Manufacturing method of oil absorbing material
By processing raw cotton into small lumps using a fiber opening machine and storing them in non-woven bags, the method enhances oil absorption performance, addressing the limitations of previous cotton-based materials.
Patent Information
- Application Number
- JP2023060231
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing oil-absorbing materials using cotton fibers housed in non-woven bags, such as those made from unused fiber cotton, fallen cotton, or raw cotton, suffer from poor oil absorption performance due to short fiber length and lack of fiber intertwining, resulting in inadequate oil absorption capabilities.
A method involving passing raw cotton through a fiber opening machine to create small cotton lumps, which are then stored in a non-woven fabric bag, utilizing a spreading machine with specific spike pin configurations to achieve optimal fiber separation and density for improved absorption.
The resulting oil-absorbing material exhibits enhanced oil absorption rates, retention, and speed, making it effective for absorbing various oils, including cooking oil, machine oil, and marine spills.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an oil-absorbing material having excellent oil absorption performance such as oil absorption rate. [Background technology]
[0002] Oil absorbents in which cotton (cotton fibers) are stored in a nonwoven bag have been known for some time. For example, Patent Document 1 discloses an oil absorbent in which unused cotton fibers are stored in a nonwoven bag. Here, unused cotton fibers refer to waste fibers and the like generated during spinning (see the Basic Policy (Basic Policy on Promoting the Procurement of Eco-Friendly Goods, etc.) established based on the Law on Promoting the Procurement of Eco-Friendly Goods, etc. by the State, etc. (Green Purchasing Law)). Patent Document 2 also discloses an oil absorbent in which unbleached cotton is stored in a nonwoven bag. Here, it is described that it is preferable to use waste cotton (unbleached cotton that has not been put through a carding machine) as the unbleached cotton.
[0003] However, unused cotton fibers and fallen cotton fibers have a short fiber length and little intertwining between the fibers, so there is a drawback that an oil absorbent material with good oil absorption performance cannot be obtained. For this reason, it is possible to use raw cotton instead of unused cotton fibers and fallen cotton fibers, but the raw cotton is too compressed, so an oil absorbent material with good oil absorption performance cannot be obtained. It is also possible to use a fiber web, fiber sliver, or nonwoven fabric made by passing raw cotton through a carding machine to open it, but since the fibers are little intertwined and not bulky, an oil absorbent material with good oil absorption performance cannot be obtained.
[0004] [Patent Document 1] JP 2011-72929 A [Patent Document 2] JP 2007-7529 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have been conducting research into obtaining an oil-absorbing material using cotton, and have found that small pieces of cotton before being passed through a carding machine from raw cotton have relatively good oil-absorbing properties. The present invention is based on this finding. Therefore, the object of the present invention is to obtain an oil-absorbing material having good oil-absorbing properties. [Means for solving the problem]
[0006] The present invention relates to a method for producing an oil-absorbing material, which comprises the steps of passing a cotton lump such as raw cotton through a fiber opener to obtain small cotton lumps, and storing the small cotton lumps in a nonwoven fabric bag. Here, "raw cotton" refers to cotton in a packed and compressed state. The "fiber opener" is a machine in which a cylinder has a number of metallic spike pins on its surface and rotates. Therefore, when a cotton lump is fed to the fiber opener at a low speed, the cotton lump is scraped off and torn by the spike pins, so that the cotton lump can be divided into small cotton lumps. The spike pins are regularly planted on the cylinder surface, and the interval between adjacent spike pins is about 2 to 4 cm in the circumferential direction of the cylinder and about 1 to 2 cm in the width direction of the cylinder.
[0007] In the present invention, first, a cotton lump is prepared. Raw cotton is suitable as the cotton lump. Specifically, raw cotton packed and transported from a production area, or unbleached raw cotton packed and transported after only bleaching treatment, etc. are used. In addition to raw cotton, cotton products such as cotton nonwoven fabrics can also be used. The cotton lump may contain a small amount of other fibers than cotton fibers. Then, the cotton lump is put into a fiber spreader. Specifically, the cotton lump is fed to a feed roller provided just before the fiber spreader, and the cotton lump is passed through the fiber spreader. Since the diameter of the feed roller is smaller than the diameter of the cylinder of the fiber spreader and the rotation speed of the feed roller is slower than the rotation speed of the cylinder of the fiber spreader, the cotton lump is scraped off and torn by the spike pins of the cylinder, the cotton lump is divided, and discharged from the fiber spreader as small cotton lumps. The diameter of the cylinder is preferably about 5 to 20 times the diameter of the feed roller. The rotation speed of the cylinder is preferably about 100 to 1000 times that of the feed rollers. The diameter of the cylinder is preferably about 30 to 100 cm, and the rotation speed of the cylinder is preferably about 300 to 900 rpm.
[0008] The cotton mass may be passed through the opener multiple times. That is, the cotton mass discharged from the opener may be passed through the opener once or twice more. When the mass is passed through the opener multiple times, the apparent density gradually decreases. However, since it is an opener, there is a limit, and unlike when the mass is passed through a carding machine, the individual cotton fibers do not become separated, but the state of small cotton masses is maintained. In the present invention, the upper limit is about 10 times through the opener, and passing the mass through the opener more than this is not rational.
[0009] The apparent density of the cotton lumps obtained through the opener is 0.0089 to 0.0136 g / cm 3 It is preferable that the apparent density of the cotton slug is about this range. It has been found that the cotton slug has good oil absorption performance. The apparent density is measured and calculated by the following measuring method. (1) Weigh out 1 g of cotton lumps and gently place them evenly into a 100 mL beaker [PYREX (registered trademark) manufactured by Iwaki Glass Co., Ltd. (now ACG Technoglass)], being careful not to crush the cotton lumps. (2) Gently place a piece of filter paper (Advantec No. 2), which has been cut into a circle to fit the inner diameter of the beaker, on top of the small piece of cotton inside the beaker. (3) Gently place a 10 g weight on top of the filter paper so that the filter paper is horizontal. (4) Read the scale on the filter paper according to the graduations on the beaker and calculate the volume of the cotton ball (X cm 3 ) (5) The weight of the cotton lump (1 g) is divided by the volume of the cotton lump (X cm3) to obtain the apparent density (g / cm 3 )
[0010] The obtained cotton lumps are placed in a nonwoven fabric bag to prepare an oil absorbent material. As the nonwoven fabric constituting the bag, a conventionally known nonwoven fabric is used. In particular, it is preferable to adopt a nonwoven fabric having excellent oil permeability, for example, a low basis weight (10 to 20 g / m 2 It is preferable to use a spunbonded nonwoven fabric that is thin (about 0.1 to 0.3 mm) and has high strength. In addition, the constituent fibers of the spunbonded nonwoven fabric are preferably thermoplastic long fibers such as polypropylene. This is because the mouth of the bag can be sealed by heat welding. A method for storing the cotton lump in a nonwoven bag is to prepare a nonwoven bag with an open mouth, put the cotton lump in through the mouth, and then seal the mouth. Specifically, two sheets of nonwoven fabric are stacked and heat-sealed on three sides, the cotton lump is put in through the mouth that is not heat-sealed, and the mouth is heat-sealed to seal it. Alternatively, one sheet of nonwoven fabric may be bent into a cylinder, both ends are stacked and heat-sealed, the lower end of the cylinder is heat-sealed, the cotton lump is put in through the mouth of the upper end of the cylinder, and the mouth is heat-sealed to seal it.
[0011] The oil-absorbing material obtained by the method according to the present invention is used to absorb and recover edible oil or machine oil used and discharged from homes, restaurants, factories, etc. It is also used to absorb and recover oil spilled on the sea due to ship accidents, etc. It is also used to absorb and dispose of various other types of oil. Effect of the Invention
[0012] The oil-absorbing material obtained by the method according to the present invention has the advantage of exhibiting good oil-absorbing performance since it is made of small cotton lumps obtained by a specific method. EXAMPLES
[0013] Example 1 The raw cotton was passed through a fiber spreader (Op-200 manufactured by Yamato Kiko Co., Ltd., cylinder diameter: 38 cm, feed roller diameter: 5 cm) once to obtain an apparent density of 0.0136 g / m 3 The cotton lumps were obtained. The operating conditions of the opening machine were a feed roller rotation speed of 2 rpm and a cylinder rotation speed of 580 rpm. On the other hand, a polypropylene long fiber spunbond nonwoven fabric (Mitsui Chemicals PS-103, basis weight 16 g / m 2 Two pieces of 7.5 cm square cotton (0.18 mm thick) were cut out, overlapped on all four sides, and three of the sides were heat sealed using a heat sealer (FI-300, manufactured by Fuji Impulse Sealer Co., Ltd.) to create a bag. 0.5 g of cotton lump was gently placed into the bag from the opening of the bag that was not heat sealed, taking care not to crush the cotton lump. The opening of the bag was then heat sealed, and the cotton lump was placed in a nonwoven bag to obtain an oil absorbent material. The width of the heat sealed part was 0.5 cm.
[0014] Example 2 Cotton raw material was passed through a fiber spreader (Op-200 manufactured by Yamato Kiko Co., Ltd.) 10 times to obtain an apparent density of 0.0089 g / m 3 The cotton lumps were then placed in nonwoven bags in the same manner as in Example 1 to obtain oil absorbent materials. The operating conditions of the fiber spreader were the same as in Example 1, and the same conditions were used for all 10 runs.
[0015] Example 3 Unbleached raw cotton was passed through a fiber spreader (Op-200 manufactured by Yamato Kiko Co., Ltd.) once to obtain an apparent density of 0.0133 g / m 3 The cotton lumps were placed in nonwoven bags in the same manner as in Example 1 to obtain oil absorbent materials. The operating conditions of the fiber spreader were the same as in Example 1.
[0016] Example 4 Unbleached raw cotton was passed through a fiber spreader (Op-200 manufactured by Yamato Kiko Co., Ltd.) 10 times to obtain an apparent density of 0.0091 g / m 3 The cotton lumps were then placed in nonwoven bags in the same manner as in Example 1 to obtain oil absorbent materials. The operating conditions of the fiber spreader were the same as in Example 1, and the same conditions were used for all 10 runs.
[0017] Comparative Example 1 Apparent density 0.0164g / m 3 0.5 g of the raw cotton was placed in the nonwoven fabric bag used in Example 1 as it was, without being passed through a fiber opener, to obtain an oil absorbent material.
[0018] Comparative Example 2 Apparent density 0.0175g / m 3 0.5 g of the unbleached raw cotton was placed in the nonwoven bag used in Example 1 as it was, without being passed through a fiber opener, to obtain an oil absorbent material.
[0019] Comparative Example 3 Four plies of cotton nonwoven fabric (Unitika Co., Ltd., cotton spunlace nonwoven fabric "CO50S / A01") cut into 5.0 cm squares were stacked and placed in the nonwoven fabric bag used in Example 1 to obtain an oil absorbent material.
[0020] The oil absorbing properties of the oil absorbing materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were measured by the following methods. [Oil absorption rate (g / g)] (1) Measure the weight W0 (g) of the oil-absorbing material. (2) Float the oil absorbent material on the oil surface and leave it to soak in the oil for 5 minutes. (3) After 5 minutes, remove from oil and hang for 3 minutes. (4) After 3 minutes, measure the weight W1 (g) of the oil-absorbing material. (5) The value calculated using the formula [(W1-W0) / W0] is the oil absorption rate (g / g).
[0021] [Retention rate (g / g)] In measuring the above oil absorption rate (g / g), the weight of the oil that has flowed off the oil-absorbent material in the process (3) above, W2 (g), is measured, and the value calculated using the formula {(W1-W0) / [(W1-W0)+W2]} is the retention rate (g / g).
[0022] [Oil absorption speed (g / 10s)] (1) Measure the weight W3 (g) of the oil-absorbing material. (2) Float the oil absorbent material on the surface of the oil and leave it to soak in the oil for 10 seconds. (3) After 10 seconds, remove it from the oil and measure the weight W4 (g) of the oil-absorbing material. (4) The value calculated using the formula (W4-W3) is the oil absorption rate (g / 10s).
[0023] [Edible oil absorption performance] The oil absorbing performance of the oil absorbing materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was evaluated for olive oil (extra virgin olive oil "BOSCO" manufactured by Nisshin Oillio Group, Ltd.) and the results are shown in Table 1.
[0024] [Table 1] ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━ Oil absorption rate (g / g) Retention rate (g / g) Oil absorption rate (g / 10s) ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━ Example 1 28.8 0.57 27.0 Example 2 39.6 0.63 33.5 Example 3 29.5 0.55 31.0 Example 4 41.6 0.64 36.9 Comparative Example 1 21.9 0.45 24.5 Comparative Example 2 19.4 0.47 24.2 Comparative Example 3 7.5 0.40 14.4 ━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━━
[0025] As is clear from the results in Table 1, the oil absorbent material obtained by the method of the embodiment has a higher oil absorption rate, a higher retention rate, and a higher oil absorption rate than the oil absorbent material obtained by the method of the comparative example, and is therefore superior in oil absorption performance.
[0026] [Machine oil absorption performance] The oil absorption performance of the oil absorbent materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was evaluated using high vacuum pump oil (high vacuum pump oil "Neovac MR-100" manufactured by MORESCO Corporation). The results (however, the oil absorption rate was not evaluated) are shown in Table 2.
[0027] [Table 2] ━━━━━━━━━━━━━━━━━━━━━━━━━ Oil absorption rate (g / g) Retention rate (g / g) ━━━━━━━━━━━━━━━━━━━━━━━━━ Example 1 28.9 0.58 Example 2 43.6 0.64 Example 3 28.1 0.62 Example 4 41.1 0.67 Comparative Example 1 22.5 0.50 Comparative Example 2 21.4 0.50 Comparative Example 3 7.9 0.41 ━━━━━━━━━━━━━━━━━━━━━━━━━
[0028] As is clear from the results in Table 2, the oil absorbent material obtained by the method of the embodiment has a higher oil absorption rate and higher retention rate than the oil absorbent material obtained by the method of the comparative example, and is therefore superior in oil absorption performance.
Claims
1. The method for producing an oil absorbent material comprises the steps of: passing a cotton lump through a fiber opener to obtain small cotton lumps; and storing the small cotton lumps in a nonwoven fabric bag.
2. 2. The method for producing an oil-absorbing material according to claim 1, wherein the cotton mass is passed through a fiber opener a number of times.
3. 2. The method for producing an oil-absorbing material according to claim 1, wherein the cotton mass is raw cotton or a cotton product.
4. The apparent density of the cotton blob is 0.0089 to 0.0136 g / cm 3 The method for producing the oil absorbing material according to claim 1,