Heat conductive sheet

A thermally conductive sheet with a thermally conductive layer and adhesive layer, optimized for improved adhesion and reworkability, addresses the challenges of peeling and assembly difficulties in semiconductor devices by enhancing adhesive strength at elevated temperatures.

JP2024146928APending Publication Date: 2024-10-15SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024057857
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Thermally conductive sheets used in semiconductor devices face challenges with reworkability and adhesion due to conflicting requirements for heat dissipation, flexibility, and adhesion strength, leading to issues like peeling and difficulty in reattachment during assembly and use.

Method used

A thermally conductive sheet with a specific configuration of a thermally conductive layer and an adhesive layer, where the adhesive strength improves at elevated temperatures, ensuring a predetermined relationship between tensile strength and adhesive forces, allowing for reworkability and strong adhesion during use.

Benefits of technology

The sheet achieves both reworkability during assembly and excellent adhesion during actual use, preventing peeling and ensuring effective heat transfer in semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146928000007
    Figure 2024146928000007
  • Figure 2024146928000008
    Figure 2024146928000008
  • Figure 2024146928000001
    Figure 2024146928000001
Patent Text Reader

Abstract

To provide a heat conductive sheet which has reworkability during assembly operations and is improved in adhesive force during actual use.SOLUTION: There is provided a heat conductive sheet comprising a heat conductive layer containing a polymer matrix and a heat conductive filler and an adhesive layer provided on at least one surface of the heat conductive layer. The tensile strength at break A [mN / mm] of the heat conductive sheet, the initial adhesive strength B1 [MPa] of the adhesive layer measured after pressurizing the heat conductive sheet at a load of 20 psi under the environment at 25°C for 12 minutes and the adhesive strength B2 [MPa] of the adhesive layer measured after pressurizing the heat conductive sheet at a load of 20 psi under the environment at 80°C for 60 minutes satisfy the relationship in the following formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive sheet. [Background technology]

[0002] It is known that thermally conductive sheets are used in semiconductor elements and various electronic devices to effectively dissipate heat from heat generating bodies. For example, it is known that semiconductor packages dissipate heat by sandwiching a heat dissipation material between a heat generating body such as a semiconductor chip and a heat dissipating body called a heat spreader, or between the heat spreader and a cooling unit such as a heat sink.

[0003] Semiconductor packages are generally heated above a certain temperature during use. Each component, such as the substrate, semiconductor chip, and heat spreader, has a different thermal expansion coefficient, so warping can occur when heated. As chips have become larger in recent years, the gaps caused by warping have also become larger.

[0004] Therefore, it is required that thermally conductive sheets used in semiconductor applications and the like have high heat dissipation properties while also having high flexibility in order to improve the ability to follow warping. However, when an attempt is made to improve both the heat dissipation properties and flexibility of a thermally conductive sheet, the adhesion to surrounding components decreases, and there is a concern that the sheet will not be able to follow warping and will peel off from each component, such as a semiconductor chip, a heat sink, or a heat spreader. For this reason, for example, Patent Document 1 attempts to suppress peeling from each component, such as a semiconductor chip, a heat sink, or a heat spreader, by blending liquid polybutene, acrylic acid ester polymer, ethylene-α-olefin copolymer, hot melt agent, etc., into the thermally conductive sheet to increase the tackiness. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 7067571 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the semiconductor element has a large surface area, the thermally conductive sheet is easily misaligned when it is placed, making the placement process more difficult and requiring ease of re-application (reworkability).However, as described in Patent Document 1, increasing the tack strength makes it difficult to re-apply the thermally conductive sheet, and increasing the flexibility reduces the strength of the thermally conductive sheet, resulting in problems such as the thermally conductive sheet being damaged when re-applied even with weak adhesive strength.

[0007] Therefore, an object of the present invention is to provide a thermally conductive sheet that has reworkability during assembly work and exhibits excellent adhesion in actual use. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above problem can be solved by using an adhesive whose adhesive strength improves at 80° C. in a configuration in which an adhesive is spray-coated onto a thermally conductive sheet, and by setting the relationship between the tensile breaking strength and adhesive strength of the thermally conductive sheet within a predetermined range. They also found that solving the above problem makes it possible to suppress peeling caused by warping, etc. That is, the present invention provides the following [1] to [7].

[0009] [1] A thermally conductive sheet comprising a thermally conductive layer containing a polymer matrix and a thermally conductive filler, and an adhesive layer provided on at least one surface of the thermally conductive layer, wherein the tensile breaking strength A [mN / mm] of the thermally conductive sheet, the initial adhesive strength B1 [MPa] of the adhesive layer measured after the thermally conductive sheet is pressurized at a load of 20 psi for 12 minutes in an environment of 25°C, and the adhesive strength B2 [MPa] of the adhesive layer measured after the thermally conductive sheet is pressurized at a load of 20 psi for 60 minutes in an environment of 80°C satisfy the relationship of the following formula (1).

number

[0010] According to the present invention, it is possible to provide a thermally conductive sheet which has reworkability during assembly work and exhibits excellent adhesion in practical use. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram of a thermal resistance measuring device. [Diagram 2] FIG. 2 is a schematic diagram showing a method for measuring die shear strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Thermal conductive sheet] The thermally conductive sheet of the present invention is a thermally conductive sheet comprising a thermally conductive layer and an adhesive layer provided on at least one surface of the thermally conductive layer, in which the tensile breaking strength A of the thermally conductive sheet, the initial adhesive strength B1 of the adhesive layer, and the adhesive strength B2 after heat treatment satisfy the relationship of the following formula (1). Here, the initial adhesive strength B1 is the adhesive strength measured after applying a pressure of 20 psi (0.138 MPa) for 12 minutes in an environment at 25° C. The adhesive strength B2 after heat treatment is the adhesive strength measured after applying a pressure of 20 psi for 60 minutes in an environment at 80° C. In addition, the adhesive strengths B1 and B2 are the adhesive strengths to a nickel-plated copper plate and a silicon die measured in a die shear strength measurement as described in the examples. In the following formula (1), the unit of the tensile breaking strength A is mN / mm, and the unit of the adhesive strengths B1 and B2 is MPa.

number

[0013] If the adhesive strength B1 is 0.00385 times or more the tensile breaking strength A, it becomes difficult to realize reworkability during assembly, particularly during the process of attaching the thermally conductive sheet. If the adhesive strength B2 is 0.00385 times or less the tensile breaking strength A, the thermally conductive sheet cannot exhibit sufficient adhesion during actual use, and there is a risk that the thermally conductive sheet will peel off from the adherend. The thermally conductive sheet of the present invention can satisfy the requirement of the above formula (1) by appropriately adjusting the tensile breaking strength of the thermally conductive layer and the adhesive strength of the adhesive layer. In addition, the adhesive layer may use an adhesive whose adhesive strength improves when heated. For example, in the case of an acrylic adhesive, as described later, it is preferable to incorporate a functional group or a reactive double bond in the side chain and appropriately adjust the content of these to satisfy the requirement of the above formula (1).

[0014] In the present invention, the ratio (B1 / A) of adhesive strength B1 to tensile breaking strength A is preferably 0.00382 or less, more preferably 0.00350 or less. By making B1 / A equal to or less than the above upper limit, it becomes easier to impart excellent reworkability to the thermal conductive sheet. From the viewpoint of reworkability, the lower the B1 / A, the better, and it is sufficient if it is 0 or more, but from the viewpoint of practicality, it is sufficient to make it about 0.0002 or more, and preferably 0.0005 or more.

[0015] In the present invention, the ratio (B2 / A) of adhesive strength B2 to tensile breaking strength A is preferably 0.00385 or more, more preferably 0.0039 or more. When B2 / A is equal to or more than the above lower limit, the adhesive strength is sufficiently exhibited during actual use of the thermal conductive sheet, and the thermal conductive sheet is less likely to peel off from the adherend. From the viewpoint of adhesive strength, the higher B2 / A is the better, but from the viewpoint of practicality, it is good to have a ratio of, for example, about 0.01 or less, preferably 0.008 or less.

[0016] <Adhesive layer> The adhesive layer of the present invention can be an acrylic adhesive layer, a rubber adhesive layer, a urethane adhesive layer, a silicone adhesive layer, or the like. Among these, an acrylic adhesive layer is preferred. By using the acrylic adhesive layer, when the adhesive layer is adhered to an adherend such as a heat spreader, a heat sink, or a semiconductor chip, and then used in a relatively high temperature environment of, for example, about 60 to 150°C in practical use, the adhesive strength is likely to improve during practical use. By improving the adhesive strength during practical use, excellent reworkability is exhibited during assembly work, and excellent adhesive strength is exhibited during practical use, preventing peeling from the adherend.

[0017] The acrylic adhesive layer is formed from an acrylic adhesive. The acrylic adhesive may contain an acrylic polymer as a main component of the adhesive. The acrylic adhesive layer can exhibit adhesiveness by containing the acrylic polymer.

[0018] The acrylic adhesive layer may or may not have a reactive double bond. When the acrylic adhesive layer has a reactive double bond, the reactive double bond reacts when heated at high temperatures during use, and the adhesive strength to the adherend may be improved, which makes it easier to improve the adhesive strength in practical use. Therefore, even if the initial adhesive strength (B1) is reduced, no problems will arise in practical use, and reworkability will also be improved. The reactive double bond is an unsaturated carbon-carbon double bond that does not constitute an aromatic ring, and is typically composed of a group having a structure represented by H2C=CH-* or H2C=CCH3-* (* indicates a bond), and specific examples thereof include a vinyl group, an acryloyl group, and a methacryloyl group. The acrylic polymer having a reactive double bond (reactive double bond-containing acrylic polymer) may have a functional group such as a hydroxyl group, a carboxyl group, an epoxy group, or an amino group in a side chain in addition to the reactive double bond. However, it preferably has at least one of a hydroxyl group and a carboxyl group in the side chain, and more preferably has both a hydroxyl group and a carboxyl group. The reactive double bond-containing acrylic polymer can be obtained, for example, by reacting an acrylic polymer having a functional group such as a hydroxyl group, a carboxyl group, an epoxy group, or an amino group in a side chain (hereinafter also referred to as an acrylic polymer (X)) with a reactive double bond-containing compound having a reactive group that reacts with the functional group and a reactive double bond (hereinafter also referred to as a reactive double bond-containing compound (Y)).

[0019] The acrylic polymer (X) may be any polymer containing a structural unit derived from (meth)acrylate, but typically contains a structural unit derived from alkyl(meth)acrylate as a main component. More specifically, the acrylic polymer (X) may be a copolymer of an alkyl(meth)acrylate and a functional group-containing monomer, or a copolymer of an alkyl(meth)acrylate, a functional group-containing monomer, and a monomer other than these. Incidentally, (meth)acrylate is used as a term meaning either or both of acrylate and methacrylate, and the same applies to other similar terms.

[0020] Alkyl (meth)acrylate is an ester of (meth)acrylic acid and an alkyl alcohol. The alkyl group in the alkyl (meth)acrylate may be linear, may have a branched structure, or may have a cyclic structure. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. The alkyl (meth)acrylate may be used alone or in combination of two or more kinds. The alkyl (meth)acrylate is preferably an alkyl (meth)acrylate having an alkyl group with a carbon number of 1 to 12, more preferably an alkyl acrylate having an alkyl group with a carbon number of 2 to 8, and even more preferably an alkyl acrylate having an alkyl group with a carbon number of 2 to 4. When the number of carbon atoms in the alkyl group is within the above range, in particular not more than the above upper limit, the adhesion of the thermal conductive sheet during actual use is improved, and while improving the adhesion, reworkability is also easily improved. The structural unit derived from an alkyl acrylate having an alkyl group with 2 to 8 carbon atoms may be the main component in the acrylic polymer, and may account for, for example, 50% by mass or more in the acrylic polymer, preferably 60% by mass or more and 95% by mass or less, and more preferably 70% by mass or more and 90% by mass or less.

[0021] As described above, the functional group in the functional group-containing monomer includes a carboxyl group, a hydroxyl group, an amino group, and an epoxy group, among which a carboxyl group and a hydroxyl group are preferred. The monomer containing a carboxyl group includes (meth)acrylic acid, crotonic acid, and the like, among which a (meth)acrylic acid is more preferred. Examples of monomers containing a hydroxyl group include (meth)acrylates having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, and allyl alcohol. Among these, (meth)acrylates having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate are preferred. The content of the constituent units derived from functional group-containing monomers in the acrylic polymer is, for example, about 1% by mass or more and 35% by mass or less, preferably 5% by mass or more and 30% by mass or less, and more preferably 10% by mass or more and 25% by mass or less. The functional group-containing monomer may be used alone or in combination of two or more kinds.

[0022] Examples of other monomers include alkyl (meth)acrylates and monomers other than the functional group-containing monomers described above, and are not particularly limited as long as they are copolymerizable with alkyl (meth)acrylates and functional group-containing monomers.Specific examples include styrene derivatives such as styrene, α-methylstyrene, p-methylstyrene, p-chlorostyrene, and divinylbenzene, compounds having vinyl ester groups such as vinyl acetate and vinyl propionate, N-vinylpyrrolidone, N-vinylmorpholine, (meth)acrylonitrile, N-cyclohexylmaleimide, N-phenylmaleimide, N-laurylmaleimide, N-benzylmaleimide, n-propyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, and tert-butyl vinyl ether.One type of other monomer may be used alone, or two or more types may be used in combination.

[0023] The reactive double bond-containing compound (Y) is a compound having a reactive group that reacts with the functional group described above and a reactive double bond. Examples of the reactive group include an isocyanate group, an epoxy group, a carboxyl group, and a hydroxyl group. Among these, the isocyanate group and the epoxy group are preferred, and the isocyanate group is more preferred. The content of the reactive double bond in the acrylic adhesive layer can be adjusted by the amount of functional groups in the acrylic polymer (X) and the ratio of the functional groups that react with the reactive double bond-containing compound (Y). The amount of functional groups in the acrylic polymer (X) can be adjusted by the ratio of functional group-containing monomers used in synthesizing the acrylic polymer (X).

[0024] The acrylic polymer contained in the acrylic adhesive layer may be an acrylic polymer containing a reactive double bond, an acrylic polymer having no reactive double bond, or a combination of an acrylic polymer containing a reactive double bond and an acrylic polymer having no reactive double bond. The acrylic polymer having no reactive double bond may have a functional group such as a hydroxyl group, a carboxyl group, an epoxy group, or an amino group in the side chain, and in this case, it is preferable that at least one of a hydroxyl group and a carboxyl group is in the side chain. In addition, it may not have a functional group in the side chain. As an example of the acrylic polymer having no reactive double bond, the above-mentioned acrylic polymer (X) is exemplified. In addition, it may be a polymer of alkyl (meth)acrylate. The acrylic pressure-sensitive adhesive may contain, in addition to the above-mentioned acrylic polymer, components that are generally blended into pressure-sensitive adhesives, and may also contain additives such as a crosslinking agent, a tackifier, a filler, an antioxidant, an ultraviolet protection agent, a plasticizer, and a viscosity adjuster, as appropriate.

[0025] The weight-average molecular weight of the acrylic polymer is not particularly limited, but is, for example, about 100,000 to 1,200,000, and preferably about 200,000 to 1,000,000. The weight-average molecular weight is measured by gel permeation chromatography (GPC) and calculated as a polystyrene equivalent value.

[0026] When the acrylic adhesive layer has a reactive double bond, the intensity ratio A / B of the peak intensity A of the C=C stretching vibration to the peak intensity B of the C=O stretching vibration in the Raman spectrum is preferably 0.2 or more. Here, the peak intensity A is a peak caused by a reactive double bond (C=C double bond). Moreover, the peak intensity B is a peak caused by a C=O bond contained in the acrylic polymer. Therefore, the intensity ratio A / B of the peak intensity A to the peak intensity B can be said to be an index showing the proportion of reactive double bonds in the acrylic polymer.

[0027] When the acrylic adhesive layer has an intensity ratio A / B of 0.2 or more, it has a sufficient amount of reactive double bonds, and when it is heated in actual use while in close contact with an adherend, the adhesive strength is likely to improve. The intensity ratio A / B is more preferably 0.3 or more, even more preferably 0.4 or more, and even more preferably 0.5 or more. The intensity ratio A / B is not particularly limited, but is, for example, 1.0 or less, preferably 0.8 or less, and more preferably 0.7 or less. The peak of the C=O stretching vibration is typically at a wavenumber of 1720 cm -1 The peak of the C=C stretching vibration typically appears around 1636 cm -1 However, these peaks may be slightly shifted depending on the structure of the acrylic polymer, etc.

[0028] The adhesive layer may be provided on one surface of the thermally conductive layer or on both surfaces of the thermally conductive layer. Note that the one surface or both surfaces referred to here are surfaces that are perpendicular to the thickness direction of the thermally conductive layer, and are also called main surfaces. By providing the adhesive layers on both surfaces of the thermally conductive layer, the adhesiveness of both surfaces of the thermally conductive sheet to the adherend can be improved. Therefore, when the thermally conductive sheet is used for semiconductor applications, it can be adhered to both the semiconductor chip and the heat spreader, or the heat spreader and the heat sink with relatively high adhesive strength, and even if it is heated at high temperature after being in actual use while being adhered to these, it is easy to prevent the thermally conductive sheet from peeling off from either the semiconductor chip and the heat spreader, or the heat spreader and the heat sink.

[0029] The weight of the adhesive layer on each surface is, for example, 0.05 mg / cm 2 or more, preferably 0.1 mg / cm 2 More preferably, 0.2 mg / cm 2 More preferably, 0.3 mg / cm 2 or more, for example, 1.0 mg / cm 2 Less than 0.75 mg / cm 2 Less than 0.6 mg / cm, more preferably 0.6 mg / cm 2 More preferably, 0.4 mg / cm 2 The adhesive layer can ensure sufficient adhesive strength to the adherend by making the weight per unit area a certain amount or more. Also, by making the weight per unit area a certain amount or less, it becomes easier to achieve excellent reworkability during assembly work. Also, it becomes easier to ensure good thermal conductivity by preventing the thermal resistance value from decreasing due to the adhesive layer.

[0030] The adhesive layer is preferably soaked into the thermally conductive layer. Typically, a part of the adhesive layer is preferably soaked into the thermally conductive layer, but the entire adhesive layer may be soaked into the thermally conductive layer as long as the adhesive layer can exert an adhesive force on the adherend. By soaking into the thermally conductive layer, the adhesive layer can reduce the amount of adhesive present on the surface of the thermally conductive layer, and can suppress the deterioration of thermal conductivity due to the adhesive layer. In addition, the thermally conductive sheet can ensure high adhesion even if the adhesive soaks into the thermally conductive layer. Although the principle behind this is unclear, it is assumed that this is because thermally conductive sheets are generally compressed or otherwise pressurized when in use, and the soaked adhesive seeps out to the surface due to the pressure, enhancing adhesion.

[0031] In addition, as described below, the adhesive layer can be impregnated into air bubbles formed by the evaporation of a volatile substance, allowing an appropriate amount of adhesive layer to soak into the thermally conductive layer. The adhesive layer may be formed so as to cover the entire surface of each of the thermally conductive layers, but may also be formed so as to cover only a portion of each of the surfaces as long as the adhesive layer can exert its adhesive strength with respect to the adherend.

[0032] The adhesive strength B1 of the adhesive layer is preferably 0.5 MPa or less, more preferably 0.3 MPa or less, and even more preferably 0.11 MPa or less. By having the adhesive strength B1 be equal to or less than the upper limit, it becomes easier to impart excellent reworkability to the thermal conductive sheet. On the other hand, the lower limit of the adhesive strength B1 of the adhesive layer is not particularly limited, but from the viewpoint of practicality, it is good to set it to about 0.005 MPa or more, and preferably 0.01 MPa or more.

[0033] In addition, the adhesive strength B2 of the adhesive layer is preferably 0.12 MPa or more, more preferably 0.13 MPa or more, and even more preferably 0.15 MPa or more. When the adhesive strength B2 is equal to or more than the lower limit, the thermal conductive sheet is likely to exhibit excellent adhesion in practical use. On the other hand, the upper limit of the adhesive strength B1 of the adhesive layer is not particularly limited, but from the viewpoint of practicality, it is preferably, for example, about 2 MPa or less, and preferably 1.5 MPa or less.

[0034] <Thermal Conduction Layer> The thermally conductive layer of the present invention comprises a polymeric matrix and a thermally conductive filler. The polymer matrix is ​​a matrix made of an organic polymer, preferably an organic polymer made of rubber or gel, and more preferably formed by curing a liquid polymer composition (curable polymer composition) made of a mixture of a base agent and a curing agent. The curable polymer composition may be, for example, one made of uncrosslinked rubber and a crosslinking agent, or one containing a monomer, a prepolymer, or the like, and a curing agent. The curing reaction may be room temperature curing or heat curing.

[0035] The polymer matrix is ​​preferably an organopolysiloxane. In the present invention, by using an organopolysiloxane, the polymer matrix after curing can be made flexible, and the filling property of the thermally conductive filler can be improved. The organopolysiloxane is preferably a silicone rubber. In addition, the organopolysiloxane is preferably a curing type silicone, and more preferably an addition reaction type silicone. In the case of addition reaction type silicone, the curable polymer composition is composed of an alkenyl group-containing organopolysiloxane (base material) and a hydrogen organopolysiloxane (curing agent), and the polymer matrix may be formed by curing these. It is considered that the use of addition reaction type silicone makes it easier to improve adhesion to the adherend by high temperature heating during actual use.

[0036] As the rubber, various synthetic rubbers can be used in addition to silicone rubber, and specific examples include acrylic rubber, nitrile rubber, isoprene rubber, urethane rubber, ethylene propylene rubber, styrene-butadiene rubber, butadiene rubber, fluororubber, and butyl rubber. When using these rubbers, the synthetic rubbers may be crosslinked or left uncrosslinked (i.e., uncured) in the thermal conductive sheet. Uncrosslinked rubbers are mainly used for flow orientation. Furthermore, when crosslinking (i.e., curing) is performed, as explained above, the polymer matrix may be a cured curable polymer composition consisting of an uncrosslinked synthetic rubber and a crosslinking agent. As the elastomer, a thermoplastic elastomer such as a polyester-based thermoplastic elastomer or a polyurethane-based thermoplastic elastomer, or a thermosetting elastomer formed by curing a mixed liquid polymer composition consisting of a base agent and a curing agent can be used. For example, a polyurethane-based elastomer formed by curing a polymer composition containing a polymer having a hydroxyl group and an isocyanate can be exemplified. Furthermore, examples of gels include silicone gels, such as those based on organopolysiloxane.

[0037] In addition, the polymer composition for forming the polymer matrix may be composed of an organic polymer alone, or may be composed of an organic polymer and a plasticizer. The plasticizer is preferably used when synthetic rubber is used, and by including the plasticizer, it is possible to increase the flexibility of the polymer matrix when not crosslinked. For example, when the polymer matrix is ​​organopolysiloxane, silicone oil is preferably used as a plasticizer. That is, the curable polymer composition may be composed of a base agent and a curing agent, or may be composed of a base agent, a curing agent, and a plasticizer. The content of the polymer matrix, expressed as a volume-based filling rate (volume filling rate), is preferably 15 volume % or more and 50 volume % or less, more preferably 17 volume % or more and 45 volume % or less, and even more preferably 20 volume % or more and 40 volume % or less, based on the total amount of the thermal conductive sheet. In terms of adjusting the tensile breaking strength, when the tensile breaking strength is adjusted to be higher, the content of the polymer matrix is ​​preferably increased, and when the tensile breaking strength is adjusted to be lower, the content of the polymer matrix is ​​preferably decreased.

[0038] (Thermal conductive filler) The thermally conductive filler contained in the thermally conductive layer may be dispersed in a polymer matrix and held in the polymer matrix. Examples of the thermally conductive filler include anisotropic fillers and non-anisotropic fillers, but it is preferable to use at least anisotropic fillers.

[0039] The anisotropic filler is preferably oriented in the thickness direction of the thermally conductive sheet. This makes it easier for the thermally conductive layer to increase its thermal conductivity. When the anisotropic filler is oriented in the thickness direction, its long axis direction does not need to be strictly parallel to the thickness direction, and even if the long axis direction is slightly tilted to the thickness direction, it is considered to be oriented in the thickness direction. Specifically, anisotropic fillers oriented in the thickness direction are also those whose long axis direction is tilted by less than 20°, and such anisotropic fillers are the majority in the thermally conductive sheet (for example, more than 60% of the total number of anisotropic fillers, preferably more than 80%).

[0040] The content of the thermally conductive filler is preferably 150 parts by mass or more and 3000 parts by mass or less, more preferably 200 parts by mass or more and 1800 parts by mass or less, and even more preferably 300 parts by mass or more and 1000 parts by mass or less, relative to 100 parts by mass of the polymer matrix. By making the content of the thermally conductive filler 150 parts by mass or more, a certain level of thermal conductivity can be imparted to the thermally conductive layer. In addition, by making the content 3000 parts by mass or less, the thermally conductive filler can be appropriately dispersed in the polymer matrix. In addition, the viscosity of the mixed composition described later can be prevented from becoming higher than necessary. The volumetric filling rate of the thermally conductive filler relative to the total amount of the thermally conductive layer is preferably 30% by volume or more and 85% by volume or less, more preferably 50% by volume or more and 83% by volume or less, and even more preferably 66% by volume or more and 80% by volume or less. By setting the volumetric filling rate to the lower limit or more, a certain level of thermal conductivity can be imparted to the thermally conductive layer. By setting the volumetric filling rate to the upper limit or less, the thermally conductive layer can be easily manufactured. In terms of adjusting the tensile breaking strength, when adjusting to increase the tensile breaking strength, it is preferable to adjust the volumetric filling rate of the thermally conductive filler to be smaller, and when adjusting to decrease the tensile breaking strength, it is preferable to adjust the volumetric filling rate of the thermally conductive filler to be larger.

[0041] (Anisotropic filling material) An anisotropic filler is a filler that has anisotropy in shape and can be oriented. Examples of anisotropic fillers include fibrous materials and scaly materials. An anisotropic filler has a high aspect ratio, specifically, an aspect ratio of more than 2, and the aspect ratio is preferably 5 or more. By making the aspect ratio larger than 2, it becomes easier to orient the anisotropic filler in one direction, such as the thickness direction, and it is easier to increase the thermal conductivity in one direction, such as the thickness direction of the thermal conductive layer. In addition, the upper limit of the aspect ratio is not particularly limited, but is practically 100. The aspect ratio is the ratio of the long axis length to the short axis length of an anisotropic filler, which in fibrous materials means fiber length / fiber diameter, and in scaly materials means the long axis length / thickness of the scaly materials.

[0042] The content of the anisotropic filler in the thermally conductive layer is preferably 10 parts by mass or more and 500 parts by mass or less, more preferably 30 parts by mass or more and 300 parts by mass or less, and even more preferably 50 parts by mass or more and 250 parts by mass or less, per 100 parts by mass of the polymer matrix. By making the content of the anisotropic filler 10 parts by mass or more, it is easy to increase the thermal conductivity. Also, by making the content 500 parts by mass or less, it is easy to make the viscosity of the mixed composition described later appropriate, and the orientation of the anisotropic filler is good. Furthermore, the dispersibility of the anisotropic filler in the polymer matrix is ​​also good. In terms of adjusting the tensile breaking strength, when adjusting to increase the tensile breaking strength, it is recommended to adjust the content of the anisotropic filler to be smaller, and when adjusting to decrease the tensile breaking strength, it is recommended to adjust the content of the anisotropic filler to be larger.

[0043] When the anisotropic filler is a fiber material, the average fiber length is preferably 10 μm to 300 μm, more preferably 20 μm to 200 μm, and even more preferably 30 μm to 100 μm. When the average fiber length is 10 μm or more, the anisotropic fillers are in proper contact with each other inside the heat conductive layer, a heat transfer path is secured, and the heat conductivity of the heat conductive layer is improved. On the other hand, when the average fiber length is 500 μm or less, the bulk of the anisotropic filler is reduced, and it becomes possible to highly fill the binder component. In addition, the average fiber length of the fiber material is preferably shorter than the thickness of the thermally conductive sheet. By having the average fiber length shorter than the thickness, the fiber material is prevented from protruding more than necessary from the surface of the thermally conductive sheet. The average fiber length can be calculated by observing the anisotropic filler under a microscope. More specifically, the fiber lengths of 50 pieces of any anisotropic filler can be measured using, for example, an electron microscope or an optical microscope, and the average value (arithmetic mean value) can be used as the average fiber length.

[0044] In addition, when the anisotropic filler is a scaly material, its average particle size is preferably 10 μm to 300 μm, more preferably 15 μm to 200 μm, and even more preferably 20 μm to 100 μm. By setting the average particle size to 10 μm or more, the anisotropic fillers in the heat conductive layer can easily come into contact with each other, a heat transfer path can be secured, and the heat conductivity of the heat conductive layer can be improved. On the other hand, by setting the average particle size to 400 μm or less, the bulk of the heat conductive sheet can be reduced, and the anisotropic filler can be highly filled in the binder component. The average particle size of the scaly filler is D50, which can be calculated by observing the scaly filler under a microscope and taking the long diameter as the diameter. More specifically, for example, using an electron microscope or optical microscope, the long diameter of 500 or more arbitrary scaly fillers is measured, and the particle size corresponds to a cumulative frequency of 50%. Specifically, it can be obtained from a particle size distribution curve in which the horizontal axis is the particle size and the vertical axis is the cumulative frequency, using the scaly filler as a sample. The particle size distribution curve is a numerical particle size distribution curve obtained by sequentially accumulating the particle sizes of the scaly fillers starting from the smallest particle size.

[0045] The anisotropic filler may be a known material having thermal conductivity, but when oriented by magnetic field orientation as described below, it is preferable that the filler has diamagnetism. On the other hand, when oriented by flow orientation or when the anisotropic filler is not oriented, the filler does not need to have diamagnetism. Specific examples of anisotropic fillers include carbon-based materials such as carbon fibers or scaly carbon powder, metal materials such as metal fibers, metal oxides, boron nitride, metal nitrides, metal carbides, metal hydroxides, polyparaphenylene benzoxazole fibers, etc. Among these, carbon-based materials are preferred because they have a low specific gravity and good dispersibility in binder components, and graphitized carbon materials with high thermal conductivity are more preferred. Graphitized carbon materials have diamagnetic properties because the graphite planes are aligned in a specific direction. Also, boron nitride is preferred as an anisotropic filler. Although boron nitride is not particularly limited, it is preferred to use it as a scaly material. The scaly boron nitride may be agglomerated or may not be agglomerated, but it is preferred that it is not agglomerated in part or in whole. Note that boron nitride and the like also have diamagnetic properties when the crystal planes are aligned in a specific direction.

[0046] Furthermore, the anisotropic filler generally has a thermal conductivity along the anisotropic direction (i.e., the long axis direction) of 30 W / m·K or more, preferably 60 W / m·K or more, more preferably 100 W / m·K or more, and even more preferably 200 W / m·K or more, though it is not particularly limited thereto. The upper limit of the thermal conductivity of the anisotropic filler is, for example, 2000 W / m·K or less. The thermal conductivity can be measured by a laser flash method or the like.

[0047] The anisotropic filler may be used alone or in combination of two or more kinds. For example, at least two anisotropic fillers having different average particle diameters or average fiber lengths may be used as the anisotropic filler. When anisotropic fillers of different sizes are used, the smaller anisotropic fillers are inserted between the relatively larger anisotropic fillers, so that the anisotropic fillers can be densely packed in the binder component and the heat conduction efficiency can be improved.

[0048] In addition, the anisotropic filler preferably contains a fiber material, and more preferably contains carbon fiber. A thermally conductive layer containing a fiber material is more likely to improve the tensile breaking strength of the thermally conductive sheet. As described below, slicing the sheet tends to cause the fiber material to fall off, resulting in unevenness on the surface and reduced adhesion. However, in the present invention, by providing an adhesive layer, the adhesive layer penetrates into the recesses, so that even a thermally conductive layer containing a fiber material can sufficiently increase adhesion. In order to improve thermal conductivity, the thermally conductive layer preferably contains a scaly material as an anisotropic filler in addition to the fibrous material. In this case, the content ratio of the scaly material to the fibrous material (scaly material / fibrous material) is, for example, 0.01 to 1, preferably 0.02 to 0.5, more preferably 0.1 to 0.3, by mass.

[0049] The carbon fiber used as the anisotropic filler is preferably a graphitized carbon fiber. The flake carbon powder is preferably a flake graphite powder. It is also preferable to use the graphitized carbon fiber and the flake graphite powder in combination as the anisotropic filler. Graphitized carbon fiber has graphite crystal planes aligned in the fiber axis direction, and has high thermal conductivity in the fiber axis direction. Therefore, by aligning the fiber axis direction in a specific direction, it is possible to increase the thermal conductivity in a specific direction. Furthermore, flake graphite powder has graphite crystal planes aligned in the in-plane direction of the flake surfaces, and has high thermal conductivity in the in-plane direction. Therefore, by aligning the flake surfaces in a specific direction, it is possible to increase the thermal conductivity in a specific direction. Graphitized carbon fiber and flake graphite powder having a high degree of graphitization are preferred.

[0050] As the graphitized carbon materials such as the graphitized carbon fiber and the flake graphite powder, the following raw materials can be graphitized. For example, condensed polycyclic hydrocarbon compounds such as naphthalene, condensed heterocyclic compounds such as PAN (polyacrylonitrile) and pitch can be mentioned, but it is preferable to use graphitized mesophase pitch, polyimide, and polybenzazole, which have a particularly high degree of graphitization. For example, by using mesophase pitch, the pitch is oriented in the fiber axis direction due to its anisotropy in the spinning process described later, and graphitized carbon fibers having excellent thermal conductivity in the fiber axis direction can be obtained. The use of mesophase pitch in graphitized carbon fiber is not particularly limited as long as it can be spun, and mesophase pitch may be used alone or in combination with other raw materials. However, it is most preferable to use mesophase pitch alone, that is, graphitized carbon fiber containing 100% mesophase pitch, from the viewpoints of high thermal conductivity, spinnability, and stability of quality.

[0051] The graphitized carbon fiber may be one which has been subjected to spinning, infusibility and carbonization in sequence, pulverized or cut to a predetermined particle size, and then graphitized, or one which has been pulverized or cut after carbonization and then graphitized. When pulverization or cutting is performed before graphitization, the newly exposed surface due to pulverization is more likely to undergo condensation polymerization and cyclization reactions during the graphitization process, and therefore it is possible to obtain graphitized carbon fiber with a higher degree of graphitization and further improved thermal conductivity. On the other hand, when spun carbon fiber is graphitized and then pulverized, the graphitized carbon fiber is easy to pulverize because it is hard, and carbon fiber powder with a relatively narrow fiber length distribution can be obtained by pulverization for a short period of time.

[0052] As described above, the average fiber length of the graphitized carbon fiber is preferably 10 μm or more and 300 μm or less, more preferably 20 μm or more and 200 μm or less, and even more preferably 30 μm or more and 100 μm or less. As described above, the aspect ratio of the graphitized carbon fiber is greater than 2, and preferably is 5 or more. The thermal conductivity of the graphitized carbon fiber is not particularly limited, but the thermal conductivity in the fiber axis direction is preferably 400 W / m·K or more, and more preferably 800 W / m·K or more.

[0053] When the thermally conductive layer contains an anisotropic filler, it may be exposed on the surface of the thermally conductive layer, but it is preferable that the filler is exposed. When the anisotropic filler is exposed, the anisotropic filler comes into contact with the adherend, such as a heating body or a heat dissipating body, and the thermal resistance value is easily reduced. When the anisotropic filler is exposed, the adhesion to the adherend is difficult to improve, but even in such a case, in the present invention, the adhesion is easily improved by providing an adhesive layer.

[0054] (non-anisotropic filler) The thermally conductive filler in the present invention may contain a non-anisotropic filler, and it is preferable to use the above-mentioned anisotropic filler and a non-anisotropic filler in combination. In particular, when used in combination with an anisotropic filler oriented in one direction such as the thickness direction, the non-anisotropic filler is interposed in the gaps between the oriented anisotropic fillers, and the thermal conductivity can be further increased. The non-anisotropic filler is a filler that does not substantially have anisotropy in shape, and is a filler that does not orient in a predetermined direction even in an environment in which the anisotropic filler is oriented in the predetermined direction, such as under the generation of magnetic lines of force or under the action of shear force, as described below.

[0055] The aspect ratio of the non-anisotropic filler is 2 or less, and preferably 1.5 or less. When a non-anisotropic filler having such a low aspect ratio is used in combination with an anisotropic filler, it is easy to be arranged in the gaps of the anisotropic filler, and it is easy to improve the thermal conductivity. In addition, by making the aspect ratio 2 or less, it is possible to prevent the viscosity of the mixed composition described later from increasing, and to achieve high filling.

[0056] Specific examples of the non-anisotropic filler include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides, nitrides, carbides other than metals, etc. Examples of the shape of the non-anisotropic filler include spherical, polyhedral, and amorphous powders. In the non-anisotropic filler, examples of metals include aluminum, copper, nickel, etc., examples of metal oxides include aluminum oxide, magnesium oxide, zinc oxide, etc., such as alumina, and examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Furthermore, examples of carbon materials include spherical graphite. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, aluminum oxide and aluminum are preferred because they have high thermal conductivity and are easily available in spherical form. The non-anisotropic filler may be used alone or in combination of two or more of the above.

[0057] The average particle size of the non-anisotropic filler is, for example, 0.1 μm or more and 200 μm or less, preferably 0.5 μm or more and 100 μm or less, and more preferably 1 μm or more and 70 μm or less. In addition, when a non-anisotropic filler is used in combination with an anisotropic filler, the average particle size of the non-anisotropic filler is preferably 0.1 μm or more and 50 μm or less, more preferably 0.5 μm or more and 35 μm or less, and even more preferably 1 μm or more and 15 μm or less. By making the average particle size 50 μm or less, even when used in combination with an anisotropic filler, problems such as disturbing the orientation of the anisotropic filler are unlikely to occur. In addition, by making the average particle size 0.1 μm or more, the specific surface area of ​​the non-anisotropic filler does not become larger than necessary, and even if a large amount is mixed, the viscosity of the mixed composition is unlikely to increase, making it easier to highly fill the non-anisotropic filler. The non-anisotropic filler may be, for example, a non-anisotropic filler having at least two different average particle sizes. The average particle size of the non-anisotropic filler can be measured by observation with an electron microscope, etc. More specifically, for example, the particle sizes of 500 or more particles of any non-anisotropic filler can be measured using an electron microscope or an optical microscope, and D50 can be calculated in the same manner as for the scaly filler.

[0058] The content of the non-anisotropic filler is preferably 50 parts by mass or more and 2500 parts by mass or less, more preferably 100 parts by mass or more and 1500 parts by mass or less, and even more preferably 200 parts by mass or more and 750 parts by mass or less, relative to 100 parts by mass of the polymer matrix. By making it 50 parts by mass or more, the thermal conductivity of the thermal conductive sheet can be improved. On the other hand, by making it 1500 parts by mass or less, the non-anisotropic filler can be appropriately dispersed in the binder component, and the effect of increasing the thermal conductivity according to the content can be obtained. In addition, the viscosity of the mixed composition can be prevented from increasing more than necessary.

[0059] The mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler is not particularly limited, but is preferably from 0.5 to 15, more preferably from 1 to 10, and more preferably from 1.1 to 7. By setting the mass ratio within the above range, the non-anisotropic filler is appropriately filled between the anisotropic fillers to form an efficient heat transfer path, thereby further improving the thermal conductivity of the thermally conductive sheet. On the other hand, from the viewpoint of adjusting the tensile breaking strength, the tensile breaking strength can be lowered by decreasing the mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler, and the tensile breaking strength can be increased by increasing the mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler. For example, from the viewpoint of lowering the tensile breaking strength, the mass ratio is preferably 0.5 or more and 5 or less, and from the viewpoint of increasing the tensile breaking strength, the mass ratio is preferably more than 5 and 15 or less.

[0060] In the heat conductive layer, the polymer matrix may further contain other components than those mentioned above within a range that does not impair the function of the heat conductive layer. Specifically, for example, at least one selected from dispersants, flame retardants, antioxidants, colorants, anti-settling agents, etc. may be mentioned. In addition, when the curable polymer composition is crosslinked or cured as described above, a crosslinking accelerator, a curing accelerator, a curing catalyst, etc. that accelerates crosslinking and curing may be added as an additive. When the polymer matrix is ​​an organopolysiloxane, a platinum catalyst may be used as the curing catalyst.

[0061] The surface of the thermally conductive layer is preferably a sliced ​​surface. By having the surface of the thermally conductive layer be a sliced ​​surface, as described above, the anisotropic filler and the like can be easily exposed to the surface of the thermally conductive layer, and the thermal resistance value can be effectively reduced. The thermally conductive sheet may have one surface or both surfaces as sliced ​​surfaces, but it is preferable that the surface on which the adhesive layer is provided is a sliced ​​surface. Note that the sliced ​​surface is a surface formed by cutting with a shear blade or a laser, as described later. The sliced ​​surface often has large irregularities due to the protrusion or falling off of the anisotropic filler, but by filling the recesses with an adhesive layer, the air gap can be reduced during use, improving the thermal resistance and increasing adhesion.

[0062] It is also preferable that the thermally conductive sheet has a polished surface. By having at least one surface of the thermally conductive sheet be a polished surface, the thermal resistance value can be more effectively reduced. The thermally conductive sheet may have one surface or both surfaces being polished, but it is preferable that the surface on which the adhesive layer is provided is a polished surface, and it is particularly preferable that the surface on which the adhesive layer is provided is a sliced ​​surface and a polished surface. The polished surface has a relatively high smoothness, and the adhesive layer is provided, which makes it easier to increase the adhesion to the adherend.

[0063] The thickness of the thermally conductive layer is not particularly limited, but is, for example, about 1200 μm or less. From the viewpoint of suitable use in semiconductor applications and from the viewpoint of preventing the thermal resistance value from increasing, it is better to make it relatively thin, preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less. The thickness of the thermally conductive layer is not particularly limited, but for practical purposes, it is, for example, 10 μm or more, preferably 20 μm or more, and more preferably 70 μm or more. The thickness of the thermally conductive layer is the initial thickness measured in a state where no load is applied in the thickness direction.

[0064] (Arithmetic mean height (Sa)) The arithmetic mean height (Sa) of the surface of the thermally conductive sheet on which the adhesive layer is provided is, for example, 20 μm or less, preferably 12 μm or less, more preferably 6 μm or less, and even more preferably 5 μm or less. The thermal resistance value of the thermally conductive sheet can be more effectively reduced by lowering the arithmetic mean height of the surface on which the acrylic adhesive layer is provided. In addition, the acrylic adhesive layer allows the thermally conductive sheet to be more effectively attached to the adherend. Note that, for example, when the surface of the thermally conductive sheet is sliced ​​as described above, the arithmetic mean height is likely to be relatively large, but by polishing after slicing, the arithmetic mean height (Sa) can be reduced as described above. The arithmetic mean height (Sa) of the surface of the thermal conductive sheet on which the acrylic adhesive layer is provided is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more. By making the arithmetic mean height (Sa) equal to or more than these lower limits, even a sliced ​​surface can be relatively easily obtained by polishing.

[0065] (E hardness) The thermally conductive layer of the present invention preferably has a type E hardness (hereinafter also referred to as "E hardness") defined by JIS K6253 of 10 or more and 80 or less, more preferably 20 or more and 70 or less, and even more preferably 30 or more and 65 or less. When the E hardness is equal to or more than the above lower limit, the mechanical strength of the thermally conductive sheet is easily increased. On the other hand, when the E hardness is equal to or less than the above upper limit, a certain degree of flexibility is imparted to the thermally conductive sheet, and the adhesion to the adherend is also easily improved. If it is desired to increase the tensile breaking strength, it is advisable to adjust the E hardness to a higher value, whereas if it is desired to decrease the tensile breaking strength, it is advisable to adjust the E hardness to a lower value.

[0066] <Thermal resistance value of thermal conductive sheet> The thermal conductive sheet of the present invention has a thermal resistance of, for example, 0.5°C cm 2 / W or less, but 0.25°C cm 2 / W or less is preferable, and 0.2°C cm 2 / W or less is more preferable, and 0.16°C cm2 / W or less is more preferable. When the thermal resistance is equal to or less than the above upper limit, the efficiency of heat transfer from the heat generating body to the heat sink via the thermal conductive sheet is improved, and excellent thermal conductivity can be obtained. In the present invention, the lower the thermal resistance is, the better, and the lower the thermal resistance is, the better the thermal conductivity is. 2 / W or more is sufficient, but in practice, it should be, for example, 0.01°C cm 2 / W or more, preferably 0.05°C cm 2 / W or more. The thermal resistance value is a thermal resistance value measured when a pressure of 20 psi is applied in the thickness direction, and specifically, can be obtained by the measurement method described in the examples.

[0067] <Tensile breaking strength> The thermal conductive sheet of the present invention preferably has a tensile breaking strength of 15 mN / mm to 60 mN / mm, more preferably 20 mN / mm to 50 mN / mm, and even more preferably 30 mN / mm to 45 mN / mm. When the tensile breaking strength is equal to or greater than the lower limit, a certain degree of workability is ensured, and it is easy to impart excellent reworkability to the thermal conductive sheet. When the tensile breaking strength is equal to or less than the upper limit, a certain degree of flexibility is imparted to the thermal conductive sheet, and it is easy to improve the ability to follow warping and adhesion. The tensile breaking strength can be obtained by the method described in the Examples.

[0068] <Tensile elongation at break> The thermal conductive sheet of the present invention preferably has a tensile elongation at break of 10% or more, more preferably 12% or more, and even more preferably 13% or more. If the tensile elongation at break is equal to or more than the lower limit, when the adherend warps, breakage due to warping is prevented, and it is easy to make the conformability to warping excellent. In addition, from the viewpoint of imparting a certain stiffness to the thermal conductive sheet and facilitating good reworkability, the tensile strength at break is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less. The above-mentioned tensile strength at break and tensile elongation at break can be adjusted, for example, by adjusting the type and amount of the polymer matrix and the thermally conductive filler that constitute the thermally conductive layer. From the viewpoint of not increasing the tensile breaking strength too much, a preferred embodiment is, for example, to use silicone rubber or silicone gel as the polymer matrix, to set the content of the polymer matrix to 40 volume % or less, to contain an anisotropic filler as the thermally conductive filler, and to set the mixing amount of the thermally conductive filler to 60 volume % or more. In order to avoid excessively lowering the tensile strength at break, it is a preferred embodiment to set the content of the polymer matrix to 15 volume % or more, while setting the amount of the thermally conductive filler containing an anisotropic filler as the thermally conductive filler to 85 volume % or less. The tensile elongation at break can be obtained by the method described in the Examples.

[0069] [Method of manufacturing thermally conductive sheets] The thermally conductive sheet of the present invention can be produced, for example, by a method including the following steps 1 to 3, although the method is not particularly limited. Step 1: A step of mixing at least a curable polymer composition and a thermally conductive filler to obtain a mixed composition. Step 2: A step of curing the mixed composition by heating to obtain a cured product. Step 3: Applying an adhesive to the surface of the cured product

[0070] (Process 1) In step 1, a mixed composition may be obtained by mixing at least the curable polymer composition and the thermally conductive filler, and it is preferable to further mix a volatile substance into the mixed composition. In addition, other components such as additives may be appropriately added to the mixed composition as needed.

[0071] In step 1, the mixing method and mixing order are not particularly limited as long as the above-mentioned components can be mixed to obtain a mixed composition, and the curable polymer composition, the thermally conductive filler, the volatile substance added as necessary, and other components added as necessary may be appropriately mixed in any order to obtain a mixed composition. As described above, the curable polymer composition may consist of, for example, a base agent and a curing agent (for example, in the case of an addition reaction type silicone, an alkenyl group-containing organopolysiloxane and a hydrogen organopolysiloxane). In such a case, the base agent, the curing agent, the thermally conductive filler, and the volatile substance and other components that are optionally added as necessary may be mixed in any order to obtain a mixed composition. The mixed composition may be in the form of a one-part type or a two-part type consisting of a first part and a second part. The two-part type is a type in which the first part and the second part are mixed together at the time of use to obtain a mixed composition.

[0072] (Volatile substances) The volatile substance used in the present invention may be any component that volatilizes in step 2 described below. The volatile substance volatilizes by heating during curing, thereby increasing the content of the thermally conductive filler in the thermally conductive sheet. In addition, the viscosity of the mixed composition is reduced by including a volatile substance. This makes it easier to increase the amount of thermally conductive filler to be mixed, and also makes it easier to orient the anisotropic filler in a predetermined direction by magnetic field orientation described below. Furthermore, as the volatile substances evaporate, numerous fine bubbles are formed in the cured product, which makes it easier for the adhesive to seep into the heat conductive layer in step 4, which will be described later.

[0073] In addition, the volatile material is preferably a compatible material that is compatible or soluble in the curable polymer composition. If the volatile material is a compatible material, the curable polymer composition and the volatile material can be mixed uniformly, making it easier to reduce the viscosity and increase the amount of the thermally conductive filler. Furthermore, the bubbles formed by the evaporation of the volatile material can be fine and uniform.

[0074] The volatile substance is preferably a substance that is liquid at room temperature (25° C.) and at 1 atmospheric pressure. Examples of the volatile substance include an alkoxysilane compound, a hydrocarbon solvent, and an alkoxysiloxane compound. These compounds can increase the solubility or compatibility with the curable polymer composition, making it easier to reduce the viscosity of the mixed composition and increase the amount of the thermally conductive filler. In addition, the volatilization of the volatile substance makes it easier to make the bubbles formed fine and uniform. The volatile substances may be used alone or in combination of two or more.

[0075] As the volatile material, it is preferable to use an alkoxysilane compound. By using an alkoxysilane compound, the surface of the thermally conductive sheet obtained by curing is free of roughness and has a good appearance. The alkoxysilane compound used as the volatile substance is a compound having a structure in which, of the four bonds possessed by a silicon atom (Si), one to three are bonded to an alkoxy group, and the remaining bonds are bonded to an organic substituent. By having an alkoxy group and an organic substituent, the alkoxysilane compound can enhance compatibility with a curable polymer composition, particularly a curable polymer composition composed of an organopolysiloxane. Examples of the alkoxy group contained in the alkoxysilane compound include a methoxy group, an ethoxy group, a protoxy group, a butoxy group, a pentoxy group, and a hexoxy group. The alkoxysilane compound may be contained in the curable polymer composition as a dimer.

[0076] Among the alkoxysilane compounds, from the viewpoint of availability, an alkoxysilane compound having at least one of a methoxy group and an ethoxy group is preferred. From the viewpoint of compatibility with the curable polymer composition, solubility, etc., the number of alkoxy groups in the alkoxysilane compound is preferably 2 or 3, more preferably 3. Specifically, the alkoxysilane compound is preferably at least one selected from a trimethoxysilane compound, a triethoxysilane compound, a dimethoxysilane compound, and a diethoxysilane compound.

[0077] Examples of functional groups contained in the organic substituent of the alkoxysilane compound include acryloyl, alkyl, carboxyl, vinyl, methacryl, aromatic, amino, isocyanate, isocyanurate, epoxy, hydroxyl, and mercapto groups. When a platinum catalyst is used as a curing catalyst for a curable polymer composition composed of an organopolysiloxane, it is preferable to select and use an alkoxysilane compound that is less likely to affect the curing reaction of the organopolysiloxane. Specifically, when an addition reaction type organopolysiloxane using a platinum catalyst is used, it is preferable that the organic substituent of the alkoxysilane compound does not include an amino group, an isocyanate group, an isocyanurate group, a hydroxyl group, or a mercapto group.

[0078] From the viewpoint of compatibility with the curable polymer composition composed of organopolysiloxane, the alkoxysilane compound preferably contains an alkylalkoxysilane compound having an alkyl group bonded to a silicon atom, i.e., an alkoxysilane compound having an alkyl group as an organic substituent. Therefore, dialkyldialkoxysilane compounds and alkyltrialkoxysilane compounds are preferred, and among them, alkyltrialkoxysilane compounds are preferred. The number of carbon atoms in the alkyl group bonded to the silicon atom may be, for example, 1 to 16. In addition, in trialkoxysilane compounds such as trimethoxysilane compounds and triethoxysilane compounds, the number of carbon atoms in the alkyl group is preferably 6 or more, more preferably 8 or more, and is preferably 12 or less, more preferably 10 or less. On the other hand, in dialkoxysilane compounds such as dimethoxysilane compounds and triethoxysilane compounds, the alkyl group may have 1 or more carbon atoms, and preferably has 10 or less carbon atoms, more preferably 6 or less, and even more preferably 4 or less carbon atoms.

[0079] Examples of alkyl group-containing alkoxysilane compounds include methyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, di-n-propyldimethoxysilane, di-n-propyldiethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, and n-decyltriethoxysilane. Among the alkyl group-containing alkoxysilane compounds, n-decyltrimethoxysilane and n-octyltriethoxysilane are even more preferred from the viewpoint of compatibility with the organopolysiloxane constituting the curable polymer composition.

[0080] The alkoxysiloxane compound used as the volatile substance has two or more siloxane bonds and has a structure in which an alkoxy group is bonded to at least one silicon atom. The alkoxysiloxane compound has a structure in which an organic substituent is bonded to at least one silicon atom among the silicon atoms constituting the siloxane bond. By having an alkoxy group and an organic substituent, the alkoxysiloxane compound can improve compatibility with the organopolysiloxane constituting the curable polymer composition. Examples of the alkoxy group and organic substituent possessed by the alkoxysiloxane compound include those exemplified in the description of the alkoxysilane compound above, and from the viewpoint of compatibility with the organopolysiloxane constituting the curable polymer composition, it is preferable for the compound to have at least an alkyl group.

[0081] Examples of the alkoxysiloxane compound include methyl methoxy siloxane oligomer, methyl phenyl methoxy siloxane oligomer, methyl epoxy methoxy siloxane oligomer, methyl mercapto methoxy siloxane oligomer, and methyl acryloyl methoxy siloxane oligomer. The alkoxysiloxane compounds may be used alone or in combination of two or more.

[0082] Examples of the hydrocarbon solvent used as the volatile material include aromatic hydrocarbon solvents. Among them, aromatic hydrocarbon solvents are preferred from the viewpoint of compatibility with the curable polymer composition. Examples of the aromatic hydrocarbon solvent include aromatic hydrocarbon solvents having about 6 to 10 carbon atoms, such as toluene, xylene, mesitylene, ethylbenzene, propylbenzene, butylbenzene, and t-butylbenzene, and preferably toluene and xylene.

[0083] In the mixed composition, the content of the volatile substance relative to 100 parts by mass of the curable polymer composition is preferably 6 parts by mass or more and 60 parts by mass or less. When the content is 6 parts by mass or more, the effect of the volatile substance is easily exhibited, for example, a moderate amount of fine bubbles can be formed in the polymer matrix. In addition, when the content is 60 parts by mass or less, an effect commensurate with the amount of the volatile substance used can be obtained. From these viewpoints, the content of the volatile substance is more preferably 8 parts by mass or more and 50 parts by mass or less, and even more preferably 10 parts by mass or more and 35 parts by mass or less. It is preferable that the volatile substance is partially or completely volatilized by the heating in step 2. Therefore, the volatile substance does not need to be contained in the thermal conductive sheet, but may be contained in the thermal conductive sheet in an amount less than the content in the mixed composition.

[0084] The detailed description of the components other than the volatile substance in the mixed composition (i.e., the curable polymer composition, the thermally conductive filler, other additives, etc.) is as described above. The content of the thermally conductive filler in the mixed composition is also as described above. However, while the content of each component is shown above as an amount based on 100 parts by mass of the polymer matrix, in the mixed composition, the amount is based on 100 parts by mass of the curable polymer composition.

[0085] (Process 2) Step 2 is a step of curing the mixed composition by heating. The temperature at which the mixed composition is heated is not particularly limited as long as the curable polymer composition can be cured by heating, and may be higher than room temperature (25°C), but is preferably 50°C or higher, more preferably 70°C or higher. The heating temperature is not particularly limited, but may be a temperature at which the thermally conductive layer and the mixed composition do not thermally deteriorate, for example, 200°C or lower, preferably 180°C or lower, more preferably 160°C or lower. The heating may be performed in one stage or in two or more stages. When performing in two or more stages, the heating temperature may be within the above range in at least one stage, but it is preferable that the heating temperature is within the above range in all stages, and it is preferable that at least the first stage is heated at a temperature lower than the boiling point of the volatile compound. The total heating time is, for example, about 10 minutes to 24 hours. When performing in two or more stages, for example, the mixed composition is semi-cured in the first stage (primary curing), and the mixed composition is fully cured by heating in the second stage or later (secondary curing). Further, the curing may be such that the resin is completely cured by a primary curing step, and the second and subsequent heating steps are not accompanied by any curing.

[0086] As described later, when slicing the molded product obtained from the mixed composition to obtain a sheet-shaped molded product, it is also preferable to carry out a first stage of heating before slicing to perform primary curing, and then further heat the product after slicing to perform a second or subsequent stage of heating (secondary curing). By heating the product after slicing, volatile substances are more likely to volatilize by the second or subsequent stage of heating. When curing in two or more stages, the heating in the first stage (primary curing) may be performed at, for example, 50°C to 120°C, preferably 60°C to 100°C, more preferably 70°C to 90°C. The heating in the second and subsequent stages (secondary curing) may be performed at a higher temperature than the primary curing, for example, 100°C to 200°C, preferably 120°C to 180°C, more preferably 140°C to 160°C. The heating time in the first stage may be, for example, about 5 minutes to 20 hours, preferably about 30 minutes to 12 hours. The heating time in the second and subsequent stages may be, for example, about 10 minutes to 15 hours, preferably about 1 hour to 10 hours. By subjecting the molded body obtained from the mixed composition to the first heating step at a relatively low temperature as described above, the volatile compound is less likely to foam and produce large bubbles, and the molded body can be cured so that the volatile compound remains in the molded body. In addition, when the molded body is sliced ​​and then heated at a relatively high temperature for the second stage, the molded body is hardened, so that even at high temperatures it does not foam and generate large bubbles, and the spaces where the volatile compounds were present become fine bubbles. The size of the bubbles is, for example, 1 μm or less, preferably 0.2 μm or less. The lower limit of the size of the bubbles is not particularly limited, but is, for example, 0.001 μm or more.

[0087] In step 2, the mixed composition may be molded into a predetermined shape such as a block or sheet, and may be heated to harden. In step 2, when the mixed composition contains an anisotropic filler as the thermally conductive filler, the anisotropic filler may be oriented in one direction and then hardened by heating. The anisotropic filler may be oriented by a magnetic field orientation method or a flow orientation method, but it is preferable to orient the anisotropic filler by the magnetic field orientation method.

[0088] In the magnetic field orientation method, the mixed composition is injected into a mold or the like and then placed in a magnetic field to orient the anisotropic filler along the magnetic field. The curable polymer composition is then cured to obtain an oriented molded product. The mixed composition is cured under the heating conditions described above. The oriented molded body is preferably in the form of a block, but may be in the form of a sheet. By forming the oriented molded body in the form of a sheet, the adhesive may be applied to the oriented molded body directly in step 3 without slicing it. On the other hand, by forming the oriented molded body in the form of a block, the orientation of the anisotropic filler is enhanced.

[0089] In the magnetic field orientation method, a release film may be placed in the part inside the mold that contacts the mixed composition. For example, a resin film with good releasability or a resin film with one side treated with a release agent is used as the release film. By using the release film, the oriented molded body can be easily released from the mold.

[0090] The viscosity of the mixed composition used in the magnetic field orientation method is preferably 10 Pa·s or more and 300 Pa·s or less in order to perform magnetic field orientation. By making it 10 Pa·s or more, the thermally conductive filler is less likely to settle. In addition, by making it 300 Pa·s or less, the fluidity is improved, the anisotropic filler is properly oriented in the magnetic field, and there is no problem such as the orientation taking too long. The viscosity is measured at 25°C using a rotational viscometer (Brookfield viscometer DV-E, spindle SC4-14) at a rotational speed of 10 rpm. However, when a thermally conductive filler that does not easily settle is used or when an additive such as an anti-settling agent is combined, the viscosity of the mixed composition may be less than 10 Pa·s.

[0091] In the magnetic field orientation method, the magnetic field generating source for applying the magnetic field lines includes a superconducting magnet, a permanent magnet, an electromagnet, etc., but a superconducting magnet is preferable because it can generate a magnetic field with a high magnetic flux density. The magnetic field generated from these magnetic field generating sources preferably has a magnetic flux density of 1 to 30 Tesla. When the magnetic flux density is 1 Tesla or more, it becomes possible to easily orient the above-mentioned anisotropic filler made of a carbon material, etc. Also, when it is 30 Tesla or less, it becomes possible to practically manufacture it.

[0092] In the flow orientation method, a shear force is applied to the mixed composition to produce a primary sheet in which the anisotropic filler is oriented along the surface direction. More specifically, in the flow orientation method, the mixed composition prepared in step 1 is first stretched flat while applying a shear force to form a sheet (primary sheet). By applying a shear force, the anisotropic filler can be oriented in the shear direction. As a means for forming the sheet, for example, the mixed composition is applied to a substrate film by a coating applicator such as a bar coater or a doctor blade, or by extrusion molding or ejection from a nozzle, and then, as necessary, the mixed composition may be dried, semi-cured, or fully cured. The thickness of the primary sheet is preferably about 50 μm or more and 5000 μm or less. In the primary sheet, the anisotropic filler is oriented in one direction along the surface direction of the sheet. The mixed composition used in the flow orientation method has a relatively high viscosity so that a shear force is applied when the mixed composition is stretched into a sheet. Specifically, the viscosity of the mixed composition is preferably 3 Pa·s or more and 500 Pa·s or less.

[0093] The primary sheet may be used as a thermally conductive sheet as it is without being formed into a block as described below. Alternatively, a laminate block (a block-shaped oriented molded product) may be formed by laminating a plurality of primary sheets so that they are oriented in the same direction, and then bonding the primary sheets together by a heat press or the like while curing them by heating as necessary. In addition, when forming a laminated block, at least one of the surfaces of the primary sheets to be laminated may be irradiated with vacuum ultraviolet light, and then the primary sheets may be laminated. When the primary sheets are laminated via the surfaces irradiated with vacuum ultraviolet light, the primary sheets can be firmly bonded to each other. In addition, when irradiating with vacuum ultraviolet light, the mixed composition may be fully cured when preparing the primary sheets, and there is no need to cure by heating or the like when the primary sheets are laminated to form a laminated block. In the flow orientation method, the mixed composition may also be cured under the heating conditions as described above.

[0094] As described above, when forming a block-shaped oriented molded body, the obtained oriented molded body may be cut by slicing or the like perpendicular to the direction in which the anisotropic filler is oriented to form a sheet-shaped molded body. Slicing may be performed, for example, with a shear blade or a laser. When the sheet-shaped molded body is cut by slicing or the like, a part of the fibrous filler may be exposed from the matrix at each surface, which is the cut surface. Most of the exposed fibrous filler is oriented in the thickness direction without falling over. However, in step 2, when the oriented molded body is cut by slicing or the like, the fibrous filler contained in the oriented molded body may be cut to an extent that does not impair the effects of the present invention.

[0095] The sheet-like molded product obtained by cutting may be coated with an adhesive as is in step 3 described below, or may be further treated. For example, each surface that is the sliced ​​surface may be polished. In addition, as described above, secondary curing may be performed. The secondary curing may be performed after or before polishing. By polishing the sheet-like molded body, the surface condition of the sheet-like molded body becomes better, and the thermal resistance value can be further reduced. By polishing the sheet-like molded body, the sheet surface can be made smooth while exposing a certain amount of anisotropic filler such as a fibrous filler on the surface. The fibrous filler can also be made to be in a collapsed state. Therefore, the surface of the thermally conductive sheet can be easily attached to other members, and the sheet surface can be easily covered with the fibrous filler over a certain area or more, and the thermal resistance value can be easily reduced.

[0096] The polishing may be performed by polishing at least one surface of the obtained sheet-like molded product, but it is preferable to polish both surfaces of the sheet-like molded product. The surface polishing may be performed using, for example, abrasive paper, abrasive film, abrasive cloth, abrasive belt, or the like. Regarding the properties of the abrasive paper, the average particle size (D50) of the abrasive grains contained therein is preferably 0.1 μm or more and 100 μm or less, more preferably 1 μm or more and 60 μm or less. The grain size of the abrasive grains in the abrasive paper is preferably #120 to 20,000, more preferably #300 to 15,000, and more preferably #320 to 4,000.

[0097] The polishing method may be, for example, polishing the surface of the sheet-like molded body by continuously contacting the abrasive paper in the same straight line, polishing by going back and forth over a fixed distance, polishing by rotating in the same direction, or polishing by contacting in various directions. The degree of polishing can be determined, for example, while observing the surface condition. In the case of reciprocating polishing, for example, reciprocating is preferably performed 1 to 300 times, more preferably 2 to 200 times, and even more preferably 3 to 50 times. The surface of the sheet-like molded body may be polished in two separate polishing steps. For example, the first polishing step may be performed using abrasive paper having a larger average grain size of abrasive grains, and the second polishing step may be performed using abrasive paper having a smaller average grain size of abrasive grains than that of the first polishing step.

[0098] (Step 3) In step 3, as described above, an adhesive is applied to the surface of the cured product such as the sheet-like molded product obtained in step 2. In the present invention, the adhesive to be applied is preferably an acrylic adhesive having a reactive double bond as described above. In the present manufacturing method, it is preferable to allow the applied adhesive to penetrate into the thermal conductive layer, but it is preferable that the adhesive penetrates into the thermal conductive layer simply by applying the adhesive. However, it is not necessary for the applied adhesive to penetrate into the thermal conductive layer.

[0099] The adhesive may be diluted with a diluent and applied to the surface of the sheet-shaped molded body as a diluted adhesive solution. Diluting the adhesive with a diluent makes it easier for the adhesive to soak into the thermal conductive layer. The diluent is not particularly limited as long as it is a liquid at 25°C and 1 atm, has solubility or compatibility with the adhesive, and is a component that volatilizes when dried as described below, but an organic solvent is preferably used.

[0100] The organic solvent used is not particularly limited, but examples thereof include ketone compounds such as acetone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbon compounds such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, tripropylene glycol monomethyl ether, and polyethylene glycol monoethyl ether; ester compounds such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; and aliphatic hydrocarbon compounds such as hexane, octane, and decane. From the viewpoint of properly penetrating the adhesive into the thermally conductive layer by spray application as described below, it is preferable to use an organic solvent that does not evaporate too quickly, such as cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, or polyethylene glycol monoethyl ether. In addition to the above organic solvents, it is preferable to further contain an organic solvent having a boiling point lower than these, specifically, methyl ethyl ketone, methyl isobutyl ketone, hexane, ethyl acetate, butyl acetate, toluene, etc.

[0101] The dilution concentration by the diluent is not particularly limited, but it is preferable to adjust the solid content concentration of the adhesive to, for example, 5% by mass or more and 50% by mass or less, preferably 8% by mass or more and 35% by mass or less, and more preferably 10% by mass or more and 25% by mass or less. When the solid content concentration is 5% by mass or more, it is possible to prevent heating more than necessary during drying, and a predetermined amount of adhesive can be appropriately soaked into the heat conductive layer together with the organic solvent. In addition, by setting the solid content concentration to 50% by mass or less, the basis weight does not become more than necessary, and the adhesive can be appropriately soaked into the heat conductive layer because the viscosity can be adjusted to an easy-to-suck viscosity. The amount of adhesive that soaks into the heat conductive layer can be adjusted by the viscosity, solid content concentration, type of solvent, etc. For example, when it is desired to increase the amount of adhesive that soaks, it is preferable to adjust the solid content concentration to a high concentration with a low viscosity. When it is desired to reduce the adhesive material that soaks, it is preferable to set the solid content concentration to a low concentration with a high viscosity.

[0102] The method of applying the adhesive is not particularly limited, and a known application method may be adopted, but spray application is preferred. By performing spray application, the basis weight is not more than necessary, and the adhesive is easily permeated into the heat conductive layer. In addition, by performing spray application and suppressing the amount of application, it is possible to provide a portion with an adhesive layer and a portion without an adhesive layer on the surface of the heat conductive layer. In addition, when performing spray application, it is preferable to spray apply an adhesive containing a fast-drying organic solvent such as ethyl acetate and a slow-drying organic solvent such as polyethylene glycol monoethyl ether or propylene glycol monomethyl ether acetate. More specifically, by including a slow-drying organic solvent, the organic solvent is prevented from volatilizing too much when the adhesive discharged from the spray is applied to the surface of the heat conductive layer, so that the adhesive is easily permeated into the heat conductive layer. On the other hand, by including a fast-drying solvent, it is preferable to adjust the viscosity to be suitable for spraying.

[0103] The applied adhesive may then be dried to volatilize the diluent. The drying temperature may be at a temperature at which the reaction of the reactive double bonds of the adhesive does not substantially proceed, for example, 80° C. or less, preferably 70° C. or less, and more preferably 60° C. or less. The drying temperature is not particularly limited in terms of its lower limit, and may be about room temperature, for example, 20° C. or more, but from the viewpoint of shortening the drying time, it is preferably 30° C. or more, more preferably 40° C. or more, and even more preferably 45° C. or more. The drying time may be a time sufficient for substantially all of the diluent contained in the applied adhesive to be evaporated, for example, 1 minute or more, preferably 2 minutes or more, and more preferably 3 minutes or more. The drying time is not particularly limited, but is preferably short from the viewpoint of workability, for example, 24 hours or less, preferably 3 hours or less, and more preferably 1 hour or less.

[0104] [Uses of thermal conductive sheets] The thermally conductive sheet is interposed between a heat generating body and a heat sink, and transfers heat generated by the heat generating body to the heat sink by thermal conduction, and dissipates the heat from the heat sink. The thermally conductive sheet is used in electronic equipment applications, semiconductor applications, and the like, and is preferably used in semiconductor applications. In semiconductor applications, the thermally conductive sheet may be used in any manner, but is preferably called TIM1 and used in applications where it is directly applied to semiconductor chips such as silicon dies, for example, between a semiconductor chip and a heat spreader. Also, called TIM2, it is preferably used in applications that are not directly applied to semiconductor chips, in which case the thermally conductive sheet may be used, for example, between a heat spreader and a cooling unit such as a heat sink or heat pipe. In addition to the above, the thermally conductive sheet may be used between various electronic components that generate heat and heat dissipation bodies such as heat spreaders, heat sinks, heat pipes, heat pumps, and metal casings of electronic devices. The thermally conductive sheet is preferably used by being placed between two components (adherends) such as a heat sink or a heat generator, and is preferably used in a state in which it is in close contact with each component (adherend) and compressed. The thermally conductive sheet of the present invention may be used in a temperature range described below in a state where it is adhered to an adherend via an adhesive layer. When the thermally conductive sheet is actually used, the thermally conductive sheet may be heated, for example, in a range of 60°C to 180°C, preferably in a range of 70°C to 150°C. The thermally conductive sheet of the present invention may be one whose adhesion is improved by being used under such an environment. EXAMPLES

[0105] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0106] The measurement and evaluation methods in the present examples are as follows.

[0107] [A / B ratio] A droplet of the adhesive coating solution prepared in the same manner as the adhesive used in each Example and Comparative Example was applied to a gold-plated stainless steel plate, and the plate was thoroughly dried after application to volatilize the solvent and form an acrylic adhesive layer on the plate. The drying was performed by leaving the plate coated with the adhesive in an 80°C environment for 15 minutes. The acrylic adhesive layer formed on the plate was analyzed by Raman analysis, and the A / B value was determined using the following device and under the following measurement conditions. -1 The intensity is "A" and the wave number is 1724.4 cm -1 The strength was rated as "B". (Equipment used) "inVia Qontor" manufactured by Renishaw (Measurement conditions) Laser power: 50 Accumulation count: 1 time Laser wavelength: 785nm Grating: 1200l / mm Magnification: 50x Focus: Adjust to the sample surface on which the acrylic adhesive layer is formed.

[0108] [Thermal resistance value] The thermal resistance value was measured by the following method using a thermal resistance measuring device as shown in FIG. Specifically, for each sample, a test piece S measuring 30 mm×30 mm was prepared for this test. Then, each test piece S was attached onto a copper block 22 with a measurement surface of 25.4 mm×25.4 mm and a side surface covered with a heat insulating material 21, and sandwiched between an upper copper block 23, and a load of 10 psi was applied by a load cell 26. Here, the lower copper block 22 was in contact with a heater 24. The upper copper block 23 was also covered with a heat insulating material 21 and connected to a heat sink 25 equipped with a fan. Next, the heater 24 was heated to 80° C., and 10 minutes after the temperature reached a substantially steady state, the temperature (θ j0 ), the temperature of the lower copper block 22 (θ j1 ) and the amount of heat generated by the heater (Q) were measured, and the thermal resistance of each sample was calculated using the following formula (1). At the same time as measuring the thermal resistance, the thickness of the thermally conductive sheet at the time of measuring the thermal resistance was also measured. Thermal resistance=(θ j1 -θ j0 ) / Q... Equation (1) In formula (1), θ j1 is the temperature of the lower copper block 22, θ j0 is the temperature of the upper copper block 23, and Q is the amount of heat generated.

[0109] The same measurements were performed by changing the pressure applied by the load cell 26 to 20 psi, 30 psi, and 40 psi, and the results are shown in Table 2. The thermal resistance value at a pressure of 20 psi was calculated as the rate of change in thermal resistance, which was calculated based on the thermal resistance value of a blank thermal conductive sheet (100%). The blank was a thermal conductive sheet having the same configuration except that it did not have an adhesive layer.

[0110] [Tensile elongation at break, tensile elongation at break, and tensile strength at break] The thermally conductive sheet was cut into a dumbbell shape No. 8 as specified in JIS K6251: 2010. Using this as a sample, a tensile test was performed twice in the MD direction at 25°C using a tensile tester (product name "MAX-1KN", manufactured by Japan Measurement Systems Co., Ltd.) in accordance with JIS K7161, and the average values ​​of these measurements were taken as the tensile breaking elongation, tensile breaking elongation percentage, and tensile breaking strength, respectively.

[0111] [Die shear strength] Two thermally conductive sheets of 3 mm×3 mm obtained in each Example and Comparative Example were prepared, and then one of the two thermally conductive sheets, thermally conductive sheet 11, was placed on nickel-plated copper plate 10 having an outer dimension of 50 mm×50 mm and a thickness of 2 mm, as shown in Fig. 2, and silicon die 12 having a dimension of 3 mm×3 mm and a thickness of 600 μm was placed on thermally conductive sheet 11. Then, thermally conductive sheet 11 was pressed in the thickness direction at a pressure of 20 psi for 720 seconds in a room temperature environment to bond thermally conductive sheet 11 to nickel-plated copper plate 10 and silicon die 12, thereby obtaining a measurement sample 15. Thereafter, using a die shear tester ("Dage-S4000", manufactured by Nordson Corporation) in a 25°C environment, the height of the tip of the tool 17 was adjusted to 300 μm above the surface of the thermally conductive sheet 11. Next, the tool 17 was applied to the silicon die 12 along the shear direction S at a speed of 150 μm / s, and the load required to break the joint was determined as the die shear strength (B1).

[0112] In addition, a measurement sample was obtained from the other thermally conductive sheet in the same manner as above, except that the sheet was pressed in the thickness direction at a pressure of 20 psi for 3,600 seconds in an 80°C environment, and then the die shear strength (B2) of the sample was measured in the same manner as above.

[0113] The ratios of the tensile breaking strength and die shear strength (B1 / A, B2 / A) measured by the above method were calculated. The failure mode during the die shear strength (B2) measurement was confirmed, and those that showed cohesive failure were marked with "O".

[0114] [Rework Test] The thermally conductive sheets of 25.4 mm x 25.4 mm obtained in each Example and Comparative Example were attached under a load of 20 psi for 1 minute in a room temperature (25°C) environment, and then evaluated whether they could be peeled off by holding one side of one end with wide tweezers ("MEISTER tweezers ARG-SA", AS ONE Corporation). The evaluation criteria are as follows. (Evaluation Criteria) A: It was possible to peel it off. B: Peeling was successful, but some deformation occurred. C: It could not be peeled off and was torn off.

[0115] [Adhesion test] The thermally conductive sheets of 25.4 mm x 25.4 mm obtained in each Example and Comparative Example were placed between the heating element and the heat sink, and after applying pressure at a load of 20 psi for 60 minutes in an 80°C environment, the presence or absence of peeling was evaluated when the gap between the heating element and the heat sink was expanded to 110% of the initial thickness to simulate warping. The evaluation criteria were as follows. (Evaluation Criteria) A: No peeling occurred. B: Peeled off.

[0116] The following components were used as raw materials for the thermally conductive sheet. (Polymer composition) Curable silicone: An addition reaction type organopolysiloxane consisting of an alkenyl group-containing organopolysiloxane as the base agent and a hydrogen organopolysiloxane as the curing agent (however, it contains a catalytic amount of platinum catalyst). (Volatile substances) n-Decyltrimethoxysilane

[0117] (Thermal conductive filler) Aluminum oxide 1: Spherical, average particle size (D50) = 3 μm, aspect ratio 1.0 Aluminum oxide 2: Polyhedral shape, average particle size (D50) = 0.5 μm, aspect ratio 1.0 Aluminum: Spherical, average particle size (D50) = 3 μm, aspect ratio 1.0 to 1.5 Graphitized carbon fiber: average fiber length (arithmetic mean) 85 μm, diameter 10 μm, aspect ratio 8.5, thermal conductivity 900 W / m K Scaly boron nitride: average particle size (D50) = 50 μm, aspect ratio 20-50, thermal conductivity 200 W / m K Flake graphite powder: average particle size (D50) = 15 μm, aspect ratio 10, thermal conductivity 550 W / m K

[0118] (Adhesive) Adhesive 1: An adhesive whose main adhesive component is an acrylic polymer whose main component is a structural unit derived from 2-ethylhexyl acrylate and has hydroxyl groups, carboxyl groups, and vinyl groups on the side chains. A / B=0.588 Adhesive 2: An adhesive whose main adhesive component is an acrylic polymer whose main component is a structural unit derived from 2-ethylhexyl acrylate and has hydroxyl groups, carboxyl groups, and vinyl groups on the side chains. A / B=0.405 Adhesive 3: An acrylic adhesive not containing a reactive double bond (manufactured by Soken Chemical Co., Ltd., "SK1720"). A / B=0.138 Adhesive 4: Acrylic adhesive not having a reactive double bond (manufactured by Soken Chemical Co., Ltd., "1604N"). A / B=0.138 Adhesive 5: Silicone adhesive (Dow Toray Co., Ltd., "DOWSIL 7646 Adhesive") *100 parts by mass of a diluted solution of the adhesive diluted with ethyl acetate to a solid content concentration of 33% by mass was further diluted with 120 parts by mass of propylene glycol monomethyl ether acetate (solvent) to prepare a coating solution with a solid content concentration of 15% by mass, which was used in each of the Examples and Comparative Examples.

[0119] [Example 1] A mixed composition was obtained by mixing the components according to Recipe 1 in Table 1 for 50 minutes at 25°C using a planetary mixer. The mixed composition was then poured into a mold set to a thickness sufficiently greater than that of the thermally conductive sheet, and a magnetic field of 8T was applied in the thickness direction to orient the carbon fibers and flake graphite in the thickness direction, followed by heating at 80°C for 8 hours for primary curing of the curable silicone, thereby obtaining a block-shaped oriented molded product. Next, the block-shaped oriented molded body was sliced ​​into a sheet having a thickness of about 120 μm using a shear blade to obtain a sheet-shaped molded body with exposed carbon fibers, which was then heated at 150° C. for 6 hours for secondary curing. Next, the sheet-like molded body was polished back and forth 25 times with coarse abrasive paper A (grain size #800) whose average abrasive grain size (D50) was 20 μm, and then further polished back and forth 10 times with coarse abrasive paper B (grain size #4000) whose average abrasive grain size (D50) was 3 μm.

[0120] The adhesive 1 coating solution was sprayed onto both surfaces of the obtained sheet-like molded body, adjusting the discharge rate so that the amount of the coating would be the amount listed in Table 1 after drying, and then dried at 50°C for 3 minutes to obtain a thermally conductive sheet having an adhesive layer on both surfaces of the thermally conductive layer. It was confirmed that there were fine bubbles inside the thermally conductive layer, and that the acrylic adhesive had permeated into the fine bubbles near both surfaces. The filling rate of the thermally conductive filler in the thermally conductive layer was 64.0%, and the anisotropic filler was oriented in the thickness direction.

[0121] [Example 2] The same procedure as in Example 1 was carried out, except that the type of adhesive was changed as shown in Table 2.

[0122] [Examples 3 and 4] The same procedure as in Example 1 was carried out, except that the type and compounding ratio of the adhesive were changed as shown in Table 2, and the spray application conditions were changed so that the basis weight of the adhesive layer after drying was as shown in Table 2.

[0123] [Example 5] According to the formulation 2 in Table 1, each component was mixed at 25°C for 50 minutes using a planetary mixer to obtain a mixed composition. The mixed composition was applied in one direction on a base film made of polyethylene terephthalate (PET) at 25°C using a bar coater as an application applicator. The anisotropic filler was oriented such that the long axis direction was along the application direction, the short axis direction was in one direction along the sheet surface direction, and along a direction perpendicular to the application direction. Next, the applied mixed composition was heated at 80°C for 8 hours to harden the liquid composition, thereby obtaining a primary sheet having a thickness of 2 mm.

[0124] Both sides of each of the obtained primary sheets were irradiated with a VUV irradiation device (product name Excimer MINI, manufactured by Hamamatsu Photonics) at room temperature (25°C) in the atmosphere with an integrated light dose of 20 mJ / cm on the surface of the primary sheet. 2 VUV was irradiated under the condition of. Next, 100 sheets of the VUV-irradiated primary sheet were stacked and pressed with a roller at a pressure of 1.6 kgf / 50 mm in an environment of 25 ° C. to obtain a laminated block. The obtained laminated block was sliced ​​with a cutter blade parallel to the stacking direction and perpendicular to the direction along which the long axis of the scale-like filler was aligned, to obtain a sheet-like molded body with a thickness of 2 mm for each unit layer and a sheet thickness of about 0.30 mm. In the sheet-like molded body, the anisotropic filler was oriented in the thickness direction. Thereafter, the sheet-like molded body was further heated at 150 ° C. for 6 hours to be secondary cured. Thereafter, the same procedure as in Example 1 was carried out, except that the weight per unit area of ​​the adhesive after drying was changed as shown in Table 2, and the block-shaped oriented molded body was sliced ​​into a sheet having a thickness of about 300 μm, to obtain a thermally conductive sheet having an acrylic adhesive layer on both surfaces of the thermally conductive layer. There were no fine bubbles inside the thermally conductive layer, and it was not possible to confirm that the acrylic adhesive had penetrated into the fine bubbles. The filling rate of the thermally conductive filler in the thermally conductive layer was 70.2%, and the anisotropic filler was oriented in the thickness direction.

[0125] [Comparative Example 1] The same procedure as in Example 1 was carried out, except that the type of adhesive was changed as shown in Table 2, and the spray application conditions were changed so that the basis weight of the adhesive layer after drying was as shown in Table 2.

[0126] [Comparative Example 2] The same procedure as in Example 1 was carried out, except that the type of adhesive was changed as shown in Table 2, and the adhesive layer was provided by screen printing.

[0127] [Reference example 1] The same procedure as in Example 1 was carried out, except that the adhesive coating liquid was not applied to the sheet-shaped molded body.

[0128] [Reference example 2] The same procedure as in Example 5 was carried out, except that the adhesive coating liquid was not applied to the sheet-shaped molded body.

[0129] [Table 1] *The values ​​for each component are parts by mass for each formulation. *The sheet hardness is a value measured for the cured products obtained from Formulations 1 and 2 in each Example and Comparative Example.

[0130] [Table 2]

[0131] As is clear from the above examples, the thermally conductive sheet satisfying the requirements of the present invention had excellent reworkability because its adhesive strength was below a certain value at room temperature. Moreover, the adhesive strength of the sheet improved when heated, and exceeded a certain value at high temperatures, demonstrating excellent adhesion. In contrast, the thermally conductive sheet produced in Comparative Example 1 had an adhesive strength above a certain value at room temperature, so it was unable to exhibit excellent reworkability, and the thermally conductive sheet was torn during the rework test. Also, the thermally conductive sheet produced in Comparative Example 2 had an adhesive strength below a certain value in a heated state, so it was unable to exhibit excellent adhesion, and peeled off from the adherend during the adhesion test.

Claims

1. A thermally conductive sheet comprising a thermally conductive layer including a polymer matrix and a thermally conductive filler, and an adhesive layer provided on at least one surface of the thermally conductive layer, A thermally conductive sheet in which a tensile breaking strength A [mN / mm] of the thermally conductive sheet, an initial adhesive strength B1 [MPa] of the adhesive layer measured after the thermally conductive sheet is pressurized at a load of 20 psi for 12 minutes in an environment of 25°C, and an adhesive strength B2 [MPa] of the adhesive layer measured after the thermally conductive sheet is pressurized at a load of 20 psi for 60 minutes in an environment of 80°C satisfy the relationship of the following formula (1). [0010]

2. The thermally conductive sheet according to claim 1 , wherein the adhesive layer is formed of an acrylic adhesive.

3. the polymer matrix is ​​made of a rubber or a gel; 3. The thermally conductive sheet according to claim 1, wherein the thermally conductive sheet has a tensile breaking strength of 15 mN / mm or more and 60 mN / mm or less.

4. the polymer matrix is ​​made of a rubber or a gel; The thermally conductive sheet according to claim 1 or 2, wherein the thermally conductive sheet has a tensile elongation at break of 10% or more.

5. The thermally conductive sheet according to claim 1 or 2, wherein the polymer matrix is ​​an organopolysiloxane.

6. The thermally conductive sheet according to claim 1 , wherein the thermally conductive layer contains an anisotropic filler oriented in a thickness direction of the thermally conductive layer.

7. The thermally conductive sheet according to claim 1 or 2, wherein a surface of the thermally conductive layer is a sliced ​​surface.

Citation Information

Patent Citations

  • Thermally conductive sheet and heat dissipation device using the thermally conductive sheet