Aluminum fin material
By integrating a copper-nonreactive antifungal agent in the lubricating film layer of aluminum fin materials, the antifungal and lubricating properties are maintained, addressing cost and corrosion issues, and ensuring effective heat exchange performance.
Patent Information
- Application Number
- JP2023060290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing aluminum fin materials for heat exchangers face challenges in maintaining antifungal performance while minimizing the addition of fungicidal agents, which can increase costs and compromise the functionality of other layers, and there is a risk of copper corrosion due to elution of antifungal agents during use.
Incorporating an antifungal agent into the lubricating film layer that does not react with copper, along with a hydrophilic and optionally a corrosion-resistant film layer, to achieve effective antifungal and lubricating properties without increasing the overall agent content, thereby preventing copper corrosion.
The solution maintains excellent antifungal and lubricating properties while preventing copper corrosion, ensuring adhesion with copper tubes and preserving heat exchange performance, reducing the risk of refrigerant leakage and copper discoloration.
Smart Images

Figure 2024147341000001 
Figure 2024147341000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum fin material, and more particularly to an aluminum fin material that is suitable for use in heat exchangers of air conditioners and the like. [Background technology]
[0002] Heat exchangers are used in products in various fields, such as room air conditioners, packaged air conditioners, freezer showcases, refrigerators, oil coolers, and radiators. Aluminum and aluminum alloys, which have excellent thermal conductivity, workability, and corrosion resistance, are generally used as materials for heat exchanger fins. Plate fin and plate and tube heat exchangers have a structure in which aluminum fin materials are arranged in parallel at close intervals.
[0003] When the surface temperature of the aluminum fin material of a heat exchanger falls below the dew point, condensation water adheres to it. If the surface of the aluminum fin material becomes wet due to the influence of this condensation water, mold and mildew are likely to occur.
[0004] In response to this, Patent Document 1 discloses an aluminum fin material for heat exchangers in which a substance having antifungal properties is contained in a first coating film (corrosion-resistant film layer) made of a corrosion-resistant resin and a second coating film (hydrophilic film layer) made of a hydrophilic resin, which is said to provide excellent hydrophilicity and immediate and long-lasting antifungal properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-186149 A Summary of the Invention [Problem to be solved by the invention]
[0006] In order to impart excellent press workability to aluminum fin materials for heat exchangers such as that described in Patent Document 1, a third coating film made of polyethylene glycol (PEG), that is, a lubricating coating layer, is sometimes provided.
[0007] However, when a further functional layer such as a lubricating coating layer is provided on the layer containing a substance having antifungal properties, it is necessary to increase the amount of antifungal agent added in order to obtain the same antifungal performance as when the functional layer is not provided. Increasing the amount of antifungal agent added leads to a decrease in the content of components necessary for the functional layer to perform its original function. In addition, the cost increases with the increase in the amount of antifungal agent added.
[0008] Therefore, an object of the present invention is to provide an aluminum fin material that has a lubricating coating layer and has both good properties due to the functional layer and good mold resistance. [Means for solving the problem]
[0009] In response to the above problem, the inventors have conducted further research and have come up with the idea that by incorporating an antifungal agent into the lubricating coating layer, good antifungal properties can be achieved without increasing the amount of the agent added. Since only a small amount of antifungal agent is required, the lubricating coating layer and the hydrophilic coating layer, which are functional layers, can provide good properties such as lubricity and hydrophilicity.
[0010] However, it was found that when a mildewproofing agent is contained in the lubricating coating layer, the mildewproofing agent is easily dissolved during use of the aluminum fin material, and easily corrodes the copper components of the heat exchanger. From this, it was thought that it is also important to use a mildewproofing agent that does not react with copper, and this led to the completion of the present invention.
[0011] The present invention relates to the following [1] to [9]. [1] An aluminum plate having a hydrophilic coating layer and a lubricating coating layer in this order on at least one surface of the aluminum plate, the lubricating coating layer containing a fungicide, and after immersing copper in 50 mL of ion-exchanged water containing 0.5 g of the fungicide at room temperature for 14 days, the infrared absorption spectrum of the copper surface shows a peak in the range of 2800 to 3000 cm originating from a C-H bond. -1 The aluminum fin material has a peak intensity of 0.15 or less. [2] The content of the antifungal agent in the lubricating coating layer is 0.35 mg / dm 2 The aluminum fin material described in [1] above. [3] The aluminum fin material according to [1] or [2], wherein the concentration of the antifungal agent in the lubricating coating layer is 5 to 65 mass %. [4] The aluminum fin material described in [1] or [2] above, wherein the lubricating coating layer further contains an antibacterial agent. [5] The coating amount of the lubricating coating layer is 1.0 to 10 mg / dm 2 The aluminum fin material according to [1] or [2] above. [6] The coating amount of the hydrophilic coating layer is 0.1 to 25 mg / dm 2 The aluminum fin material according to [1] or [2] above. [7] The aluminum fin material described in [1] or [2], further comprising a corrosion-resistant coating layer between the aluminum plate and the hydrophilic coating layer. [8] The aluminum fin material described in [7] above, wherein the corrosion-resistant coating layer contains an antibacterial agent. [9] The coating amount of the corrosion-resistant coating layer is 3 to 60 mg / dm 2 The aluminum fin material according to [7] above. Effect of the Invention
[0012] The aluminum fin material according to the present invention has a lubricating coating layer, and has good properties due to the functional layer and good antifungal properties. In addition, since the corrosion of copper caused by the antifungal agent can be prevented, even if the antifungal agent dissolves during use of the aluminum fin material, it does not corrode the copper members of the heat exchanger. As a result, adhesion with the copper tube can be maintained, and a decrease in heat exchange performance can be suppressed. In addition, leakage of the internal refrigerant due to holes in the copper tube and changes in appearance due to discoloration of the copper members can be prevented. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the aluminum fin material according to the present invention will be described in detail. Note that the symbol "to" indicating a numerical range is used to mean that the numerical range includes the numerical ranges before and after the symbol as the lower and upper limits.
[0014] <Aluminum fin material> The aluminum fin material (hereinafter sometimes simply referred to as "fin material") of this embodiment comprises an aluminum plate and, on at least one surface of the aluminum plate, a hydrophilic coating layer and a lubricating coating layer, in that order.
[0015] (Lubricant coating layer, anti-mold agent) The antifungal agent is contained in the lubricating coating layer. Then, copper is immersed in 50 mL of ion-exchanged water containing 0.5 g of the antifungal agent at room temperature for 14 days. In the infrared absorption spectrum (IR spectrum) of the copper surface, a peak in the range of 2800 to 3000 cm originating from a C-H bond is observed. -1 The intensity of the peak observed at 1000 nm is 0.15 or less. This means that it can be determined that the aluminum fin material has the necessary non-reactivity with copper in this embodiment, and even if the antifungal agent elutes from the lubricating coating layer when the aluminum fin material is in use, corrosion of the copper member of the heat exchanger due to the antifungal agent can be suppressed. The intensity of the peak is preferably 0.1 or less, more preferably less than 0.1, and even more preferably 0.05 or less. The lower limit of the intensity of the peak is not particularly limited, and may be 0, that is, the peak may not be detected.
[0016] Alternatively, simply, if no discoloration or other changes are visually observed on the copper surface before and after contacting the copper with the antifungal agent, it can be determined that the intensity of the above peak is likely to be 0.15 or less.
[0017] The mold targeted by the antifungal agent in this specification refers to multicellular fungi of about 2 to 10 μm in size, and examples thereof include Penicillium niger, Aspergillus niger, Aspergillus niger, Trichophyton niger, and the like, but are not limited to these.
[0018] The antifungal agent is not particularly limited as long as it does not react with copper, and examples thereof include imidazoles, thiazoles, isothiazolines, pyridines, triazines, aldehydes, phenols, piguanides, nitriles, halogens, anilides, disulfides, thiocarbamates, quaternary ammonium salts, organometallics, alcohols, carboxylic acids, natural products, etc. Among these, imidazoles and thiazoles are preferred. Also preferred is an antifungal agent made of silver ions and zeolite. The antifungal agent may be one type only, or two or more types may be included. The antifungal agent may also have other properties such as antibacterial properties.
[0019] More preferred specific examples of the antifungal agent that does not react with copper include Amolden D-CL50P (product name), Amolden NBP-8 (product name), Amolden PPC (product name), Amolden V-GPZ (product name), Amolden V-CHG (product name), and Amolden MCD (product name), all manufactured by Yamato Chemical Industry Co., Ltd., and Zeomic manufactured by Sinanen Zeomic Co., Ltd. Among these, Amolden MCD is preferred.
[0020] The content of the antifungal agent in the lubricating coating layer is 0.35 to 6.0 mg / dm 2 Here, from the viewpoint of obtaining a better antifungal property, the content of the antifungal agent is preferably 0.35 mg / dm 2 More than 0.50 mg / dm 2 More preferably, 0.70 mg / dm 2The content of the antifungal agent is more preferably 6.0 mg / dm from the viewpoint of obtaining better lubricity as a lubricating coating layer. 2 Less than 5.9 mg / dm 2 In addition, since the fin material according to the present embodiment can contain a fungicide in the lubricating coating layer, the content of the fungicide is set to the above-mentioned 0.35 mg / dm2, which is lower than the conventional amount. 2 In terms of degree, a sufficiently good antifungal effect can be obtained.
[0021] The concentration of the antifungal agent in the lubricating coating layer is preferably 5 to 65% by mass. From the viewpoint of obtaining better antifungal properties, the concentration of the antifungal agent is preferably 5% by mass or more, more preferably 15% by mass or more. Also, from the viewpoint of the lubricating coating layer exhibiting better lubricity, the concentration of the antifungal agent is preferably 65% by mass or less, more preferably 60% by mass or less.
[0022] The lubricating coating layer is a layer formed on the surface of the hydrophilic coating layer, and is intended to obtain good processability by increasing the lubricity of the fin material surface. The resin constituting the lubricating coating layer can be a conventionally known resin that enhances lubricity. This reduces the friction coefficient of the fin material surface, making it lubricating, and improves press formability when processing the fin material into a fin.
[0023] Examples of resins that enhance lubricity include resins having hydrophilic groups, such as hydroxyl groups, carboxyl groups, sulfonic acid groups, and polyether groups.
[0024] Examples of resins having hydroxyl groups include polyethylene glycol (PEG) and polyvinyl alcohol (PVA). Examples of resins having carboxyl groups include polyacrylic acid (PAA). Examples of resins having hydroxyl groups and carboxyl groups include carboxymethyl cellulose (CMC). Examples of resins having sulfonic acid groups include sulfoethyl acrylate. Examples of resins having polyether groups include polyethylene glycol (PEG) and modified compounds thereof. Examples of modified compounds of polyethylene glycol (PEG) include urethane modified PEG and ether modified PEG. In addition to these, copolymers of two or more types of monomers having hydrophilic groups can also be applied.
[0025] In addition to the above resin and antifungal agent, the lubricating coating layer may contain other optional components within the scope of the present invention, such as various water-based solvents and paint additives for improving the coatability, workability, and physical properties of the coating layer. Examples of paint additives include water-soluble organic solvents, crosslinking agents, surfactants, surface conditioners, wetting and dispersing agents, antisettling agents, antioxidants, defoamers, antifouling agents, rust inhibitors, and antibacterial agents. Among these, it is preferable to include an antibacterial agent. These paint additives may be included in one type or in two or more types.
[0026] The bacteria targeted by the antibacterial agent in this specification are fungi of about 0.5 to 5 μm in size that are composed of a single cell and reproduce by division, and examples thereof include, but are not limited to, Escherichia coli, Salmonella, Staphylococcus aureus, and Helicobacter pylori.
[0027] The antibacterial agent contained in the lubricating coating layer is preferably one that does not react with copper, similar to the antifungal agent. For example, imidazole-based, thiazole-based, isothiazolin-based, pyridine-based, triazine-based, aldehyde-based, phenol-based, piguanide-based, nitrile-based, halogen-based, anilide-based, disulfide-based, thiocarbamate-based, quaternary ammonium salt-based, organometallic, alcohol-based, carboxylic acid-based, natural, etc. are listed. Among them, imidazole-based and organometallic are preferred. The antibacterial agent may be one type or two or more types.
[0028] A more preferred example of the antibacterial agent that does not react with copper is Amolden AG-S1000 (product name) manufactured by Yamato Chemical Industry Co., Ltd. When the lubricating coating layer contains an antibacterial agent in addition to the antifungal agent, the content of the antibacterial agent in the lubricating coating layer is 0.0001 mg / dm 2 Super 15mg / dm 2 Here, from the viewpoint of obtaining good antibacterial properties, the content of the antibacterial agent is preferably 0.0001 mg / dm 2 More than 0.0005 mg / dm is preferred. 2 More preferably, 0.001 mg / dm 2 More preferably, the content of the antibacterial agent is 15 mg / dm2 or more, from the viewpoint of obtaining better lubricity as the lubricating coating layer. 2 Less than 10 mg / dm 2 The following is more preferred:
[0029] The lubricating coating layer can be formed by applying a coating composition containing a resin that enhances lubricity, such as a resin having a hydroxyl group, onto the hydrophilic coating layer and solidifying it by drying or the like. The lubricating coating layer is preferably the outermost layer.
[0030] The amount of the lubricating coating layer is 0.5 to 15 mg / dm 2 is preferable, and 1.0 to 10 mg / dm 2 Here, from the viewpoint of obtaining sufficient lubricity, the coating amount of the lubricating coating layer is more preferably 0.5 mg / dm 2More than 1.0 mg / dm 2 More preferably, 1.5 mg / dm 2 More preferably, 2.0 mg / dm 2 On the other hand, from the viewpoint of obtaining good lubricity, the coating amount of the lubricating coating layer is preferably 15 mg / dm 2 Less than 10 mg / dm 2 The following is more preferred:
[0031] The thickness and amount of the lubricating coating layer can be adjusted by the concentration of the coating composition used to form the lubricating coating layer, the selection of the bar coater number, and the like.
[0032] 《Hydrophilic film layer》 The hydrophilic coating layer is a coating layer that imparts hydrophilicity to the surface of the fin material, and contains a conventionally known hydrophilic resin. The hydrophilic resin may contain one type of resin or two or more types of resins as long as it has a hydrophilic group. Examples of the hydrophilic group include a hydroxyl group, a carboxyl group, a sulfonic acid group, and a polyether group.
[0033] Examples of those having a hydroxyl group include polyethylene glycol (PEG) and polyvinyl alcohol (PVA). Examples of those having a carboxyl group include polyacrylic acid (PAA). Examples of those having a hydroxyl group and a carboxyl group include carboxymethyl cellulose (CMC). Examples of those having a sulfonic acid group include sulfoethyl acrylate. Examples of those having a polyether group include polyethylene glycol (PEG) and modified compounds thereof.
[0034] Among these, from the viewpoint of more suitably expressing the desired hydrophilicity even when a lubricating coating layer is formed on the surface of the hydrophilic coating layer, the hydrophilic resin is preferably one containing a sulfonic acid group or a polyether group, i.e., one containing an ether bond, more preferably one containing a sulfonic acid group and an ether bond, and particularly preferably an acrylic acid resin containing a sulfonic acid group and an ether bond.
[0035] The acrylic acid resin containing sulfonic acid and ether bonds is an acrylic acid resin containing an unsaturated double bond group and a sulfonic acid group, and is typically 3-allyloxy-2-hydroxy-1-propanesulfonic acid sodium salt (HAPS), but other examples include acrylamidomethylpropanesulfonic acid, etc. The acrylic acid resin containing sulfonic acid and ether bonds is not limited to these.
[0036] In addition to the above, the hydrophilic resin may be a copolymer of two or more monomers having a hydrophilic group. For example, a copolymer of acrylic acid and sulfoethyl acrylate may be used. The copolymer may be an alternating copolymer, a block copolymer, a graft copolymer, a random copolymer, or the like, and the arrangement of the monomers is not particularly limited.
[0037] It is preferable that the hydrophilic coating layer further contains a surfactant in addition to the hydrophilic resin. This allows for both better hydrophilicity and workability due to the lubricating coating layer formed on the hydrophilic coating layer. This is believed to be due to the exposure action of the surfactant.
[0038] The surfactant may be any of anionic, cationic and nonionic types, but nonionic surfactants are preferred from the viewpoint of ease of dispersion in the hydrophilic coating layer.
[0039] Examples of nonionic surfactants include ethylenediamine polyoxypropylene-polyoxyethylene condensates, polyoxyethylene sorbitan monolaurate, polyoxyethylene polyoxypropylene block polymers, polyoxyethylene sorbitan monostearate, and the like.
[0040] The hydrophilic coating layer can be formed by applying a coating composition containing a hydrophilic resin onto an aluminum plate, a base treatment layer, or a corrosion-resistant coating layer, as described below, and solidifying the composition by drying or the like.
[0041] In addition to the hydrophilic resin and surfactant, the hydrophilic coating layer may contain other optional components within the range that does not impair the effects of the present invention. Examples of the optional components include various water-based solvents and paint additives for improving the coatability, workability, and physical properties of the coating layer. Examples of paint additives include water-soluble organic solvents, crosslinking agents, surface conditioners, wetting and dispersing agents, antisettling agents, antioxidants, defoamers, rust inhibitors, antibacterial agents, antifungal agents, etc. These paint additives may be contained alone or in combination of two or more.
[0042] The thickness and amount of the hydrophilic coating layer can be adjusted by the concentration of the coating composition used to form the hydrophilic coating layer, the selection of the bar coater number, and the like.
[0043] The amount of the hydrophilic coating layer is 0.1 to 28 mg / dm 2 is preferable, and 0.1 to 25 mg / dm 2 Here, from the viewpoint of obtaining better hydrophilicity, the coating amount of the hydrophilic coating layer is more preferably 0.1 mg / dm 2 More than 0.3 mg / dm 2 More preferably, 0.5 mg / dm 2 The above is even more preferable. From the viewpoint of obtaining good coating workability when forming the hydrophilic coating layer, and from the viewpoint of exhibiting the other functions of a coating layer having another function, such as a corrosion-resistant coating layer, formed on the aluminum plate side of the hydrophilic coating layer, the coating amount of the hydrophilic coating layer is 28 mg / dm 2 Less than 25 mg / dm 2 The following is more preferred:
[0044] <Corrosion-resistant coating layer> The corrosion-resistant coating layer is a layer formed on the aluminum plate mainly to enhance the corrosion resistance of the aluminum plate. Therefore, it is preferable to further provide a corrosion-resistant coating layer between the aluminum plate and the hydrophilic coating layer. When a base treatment layer described later is formed on the surface of the aluminum plate, the corrosion-resistant coating layer is preferably provided between the base treatment layer and the hydrophilic coating layer. In addition, when a coating layer having another function such as an anti-frost coating layer is formed on the aluminum plate or on the base treatment layer, the corrosion-resistant coating layer may be formed on the coating layer.
[0045] The corrosion-resistant coating layer preferably contains a hydrophobic resin, and can be formed, for example, by applying a coating composition containing a hydrophobic resin onto an aluminum plate, an undercoat treatment layer, or a coating layer such as an anti-frost coating layer, and then solidifying it by drying or the like.
[0046] The corrosion-resistant coating layer makes it difficult for moisture such as condensation water, oxygen, chloride ions and other ionic species to penetrate the aluminum plate, thereby suppressing corrosion of the aluminum plate and the production of odorous aluminum oxides.
[0047] The hydrophobic resin in the corrosion-resistant coating layer may be a conventionally known resin, such as polyester, polyolefin, melamine, epoxy, urethane, or acrylic resin, or a mixture of two or more of these resins.
[0048] In addition to the above, the corrosion-resistant coating layer may contain other optional components within the range that does not impair the effects of the present invention. Examples of optional components include various water-based solvents and paint additives for improving the paintability, workability, and physical properties of the coating. Examples of paint additives include water-soluble organic solvents, crosslinking agents, surfactants, surface conditioners, wetting and dispersing agents, antisettling agents, antioxidants, defoamers, rust inhibitors, and antibacterial agents. Among these, it is preferable to include an antibacterial agent. These paint additives may be included in one type or in two or more types.
[0049] The antibacterial agent contained in the corrosion-resistant coating layer may be a conventionally known antibacterial agent, such as imidazole-based, thiazole-based, isothiazolin-based, pyridine-based, triazine-based, aldehyde-based, phenol-based, piguanide-based, nitrile-based, halogen-based, anilide-based, disulfide-based, thiocarbamate-based, quaternary ammonium salt-based, organometallic, alcohol-based, carboxylic acid-based, natural, etc. In addition, since a hydrophilic coating layer and a lubricating coating layer are further formed on the surface of the corrosion-resistant coating layer, an antibacterial agent that reacts with copper can be used, unlike the antibacterial agent contained in the lubricating coating layer.
[0050] The amount of the corrosion-resistant coating layer is not particularly limited, but is preferably 3 to 60 mg / dm 2 Here, from the viewpoint of imparting sufficient corrosion resistance to the aluminum plate, the coating amount of the corrosion-resistant coating layer is preferably 3 mg / dm 2 On the other hand, even if the coating amount of the corrosion-resistant coating layer is increased, the obtained corrosion resistance effect reaches a plateau, and from the viewpoint of suppressing the decrease in the heat exchange efficiency of the fin material, the coating amount of the corrosion-resistant coating layer is preferably 60 mg / dm 2 The following is preferred:
[0051] The thickness of the corrosion-resistant coating layer is preferably 0.05 μm or more from the viewpoint of obtaining good corrosion resistance, and is preferably 15 μm or less from the viewpoints of good film-forming properties, reduced defects such as cracks, low heat transfer resistance of the corrosion-resistant coating layer, and good heat exchange efficiency of the fin. The thickness and amount of the corrosion-resistant coating layer can be adjusted by the concentration of the coating composition used to form the corrosion-resistant coating layer, the selection of the bar coater number, and the like.
[0052] In the fin material, the total thickness of the lubricating coating layer, the hydrophilic coating layer, and the lubricating coating layer is preferably 5 μm or less in order to suppress a decrease in the heat exchange efficiency of the fin material.
[0053] Aluminum plate The aluminum plate is a concept that includes a plate made of aluminum and a plate made of an aluminum alloy, and an aluminum plate that has been conventionally used for aluminum fin materials can be used. As the aluminum plate, 1000 series aluminum as specified in JIS H 4000:2014 is preferable because of its excellent thermal conductivity and workability. More specifically, aluminum alloy numbers 1050, 1070, and 1200 are more preferable as the aluminum plate. However, the above description does not exclude the use of 2000 series to 9000 series aluminum alloys or other aluminum plates as the aluminum plate.
[0054] The aluminum plate is made to have a desired thickness depending on the application and specifications of the fin material. For fin materials for heat exchangers, the thickness is preferably 0.08 mm or more, more preferably 0.1 mm or more, from the viewpoint of fin strength, etc. On the other hand, the thickness is preferably 0.3 mm or less, more preferably 0.2 mm or less, from the viewpoint of processability into fins and heat exchange efficiency, etc.
[0055] At least one surface of the aluminum plate is provided with a hydrophilic coating layer and a lubricating coating layer in this order, but a hydrophilic coating layer and a lubricating coating layer may be provided on both surfaces. Even if a hydrophilic coating layer and a lubricating coating layer are provided on both surfaces, the configuration of the coating layers on both surfaces does not necessarily have to be the same.
[0056] << Base treatment layer >> If desired, a primer layer can be provided on the aluminum plate. When the fin material has a corrosion-resistant coating layer, it is preferable to provide a primer layer between the aluminum plate and the corrosion-resistant coating layer. By providing a base treatment layer, the corrosion resistance of the aluminum plate can be improved, and when the fin material is provided with a corrosion-resistant coating layer, the adhesion between the aluminum plate and the corrosion-resistant coating layer can be improved.
[0057] The undercoat treatment layer may be any layer that can impart corrosion resistance to the aluminum plate, and may be any layer known in the art, such as a layer made of an inorganic oxide or an inorganic-organic composite compound. As the inorganic material constituting the inorganic oxide or inorganic-organic composite compound, chromium (Cr), zirconium (Zr) or titanium (Ti) is preferred as the main component.
[0058] The layer made of an inorganic oxide that serves as the undercoat treatment layer can be formed, for example, by subjecting an aluminum plate to a chromate phosphate treatment, a zirconium phosphate treatment, a zirconium oxide treatment, a chromate chromate treatment, a zinc phosphate treatment, a titanic acid phosphate treatment, etc. However, the type of inorganic oxide is not limited to those formed by these treatments.
[0059] The layer made of an inorganic-organic composite compound that serves as the undercoat treatment layer can be formed, for example, by subjecting an aluminum plate to coating-type chromate treatment, coating-type zirconium treatment, etc. Specific examples of such inorganic-organic composite compounds include, for example, acrylic-zirconium composites.
[0060] The thickness of the undercoat treatment layer is not particularly limited and may be set appropriately, but the amount of the coating per unit area should be 1 to 100 mg / m2 in terms of metal (Cr, Zr, Ti). 2 The thickness of the film is preferably 1 to 100 nm. The deposition amount and film thickness of the undercoat treatment layer can be adjusted by adjusting the concentration of the chemical conversion treatment solution used in forming the undercoat treatment layer and the film formation treatment time.
[0061] Before forming the primer layer, the surface of the aluminum plate may be degreased in advance using an alkaline degreasing solution, which improves the reactivity of the primer treatment and also improves the adhesion of the formed primer layer.
[0062] <Characteristics of aluminum fin material> In the aluminum fin material according to this embodiment, even if a mildewproofing agent with a small average particle size is used, the mildewproofing agent is contained in the lubricating coating layer, so that the aluminum fin material has both good hydrophilicity and mildewproofing properties, and does not corrode copper even during use of the fin material.
[0063] The hydrophilicity of the fin material can be evaluated by the following method. The fin material is immersed in a water tank filled with tap water for 8 hours, and then dried at 80°C for 16 hours, which constitutes one cycle. This immersion and drying process is repeated 14 times. After 10 cycles and 14 cycles, the material is returned to room temperature, and approximately 2 μL of ion-exchanged water is dropped onto the fin material surface, and the contact angle of the droplet is measured with a contact angle meter (Kyowa Interface Science Co., Ltd.: CA-05 type). The contact angle is measured three times for each sample, and the average value is taken as the contact angle. The contact angle of the droplet is judged to be good if at least one of the contact angles after 10 cycles and after 14 cycles is 45° or less, and it is preferable that both are 45° or less. The contact angle is more preferably 40° or less, and even more preferably 30° or less. The smaller the contact angle, the better, but it is usually 5° or more.
[0064] The mold resistance of fin material can be evaluated by a mold halo test based on the mold resistance test method (Halo method) (revised in 2007) set forth in the appendix to the "Terminology Usage Standards for the Suppression of Bacteria, etc." set forth by the National Household Electrical Appliances and Materials Fair Trade Council (public corporation). If no halo width is observed against Aspergillus niger, Penicillium niger, or Aspergillus niger, it is determined to have good mold resistance.
[0065] The antibacterial properties of the fin material can be evaluated using the fin material in an antibacterial evaluation test against Escherichia coli using the film adhesion method in accordance with JIS Z 2801:2012. The antibacterial activity value is calculated by the above evaluation test, and when the value is 2.0 or more, it is determined that the antibacterial property is good.
[0066] The lubricity, i.e., processability, of a fin material can be evaluated using the coefficient of friction. Specifically, a load of 200 g is applied to the fin material using a Bowden testing machine, and the material is slid back and forth three times while changing the position, and the average value is taken as the coefficient of friction. A friction coefficient of less than 0.20 is deemed to be good lubricity, and a friction coefficient of less than 0.15 is preferable, and less than 0.10 is more preferable. The smaller the friction coefficient, the better, but it is usually 0.20 or more.
[0067] <Method of manufacturing aluminum fin material> An example of a manufacturing method for the aluminum fin material according to this embodiment will be described, but the present invention is not limited to this embodiment, and other manufacturing methods can also be used as long as they do not interfere with the effects of this embodiment. In addition, the following example is an explanation of the case where a base treatment layer, a corrosion-resistant film layer, a hydrophilic film layer, and a lubricating film layer are formed in this order on the surface of an aluminum plate, but the formation of the base treatment layer and the corrosion-resistant film layer is optional. In addition, a film layer having another function may be further provided. In addition, as long as a lubricating film layer is formed on the surface of the hydrophilic film layer, the order of each of the other layers can be appropriately changed.
[0068] A base treatment layer is formed on the surface of an aluminum plate by a known method, and a corrosion-resistant coating layer and a hydrophilic coating layer are formed on the base treatment layer in this order by known methods.
[0069] Next, a coating composition containing a resin that enhances lubricity and a fungicide that does not react with copper is prepared as a coating composition for the lubricating coating layer, and the coating composition is applied to the surface of the hydrophilic coating layer, dried, and baked to form a lubricating coating layer. The coating composition may further contain other optional additives such as an antibacterial agent that does not react with copper and a surfactant.
[0070] The baking temperature is not particularly limited as long as the lubricating coating layer does not peel off, but is preferably 100° C. or higher, and more preferably 150° C. or higher. From the viewpoint of preventing oxidation of the resin of the lubricating coating layer, the baking temperature is preferably 250° C. or lower, and more preferably 200° C. or lower. The baking temperature is the temperature of the oven in which baking is performed.
[0071] The baking time is not particularly limited as long as the lubricating coating layer does not peel off, but is preferably 3 seconds or more, more preferably 5 seconds or more, and is preferably 30 seconds or less, more preferably 20 seconds or less, from the viewpoint of preventing oxidation of the resin of the lubricating coating layer.
[0072] The solvent for the coating composition is not particularly limited, and examples thereof include water, alcohol, ether, etc. Among these, water and alcohol are preferred, and as the alcohol, butanol, ethanol, etc. are preferred. The solvent may be used alone or in combination of two or more. For example, in the case of a mixed solvent of water and alcohol, it is preferable from the viewpoint of coatability that the amount of alcohol is 1 to 20 parts by mass per 100 parts by mass of water.
[0073] The aluminum fin material according to this embodiment has been described in detail above, but another aspect according to this embodiment is as follows. [1]' An aluminum plate having a hydrophilic coating layer and a lubricating coating layer on at least one surface of the aluminum plate, in this order; The lubricating coating layer contains a fungicide, After copper was immersed in 50 mL of ion-exchanged water containing 0.5 g of the antifungal agent at room temperature for 14 days, the infrared absorption spectrum of the copper surface showed a peak in the range of 2800 to 3000 cm originating from a C-H bond. -1 The aluminum fin material has a peak intensity of 0.15 or less. [2]' The content of the antifungal agent in the lubricating coating layer is 0.35 mg / dm 2 The aluminum fin material described in [1]' above. [3]' The aluminum fin material according to [1]' or [2]', wherein the concentration of the antifungal agent in the lubricating coating layer is 5 to 65 mass %. [4]' The aluminum fin material according to any one of [1]' to [3]' above, wherein the lubricating coating layer further contains an antibacterial agent. [5] The coating amount of the lubricating coating layer is 1.0 to 10 mg / dm2 The aluminum fin material according to any one of the above [1]' to [4]'. [6] The coating amount of the hydrophilic coating layer is 0.1 to 25 mg / dm 2 The aluminum fin material according to any one of the above [1]' to [5]'. [7]' The aluminum fin material according to any one of [1]' to [6]', further comprising a corrosion-resistant coating layer between the aluminum plate and the hydrophilic coating layer. [8]' The aluminum fin material according to [7]', wherein the corrosion-resistant coating layer contains an antibacterial agent. [9]' The coating amount of the corrosion-resistant coating layer is 3 to 60 mg / dm 2 The aluminum fin material according to [7]' or [8]'. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples, and can be practiced with modifications within the scope of the invention, all of which are included in the technical scope of the present invention.
[0075] Example 1 The aluminum plate used was an aluminum plate having a thickness of 0.1 mm and conforming to the alloy number 1070 standard specified in JIS H 4000: 2014. A primer layer was formed on one surface of the aluminum plate by phosphate chromate treatment. Next, a coating composition was prepared by dispersing the epoxy resin in ion-exchanged water, and the coating amount was adjusted to 10 mg / dm 2 The coating was applied to the surface of the undercoat treatment layer using a bar coater so as to obtain a coating having a corrosion-resistant coating layer. After drying, the coating was baked to form a corrosion-resistant coating layer. Next, a coating composition was prepared by dispersing an acrylic sulfonic acid resin in ion-exchanged water, and the coating amount was set to 6 mg / dm 2 The coating was applied to the surface of the corrosion-resistant coating layer using a bar coater so as to obtain a hydrophilic coating layer by drying and baking the coating. Next, a coating composition was prepared by dispersing urethane-modified polyethylene glycol and a fungicide (Amolden MCD, manufactured by Yamato Chemical Industry Co., Ltd.) in ion-exchanged water, and the coating amount was 1.2 mg / dm 2 The lubricating coating layer was formed by applying the antifungal agent to the surface of the hydrophilic coating layer using a bar coater so that the antifungal agent was applied to the surface of the hydrophilic coating layer using a bar coater, drying the antifungal agent, and baking the antifungal agent at 180° C. for 10 seconds. The content and concentration of the antifungal agent in the lubricating coating layer are shown in Table 1. In this manner, an aluminum fin material was obtained.
[0076] Examples 2 and 3 An aluminum fin material was obtained in the same manner as in Example 1, except that the content and concentration of the antifungal agent in the lubricating coating layer were changed to the values shown in Table 1.
[0077] Examples 4 to 21 Aluminum fin material was obtained in the same manner as in Example 1, except that the coating amount of the corrosion-resistant coating layer and the coating amount of the hydrophilic coating layer were changed to the values shown in Table 1, and further, for the lubricating coating layer, an antibacterial agent (Amolden AG-S1000, manufactured by Yamato Chemical Industry Co., Ltd.) was added in the amount shown in Table 1, and the coating amount and the content and concentration of the antifungal agent were changed to the values shown in Table 1.
[0078] Comparative Example 1 In the same manner as in Example 1, a base treatment layer and a corrosion-resistant coating layer were formed on the surface of an aluminum plate. Next, a coating composition was prepared by dispersing an epoxy resin and a fungicide (Amolden MCD, manufactured by Yamato Chemical Industry Co., Ltd.) in ion-exchanged water, and the coating amount was set to 8 mg / dm 2 The hydrophilic coating layer was formed by applying the antifungal agent to the surface of the corrosion-resistant coating layer using a bar coater so that the antifungal agent was applied to the surface of the corrosion-resistant coating layer using a bar coater, drying the antifungal agent, and baking the antifungal agent to form the hydrophilic coating layer. The content and concentration of the antifungal agent in the hydrophilic coating layer are shown in Table 1. Next, a coating composition was prepared by dispersing urethane-modified polyethylene glycol in ion-exchanged water, and the coating amount was adjusted to 0.5 mg / dm 2After drying, the lubricating coating layer was baked at 180° C. for 10 seconds to form a lubricating coating layer. In this manner, an aluminum fin material was obtained.
[0079] 《Reference example 1》 In the same manner as in Example 1, a primer layer was formed on the surface of an aluminum plate. Next, a coating composition was prepared by dispersing an epoxy resin and zinc pyrithione (manufactured by Yamato Chemical Industry Co., Ltd., Amolden PT-50), which is an antifungal and antibacterial agent, in ion-exchanged water, and the coating amount was adjusted to 2 mg / dm 2 The coating was applied to the surface of the undercoat treatment layer using a bar coater so that the coating was as follows: after drying, the coating was baked to form a corrosion-resistant coating layer. The content and concentration of zinc pyrithione, which acts as a fungicide and antibacterial agent in the corrosion-resistant coating layer, are shown in Table 1. Note that since zinc pyrithione is both a fungicide and antibacterial agent, the antibacterial agent item is not listed in Table 1. Next, a coating composition was prepared by dispersing the epoxy resin in ion-exchanged water, and the coating amount was 4.3 mg / dm 2 The coating was applied to the surface of the corrosion-resistant coating layer using a bar coater so as to obtain a hydrophilic coating layer by drying and baking the coating. Next, a coating composition was prepared by dispersing urethane-modified polyethylene glycol in ion-exchanged water, and the coating amount was 1.3 mg / dm 2 After drying, the lubricating coating layer was baked at 180° C. for 10 seconds to form a lubricating coating layer. In this manner, an aluminum fin material was obtained.
[0080] [Table 1]
[0081] "evaluation" Copper reactivity of fungicides and antibacterial agents Copper cut to a length of 1 cm was immersed for 14 days in 50 mL of ion-exchanged water containing 0.5 g of the antifungal agent, antibacterial agent, or antifungal and antibacterial agent listed in Table 2 at room temperature. The copper surface was then washed with ion-exchanged water, dried, and measured with an infrared spectrophotometer (Nicolet IN10, manufactured by Thermo Fisher Scientific). In the obtained IR spectrum, the 2800 to 3000 cm -1 The peak observed in the graph was determined to be due to a C-H bond, and its intensity was calculated. The results are shown in Table 2. If the peak intensity was 0.15 or less, it was determined that the compound did not react with copper.
[0082] [Table 2]
[0083] The fungicide Amolden FS-300 (product name, manufactured by Yamato Chemical Industry Co., Ltd.) and zinc pyrithione, a fungicide and antibacterial agent, have been added to corrosion-resistant and hydrophilic coating layers in the past, but their peak strength exceeds 0.15 and they react with copper. Therefore, when they are added to the lubricating coating layer, which is the outer layer of the corrosion-resistant and hydrophilic coating layers, there is a concern that the corrosion of copper may occur during the use of aluminum fin materials, due to the ease of elution of the fungicide. On the other hand, the fungicides Amorden D-CL50, Amorden NBP-8, Amorden PPC, Amorden V-GPZ, Amorden V-CHG, and Amorden MCD (all product names, manufactured by Yamato Chemical Industry Co., Ltd.), the antibacterial agent Amorden AG-S1000 (product name, manufactured by Yamato Chemical Industry Co., Ltd.), and the fungicide and antibacterial agent Zeomic (product name, manufactured by Sinanen Zeomic Co., Ltd.) do not react with copper. Therefore, they can be added to the lubricating coating layer without worrying about copper corrosion during the use of aluminum fin materials.
[0084] ·Hydrophilicity The fin material was immersed in a water tank filled with tap water for 8 hours, and then dried at 80°C for 16 hours, which constituted one cycle. This immersion and drying process was repeated 14 times. After 10 cycles and 14 cycles, the material was returned to room temperature, and about 2 μL of ion-exchanged water was dropped onto the fin material surface, and the contact angle of the droplet was measured with a contact angle meter (Kyowa Interface Science Co., Ltd.: CA-05 type). The contact angle was measured three times for each sample, and the average value was taken as the contact angle. The results are shown in "hydrophilicity" in Table 1. If the contact angle after both 10 cycles and 14 cycles was 45° or less, it was judged to be very good, and the "evaluation" was rated "○". If at least one of the contact angles after 10 cycles and 14 cycles was 45° or less, it was judged to be pass, and the "evaluation" was rated "△". If both the contact angles after 10 cycles and 14 cycles were more than 45°, it was judged to be poor, and the "evaluation" was rated "×".
[0085] ·Mold and mildew resistant A mold halo test was conducted on the fin material based on the mold prevention test method (halo method) (revised in 2007) stipulated in the appendix of the "Standards for the Use of Terms Concerning the Inhibition of Bacteria, etc." by the National Household Electrical Appliances Fair Trade Council (public corporation). The results are shown in "Mold Prevention" in Table 1, and when no halo width was observed for Aspergillus niger, Penicillium niger, or Black Mold, the mold prevention was judged to be good and given a rating of "○."
[0086] ·Antibacterial The fin material was used to carry out an antibacterial evaluation test against Escherichia coli by a film adhesion method in accordance with JIS Z 2801:2012. The results are shown in "Antibacterial Property" in Table 1. An antibacterial activity value was calculated by such an evaluation test, and when the antibacterial activity value was 2.0 or more, the antibacterial property was judged to be good and marked with "○". When the antibacterial activity value was less than 2.0, the antibacterial property was judged to be poor and marked with "×". Note that, since no evaluation test was carried out for Examples 1 to 3 and Comparative Example 1, they are marked with "-" in Table 1.
[0087] ·Lubricity The lubricity of the fin material, i.e., the workability, was evaluated by the friction coefficient. The friction coefficient was measured by applying a load of 200 g to the fin material using a Bowden tester, sliding it back and forth three times while changing the position, and the average value was used. The results are shown in "Lubricity" and "Friction Coefficient (-)" in Table 1. If the friction coefficient is less than 0.15, it is judged to be very good, and the "Evaluation" is "○". If the friction coefficient is 0.15 or more and less than 0.20, it is judged to be good, that is, pass, and the "Evaluation" is "△". If the friction coefficient is 0.20 or more, it is poor, that is, fail. Since no evaluation test was performed in Comparative Example 1, it is marked as "-" in Table 1.
[0088] From the results in Table 1, all of the aluminum fin materials of Examples 1 to 21 contained an antifungal agent that does not react with copper in the lubricating coating layer, and while realizing good antifungal properties, they also had good hydrophilicity and lubricity. In contrast, the aluminum fin material of Comparative Example 1 contained an antifungal agent in the hydrophilic coating layer, but despite the content and concentration of the antifungal agent being higher than those of Examples 1 to 21, its antifungal properties were poor. Furthermore, in Comparative Example 1, the content and concentration of the antifungal agent were higher, which reduced the relative amount of hydrophilic resin. Therefore, the amount of hydrophilic coating was increased to 8 mg / dm 2 From these results, it can be seen that the aluminum fin materials of Examples 1 to 21 do not inhibit the good hydrophilicity of the hydrophilic coating layer by including an antifungal agent in the lubricating coating layer. Furthermore, the results of Examples 4 to 21 showed that by further adding an appropriate amount of an antibacterial agent that does not react with copper to the lubricating coating layer, an aluminum fin material that also had good antibacterial properties was obtained. From the above, it has been found that the aluminum fin material of this embodiment has both good hydrophilicity due to the hydrophilic coating layer, which is the functional layer, and good mold resistance, and does not corrode copper even when in use.
[0089] The aluminum fin material of Reference Example 1 is a conventional example in which zinc pyrithione, which has antifungal and antibacterial properties, is contained in the corrosion-resistant coating layer, and is an example that serves as an indicator of the antifungal and antibacterial properties and hydrophilicity of the hydrophilic coating layer. Although the aluminum fin material of Reference Example 1 showed good results in both antifungal and antibacterial properties, the inclusion of zinc pyrithione in the lubricating coating layer caused the aluminum in the aluminum fin material to corrode, and the corrosion-resistant coating layer was unable to provide the intended function of corrosion resistance.
Claims
1. An aluminum plate having a hydrophilic coating layer and a lubricating coating layer on at least one surface of the aluminum plate, in this order; The lubricating coating layer contains a fungicide, After copper was immersed in 50 mL of ion-exchanged water containing 0.5 g of the fungicide at room temperature for 14 days, the infrared absorption spectrum of the copper surface showed a peak in the range of 2800 to 3000 cm originating from a C—H bond. -1 The aluminum fin material has a peak intensity of 0.15 or less.
2. The content of the antifungal agent in the lubricating coating layer is 0.35 mg / dm 2 The aluminum fin material according to claim 1.
3. The aluminum fin material according to claim 1 or 2, wherein the concentration of the antifungal agent in the lubricating coating layer is 5 to 65 mass%.
4. The aluminum fin material according to claim 1 or 2, wherein the lubricating coating layer further contains an antibacterial agent.
5. The coating amount of the lubricating coating layer is 1.0 to 10 mg / dm 2 The aluminum fin material according to claim 1 or 2.
6. The coating amount of the hydrophilic coating layer is 0.1 to 25 mg / dm 2 The aluminum fin material according to claim 1 or 2.
7. The aluminum fin material according to claim 1 or 2, further comprising a corrosion-resistant coating layer between the aluminum plate and the hydrophilic coating layer.
8. The aluminum fin material according to claim 7, wherein the corrosion resistant coating layer includes an antibacterial agent.
9. The coating amount of the corrosion-resistant coating layer is 3 to 60 mg / dm 2 The aluminum fin material according to claim 7 .
Citation Information
Patent Citations
Aluminum fin material for heat exchanger
JP1996313191A
Fungicide
JP2002187803A
Surface-treated fin material for heat exchanger
JP2007268387A
Aluminum fin material for heat exchanger
JP2011214787A
Coating composition and aluminum fin material using the same
JP2012072336A