Floor coating composition

A water-based polyurethane resin floor coating with high biomass content polyols and PDI addresses weather resistance and yellowing issues, ensuring durable and environmentally friendly flooring.

JP2024148240AInactive Publication Date: 2024-10-18NIHON TOKUSHU TORYO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023061196
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing water-based polyurethane resin flooring materials suffer from weather resistance issues and yellowing of the coating film, and there is a need for environmentally friendly alternatives.

Method used

A water-based polyurethane resin floor coating composition using water-dispersed polyols and pentamethylene diisocyanate (PDI) with a biomass content of 55% or more, combined with biomass polyols, to enhance weather resistance and prevent yellowing.

Benefits of technology

The composition achieves excellent weather resistance and prevents yellowing, maintaining a long-lasting beautiful appearance both indoors and outdoors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148240000001
    Figure 2024148240000001
Patent Text Reader

Abstract

To resolve deficiencies in floor coatings, such as weather resistance and yellowing of the coating layer, and reduce the use of resins derived from fossil-based resources, such as petroleum, thereby resolving the environmental issues.SOLUTION: An aqueous polyurethane resin-based floor coating composition includes: water-dispersed polyols, including a biomass polyol; and PDI (pentamethylene diisocyanate / polyisocyanate of pentamethylene diisocyanate), including PDI with a biomass level of 55% or more on a dry basis.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a floor coating composition. [Background technology]

[0002] So-called coated flooring materials, which are formed by applying paint to floors, are widely used both indoors and outdoors. Examples of resin-based materials include epoxy resin-based materials, which can form a coating film with high hardness, and polyurethane resin-based materials, which are highly versatile and can form a durable coating film. Compared to solvent-based resins, water-based resins are more environmentally friendly and have the advantages of being easier to handle and having less odor. However, even water-based polyurethane resin-based floor coating materials that use crude MDI (4,4'-diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate) have issues with weather resistance and the coating film yellowing.

[0003] In addition, due to the growing awareness of environmental issues, paint products that use resin raw materials derived from fossil resources instead of biomass-derived resin raw materials such as animals and plants have been attracting attention in recent years. For example, Patent Document 1 discloses a coating agent containing a biomass polyol composition in a polyol resin as an anchor coating agent for melt extrusion lamination. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6948485 Summary of the Invention [Problem to be solved by the invention]

[0005] There is a demand for floor coating materials that can improve the inherent shortcomings of water-based polyurethane resin-based floor coating materials and also respond to the growing awareness of environmental issues.

[0006] Therefore, an object of the present invention is to develop a water-based polyurethane resin-based floor coating material that has excellent weather resistance and does not cause yellowing of the coating film. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by the following configuration.

[0008] <1> A water-based polyurethane resin-based coating flooring composition comprising a water-dispersible polyol and PDI (polyisocyanate of pentamethylene diisocyanate-pentamethylene diisocyanate). The water-dispersible polyol includes a biomass polyol. The PDI is characterized by having a biomass content of 55% or more per dry weight. A floor coating composition. <2> A water-based polyurethane resin-based coating floor material composition comprising a water-dispersible polyol and PDI. The water-dispersible polyol contains a biomass polyol, and the biomass content of the total polyol resin is 20% or more. PDI is characterized by having a biomass content of 35% or more per dry weight in polyurethane resin produced by polymerization reaction of PDI with a biomass content of 55% or more. A floor coating composition. Effect of the Invention

[0009] The aqueous polyurethane resin-based coating floor material composition of the present invention has excellent weather resistance and can be used both indoors and outdoors. In addition, the coating film does not yellow, so the beauty of the coated floor can be maintained for a long period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The floor coating composition according to the present invention will be described below. Each of the configurations and combinations thereof in the following embodiments is merely an example, and the present invention is not limited to the embodiments. In this specification, the symbol "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0011] <Solvent> The aqueous polyurethane resin-based floor coating composition of the present invention uses water as a solvent. The mixing ratio of water is adjusted as desired, taking into consideration the mixing and dispersing properties, coating workability, dry film-forming properties, white cement ratio, etc., of the floor coating composition of the present invention.

[0012] <Polyol> The polyol may be a polyether polyol, a polymer polyol, or a polyester polyol. In the present invention, it is essential that the polyols used include a biomass polyol having a biomass degree of 20% or more.

[0013] Biomass polyol is a polyol whose raw material is not derived from fossil raw materials, but from raw materials derived from animals and plants. The biomass polyol to be mixed in the floor coating material of the present invention can be substituted for the total amount of polyol at any ratio. That is, it is also possible to use the total amount as biomass polyol. When the biomass polyol used in the present invention is used in a floor coating material, the effect on the physical properties of the floor coating material is small when the hydroxyl value and molecular weight are the same as those of the polyols used in conventional floor coating materials.

[0014] <Isocyanate> The floor coating material of the present invention can use, as an isocyanate, biomass PDI (polyisocyanate of pentamethylene diisocyanate and pentamethylene diisocyanate) with a biomass content of 55% or more. Biomass PDI can be substituted for the total amount of isocyanate at any ratio. In other words, it is possible to use the entire amount as biomass PDI. As an isocyanate other than biomass PDI, it is possible to use conventionally known isocyanates in combination, but in order to avoid the problem of yellowing of the coating film, it is preferable to use HDI (hexamethylene diisocyanate) in combination with various conventionally known petroleum-derived isocyanates.

[0015] Both biomass polyol and biomass PDI are resins made from animal and plant-derived raw materials, rather than from conventional fossil-derived raw materials. Plant-derived raw materials include sugar and starch from castor beans (castor oil), corn, sugar cane, sugar beet, sorghum, cashew nuts, soybeans, oil palm, etc., which are transformed into different substances through fermentation, etc., to synthesize monomers, which are then polymerized into polymers.

[0016] <Other ingredients> In addition to the above-mentioned compounds, the coated floor material of the present invention can contain additives such as thickeners, thixotropy-imparting agents, defoamers, dispersants, UV absorbers, rust inhibitors, and mildew inhibitors, as well as other additives used in conventionally known coated floor materials, if necessary, within the range that does not impair the effects of the present invention.

[0017] The floor coating material of the present invention can be colored by adding color pigments, dyes, etc. as necessary. Colorants such as color pigments and dyes can be used in the form of powder or paste.

[0018] The floor coating material of the present invention can be produced by a conventionally known paint production method and production process, using a high-speed blade type agitator, an open or pressure kneader, a roll mill, a grain mill, or other paint production equipment.

[0019] The coated floor material of the present invention can be painted by a conventionally known painting method. That is, painting using various on-site painters such as brush painting, roller painting, flow painting, trowel painting, air spray painting, and airless spray painting can be applied. EXAMPLES

[0020] The present invention will be described in more detail with reference to the following examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention.

[0021] As shown in Table 1 below, floor coating materials were prepared using the compositions of Examples to Comparative Example 3, and were applied to mortar boards using a trowel. Each coated test board was cured for 48 hours at 23°C. The dry coating thickness of each coated test board was 1.5 to 2 mm. By increasing the ratio of powder and pigment, a coating film of about 10 mm can be formed. [Table 1] (The values ​​in the table are parts by weight) TIFF2024148240000001.tif49108

[0022] [Yellowing resistance] Each test panel was painted in a pale color that allows easy identification of changes in hue, and placed in a xenon lamp accelerated weathering tester. After 240 hours, Δb was measured using a color difference meter, and yellowing resistance was evaluated based on the Δb value. A Δb value of 1.5 or less was evaluated as ◯, and a value of over 10.0 was evaluated as ×.

[0023] [Impact resistance] Each painted test panel was subjected to an impact test as specified in the "Test Method for Impact Strength of Coated Floors (NNK-002 2020)" in the Coated Floor Handbook compiled by the Japan Coating Floor Industry Association. The coating surface was visually inspected after dropping a weight five times, and if cracks, lifting, peeling, or other abnormalities were found on the coating surface, it was marked as "X", and if there were no abnormalities on the coating surface, it was marked as "O".

[0024] [Coating film appearance] After each coated test panel was left to cure for 48 hours at 23°C, the dried coating surface was visually observed. If the surface was smooth and uniform, it was rated as ◯, and if any abnormalities such as noticeable foaming marks or unevenness were observed on the surface, it was rated as ×.

[0025] 〔result〕 According to the test results of the examples to the comparative example 3, the coated floor material of the present invention has a high biomass content of 45% in the urethane crosslinking component resin, and is an excellent coated floor material in terms of environmental issues compared to conventional coated floor materials derived from fossil raw materials. Furthermore, the coated floor material has been realized with significant improvements in the yellowing resistance of the coating film, the appearance of the coating film, and the impact resistance of the coating film, which were considered to be problems with conventional water-based polyurethane resin-based coated floor materials.

[0026] Other embodiments The above-mentioned embodiments are merely examples of the present invention, and the present invention is not limited to these examples, and these examples may be combined with well-known, commonly used, or publicly known techniques, or may be partially replaced. In addition, modified inventions that can be easily conceived by a person skilled in the art are also included in the present invention.

Claims

1. A water-based polyurethane resin-based coating flooring composition comprising a water-dispersible polyol and PDI (pentamethylene diisocyanate-pentamethylene diisocyanate polyisocyanate). The water-dispersible polyol includes a biomass polyol. The PDI includes a PDI with a biomass content of 55% or more per dry weight. A floor coating composition.

2. A water-based polyurethane resin-based coating floor material composition comprising a water-dispersible polyol and PDI. The water-dispersible polyol contains a biomass polyol, and the biomass content of the total polyol resin is 20% or more. PDI is characterized in that the biomass content per dry weight of the polyurethane resin produced by polymerization of PDI with a biomass content of 55% or more is 35% or more. A floor coating composition.

Citation Information

Patent Citations

  • Cement composition and polyol composition for formation of coating floor

    JP2020015647A

  • Curable polyurethane resin composition, cured object, and layered product

    WO2022210112A1

  • Anchor coating agent for melt extrusion lamination and laminate