13] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone pattern design. Furthermore, the following release layer forming ink 15 was laminated on the picture layer in synchronization with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0203] <Release layer forming ink 15> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 44 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 9 parts by weight (15.0 parts by weight per 100 parts by weight of total solids) Hindered amine light stabilizer (BASF Ltd., Tinuvin 123) 3 parts by mass (5.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by weight
[0204] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0205] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0206] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, thereby obtaining the melamine decorative board of Example 13.
[0207] [Comparative Example 6] (Making decorative sheets) As a porous substrate, a paper substrate (basis weight 100 g / m 2Titanium paper (KW-1002P, manufactured by KJ Specialty Paper Co., Ltd.) was prepared. The ash content of the paper substrate was measured according to JIS-P8252 and was found to be 36%. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate so as to form a stone grain design by a gravure printing method using the above printing ink. In addition, release layer forming ink 1 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0208] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0209] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0210] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 6.
[0211] [Comparative Example 7] (Making decorative sheets) A paper substrate (titanium base paper for building materials, PM-77P manufactured by KJ Specialty Paper Co., Ltd.) was prepared as a porous substrate. A design layer (picture layer) having a thickness of 2 μm was partially laminated on the paper substrate by a gravure printing method using the above printing ink so as to form a stone grain pattern design. Furthermore, the following release layer forming ink 16 was laminated on the picture layer in sync with the picture layer, and then an electron beam of 3 Mrad was irradiated at an acceleration voltage of 165 kV to form a release layer having a thickness of 2 μm. This produced a decorative sheet in which a porous substrate, a design layer, and a release layer were laminated in this order.
[0212] <Release layer forming ink 16> Ionizing radiation curable monomer (Aronix M-400, manufactured by Toagosei Co., Ltd.) 42 parts by weight Reactive silicone (X-22-164B, manufactured by Shin-Etsu Chemical Co., Ltd.) 4 parts by weight (6.7 parts by weight per 100 parts by weight of total solids) Silane coupling treated silica (particle size 2 μm) 8 parts by weight (13.3 parts by weight per 100 parts by weight of total solids) Hindered amine light stabilizer (BASF Ltd., Tinuvin 123) 6 parts by mass (10.0 parts by mass per 100 parts by mass of total solids) Methyl ethyl ketone 40 parts by weight
[0213] (Manufacture of melamine laminates) A liquid uncured melamine resin composition containing 60 parts by mass of uncured melamine resin (water-soluble methylol melamine resin, NikaResin S-260 manufactured by Nippon Carbide Industries Co., Ltd.), 35 parts by mass of water, and 5 parts by mass of isopropyl alcohol was applied to the prepared decorative sheet using an impregnation device so that the uncured melamine resin composition was 80 g / m 2 The mixture was impregnated so as to obtain the ratio (when dry) and then dried to produce an impregnated decorative sheet (precursor laminate).
[0214] The impregnated decorative sheet was laminated on the above-mentioned core substrate, and the above-mentioned release film was further laminated on the impregnated decorative sheet so that the peeling layer of the release film was in contact with the printed surface of the impregnated decorative sheet, to obtain a laminate.
[0215] The laminate was sandwiched between two mirror-finished plates and heated at a pressure of 100 kg / cm using a heat press. 2 The uncured melamine resin composition was heat-molded at a molding temperature of 150°C for 10 minutes to heat-cure the uncured melamine resin composition, thereby forming a cured resin layer containing a cured product of the melamine resin. This resulted in a cured laminate. The cured laminate was then removed from between the two mirror-finished plates, and the release film was peeled off from the cured resin layer containing the cured product of the melamine resin, to obtain the melamine decorative board of Comparative Example 7.
[0216] [Pure water contact angle of release layer of decorative sheet] The pure water contact angles of the release layers of the decorative sheets obtained in Examples 9 to 12 and Comparative Examples 6 and 7 were measured. The measurement method was the same as above. The results are shown in Table 3.
[0217] [60° gloss value of release layer of decorative sheet] The 60° gloss value of the release layer was measured in the decorative sheets obtained in Examples 9 to 12 and Comparative Examples 6 and 7. The measurement method was the same as above. The results are shown in Table 3.
[0218] [Spc of release layer for decorative sheet and melamine laminate] The release layers of the decorative sheets and melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7 were measured for Spc (arithmetic mean curvature of peaks). The measurement method was the same as above. The results are shown in Table 3.
[0219] [Melamine peelability evaluation] The melamine peelability was evaluated using the melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7. The evaluation criteria were the same as above. The results are shown in Table 3.
[0220] [Gloss Matte Design Evaluation] The gloss and matt design properties of the melamine decorative boards obtained in Examples 9 to 12 and Comparative Examples 6 and 7 were evaluated. The evaluation criteria were the same as above. The results are shown in Table 3.
[0221] [Table 3]
[0222] As shown in Table 3, for example, in both Example 9 and Example 1 described above, the ink 1 for forming a release layer is used, but the type of the porous substrate is different. Specifically, the porous substrate (PM-83P) used in Example 9 has a lower ash content than the porous substrate (PM-77P) used in Example 1, and the ink 1 for forming a release layer is less likely to penetrate. As a result, the pure water contact angle and 60° gloss value of Example 9 are increased and the Spc is slightly decreased compared to Example 1. Thus, the type of porous substrate affects the pure water contact angle, 60° gloss value, and Spc. Therefore, it is necessary to adjust the pure water contact angle, 60° gloss value, and Spc to a predetermined range while taking into consideration the type of porous substrate. In the present disclosure, good releasability and good gloss matte design can be obtained by adjusting the pure water contact angle, 60° gloss value, and Spc to a predetermined range while taking into consideration the type of porous substrate. A similar relationship was also confirmed between Example 10 and Example 3.
[0223] On the other hand, in both Comparative Example 6 and the above-mentioned Example 1, the ink 1 for forming a release layer is used, but the type of the porous substrate is different. Specifically, the porous substrate (KW-1002P) used in Comparative Example 6 has a higher ash content than the porous substrate (PM-77P) used in Example 1, and the ink 1 for forming a release layer is more likely to penetrate. As a result, the pure water contact angle and 60° gloss value of Comparative Example 6 are lower than those of Example 1, and the Spc is increased. Thus, the type of porous substrate affects the pure water contact angle, 60° gloss value, and Spc. In Comparative Example 6, the pure water contact angle is low, and therefore the releasability is poor.
[0224] In addition, in Example 11 and Example 12, the same porous substrate is used in both, but the amount of light stabilizer added in the ink for forming the release layer is different. The amount of light stabilizer added does not have a significant effect on the pure water contact angle, but when the amount of light stabilizer added is increased, the 60° gloss value tends to increase and the Spc tends to decrease. In this way, the presence or absence of light stabilizer addition and the amount of light stabilizer added affect the 60° gloss value and Spc. Therefore, it is necessary to adjust the pure water contact angle, 60° gloss value and Spc to a predetermined range while considering the presence or absence of light stabilizer addition and the amount of light stabilizer added. In the present disclosure, good releasability and good gloss matte design can be obtained by adjusting the pure water contact angle, 60° gloss value and Spc to a predetermined range while considering the presence or absence of light stabilizer addition and the amount of light stabilizer added.
[0225] On the other hand, in Comparative Example 7, Examples 11 and 12, the same porous substrate is used, but the amount of light stabilizer added to the ink for forming the release layer is different. When the amount of light stabilizer added is increased, the 60° gloss value tends to increase and the Spc tends to decrease. In Comparative Example 7, the 60° gloss value was high, so the gloss matte design was poor. In addition, when comparing Examples 12 and 13, in Example 13, the proportion of the matting agent was increased compared to Example 12, so the 60° gloss value decreased and the Spc increased, resulting in better gloss matte design.
[0226] Thus, in the present disclosure, for example, the following inventions are provided:
[0227] [1] A decorative sheet used in the manufacture of a resin-impregnated decorative board, The decorative sheet has a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction, The release layer has a 60° gloss value of 10 or less; The release layer has a pure water contact angle of 85° or more; The release layer has an Spc (arithmetic mean curvature of the peaks) of 80 mm-1 That's it, the decorative sheet.
[0228] [2] The decorative sheet according to [1], wherein the release layer has a contact angle with pure water of 100° or more.
[0229] [3] The decorative sheet according to [1] or [2], wherein the release layer has a 60° gloss value of 6.5 or less.
[0230] [4] The release layer has an Spc (arithmetic mean curvature of the peaks) of 120 mm -1 The decorative sheet according to any one of [1] to [3] above.
[0231] [5] The decorative sheet according to any one of [1] to [4], wherein the release layer contains a release agent.
[0232] [6] The decorative sheet according to [5], wherein the release agent contains a reactive silicone oil.
[0233] [7] The decorative sheet according to [5] or [6], wherein the content of the release agent is 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the release layer.
[0234] [8] The decorative sheet according to any one of [1] to [7], wherein the release layer contains a mattifying agent.
[0235] [9] The decorative sheet according to [8], wherein the mattifying agent contains inorganic particles.
[0236]
[10] The decorative sheet according to [8] or [9], wherein the content of the matting agent is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the release layer.
[0237]
[11] The decorative sheet according to any one of [8] to
[10] , wherein the average particle size of the matting agent is 1 μm or more and 5 μm or less.
[0238]
[12] The decorative sheet according to any one of [1] to
[11] , wherein the thickness of the release layer is 0.5 μm or more and 8 μm or less.
[0239]
[13] The decorative sheet according to any one of [1] to
[12] , wherein the release layer contains a cured product of a curable resin X.
[0240]
[14] The decorative sheet according to
[13] , wherein the curable resin X in the release layer is an ionizing radiation curable resin.
[0241]
[15] The decorative sheet according to any one of [1] to
[14] , wherein the resin-impregnated decorative board is a melamine decorative board.
[0242]
[16] A resin-impregnated decorative board, A decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction; A core substrate arranged to face the porous substrate in the decorative sheet; a cured resin layer disposed between the patterns of the release layer, the cured resin layer being thicker than the release layer and containing a cured product of the curable resin Y; The porous substrate contains a cured product of the curable resin Y, The release layer has a pure water contact angle of 85° or more; The release layer has an Spc (arithmetic mean curvature of the peaks) of 10 mm -1 That is all about the resin-impregnated decorative panel.
[0243]
[17] The resin-impregnated decorative board according to
[16] , wherein the release layer has a 60° gloss value of 10 or less.
[0244]
[18] The resin-impregnated decorative board according to
[16] or
[17] , wherein the ratio of the 60° gloss value of the cured resin layer to the 60° gloss value of the release layer is 1.2 or more.
[0245]
[19] A method for producing a resin-impregnated decorative board, comprising: A preparation step of preparing a decorative sheet according to any one of [1] to
[15] ; (i) a laminate formation step of forming a laminate having a core substrate, the decorative sheet, a curable resin layer containing a curable resin Y, and a release film in this order in the thickness direction, (ii) a surface of the decorative sheet facing the porous substrate is arranged to face the core substrate, and (iii) the decorative sheet is impregnated with the curable resin Y; a heating and pressurizing step of heating and pressurizing the laminate to cure the curable resin Y and form a cured resin layer from the curable resin layer to obtain a cured laminate; a peeling step of peeling the release film from the cured laminate to remove the cured resin layer arranged at a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between patterns of the release layer; A method for producing a resin-impregnated decorative board comprising the steps of: [Explanation of symbols]
[0246] 1...Porous base material 2…Design layer 3…Matte layer 10...Decorative sheet 20…Core substrate 30…Curable resin layer 40...Release film 100...Resin-impregnated decorative board
Claims
1. A decorative sheet used in the manufacture of a resin-impregnated decorative board, The decorative sheet has a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction, The release layer has a 60° gloss value of 10 or less, The release layer has a pure water contact angle of 85° or more; The Spc (arithmetic mean curvature of the peaks) of the release layer is 80 mm -1 That's it, the decorative sheet.
2. 2. The decorative sheet according to claim 1, wherein the release layer has a contact angle with pure water of 100° or more.
3. 2. The decorative sheet according to claim 1, wherein the release layer has a 60° gloss value of 6.5 or less.
4. The Spc (arithmetic mean curvature of the peaks) of the release layer is 120 mm -1 The decorative sheet according to claim 1 .
5. The decorative sheet according to claim 1 , wherein the release layer contains a release agent.
6. The decorative sheet according to claim 5 , wherein the release agent comprises a reactive silicone oil.
7. 6. The decorative sheet according to claim 5, wherein the content of the release agent is 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the release layer.
8. The decorative sheet according to claim 1 , wherein the release layer contains a matting agent.
9. The decorative sheet according to claim 8 , wherein the mattifying agent comprises inorganic particles.
10. 9. The decorative sheet according to claim 8, wherein the content of the matting agent is 5 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the release layer.
11. 9. The decorative sheet according to claim 8, wherein the average particle size of said matting agent is 1 μm or more and 5 μm or less.
12. 2. The decorative sheet according to claim 1, wherein the release layer has a thickness of 0.5 μm or more and 8 μm or less.
13. The decorative sheet according to claim 1 , wherein the release layer contains a cured product of a curable resin X.
14. 14. The decorative sheet according to claim 13, wherein the curable resin X in the release layer is an ionizing radiation curable resin.
15. The decorative sheet according to claim 1 , wherein the resin-impregnated decorative board is a melamine decorative board.
16. A resin-impregnated decorative board, A decorative sheet having a porous substrate, a design layer, and a release layer having a pattern shape, in this order in the thickness direction; A core substrate arranged to face the porous substrate in the decorative sheet; a cured resin layer disposed between the patterns of the release layer, the cured resin layer being thicker than the release layer and containing a cured product of the curable resin Y; The porous substrate contains a cured product of the curable resin Y, The release layer has a pure water contact angle of 85° or more; The Spc (arithmetic mean curvature of the peaks) of the release layer is 10 mm -1 That is all about the resin-impregnated decorative panel.
17. 17. The resin-impregnated decorative board according to claim 16, wherein the release layer has a 60[deg.] gloss value of 10 or less.
18. 17. The resin-impregnated decorative board according to claim 16, wherein a ratio of a 60° gloss value of the cured resin layer to a 60° gloss value of the release layer is 1.2 or greater.
19. A method for producing a resin-impregnated decorative board, comprising: A preparation step of preparing a decorative sheet according to any one of claims 1 to 15; (i) a laminate formation step of forming a laminate having a core substrate, the decorative sheet, a curable resin layer containing a curable resin Y, and a release film in this order in the thickness direction, (ii) a surface of the decorative sheet facing the porous substrate is arranged to face the core substrate, and (iii) the decorative sheet is impregnated with the curable resin Y; a heating and pressurizing step of heating and pressurizing the laminate to cure the curable resin Y while forming a cured resin layer from the curable resin layer, thereby obtaining a cured laminate; a peeling step of peeling the release film from the cured laminate to remove the cured resin layer arranged at a position overlapping with the release layer in the thickness direction, while leaving the cured resin layer arranged between patterns of the release layer; A method for producing a resin-impregnated decorative board comprising the steps of:
Citation Information
Patent Citations
decorative panels
JP6716877B2
Cited By
Resin-impregnated decorative plate including release film, release film, and method for producing resin-impregnated decorative plate
WO2026074835A1
Decorative paper and decorative plate
WO2026163707A1