Silane coupling agent, surface-treated inorganic oxide, and article

The silane coupling agent with a polyalkylene glycol chain addresses the limitations of existing agents by improving dispersibility and compatibility of inorganic oxides, enhancing their performance in composite materials and dispersions.

JP2024148061AActive Publication Date: 2024-10-17DAINICHISEIKA COLOR & CHEMICALS MFG CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023060951
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing silane coupling agents do not adequately improve the dispersibility, compatibility, and filling properties of inorganic oxides in various media, particularly inorganic fillers and pigments, limiting their application in composite materials and dispersions.

Method used

A silane coupling agent with a polyalkylene glycol chain and alkoxy group, represented by specific general formulas, is used to treat the surface of inorganic oxides, enhancing dispersibility and compatibility through chemical bonding and polyalkylene glycol chain affinity with the dispersion medium.

Benefits of technology

The treated inorganic oxides exhibit improved dispersibility, compatibility, and filling properties, allowing for better dispersion in liquids and enhanced mechanical properties in composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148061000001
    Figure 2024148061000001
  • Figure 2024148061000002
    Figure 2024148061000002
  • Figure 2024148061000003
    Figure 2024148061000003
Patent Text Reader

Abstract

To provide a silane coupling agent for use in surface treatment that can improve properties of inorganic oxides such as the dispersibility in, compatibility with and fillability into various media.SOLUTION: The invention provides a compound represented by the general formula (1) or (2) in the figure. (In the formula, R is a C1-18 hydrocarbon group; R1 is a hydrogen atom or a C1-3 hydrocarbon group; R2 is a methyl, ethyl, n-propyl or isopropyl group; multiple occurrences of R3 are each independent a hydrogen atom or methyl group; m is a number from 0 to 2; and n is a number from 10 to 70.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silane coupling agent, a surface-treated inorganic oxide, and an article. [Background technology]

[0002] Silane coupling agents having an alkoxysilyl group in their molecular structure are used as surface modifiers for improving the physical properties, such as wettability, adhesion, compatibility, dispersibility, mechanical strength, water resistance, and bleed-out resistance, of inorganic oxides, such as inorganic fillers and inorganic pigments, including silica, alumina, titanium oxide, and zinc oxide.

[0003] When the surface of an inorganic oxide is treated with a silane coupling agent, the alkoxysilyl group of the silane coupling agent and the hydroxyl group of the inorganic oxide undergo dealcoholization and dehydration condensation. The silane coupling agent is chemically bonded to the surface of the inorganic oxide, and the silane coupling agent also undergoes self-condensation. This allows the organic group of the silane coupling agent to be introduced to the surface of the inorganic oxide, and the physical properties of the inorganic oxide can be improved by the characteristics of the introduced organic group.

[0004] Various silane coupling agents for surface-treating inorganic oxides, and inorganic oxides such as glass, inorganic fillers, and inorganic pigments that have been surface-treated with a silane coupling agent have been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-095457 A [Patent Document 2] JP 2011-190179 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, with further technological development, there is a demand for further improvement in the properties of inorganic oxides, such as dispersibility and compatibility, in order to provide a dispersion in which an inorganic oxide, such as a pigment, is dispersed in a liquid medium, or a composite material in which an inorganic oxide is dispersed in a resin.

[0007] The present invention has been made in consideration of the problems of the prior art, and its objective is to provide a silane coupling agent that can give inorganic oxides such as inorganic fillers and inorganic pigments surface treatment, and can improve these characteristics of inorganic oxides, such as dispersibility in various media, compatibility, and filling property.The present invention also aims to provide a surface-treated inorganic oxide using this silane coupling agent, and an article containing this surface-treated inorganic oxide. [Means for solving the problem]

[0008] That is, according to the present invention, there is provided the following silane coupling agent. [1] A silane coupling agent used for surface treatment of an inorganic oxide, which is a compound represented by the following general formula (1) or (2):

[0009] TIFF2024148061000001.tif63170 (in the general formulas (1) and (2), R represents a hydrocarbon group having 1 to 18 carbon atoms, R1 represents a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, R2 represents a methyl group, an ethyl group, an n-propyl group, or an isopropyl group, a plurality of R3s each independently represent a hydrogen atom or a methyl group, m represents a number from 0 to 2, and n represents a number from 10 to 70)

[0010] Furthermore, according to the present invention, there is provided the following surface-treated inorganic oxide. [2] A surface-treated inorganic oxide, which is an inorganic oxide surface-treated with the silane coupling agent described in [1] above. [3] The surface-treated inorganic oxide according to the above [2], wherein the inorganic oxide is inorganic oxide fine particles having an average particle size of 10 nm to 100 μm. [4] The surface-treated inorganic oxide according to the above [3], which is a treated product obtained by surface-treating 100 parts by mass of the inorganic oxide fine particles with 0.5 to 50 parts by mass of the silane coupling agent. [5] The surface-treated inorganic oxide according to [3] or [4], wherein the inorganic oxide fine particles are at least one selected from the group consisting of titanium dioxide, zinc oxide, silica, alumina, and composite oxide pigments.

[0011] Further, according to the present invention, there are provided the following articles: [6] An article containing the surface-treated inorganic oxide according to any one of [2] to [5] above. Effect of the Invention

[0012] According to the present invention, it is possible to provide a silane coupling agent that can impart properties such as dispersibility in various media, compatibility, and packing property to the inorganic oxide or improve these properties of the inorganic oxide by treating the surface of the inorganic oxide such as an inorganic filler or an inorganic pigment. Also, according to the present invention, it is possible to provide a surface-treated inorganic oxide using this silane coupling agent, and an article containing this surface-treated inorganic oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Silane coupling agent> Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. One embodiment of the present invention is a silane coupling agent used for surface treatment of inorganic oxides, which is a compound represented by the following general formula (1) or (2) and has a polyalkylene glycol chain and an alkoxysilyl group in its molecular structure.

[0014] TIFF2024148061000002.tif33170 (in the general formula (1), R represents a hydrocarbon group having 1 to 18 carbon atoms, R1 represents a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, R2 represents a methyl group, an ethyl group, an n-propyl group, or an isopropyl group, and multiple R3s each independently represent a hydrogen atom or a methyl group, m represents a number from 0 to 2, and n represents a number from 10 to 70)

[0015] TIFF2024148061000003.tif36170 (in the general formula (2), R represents a hydrocarbon group having 1 to 18 carbon atoms, R1 represents a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, R2 represents a methyl group, an ethyl group, an n-propyl group, or an isopropyl group, and multiple R3s each independently represent a hydrogen atom or a methyl group, m represents a number from 0 to 2, and n represents a number from 10 to 70)

[0016] When the surface of an inorganic oxide is treated with the silane coupling agent of this embodiment, the alkoxysilyl group of the silane coupling agent reacts with the hydroxyl group on the surface of the inorganic oxide, and undergoes dealcoholization and dehydration condensation. This causes the silane coupling agent to chemically bond to the surface of the inorganic oxide. In addition, the polyalkylene glycol chain, which is the organic group of the silane coupling agent, is a polymer chain of a certain molecular weight having repeating units. Therefore, this polyalkylene glycol chain has affinity and compatibility with the medium that disperses the inorganic oxide, and can improve the properties of the inorganic oxide, such as dispersibility, filling property, and flowability.

[0017] One end of the polyalkylene glycol chain of the silane coupling agent is an alkyl ether. In the general formulas (1) and (2), the number of carbon atoms of the hydrocarbon group represented by R is 1 to 18, preferably 1 to 4. Examples of the polyalkylene glycol chain include a polyethylene glycol chain, a polypropylene glycol chain, a polyethylene glycol polypropylene glycol random polymer chain, and a polyethylene glycol polypropylene glycol block polymer chain. Among them, a polyethylene glycol polypropylene glycol chain having one end that is a methyl group is preferred, since it is commercially available and the hydrophilicity and hydrophobicity can be easily controlled.

[0018] In the general formulas (1) and (2), n is a number from 10 to 70, preferably from 20 to 50. The molecular weight of the silane coupling agent of the present embodiment is usually in the range of about 400 to 4,000. When n is less than 10, the molecular weight is too small, and compatibility with the dispersion medium is likely to be insufficient. On the other hand, when n is more than 70, the molecular weight is too large, and the physical properties of the dispersion medium are impaired due to the effect of the polyalkylene glycol chain on the dispersion medium, and the reactivity is reduced, making it difficult to treat the surface of the inorganic oxide.

[0019] The alkoxysilyl group of the silane coupling agent is an alkyldialkoxysilyl group or a trialkoxysilyl group. In the general formulas (1) and (2), the hydrocarbon group having 1 to 3 carbon atoms represented by R1 is preferably a methyl group or an ethyl group in consideration of reactivity. In the general formulas (1) and (2), R2 is a methyl group, an ethyl group, an n-propyl group, or an isopropyl group, and is preferably a methyl group in consideration of reactivity, and is preferably an ethyl group in consideration of stability.

[0020] The silane coupling agent represented by general formula (1) has a urea bond in its structure. The silane coupling agent represented by general formula (2) has an amide bond in its structure. Therefore, the silane coupling agent of the present embodiment has excellent hydrolysis resistance even when a dispersion medium such as water or alkaline water is used, and has good water resistance and chemical resistance. In addition, the urea bond or amide bond can easily be adsorbed by hydrogen bonding with oxygen atoms on the surface of the inorganic oxide.

[0021] The silane coupling agent represented by the general formula (2) has a carboxyl group in its structure. By neutralizing and ionizing this carboxyl group, the hydrophilicity of the surface-treated inorganic oxide (surface-treated inorganic oxide) can be increased. Furthermore, when the polyalkylene glycol chain is a polyethylene glycol chain, the water solubility of the polyethylene glycol chain and the neutralized and ionized carboxyl group act to finely disperse the surface-treated inorganic oxide (surface-treated inorganic oxide) in water in a better state. Furthermore, when an inorganic oxide having a polyalkylene glycol chain bonded to its surface is dispersed in a liquid medium such as water or an organic solvent, even if the inorganic oxide settles, the inorganic oxides can be inhibited from coagulating due to the properties of the polyalkylene glycol chain, and even if the inorganic oxides coagulate, they can be returned to a state close to the original dispersion state simply by stirring and mixing.

[0022] When an inorganic oxide surface-treated with a silane coupling agent represented by general formula (2) (surface-treated inorganic oxide) is dispersed in a dispersion medium without being neutralized, and a polymer-type dispersant containing an amino group is used, the carboxy group and the amino group in the dispersant form an ionic bond, improving the dispersion effect of the dispersant. In addition, when a resin having a group that reacts with a carboxy group, such as an epoxy resin, is used as a dispersion medium to produce a composite material, the epoxy group in the resin and the carboxy group undergo a crosslinking reaction, improving the mechanical properties of the resulting composite material.

[0023] The silane coupling agent of the present embodiment can be produced by reacting polyalkylene glycol monoalkyl ether monoamine with a general silane coupling agent having a group capable of reacting with the amino group in the polyalkylene glycol monoalkyl ether monoamine. That is, the silane coupling agent represented by general formula (1) can be produced, for example, by reacting polyalkylene glycol monoalkyl ether monoamine with a compound having an isocyanate group and an alkoxysilyl group. In addition, the silane coupling agent represented by general formula (2) can be produced, for example, by reacting with a compound having a succinic anhydride group and an alkoxysilyl group.

[0024] As the compound having an isocyanate group and an alkoxysilyl group, a conventionally known silane coupling agent can be used. Examples of such a silane coupling agent include 3-isocyanate propyl methyl dimethoxy silane, 3-isocyanate propyl methyl diethoxy silane, 3-isocyanate propyl trimethoxy silane, and 3-isocyanate propyl triethoxy silane.

[0025] Examples of compounds having a succinic anhydride group and an alkoxysilyl group include 3-methyldimethoxysilylpropyl succinic anhydride, 3-methyldiethoxysilylpropyl succinic anhydride, 3-trimethoxysilylpropyl succinic anhydride, and 3-triethoxysilylpropyl succinic anhydride. The alkoxysilyl group may be hydrolyzed. The silane coupling agent of the present embodiment may contain a silanol group in which a part of the alkoxy group is hydrolyzed.

[0026] The polyalkylene glycol monoalkyl ether monoamine and the compound having a group capable of reacting with an amino group (reactive group-containing compound) can be mixed and reacted by a conventionally known method. For example, one of the polyalkylene glycol monoalkyl ether monoamine and the reactive group-containing compound is placed in a reaction vessel and usually maintained at room temperature (25°C) to 100°C, preferably at room temperature (25°C) to 40°C. The other compound is then added, preferably dropped, more preferably diluted with an organic solvent. Since this is an exothermic reaction, it is preferable to react while maintaining the temperature at a moderate level. The reaction may be continued until the isocyanate group or acid anhydride group disappears. The disappearance of the isocyanate group or the like can be confirmed, for example, by measuring infrared absorption (IR) using an infrared spectrophotometer, and by the disappearance of an absorption peak derived from the isocyanate group or the like, or the generation of an absorption peak derived from the urea bond or the like. The amine value may also be measured by titration or the like, and the reaction may be continued until the amine value derived from the amino group of the polyalkylene glycol monoalkyl ether monoamine becomes 0 mgKOH / g.

[0027] Examples of organic solvents for diluting the polyalkylene glycol monoalkyl ether monoamine or the reactive group-containing compound include hydrocarbon solvents such as toluene, ketone solvents such as methyl ethyl ketone, ester solvents such as ethyl acetate, cyclic ether solvents such as tetrahydrofuran, glycol solvents such as ethylene glycol dimethyl ether, amide solvents such as dimethylacetamide, urea solvents such as tetramethylurea, carbonate solvents such as ethylene carbonate, etc. Among these, in consideration of the post-treatment process in which the reaction solution is poured into water to precipitate the product, it is preferable to use an organic solvent that has affinity for water, preferably one that dissolves in water.

[0028] The desired surface-treated inorganic oxide can be obtained by treating the surface of the inorganic oxide with a silane coupling agent having an isocyanate group or an acid anhydride group according to a conventionally known method, and then reacting with a polyalkylene glycol monoalkyl ether monoamine.

[0029] The silane coupling agent of the present embodiment may react with the alkoxysilyl group with moisture absorbed over time. Therefore, a dehydrating agent may be added to the produced silane coupling agent or a solution of the silane coupling agent. As the dehydrating agent, it is preferable to use an orthocarboxylate such as trimethyl orthoacetate or triethyl orthoacetate. The amount of the dehydrating agent added may be 0.1 to 5 parts by mass with respect to 100 parts by mass of the silane coupling agent.

[0030] <Surface treatment inorganic oxide> One embodiment of the surface-treated inorganic oxide of the present invention is a treated product obtained by treating the surface of an inorganic oxide with the above-mentioned silane coupling agent. The surface-treated inorganic oxide of this embodiment can be obtained by treating the surface of an inorganic oxide with the above-mentioned silane coupling agent and introducing a polyalkylene glycol chain derived from the silane coupling agent into the surface of the inorganic oxide.

[0031] Examples of inorganic oxides include silica, alumina, zinc oxide, titanium dioxide, zirconium oxide, iron oxide, copper oxide, yttria, molybdenum oxide, indium oxide, tin oxide, tungsten oxide, bismuth oxide, antimony oxide, and composite oxides thereof; composite oxides of alkaline earth metals such as magnesium, strontium, and calcium with iron, manganese, cobalt, nickel, and the like; composite oxides of cobalt, chromium, titanium, aluminum, and the like; natural minerals such as clay and mica; and the like.

[0032] The shape of the inorganic oxide can be a plate shape such as a glass plate, an amorphous shape, a fine particle shape, etc. Among them, the shape of the inorganic oxide is preferably a fine particle shape. That is, the inorganic oxide is preferably an inorganic oxide fine particle. By treating the surface of the inorganic oxide fine particle with the silane coupling agent of the present embodiment, the properties of the inorganic oxide fine particle can be improved.

[0033] Examples of inorganic oxide fine particles include pigments, plastic fillers, inorganic fillers such as titanium dioxide, zinc oxide, silica, alumina, and composite oxide pigments used as packing agents, etc. By surface-treating these inorganic oxide fine particles with the silane coupling agent of the present embodiment, it is possible to improve properties such as dispersibility, packing property, and fluidity.

[0034] Examples of the shape of inorganic oxide fine particles include amorphous, spherical, cubic, rectangular, confetti-like, flat, discoid, cone-like, plate-like, needle-like, uneven, and porous. The average particle size of inorganic oxide particles is preferably 10 nm to 100 μm, and more preferably 50 nm to 20 μm. The average particle size of inorganic oxide fine particles can be calculated as the average value of values ​​measured by image processing of electron microscope photographs. In the case of non-spherical shapes such as needle-like, the average value of the major axis and minor axis is taken as the particle size. It can also be measured by dispersing in a liquid medium and using a dynamic light scattering method.

[0035] The inorganic oxide may be previously surface-treated with a surface treatment agent other than the silane coupling agent of the present embodiment. Examples of the surface treatment include inorganic treatments such as silica treatment, alumina treatment, silica-alumina treatment, and zirconia treatment; organic acid treatments such as oleic acid treatment; and conventionally known silane coupling agent treatments and silazane treatments. Examples of conventionally known silane coupling agents include methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, phenyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane. Examples of silazane include tetramethyldisilazane, hexamethyldisilazane, and pentamethyldisilazane.

[0036] The amount of the silane coupling agent used may be appropriately set according to the amount of inorganic oxide, surface area, etc. For example, when inorganic oxide fine particles are used as the inorganic oxide, it is preferable to surface treat 100 parts by mass of inorganic oxide fine particles with 0.5 to 50 parts by mass of the silane coupling agent, and more preferably with 1 to 20 parts by mass. If the amount of the silane coupling agent relative to 100 parts by mass of inorganic oxide fine particles is less than 0.5 parts by mass, the effect obtained by surface treatment may be insufficient. On the other hand, if it exceeds 50 parts by mass, the viscosity of the dispersion liquid, etc. may be excessively increased due to the excess silane coupling agent.

[0037] The surface-treated inorganic oxide can be manufactured by a dry method, a wet method, a coating method, and the like. In the dry method, an inorganic oxide such as inorganic oxide fine particles is placed in a tumbler, a high-speed stirrer, a grinder, and the like, and the above-mentioned silane coupling agent is added. The mixture is diluted with water or an organic solvent, and an acid component such as hydrochloric acid and acetic acid, or an alkali component such as ammonia water and sodium hydroxide aqueous solution is added as a catalyst as necessary. The contents are stirred and mixed, or sprayed little by little while stirring and mixing, to fix the silane coupling agent to the surface of the inorganic oxide. After the treatment, it is preferable to dry it, and more preferably to heat it to 80°C or higher and dry it, and even more preferably to heat it to 120°C or higher and dry it. By heating it appropriately, the reaction between the surface of the inorganic oxide and the silane coupling agent can be completed. After drying, the desired surface-treated inorganic oxide of this embodiment can be obtained by pulverizing it as necessary.

[0038] In the wet method, the inorganic oxide is mixed with the silane coupling agent in a liquid medium such as water or an organic solvent. If necessary, a dispersion treatment is performed to react the silane coupling agent with the surface of the inorganic oxide. In addition to water, an aqueous solution of an acid component or an alkali component may be added as a catalyst to promote hydrolysis. A mixer such as a disperser or homogenizer can be used to mix the inorganic oxide with the silane coupling agent. By using a ball mill, a vertical bead mill, a horizontal bead mill, or a high-pressure homogenizer as a dispersing machine used in the dispersion treatment, the inorganic oxide in the form of fine particles can be reacted with the silane coupling agent in a state where the inorganic oxide in the form of fine particles is finely dispersed to the vicinity of the primary particles, and the inorganic oxide in the form of fine particles can be treated individually.

[0039] The mixed liquid containing the treated inorganic oxide (surface-treated inorganic oxide) and the silane coupling agent may be filtered, or coarse particles may be removed using a filter. Next, the silane coupling agent is precipitated in a poor solvent in which the polyalkylene glycol chain is not dissolved, and then filtered to obtain a paste state. For example, when the ratio of oxypropylene units (PO) in the polyalkylene glycol chain is 70 mass% or more, it can be obtained in a paste state by precipitating in water. In addition, the mixed liquid can be made into a paste state by distilling at least a part of the liquid medium from the mixed liquid using an evaporator or the like. Furthermore, the mixed liquid can be made into a solid state by completely distilling the liquid medium from the mixed liquid. In addition, the mixed liquid can be made into a powder state by spraying the mixed liquid while drying it using a spray dryer or the like. It is preferable to complete the reaction between the alkoxysilyl group of the silane coupling agent and the hydroxyl group present on the surface of the inorganic oxide by heating and drying the obtained paste, solid, and powder. It is preferable to crush the obtained dried product into a powder state using a crusher as necessary.

[0040] When the inorganic oxide is in the form of a plate such as a glass plate or a film, for example, a silane coupling agent or a silane coupling agent solution dissolved in a solvent such as water or an organic solvent is applied or sprayed onto the surface of the inorganic oxide. The content of the silane coupling agent in the silane coupling agent solution is preferably less than 10% by mass. After the silane coupling agent solution is applied or sprayed, it is preferable to complete the reaction between the alkoxysilyl group of the silane coupling agent and the hydroxyl group present on the surface of the inorganic oxide by heating to 120°C or higher and drying and curing. This allows the cured film formed by the silane coupling agent to be fixed onto the surface of the inorganic oxide to obtain the desired inorganic oxide.

[0041] <Goods> One embodiment of the article of the present invention contains the above-mentioned surface-treated inorganic oxide. As described above, the surface-treated inorganic oxide used in the article of this embodiment is an inorganic oxide having a polyalkylene glycol chain derived from a silane coupling agent introduced onto its surface, so that the surface is hydrophilic. Therefore, it is useful as an article such as glass or mirror having a functional surface with anti-fogging and anti-frosting properties.

[0042] Furthermore, when a surface-treated inorganic oxide in the form of fine particles (surface-treated fine particles) is used, by dispersing the surface-treated fine particles in a liquid medium capable of dissolving the polyalkylene glycol chains bonded to the surface, it is possible to obtain a dispersion liquid with excellent redispersibility, in which even if the fine particles settle, the original dispersed state can be easily restored simply by stirring, etc., due to the effect of preventing interparticle adhesion caused by the solvent content of the polyalkylene glycol chains.

[0043] The surface-treated fine particles can be used as functional fillers or bulking agents in paints, inks, coating agents, etc. For example, by dispersing the surface-treated fine particles in paints or inks containing a solvent capable of dissolving polyalkylene glycol chains, paints and inks with excellent dispersibility can be obtained. In addition, by blending the surface-treated fine particles as a filler in a coating agent such as an ultraviolet- or electron-beam-curable coating agent, a coating agent with a high filling rate and excellent fluidity can be obtained. Furthermore, the surface-treated fine particles can be filled in thermoplastic resins such as polystyrene, polyester, and polyacrylic, and thermosetting resins such as acrylic resins, melamine resins, epoxy resins, and alkyd resins at a filling rate of, for example, 50% by mass or more, preferably 70% by mass or more, and the fluidity and processability are also good. EXAMPLES

[0044] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are by mass unless otherwise specified.

[0045] <Synthesis of silane coupling agent> (Example 1 of Synthesis) 222.2 parts (0.1 mol) of polypropylene glycol polyethylene glycol monomethyl ether monoamine (trade name "Jeffamine M2005", Huntsman, PO / EO = 29 / 5 (molar ratio), actual amine value 25.25 mg KOH / g) (M2005) was placed in a reaction vessel. 27.5 parts (0.105 mol) of a compound represented by the following formula (3) (silane coupling agent, trade name "X-12-967C", Shin-Etsu Chemical Co., Ltd., Mw 262.1) and 27.5 parts of diethylene glycol dimethyl ether (DMDG) were placed in another vessel and mixed to prepare a uniform solution. The prepared solution was dropped into the reaction vessel over 30 minutes under room temperature conditions. Heat was generated during the dropwise addition, and it was confirmed that the reaction was proceeding. After the dropwise addition was completed, the temperature was raised to 45 ° C and stirred for 1 hour to obtain a silane coupling agent solution TQ-1 containing a polymer-type silane coupling agent having a carboxy group. A portion of the solution was sampled and infrared absorption (IR) was measured, and it was confirmed that the reaction was almost complete due to the disappearance of the peak derived from the acid anhydride. The solid content measured using a halogen lamp moisture meter was 90.7%. The amine value of the silane coupling agent in the obtained silane coupling agent solution TQ-1 was about 0 mg KOH / g. The amine value was calculated by dissolving the sample in a 2-propanol / toluene mixed solvent and titrating and calculating using a potentiometric titrator using a 2-propanol 0.1N-HCl solution as the titration solution. It was confirmed that the silane coupling agent in the obtained silane coupling agent solution TQ-1 was substantially insoluble in water.

[0046] TIFF2024148061000004.tif33170

[0047] (Example 2 of Synthesis) Polypropylene glycol polyethylene glycol monomethyl ether monoamine (trade name "Jeffamine M600", Huntsman, PO / EO = 9 / 1 (molar ratio), actual amine value 96.51 mgKOH / g) (M600) 116.3 parts (0.2 mol) and DMDG 116.3 parts were placed in a reaction vessel. 55.1 parts (0.21 mol) of the compound represented by formula (3) and 55.1 parts of DMDG were placed in another vessel and mixed to prepare a uniform solution. The prepared solution was dropped into the reaction vessel over 30 minutes under room temperature conditions. Heat was generated during the dropwise addition, and it was confirmed that the reaction was proceeding. After the dropwise addition was completed, the temperature was raised to 45 ° C and stirred for 1 hour to obtain a silane coupling agent solution TQ-2 containing a polymer-type silane coupling agent having a carboxy group. A portion was sampled and infrared absorption (IR) was measured, and it was confirmed that the reaction was almost complete by the disappearance of the peak derived from the acid anhydride. The solid content measured using a halogen lamp moisture meter was 49.8%. The amine value of the silane coupling agent in the obtained silane coupling agent solution TQ-2 was about 0 mg KOH / g. It was confirmed that the silane coupling agent in the obtained silane coupling agent solution TQ-2 was substantially insoluble in water.

[0048] (Synthesis Examples 3 to 5) Silane coupling agent solutions TQ-3 to 5 containing a polymer-type silane coupling agent having a carboxy group were obtained in the same manner as in the above-mentioned Synthesis Examples 1 and 2, except that the types and amounts of materials shown in Table 1 were used. Details of the obtained silane coupling agent solutions TQ-3 to 5 are shown in Table 1. The meanings of the abbreviations in Table 1 are shown below. M1000: Trade name "Jeffamine M1000", manufactured by Huntsman, PO / EO = 3 / 19 (molar ratio), actual amine value 57.23 mg KOH / g M41: Trade name "Genamine M41 / 2000", manufactured by Clariant, PO / EO = 1 / 4 (molar ratio), measured amine value 26.10 mg KOH / g M3085: Trade name "Jeffamine M3085", manufactured by Huntsman, PO / EO = 8 / 58 (molar ratio), actual amine value 18.48 mg KOH / g

[0049] TIFF2024148061000005.tif104170

[0050] (Example 6 of Synthesis) 222.2 parts (0.1 mol) of M2005 were placed in a reaction vessel. 24.7 parts (0.1 mol) of a compound represented by the following formula (4) (silane coupling agent, product name "KBE-9007N", Shin-Etsu Chemical Co., Ltd., Mw247.4) and 24.7 parts of DMDG were placed in another vessel and mixed to prepare a uniform solution. The prepared solution was dropped into the reaction vessel over 30 minutes under room temperature conditions. Heat was generated during the dropwise addition, and it was confirmed that the reaction was proceeding. After the dropwise addition was completed, the mixture was stirred at room temperature for 30 minutes to obtain a silane coupling agent solution TQ-6 containing a polymer type silane coupling agent. A portion was sampled and infrared absorption (IR) was measured, and it was confirmed that the reaction was almost complete by the disappearance of the peak derived from the isocyanate group. The solid content measured using a halogen lamp moisture meter was 90.8%. In addition, the amine value of the silane coupling agent in the obtained silane coupling agent solution TQ-6 was about 0 mgKOH / g.

[0051] TIFF2024148061000006.tif25170

[0052] (Synthetic Examples 7 to 10) Silane coupling agent solutions TQ-7 to 10 containing a polymer-type silane coupling agent having a carboxy group were obtained in the same manner as in the above-mentioned Example Synthesis 6, except that the types and amounts of materials shown in Table 2 were used. Details of the obtained silane coupling agent solutions TQ-7 to 10 are shown in Table 2.

[0053] TIFF2024148061000007.tif103170

[0054] (Comparative Synthesis Example 1) 81.6 parts (0.5 mol) of 2-(2-(2-methoxyethoxy)ethoxy)ethanamine (Mw163.2) (MEEEA) and 81.6 parts of DMDG were placed in a reaction vessel. 123.7 parts (0.5 mol) of the compound represented by formula (3) and 123.7 parts of DMDG were placed in another vessel and mixed to prepare a homogeneous solution. The prepared solution was dripped into the reaction vessel over 1 hour while cooling with water. Heat was generated during the dripping, and it was confirmed that the reaction was proceeding. After the dripping was completed, the mixture was stirred at room temperature for 30 minutes to obtain a silane coupling agent solution HS-1 containing a silane coupling agent. A portion was sampled and infrared absorption (IR) was measured, and it was confirmed that the reaction was almost complete by the disappearance of the peak derived from the acid anhydride. The solid content measured using a halogen lamp moisture meter was 49.7%. In addition, the amine value of the silane coupling agent in the obtained silane coupling agent solution HS-1 was about 0 mg KOH / g. It was confirmed that the silane coupling agent in the resulting silane coupling agent solution HS-1 was soluble in water.

[0055] (Comparative Synthesis Example 2) 81.6 parts (0.5 mol) of MEEEA and 81.6 parts of DMDG were placed in a reaction vessel. 137.6 parts (0.525 mol) of the compound represented by formula (4) and 137.6 parts of DMDG were placed in another vessel and mixed to prepare a homogeneous solution. The prepared solution was dripped into the reaction vessel over 1 hour while cooling with water. Heat was generated during the dripping, and it was confirmed that the reaction was proceeding. After the dripping was completed, the temperature was raised to 45°C and stirred for 1 hour to obtain a silane coupling agent solution HS-2 containing a silane coupling agent. A portion was sampled and infrared absorption (IR) was measured, and it was confirmed that the reaction was almost complete by the disappearance of the peak derived from the isocyanate group. The solid content measured using a halogen lamp moisture meter was 50.1%. In addition, the amine value of the silane coupling agent in the obtained silane coupling agent solution HS-2 was about 0 mgKOH / g. It was confirmed that the silane coupling agent in the obtained silane coupling agent solution HS-2 was soluble in water.

[0056] <Production of Surface-Treated Inorganic Oxides (Surface-Treated Fine Particles) (1)> Example 1 100 parts of titanium oxide pigment (product name "R-900", manufactured by Chemours), 39.0 parts of methanol, 11.0 parts of silane coupling agent solution TQ-1 (10 parts of silane coupling agent), 50 parts of ion-exchanged water, and 0.1 parts of acetic acid were placed in a resin container. 400 parts of 0.5 mm zirconia beads were filled into the container, and the mixture was shaken for 2 hours using a paint conditioner for dispersion treatment to obtain a pigment dispersion. The pigment dispersion obtained by separating the zirconia beads was poured into a large amount of water, and the resulting precipitate was filtered and washed with ion-exchanged water to obtain a water paste. The obtained water paste was dried in a dryer at 120 ° C. for 12 hours to obtain a lump-shaped dried product. The obtained dried product was pulverized in a grinder to obtain surface-treated fine particles MB-1, which are fine particles of a surface-treated inorganic oxide.

[0057] When the infrared absorption (IR) of the obtained surface-treated fine particles was measured, a small amount of peaks derived from carbonyl groups were confirmed. This is considered to be a peak derived from the carbonyl group in the amide bond of the silane coupling. On the other hand, the peak derived from the ether bond of the polyalkylene glycol chain in the silane coupling agent overlapped with the peak derived from titanium oxide and could not be confirmed. The non-volatile content measured using a halogen lamp moisture meter was 99.8%. In addition, the inorganic residue was measured by thermal analysis in which the organic matter was burned by heating to 400°C and was 91.3%. From the above results, it is considered that a predetermined amount of silane coupling agent is bonded to the surface of titanium oxide.

[0058] (Examples 2 to 4, Comparative Examples 1 and 2) Surface-treated fine particles MB-2 to 4, HB-1, and 2, which are fine-particle surface-treated inorganic oxides, were obtained in the same manner as in Example 1 described above, except that the types and amounts of silane coupling agent solutions or silane coupling agents shown in Table 3 were used. Details of the obtained surface-treated fine particles MB-2 to 4, HB-1, and 2 are shown in Table 3. The meanings of the abbreviations in Table 3 are as follows. 573: N-phenyl-3-aminopropyltrimethoxysilane, product name "KBM-573, Shin-Etsu Chemical Co., Ltd. OTMS: Octadecyltrimethoxysilane, manufactured by Tokyo Chemical Industry Co., Ltd.

[0059] TIFF2024148061000008.tif70170

[0060] <Evaluation (1)> 120 parts of surface-treated fine particles of the type shown in Table 4, 40 parts of toluene, and 40 parts of methyl ethyl ketone were placed in a resin container. 0.5 mm zirconia beads were filled into the container, and a paint conditioner was used to shake and disperse the particles for 2 hours to obtain pigment dispersions W-1 to W-6. Of the resulting pigment dispersions, those that had fluidity were measured for viscosity using a B-type viscometer. In addition, a dynamic light scattering particle size distribution measuring device (product name "nanoSAQRA", manufactured by Otsuka Electronics Co., Ltd.) was used to measure the average particle size (median diameter (D 50 )) were measured. Furthermore, the dispersibility of the pigment dispersion was evaluated according to the following evaluation criteria. The results are shown in Table 4. ◯: Liquid, with an average particle size of 300 nm or less. ×: Gel or thixotropic, average particle size exceeding 300 nm.

[0061] TIFF2024148061000009.tif64170

[0062] <Production of Surface-Treated Inorganic Oxides (Surface-Treated Fine Particles) (2)> Example 5 A pigment dispersion was obtained in the same manner as in Example 1 described above, except that the silane coupling agent solution TQ-3 was used instead of the silane coupling agent solution TQ-1, and 5 parts of the silane coupling agent were used per 100 parts of titanium oxide pigment. The obtained pigment dispersion was placed in a separable flask, and the volatile matter was removed using an evaporator to concentrate, thereby obtaining an aqueous paste. The obtained aqueous paste was dried in a dryer at 120°C for 12 hours to obtain a lump-shaped dried product. The obtained dried product was pulverized in a pulverizer to obtain surface-treated fine particles MB-5, which are fine particles of a surface-treated inorganic oxide. The non-volatile matter of the obtained surface-treated fine particles MB-5 was 99.8%, and the inorganic residue was 96.2%.

[0063] (Examples 6 to 10, Comparative Examples 3 and 4) Surface-treated fine particles MB-6 to 10, HB-3, and 4, which are fine-particle surface-treated inorganic oxides, were obtained in the same manner as in Example 5 described above, except that the type and amount of silane coupling agent solution shown in Table 5 was used. Details of the obtained surface-treated fine particles MB-6 to 10, HB-3, and 4 are shown in Table 5.

[0064] TIFF2024148061000010.tif64170

[0065] <Evaluation (2)> 55 parts of surface-treated fine particles of the type shown in Table 6, 41 parts of water, 2 parts of hexanediol, and 2 parts of a 5% aqueous sodium hydroxide solution were placed in a container. 0.5 mm zirconia beads were filled into the container, and the container was shaken for 2 hours using a paint conditioner for dispersion treatment, to obtain pigment dispersions W-7 to W-14. Of the resulting pigment dispersions, those that had fluidity were measured for viscosity using a B-type viscometer. In addition, the average particle diameter (median diameter (D 50 )) were measured. Furthermore, the dispersibility of the pigment dispersion was evaluated according to the following evaluation criteria. The results are shown in Table 6. ◯: Liquid, with an average particle size of 300 nm or less. ×: Gel or thixotropic, average particle size exceeding 300 nm.

[0066] TIFF2024148061000011.tif63170

[0067] The surface-treated fine particles MB-5 to MB-7 were prepared using a silane coupling agent having a carboxy group, and it is believed that the carboxy group was neutralized and ionized, which improved the dispersibility.

[0068] <Production of Surface-Treated Inorganic Oxides (Surface-Treated Fine Particles) (3)> Example 11 200 parts of silica sol (trade name "Snowtex ST-OS", manufactured by Nissan Chemical Industries, Ltd., silica content 20%, average particle size 9 nm) were placed in a separable flask. 3.3 parts of silane coupling agent solution TQ-6, 200 parts of isopropanol (IPA), and 0.5 parts of 28% ammonia water were added, and the mixture was heated and reacted for 5 hours under reflux. 100 parts of propylene glycol monomethyl ether (MPG) were added to the removed content, and the volatile matter was removed using an evaporator to obtain an MPG dispersion of surface-treated fine particles MB-11. The resulting dispersion was a very thin, translucent dispersion with a solid content of 23.9%.

[0069] <Evaluation (3)> 100 parts of pentaerythritol triacrylate (trade name "Aronix M-305", manufactured by Toagosei Co., Ltd.), 31.4 parts of MPG dispersion of surface-treated fine particles MB-11, and 4 parts of photoinitiator (trade name "Irgacure 2959", manufactured by BASF Japan Ltd.) were mixed to obtain an ultraviolet-curable coating agent. The obtained coating agent was applied to a PET film (trade name "Cosmoshine A4300", manufactured by Toyobo Co., Ltd., film thickness 100 μm) using a bar coater so that the dry film thickness was 3 μm, and then dried at 100 ° C for 5 minutes. The accumulated light amount was 300 mJ / cm with an 80 W / cm high-pressure mercury lamp. 2The coating agent was cured by irradiating light so that a coating film was obtained. The total light transmittance of the coating film measured using a haze meter was 92.2%, and the haze value was 0.5, indicating that a coating film with excellent transparency and no lumps or foreign matter was formed.

[0070] <Production of Surface-Treated Inorganic Oxides (Surface-Treated Fine Particles) (4)> Example 12 500 parts of spherical powder of alumina (average particle size 10 μm, surface untreated), 500 parts of methanol, 13.7 parts of silane coupling agent solution TQ-1, and 1 part of 28% ammonia water were placed in a tray and mixed and stirred for 30 minutes at 2,000 rpm using a homogenizer to obtain a mixed liquid. The resulting mixed liquid was added to a container containing a large amount of water while stirring. The resulting precipitate was filtered and washed with ion-exchanged water to obtain a water paste. The resulting water paste was dried in a dryer at 120 ° C for 12 hours to obtain a lump-shaped dried product. The resulting dried product was pulverized in a grinder to obtain surface-treated fine particles MB-12, which are fine particles of a surface-treated inorganic oxide. The non-volatile content of the resulting surface-treated fine particles MB-12 was 99.9%, and the inorganic residue was 98.9%.

[0071] Comparative Example 5 Surface-treated fine particles HB-5 were obtained in the same manner as in Example 12, except that 2.5 parts of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (trade name "KBM603", manufactured by Shin-Etsu Chemical Co., Ltd.) was used instead of the silane coupling agent solution TQ-1. The non-volatile content of the obtained surface-treated fine particles HB-5 was 99.9%, and the inorganic residue was 99.7%.

[0072] <Rating (4)> (i) 80 parts of spherical powder of alumina (average particle size 10 μm, surface untreated), (ii) 80 parts of surface-treated fine particles MB-12, or (iii) 80 parts of surface-treated fine particles HB-5 were placed in a resin container. 20 parts of epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name jER-871) was added to each and stirred to obtain mixtures (i) to (iii). Mixture (i) was a high-viscosity liquid that barely flowed. Mixture (iii) was a high-viscosity liquid with a viscosity of 15 Pa s. In contrast, mixture (ii) was a low-viscosity liquid with a viscosity of 6.3 Pa s. It is believed that the compatibility of alumina and epoxy resin was improved by the surface treatment, resulting in high loading and improved flowability.

[0073] <Production of surface-treated inorganic oxide (surface-treated substrate) (5)> (Example 13) A coating solution was obtained by mixing 10 parts of silane coupling agent solution TQ-5, 190 parts of IPA, and 200 parts of propylene glycol monomethyl ether acetate. A glass plate (7 cm x 7 cm) was washed with tetrahydrofuran and methanol, respectively, and then set on a spin coater. The coating agent was dropped onto the glass plate, coated at 2,000 rpm for 30 seconds, and then dried at 80°C for 10 minutes and at 120°C for 30 minutes to obtain a surface-treated substrate MB-13. The thickness of the coating film measured using a film thickness meter (trade name "F20-UV", Filmetrics, Inc.) was 213 nm.

[0074] Example 14 Except for using the silane coupling agent solution TQ-10 instead of the silane coupling agent solution TQ-5, the surface-treated substrate MB-14 was obtained in the same manner as in Example 13. The thickness of the coating film measured using a film thickness meter was 198 nm.

[0075] <Rating(5)> The contact angles of the surface-treated substrates MB-13 and 14 and the untreated glass plate with water were measured. The contact angle of the untreated glass plate with water was about 68°. In contrast, the contact angle of the surface-treated substrate MB-13 was about 40°, and that of the surface-treated substrate MB-14 was about 41°. The surface-treated substrate MB-13 was immersed in a 0.1% aqueous sodium hydroxide solution for 30 seconds and then dried. The contact angle of the surface measured in the same manner was about 31°. It is believed that the carboxyl group in the silane coupling agent used was neutralized and ionized, improving the hydrophilicity of the surface and decreasing the contact angle. [Industrial Applicability]

[0076] By using the silane coupling agent of the present invention, it is possible to produce a surface-treated inorganic oxide having improved dispersibility, filling property, fluidity, hydrophilicity, etc. This surface-treated inorganic oxide is useful as a filler or colorant to be blended into various coating agents, etc., and is expected to be developed into articles used in various fields, such as water-based paints, oil-based paints, water-based inks, water-based inkjet inks, solvent-based inkjet inks, ultraviolet-curable inkjet inks, semiconductor encapsulants, display members, electronic component members, refractive index control films, heat-shielding films, magnetic fluids, and phosphors.

Claims

1. A silane coupling agent used in surface treatment of an inorganic oxide, A silane coupling agent which is a compound represented by the following general formula (1) or (2): (In the general formulas (1) and (2), R represents a hydrocarbon group having 1 to 18 carbon atoms, and R 1 represents a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms; R 2 represents a methyl group, an ethyl group, an n-propyl group, or an isopropyl group; 3 each independently represents a hydrogen atom or a methyl group, m represents a number from 0 to 2, and n represents a number from 10 to 70.

2. 2. A surface-treated inorganic oxide, which is an inorganic oxide surface-treated with the silane coupling agent according to claim 1.

3. The surface-treated inorganic oxide according to claim 2, wherein the inorganic oxide is inorganic oxide fine particles having an average particle size of 10 nm to 100 μm.

4. The surface-treated inorganic oxide according to claim 3, which is a treated product obtained by surface-treating 100 parts by mass of the inorganic oxide fine particles with 0.5 to 50 parts by mass of the silane coupling agent.

5. The surface-treated inorganic oxide according to claim 3, wherein the inorganic oxide fine particles are at least one selected from the group consisting of titanium dioxide, zinc oxide, silica, alumina, and composite oxide pigments.

6. An article comprising the surface-treated inorganic oxide according to any one of claims 2 to 5.

Citation Information

Patent Citations

  • Moisture-curable composition

    JP1991168245A

  • Optical disk player and optical disk playback method

    JP2004071003A

  • Hardened hydrophilic components

    JP2009538376A

  • Surface-modified pigment particles, method for preparing them, and their applications

    JP2015516022A

  • Bifunctional poly(alkylene oxides) with aminoalkyl and unsaturated ends and derivatives thereof

    JP2018522991A