Method for estimating intensity of sludge-containing solidified body and method for managing quality of the same

The method estimates sludge-containing solidified material strength by mixing sludge and admixture, measuring hydration values, and using regression equations to address variability in hydration and aggregate content, ensuring accurate strength design and quality control.

JP2024147878APending Publication Date: 2024-10-17SHIMIZU CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023060581
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The variability in hydration degree and fine aggregate content of sludge affects the strength development of soil cement, making it difficult to accurately estimate and design the strength of sludge-containing solidified materials.

Method used

A method involving the preparation of a specimen by mixing standard sludge and an admixture at a predetermined ratio, determining compressive strength, measuring hydration calorific values, and using a multiple regression equation to estimate the compressive strength based on the mixing ratio of sludge and admixture.

Benefits of technology

Enables accurate estimation of the compressive strength of sludge-containing solidified materials, allowing for effective strength design and quality control, even with varying hydration activities and aggregate contents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147878000001_ABST
    Figure 2024147878000001_ABST
Patent Text Reader

Abstract

To provide a method for estimating the intensity of a sludge-containing solidified body which can precisely estimate the intensity of a sludge-containing solidified body, and a method for managing the quality of the solidified body.SOLUTION: The method according to the present invention includes the steps of: determining the compression intensity of a sample at a predetermined material age (Step S1); determining the intensity contribution rate of a reference sludge when a compression intensity is applied and the intensity contribution rate of a mixture material (Steps 2, 3); determining the respective accumulated heat generation amounts of a reference sludge and a sludge used for a sludge-containing solidified body as an estimation target, and determining the ratio of the accumulated heat generation amount of the reference sludge and the accumulated heat generation amount of the sludge (Steps S4 to S6); determining the intensity contribution rate of the sludge on the basis of the determined ratio of the accumulated heat generation amount and the intensity contribution rate of the reference sludge (Step S7); and estimating the compression intensity on the basis of the determined intensity contribution rate of the sludge, the intensity contribution rate of the mixture material, and the mixture ratio of the sludge and the mixture material (step S8).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for estimating the strength and a method for quality control of a sludge-containing solidified body such as soil cement using sludge. [Background technology]

[0002] In the past, one method of effectively utilizing concrete sludge generated during the treatment of returned concrete or the cleaning of ready-mix concrete trucks has been to dry and crush the sludge and reuse the resulting fine powder in concrete or soil cement. For example, the sludge can be reused as a substitute for cement in soil cement used in ground improvement work, earth retaining work, and backfill work.

[0003] On the other hand, a method for evaluating the quality of soil cement is known, as described in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-59851 Summary of the Invention [Problem to be solved by the invention]

[0005] However, depending on the age of the sludge before drying, the degree of hydration of the cement may differ, and depending on the amount of fine aggregate remaining in the sludge, the strength development may differ even when the same amount of dried sludge is added as a substitute for cement, which may make it difficult to design the strength of soil cement that uses sludge. Also, there are cases where strength development is insufficient when only dried sludge is added.

[0006] The present invention has been made in consideration of the above, and aims to provide a strength estimation method and quality control method for sludge-containing solidified body that can accurately estimate the strength of sludge-containing solidified body. [Means for solving the problem]

[0007] In order to solve the above problems and achieve the object, a method for estimating strength of a sludge-containing solidified body according to the present invention is a method for estimating the strength of a sludge-containing solidified body containing sludge and an admixture, and includes the steps of: preparing a specimen of a sludge-containing solidified body in which a predetermined standard sludge and the admixture are mixed in a predetermined ratio, and determining the compressive strength of the specimen at a predetermined material age; determining the strength contribution rate of the standard sludge and the strength contribution rate of the admixture in the compressive strength; and calculating the strength contribution rate of the standard sludge and the strength contribution rate of the admixture in the compressive strength. the step of measuring the heat release from hydration of each of the sludges and calculating an accumulated heat release up to an earlier material age than the above-mentioned material age; the step of calculating a ratio between the accumulated heat release of the standard sludge and the accumulated heat release of the sludge; the step of calculating a strength contribution rate of the sludge based on the calculated ratio of the accumulated heat release rates and the strength contribution rate of the standard sludge; and the step of estimating the compressive strength of the sludge-containing solidified body to be estimated based on the calculated strength contribution rate of the sludge, the strength contribution rate of the admixture, and the mixing ratio of the sludge and the admixture.

[0008] In addition, another method for estimating the strength of sludge-containing solidified material according to the present invention is characterized in that, in the above-mentioned invention, the compressive strength is estimated using a multiple regression equation in which the compressive strength is the objective variable and the mixing ratio of the sludge and the admixture is the explanatory variable.

[0009] In addition, the quality control method for sludge-containing solidified bodies of the present invention is a method for controlling the quality of sludge-containing solidified bodies formed by mixing soil material with a binder consisting of sludge and an admixture, and is characterized in having a step of estimating the compressive strength by the above-mentioned estimation method for sludge-containing solidified bodies, and a step of determining whether the estimated compressive strength satisfies specified design conditions. Effect of the Invention

[0010] According to the method for estimating strength of a sludge-containing solidified body of the present invention, there is provided a method for estimating the strength of a sludge-containing solidified body containing sludge and an admixture, comprising the steps of: preparing a specimen of the sludge-containing solidified body by mixing a prescribed standard sludge with the admixture in a prescribed ratio; determining the compressive strength of the specimen at a prescribed material age; determining the strength contribution rate of the standard sludge and the strength contribution rate of the admixture in the compressive strength; measuring the calorific value of hydration of the standard sludge and the sludge used in the sludge-containing solidified body to be estimated; and determining the compressive strength of the specimen at a prescribed material age. The method includes the steps of: calculating the accumulated heat generation amount up to an early material age prior to the age of sludge; calculating the ratio between the accumulated heat generation amount of the standard sludge and the accumulated heat generation amount of the sludge; calculating the strength contribution rate of the sludge based on the calculated ratio of the accumulated heat generation amounts and the strength contribution rate of the standard sludge; and estimating the compressive strength of the sludge-containing solidified body to be estimated based on the calculated strength contribution rate of the sludge, the strength contribution rate of the admixture, and the mixing ratio of the sludge and the admixture, thereby achieving the effect of being able to accurately estimate the strength of the sludge-containing solidified body.

[0011] In addition, according to another method for estimating the strength of sludge-containing solidified material of the present invention, the compressive strength is estimated using a multiple regression equation in which the compressive strength is the objective variable and the mixing ratio of the sludge and the admixture is the explanatory variable, thereby achieving the effect of easily estimating the compressive strength.

[0012] In addition, according to the quality control method for sludge-containing solidified bodies of the present invention, which is a method for controlling the quality of sludge-containing solidified bodies formed by mixing soil material with a binder consisting of sludge and an admixture, the method includes a step of estimating the compressive strength using the above-mentioned estimation method for sludge-containing solidified bodies, and a step of determining whether the estimated compressive strength satisfies specified design conditions, thereby achieving the effect of easily performing strength design and quality control of sludge-containing solidified bodies such as soil cement. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic flow diagram showing an embodiment of a method for estimating strength and a method for quality control of a sludge-containing solidified material according to the present invention. [Diagram 2] FIG. 2 is a table showing an example of mix conditions and compressive strength. [Diagram 3] FIG. 3 is a graph showing an example of the change over time in the calorific value of hydration of each dried sludge. [Figure 4] FIG. 4 is a table showing an example of the integrated calorific value of dried sludge. [Diagram 5] FIG. 5 is a table showing an example of the 28-day strength and estimated strength when using dried sludge and ground granulated blast furnace slag with different hydration activities from the base. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiment of the method for estimating strength and quality control of a sludge-containing solidified material according to the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the embodiment.

[0015] In this embodiment, the strength of soil cement (sludge-containing solidified body), which contains a binder made from dried sludge and admixtures and soil material, is estimated by a simple evaluation of the reactivity of dried sludge at the planning stage before construction is carried out at the actual site. By accurately estimating the developed strength at the planning stage, it is possible to appropriately design the strength of the soil cement. The admixture is assumed to be alkaline activated powder (for example, ground granulated blast furnace slag or fly ash). As dried sludge and alkaline activated powder are construction by-products, CO2 from the materials origin is not estimated. 2 This will result in zero emissions, which will also contribute to reducing the environmental impact.

[0016] 1, this embodiment is carried out in the procedure of steps S1 to S8. The process contents of each step will be described below.

[0017] First, in step S1, a blending test is performed by mixing the base dry sludge and alkaline activated powder in multiple (e.g., at least three) blending ratios. Specifically, a soil cement specimen is prepared by mixing a binder consisting of the base dry sludge and alkaline activated powder with water and moist soil (soil material), and the compressive strength of the specimen at a predetermined age is determined. The compressive strength is preferably determined at a material age of 28 days in a compressive strength test conforming to JIS A 1108. The base dry sludge corresponds to the standard sludge of the present invention, and it is preferable to use, for example, the dried sludge used at the construction site. The alkaline activated powder and moist soil are those actually used at the construction site.

[0018] In the next steps S2 and S3, the strength contribution ratios of the base dry sludge and the alkaline activated powder are calculated by multiple regression analysis. In this case, for example, the compressive strength at 28 days is used as the objective variable, and the mixing ratio of the base dry sludge and the mixing ratio of the alkaline activated powder are used as explanatory variables to calculate a multiple regression equation. The coefficients related to the explanatory variables correspond to the strength contribution ratios.

[0019] In the next step S4, the heat of hydration is measured for up to 12 hours using a conduction calorimeter. Specifically, the amount of heat generated by hydration when the base dry sludge and water are mixed in a predetermined weight ratio (for example, a 1:1 ratio) is measured using a conduction calorimeter, and the integrated heat generation amount from the start of measurement to a predetermined time (for example, about 12 hours to 3 days) is obtained. Meanwhile, in step S5, the integrated heat generation amount from the start of measurement to 12 hours is obtained in the same manner for dried sludge collected at a different time or from a different lot (hereinafter referred to as different lot dried sludge).

[0020] In the next step S6, the ratio of the integrated heat generation amount of the separate lot dried sludge to the integrated heat generation amount of the base dried sludge is calculated from the acquired integrated heat generation amounts.

[0021] In the next step S7, the strength contribution rate of the different lot of dried sludge is calculated by multiplying the ratio of the integrated heat generation amounts by the strength contribution rate of the base dried sludge.

[0022] In the next step S8, the compressive strength of the soil cement using the other lot of dried sludge and the alkaline activated powder is estimated from the strength contribution rate of the other lot of dried sludge and the strength contribution rate of the alkaline activated powder, and the strength design of the soil cement is performed based on this. Specifically, the compressive strength at 28 days is estimated using the strength contribution rate of the other lot of dried sludge as the coefficient of the explanatory variable (mixture ratio of base dried sludge) of the multiple regression equation obtained by the multiple regression analysis in the above steps S2 and S3. In this way, the compressive strength of the soil cement at medium to long-term ages can be easily and accurately estimated in a short time (for example, about 12 hours to several days) at an early age. This makes it possible to design the strength of the soil cement when dried sludge and alkaline activated powder with different hydration activities are used. In addition, the compressive strength can be applied to the quality control of soil cement production by routinely estimating the compressive strength for each lot of dried sludge.

[0023] When using this embodiment to evaluate and manage the quality of soil cement, the compressive strength is estimated using the above estimation method, and it is determined whether or not the estimated compressive strength meets the strength required for design (design conditions). This determination can be made in a short time before actual construction. If the result of this determination is that the strength required for design is met, it is evaluated as being of high quality, and construction is carried out using the considered mix, but if it is not met, the mix plan may be revised before actual construction. In this way, the quality of the soil cement can be easily managed.

[0024] (Example) In order to confirm the effect of the present invention, a laboratory blending test was carried out. Ground granulated blast furnace slag was used as the alkaline activated powder. First, a mix test was conducted using the binder with the composition shown in Figure 2 and local soil, and the compressive strength at 28 days was calculated. The mix conditions were dried sludge and ground granulated blast furnace slag as the binder, the water / binder ratio was 190%, and soil content was 72 mass% of the total. A soil cement specimen was prepared and a compressive strength test was conducted. The soil had a soil particle density of 2.69 g / cm3. 3 Sandy soil with a water content of 0.6% was used.

[0025] Next, the strength contribution ratios of the base dried sludge and ground granulated blast furnace slag were obtained by multiple regression analysis. As a result, the following multiple regression equation was obtained. In the following multiple regression equation, the coefficient value 0.0187 corresponds to the strength contribution ratio of the dried sludge, and the coefficient value 0.0731 corresponds to the strength contribution ratio of the ground granulated blast furnace slag.

[0026] [Compressive strength] = -1.096 + 0.0187 [proportion of dry sludge (mass%)] + 0.0731 [proportion of ground granulated blast furnace slag (mass%)] (1)

[0027] Next, heat of hydration measurements were carried out for the base dried sludge and two types of dried sludge A and B, which take longer to dry than the base dried sludge. The drying time is long for dried sludge A, followed by B. Figures 3 and 4 show the measurement results of the heat of hydration and the calculation results of the accumulated heat value. In Figure 4, the column for accumulated 12 hours shows the accumulated heat value from the start of measurement to 12 hours. Similarly, the columns for accumulated 1 day and accumulated 3 days show the accumulated heat value from the start of measurement to 1 day and the accumulated heat value from the start of measurement to 3 days, respectively. As shown in Figure 4, it can be seen that the longer the drying time of the dried sludge, the smaller the accumulated heat value.

[0028] Next, the ratio of the integrated heat generation of each dried sludge A and B to the base dried sludge was calculated using the integrated heat generation from the start of measurement for 12 hours, and the strength contribution rate of the base dried sludge was multiplied by this ratio to calculate the strength contribution rate of dried sludge A and B. Note that since the ratio of integrated heat generation is almost the same whether the value for 1 day or 3 days is used, it can be seen that any value for the material age after 12 hours can be used. The compressive strength of soil cement containing dried sludge A (or dried sludge B) can be estimated by using an equation in which the coefficient value 0.0187 in the above multiple regression equation (1) is replaced with the strength contribution rate of dried sludge A (or dried sludge B).

[0029] The relationship between the compressive strength at 28 days old (estimated strength) estimated using the strength contribution rates of dried sludge A and B and the compressive strength at 28 days old (measured strength) is shown in Figure 5. As shown in this figure, the estimated strength is very close to the measured strength, indicating that the measured strength can be estimated with high accuracy.

[0030] As described above, the strength estimation method of the present invention for estimating the strength of a sludge-containing solidified body containing sludge and an admixture includes the steps of: preparing a specimen of the sludge-containing solidified body by mixing a predetermined standard sludge with the admixture in a predetermined ratio; determining the compressive strength of the specimen at a predetermined material age; determining the strength contribution rate of the standard sludge and the strength contribution rate of the admixture in the compressive strength; and calculating the amount of heat of hydration of the standard sludge and the sludge used in the sludge-containing solidified body to be estimated. and calculating an integrated heat generation amount up to an earlier material age than the above-mentioned material age; calculating a ratio between the integrated heat generation amount of the standard sludge and the integrated heat generation amount of the sludge; calculating a strength contribution rate of the sludge based on the calculated ratio of the integrated heat generation amounts and the strength contribution rate of the standard sludge; and estimating the compressive strength of the sludge-containing solidified body to be estimated based on the calculated strength contribution rate of the sludge, the strength contribution rate of the admixture, and the mixing ratio of the sludge and the admixture, thereby making it possible to accurately estimate the strength of the sludge-containing solidified body.

[0031] In addition, according to another method for estimating the strength of sludge-containing solidified material of the present invention, the compressive strength is estimated using a multiple regression equation in which the compressive strength is the objective variable and the mixing ratio of the sludge and the admixture is the explanatory variable, so that the compressive strength can be easily estimated.

[0032] Furthermore, according to the quality control method for sludge-containing solidified bodies of the present invention, which is a method for controlling the quality of sludge-containing solidified bodies formed by mixing an earthen material with a binder consisting of sludge and an admixture, the method includes a step of estimating the compressive strength by the above-mentioned estimation method for sludge-containing solidified bodies, and a step of determining whether the estimated compressive strength satisfies specified design conditions, thereby making it possible to easily design the strength and control the quality of sludge-containing solidified bodies such as soil cement.

[0033] The "Sustainable Development Goals (SDGs)" are 17 international goals that were adopted at the United Nations Summit in September 2015. The strength estimation method and quality control method for sludge-containing solidified body according to the present embodiment can contribute to the achievement of, for example, "11. Sustainable urban and human settlements" among the 17 SDGs. [Industrial Applicability]

[0034] As described above, the strength estimation method and quality control method for sludge-containing solidified bodies of the present invention are useful for soil cement used in ground improvement works, earth retaining works, backfilling works, etc., and are particularly suitable for estimating the compressive strength of soil cement containing sludge.

Claims

1. A method for estimating the strength of a sludge-containing solidified body containing sludge and an admixture, comprising the steps of: A step of preparing a specimen of a sludge-containing solidified body by mixing a predetermined standard sludge with the admixture in a predetermined ratio, and determining a compressive strength of the specimen at a predetermined material age; A step of determining a strength contribution rate of the reference sludge and a strength contribution rate of the admixture in the compressive strength; A step of measuring the calorific value of hydration of each of the reference sludge and the sludge used in the sludge-containing solidified body to be estimated, and calculating an integrated calorific value up to an early material age before the material age; A step of determining a ratio between the integrated calorific value of the reference sludge and the integrated calorific value of the sludge; A step of determining a strength contribution rate of the sludge based on the determined ratio of the integrated heat generation amount and the strength contribution rate of the reference sludge; A method for estimating the strength of a sludge-containing solidified body, comprising the steps of estimating the compressive strength of the sludge-containing solidified body to be estimated based on the calculated strength contribution rate of the sludge, the strength contribution rate of the admixture, and the mixing ratio of the sludge and the admixture.

2. The strength estimation method for sludge-containing solidified body according to claim 1, characterized in that the compressive strength is estimated using a multiple regression equation in which the compressive strength is a dependent variable and the mixing ratio of the sludge and the admixture is an explanatory variable.

3. A method for controlling the quality of a sludge-containing solidified body obtained by mixing a soil material with a binder made of sludge and an admixture, comprising the steps of: A step of estimating the compressive strength by the method for estimating the compressive strength of a sludge-containing solidified body according to claim 1 or 2; and determining whether the estimated compressive strength satisfies predetermined design conditions.