Desulfurization method of molten pig iron
By accurately predicting the hot metal surface position at the vortex center and adjusting the impeller's relative position, the desulfurization efficiency is enhanced, reducing quicklime usage and slag generation, thus improving steel production efficiency and environmental sustainability.
Patent Information
- Application Number
- JP2023061680
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing desulfurization methods using KR equipment face challenges in achieving high desulfurization efficiency, leading to excessive quicklime usage and slag generation, which affects steel production efficiency and environmental impact.
The method involves controlling the impeller's relative position (R-dip) by accurately predicting the hot metal surface position at the vortex center using Gaussian, sigmoid, or Lorentzian functions, allowing precise adjustment of impeller speed and position to enhance desulfurization efficiency.
This approach significantly improves desulfurization efficiency, reducing quicklime consumption and slag generation, thereby enhancing steel production productivity and minimizing environmental impact.
Smart Images

Figure 2024148498000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for removing sulfur (desulfurization) from molten iron in the steelmaking industry. [Background technology]
[0002] Molten iron (hot metal) obtained by reducing iron ore contains impurities, and steel with a desired composition is produced by removing unnecessary components from the hot metal and adding necessary elements. As a method for desulfurizing hot metal, a method (mechanical stirring method) has been known in which a desulfurizing agent such as quicklime is added to the hot metal, and the desulfurizing agent is diffused into the hot metal and reacted with the hot metal by stirring with an impeller. Such a method in which an impeller is immersed in the hot metal and rotates to stir the hot metal is usually called the KR (Kanbara Reactor) method, and the equipment is called the KR equipment. Patent Documents 1 to 3 disclose methods for desulfurizing hot metal using the KR method. Hereinafter, unless otherwise specified, "desulfurization" simply means desulfurization of hot metal.
[0003] The desulfurization method using the KR method is briefly explained. Figure 1 shows a cross-sectional view of the state of molten iron in a vessel (also called a molten iron vessel or ladle), with molten iron (molten iron) 2 contained in the molten iron vessel 1. The surface position of the molten iron when stationary is indicated by dotted line 6 in Figure 1. First, prior to the start of the desulfurization process, an impeller is inserted into the stationary molten iron and begins to rotate. When the impeller is rotated, a vortex is generated in the molten iron, and centrifugal force causes the peripheral parts to rise and the center of the molten iron (the impeller shaft) to become depressed, resulting in the molten iron at position 4 in Figure 1.
[0004] After that, the desulfurization agent is added to start the desulfurization process. Immediately after the start of the desulfurization process (the initial stage of the process), the temperature of the added desulfurization agent is low, so it does not turn into slag but floats on the surface of the molten pig iron. The desulfurization agent becomes hot as it is stirred by the rotation of the impeller and repeatedly comes into contact with the high-temperature molten pig iron, and is mixed with slag containing SiO2 (hereinafter sometimes referred to as molten pig iron slag) that has been mixed in from the molten pig iron container and with components that promote a low melting point (e.g. Al2O3, FeO) that are mixed into the desulfurization agent to form low-melting point complex oxides such as CaO-SiO2-Al2O3-FeO. Some of these oxides and other materials liquefy at approximately 800°C or higher and incorporate solids such as quicklime to become slag, a mixture of solid and liquid, which turns into slag (liquefaction).
[0005] The slag-formed desulfurization agent becomes pseudo-particles, which are entrained in the vortex of the molten iron, are thrown outward by the rotational energy of the impeller and diffuse into the molten iron, and then float to the surface of the molten iron by the molten iron flow. In this way, the entire desulfurization agent is entrained in the molten iron, and there is no more remaining desulfurization agent on the molten iron surface. As this process is repeated and the desulfurization of the desulfurization agent progresses, the liquid phase of the pseudo-particles approaches CaO saturation, improving the desulfurization ability, and desulfurization progresses through this liquid phase. As desulfurization progresses, the sulfur in the molten iron reacts with quicklime to produce calcium sulfide, which becomes slag (dotted line 5 in Figure 1) and is separated from the molten iron. By repeating this process, the sulfur can be removed from the molten iron. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-247910 A [Patent Document 2] JP 2007-262501 A [Patent Document 3] JP 2010-185114 A [Patent Document 4] JP 2004-250742 A Summary of the Invention [Problem to be solved by the invention]
[0007] Desulfurization treatment using KR equipment generally shows high desulfurization efficiency, but several proposals have been made to further increase the desulfurization efficiency. Patent Document 1 proposes that a higher desulfurization efficiency can be obtained by setting the ratio of the bath depth to the inner diameter of the treatment vessel to 1.2 to 2.0. Patent Document 2 proposes that a higher desulfurization efficiency can be obtained by making the depth of the molten pig iron recess at the vortex center greater than the sum of the impeller immersion depth, which is the distance from the still molten iron surface to the upper end of the impeller, and the impeller height. Patent Document 3 proposes that a higher desulfurization efficiency can be obtained by setting the ratio of the impeller immersion depth to the molten pig iron recess depth at the vortex center to 0.6 to 0.8. Patent Document 4 proposes measuring the surface level of the molten pig iron in the ladle with microwaves at two points, calculating the stirring flow rate of the molten pig iron from the level difference, and controlling the impeller rotation speed and position so that the calculated stirring flow rate becomes a preset flow rate.
[0008] However, even if these methods are used, the total amount of quicklime added does not contribute to the desulfurization of the molten pig iron, and there is room for further improvement in desulfurization efficiency. If the desulfurization efficiency is improved, the amount of quicklime added can be reduced, and the amount of slag generated can be reduced accordingly. Reducing the amount of slag generated can reduce the amount of iron (Fe) taken out of the molten pig iron together with the slag, thereby improving the productivity of steel from iron ore. Furthermore, reducing the amount of slag generated leads to a reduction in the environmental load. For these reasons, there is a demand for further improvement in desulfurization efficiency. An object of the present invention is to further improve the desulfurization efficiency in desulfurization treatment using KR equipment. [Means for solving the problem]
[0009] In the desulfurization process using the KR equipment, as proposed in Patent Document 3, the ratio of the impeller immersion depth to the molten pig iron recession depth at the vortex center is controlled to be within a certain range, and a certain degree of effectiveness is achieved. However, when observing the desulfurization process, it is observed that the desulfurization agent floats on the surface of the molten pig iron immediately after it is added. At this time, most of the desulfurization agent is not incorporated into the molten pig iron, so it is considered that the added desulfurization agent does not exert a sufficient desulfurization effect. Eventually, it is observed that the desulfurization agent turns into slag and begins to be incorporated into the vortex of the molten pig iron.
[0010] In actual operation, the surface position of the vortex center of the molten iron being stirred cannot be confirmed from the outside. For example, since the impeller is at the vortex center, it is actually impossible to observe the exact surface position of the vortex center (see Figure 2). For this reason, the surface position of the vortex center is estimated in advance from the impeller rotation speed, etc., and this position is controlled as being constant during operation. Even if the molten iron surface could be observed from outside the molten iron vessel with a camera, etc., the vortex center cannot be seen, so the most that could be done was to assume a constant depth of the vortex center and control the impeller rotation speed so that the molten iron position that can be observed would be constant.
[0011] Furthermore, even if the molten iron stirring flow velocity is calculated from the level difference between two points on the molten iron surface as proposed in Patent Document 4 and the impeller position is controlled so that the flow velocity becomes a preset flow velocity, this cannot be immediately applied to desulfurization treatment as proposed in Patent Document 3, which controls the desulfurization process by the ratio of the impeller immersion depth to the molten iron recession depth at the vortex center.
[0012] Furthermore, the method proposed in Patent Document 4 involves comparing a level difference previously determined by an experiment with a data table of flow velocity, and determining flow velocity from calculations based on fluid mechanics. However, these methods require the preparation of a huge amount of experimental data to determine the fluid velocity, and the comparison takes time. In addition, fluid mechanics calculations take a long time to perform, so they cannot be applied to practical feedback control.
[0013] That is, when controlling the ratio of the impeller immersion depth to the molten pig iron recession depth at the vortex center to a specified value, it is difficult to accurately grasp the molten pig iron recession depth at the vortex center, and it was thought that the actual ratio of the impeller immersion depth to the molten pig iron recession depth at the vortex center was not correctly grasped in real time (time including a time delay to an extent that is tolerable for actual control). Therefore, it was envisioned that if the molten pig iron surface position of the vortex center of the molten pig iron during desulfurization treatment could be predicted accurately and in real time, the control accuracy of the ratio of the impeller immersion depth to the molten pig iron recession depth at the vortex center (hereinafter, this ratio will be referred to as the impeller relative position R-dip) would improve and desulfurization efficiency could be improved, and the development was continued, leading to the following findings.
[0014] (A) The surface shape of the molten iron being stirred by the impeller is symmetrical around the impeller's rotation axis, and can be expressed two-dimensionally when viewed in a cross section including the rotation axis. Therefore, it was thought that if only the surface shape of the molten iron during stirring could be grasped, the position of the molten iron surface at the vortex center could be predicted in a short time. Therefore, it was found that the surface shape of the molten iron during stirring can be approximated by a function, by carrying out observations of the actual molten iron surface and simulation analysis of the surface shape of the molten iron during stirring. In particular, it was found that the surface shape of the molten iron during stirring can be approximated with a high degree of accuracy by Gaussian functions and sigmoid functions. These function approximations make it possible to perform calculations in an extremely short time compared to fluid dynamics calculations.
[0015] (A) In the case of function approximation, particularly approximation using a Gaussian function or a sigmoid function, it was found that an approximation formula can be determined and the molten iron level position of the vortex center can be obtained with high accuracy if at least two positions of the molten iron surface that are at different horizontal distances from the vortex center are known. According to this, the molten iron level position of the vortex center of the molten iron flow can be obtained directly by measuring the levels of two points on the molten iron surface, so there is no need to first obtain the flow velocity as in Patent Document 4, and the molten iron level position of the vortex center can be obtained with high accuracy in an extremely short time.
[0016] (c) The means for measuring the molten iron surface position is not particularly limited. For example, a measurement method using an external laser, microwave, or ultrasonic wave can be adopted. A laser emitter and a receiver, or an ultrasonic oscillator and a receiver, may be placed directly above the molten iron surface. Moreover, as a measure against radiant heat from the molten iron, these emitters and receivers may be placed obliquely to the molten iron surface. The position may be set according to the compatibility with surrounding equipment.
[0017] From the above findings, it is possible to quickly and accurately predict the impeller relative value (R-dip), and the R-dip of the impeller position during desulfurization can be controlled with high accuracy by suppressing the effect of time delay. It has been confirmed that this makes it possible to increase the desulfurization efficiency throughout the entire KR process (desulfurization process). The present invention has been made based on these findings, and the gist of the invention is as follows.
[0018] [1] A molten iron desulfurization method for performing a desulfurization treatment by stirring molten iron in a vessel by rotation of an impeller and introducing a desulfurization agent into the molten iron, When the distance from the surface position of the molten iron when the molten iron is stationary in the vessel (the reference position of the molten iron surface) to the deepest position of the depression in the molten iron surface caused by stirring the molten iron is H, and the distance to the top end of the impeller is h, measuring the positions of at least two points on the surface of the molten iron, and predicting a distance H from the measured positions on the surface of the molten iron to a deepest position of a depression on the surface of the molten iron using a preset function; A molten metal desulfurization method, characterized in that one or both of the impeller position and the impeller rotation speed are controlled in accordance with R-dip, which is expressed as the ratio h / H of the distance h to the top end of the impeller and the distance H to the deepest position of a depression in the molten metal surface. [2] The molten metal desulfurization method according to [1], wherein the predetermined function is one or a combination of two or more functions selected from a Gaussian function, a sigmoid function, a Lorentz function, and a multi-order function. [3] The method for desulfurizing molten metal according to [1] or [2], wherein when the R-dip is greater than a predetermined R-dip target upper limit value or smaller than a predetermined R-dip target lower limit value, one or both of the rotation speed of the impeller and the distance h to the upper end of the impeller are changed. [4] The molten metal desulfurization method according to [3], wherein a rotation speed of the impeller is increased when the R-dip is greater than the target R-dip upper limit value, and the rotation speed of the impeller is decreased when the R-dip is smaller than the target R-dip lower limit value. [5] The molten metal desulfurization method according to [3] or [4], wherein the distance h to the upper end of the impeller is decreased when the R-dip is greater than the target R-dip upper limit value, and the distance h to the upper end of the impeller is increased when the R-dip is smaller than the target R-dip lower limit value. Effect of the Invention
[0019] According to the present invention, the efficiency of desulfurization of molten iron can be increased. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the state of molten iron in a molten iron vessel. [Diagram 2] Figure 2 is a conceptual diagram showing the molten iron surface position in a molten iron vessel, where Figure 2(a) is a conceptual diagram showing the molten iron surface position in an actual vessel, and Figure 2(b) is a conceptual diagram showing the molten iron surface position obtained by conventional observation. [Diagram 3] FIG. 3 is a conceptual diagram showing the molten iron surface position estimated from the Gaussian function. [Figure 4] FIG. 4 is a conceptual diagram showing the molten iron surface position estimated from the sigmoid function. [Diagram 5] FIG. 5 is a conceptual diagram showing the molten iron surface position estimated from the Lorentz function. [Figure 6] FIG. 6 is a flow diagram for explaining an example of a control flow of a desulfurization method to which the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention can be used to remove sulfur components from molten iron (hot metal). For example, the present invention can be used to remove sulfur components from molten iron (hot metal) obtained by reducing iron ore in a blast furnace. The present invention can also be applied to remove excess sulfur from molten iron (this molten iron is sometimes called molten iron) melted in an electric furnace.
[0022] [Desulfurization equipment] The present invention can be applied to a molten pig iron desulfurization method in which the molten pig iron in a molten pig iron vessel (sometimes called a ladle) is stirred by the rotation of an impeller and a desulfurization agent is added to the molten pig iron to perform desulfurization. There are no particular limitations on the type of desulfurization device as long as it stirs the molten pig iron by the rotation of an impeller, but generally, a mechanical stirring desulfurization device or a KR facility is applicable.
[0023] [Impeller relative position (R-dip): h / H] Figure 1 shows a cross-sectional view of the state of molten iron in a molten iron vessel. Molten iron (molten pig iron) 2 is contained in the molten pig iron vessel 1. The surface position 6 of the molten pig iron 2 when stationary (sometimes simply called the molten pig iron stationary position) is shown by a dotted line. The molten pig iron is stirred by the rotation of the impeller 3, and a vortex is generated as the impeller rotates. Looking at the vortex in cross section, the molten pig iron position 4 forms a depression 7 centered on the impeller axis (solid line in Figure 1). The vertical distance between the deepest position of the depression 7 of this molten pig iron position (also called the vortex center, usually located on the impeller axis) and the molten pig iron stationary position is defined as H (depression depth). The vertical distance between the top of the impeller and the molten pig iron stationary position is defined as h (impeller depth). At this time, the ratio h / H (impeller relative position (R-dip)) of the distance h from the stationary position of the molten iron to the top end of the impeller to the distance H to the deepest position of the depression on the surface of the molten iron is used as an index of how deep the impeller is located relative to the depression in the molten iron (the depression caused by the vortex). That is, when h / H=1, the top end of the impeller is at the deepest part of the depression caused by the vortex. In other words, this means that the entire impeller is just submerged in the molten iron. When h / H exceeds 1, this indicates that the entire impeller is submerged in the molten iron. Conversely, when h / H is less than 1, this indicates that a part or the entire impeller is at least above the depression in the molten iron.
[0024] [Impeller position control] By making the impeller position relatively shallow at the beginning of the desulfurization process, a strong stirring flow can be formed on the surface, and the desulfurization agent can be promoted. This is thought to be because the mixed hot metal slag and the partially liquefied desulfurization agent diffuse shallowly into the hot metal and float to the surface of the hot metal in a short time, promoting the slag formation of the remaining desulfurization agent. When the desulfurization agent turns into slag, it is taken into the hot metal as described above, so by deepening the impeller position accordingly, the stirring flow reaches a deep position in the hot metal, promoting the diffusion of the desulfurization agent. For this reason, it is recommended to make the impeller position shallow at the start of the desulfurization process and deepen it as the desulfurization process progresses. In other words, it is recommended to control the impeller position by changing the impeller relative position (R-dip) h / H according to the progress of the desulfurization process. Of course, the impeller relative position (R-dip) may be controlled to be constant during the desulfurization process. Conventionally, the main practice during desulfurization was to control R-dip to a constant value.
[0025] The position of the molten iron when a vortex is occurring (line 4 in Figure 1) naturally changes as the impeller rotation speed and other factors change. In this case, the impeller top end position h can be easily determined from the impeller shape and the position of the impeller shaft. Meanwhile, the deepest position of the molten iron depression (the molten iron surface position at the center of the molten iron vortex) cannot actually be confirmed due to the presence of the impeller. However, as will be explained below, this can be quickly estimated by the present invention. As a result, the impeller relative position (R-dip)h / H can be determined in real time according to each situation.
[0026] [Observation of the molten iron surface position] When controlling the impeller relative position R-dip, it is extremely important to accurately grasp the distance H from the stationary position of the molten iron to the deepest position of the depression on the molten iron surface in order to improve control accuracy. An image of the relationship between the molten iron surface position and the position of the impeller during actual operation is shown in Figure 2(a). As can be seen from Figure 2(a), the impeller 3 rotates around the impeller rotation axis 12, and the only molten iron surface position that can actually be observed is the outside of the impeller 3. An image of only the actually measured molten iron surface position is shown in Figure 2(b). The dotted line in Figure 2(b) indicates the observed molten iron surface position 13. As such, the distance H to the deepest position of the depression in the molten iron surface cannot be observed, and must be estimated. Conventionally, it was merely determined empirically from the impeller rotation speed, and no control method was implemented that fed back the actual molten iron surface position to the control.
[0027] [Measurement of the molten iron surface position] The means for measuring the molten iron surface position is not particularly limited. For example, a measurement method using an external laser, microwave, or ultrasonic wave can be adopted. A laser emitter and a receiver, or an ultrasonic oscillator and a receiver, may be placed directly above the molten iron surface. Moreover, as a measure against radiant heat from the molten iron, these emitters and receivers may be placed obliquely to the molten iron surface. The position may be set according to the compatibility with surrounding equipment. Note that FIG. 1 shows a schematic diagram of two laser length measuring devices 11 placed directly above the molten iron 2 to measure the distance to the molten iron surface 4.
[0028] The positions of the measurement points of the molten pig iron surface position are not particularly limited as long as at least two measurement points at different distances from the impeller rotation axis are secured. Since the molten pig iron surface is symmetrical with respect to the rotation axis (impeller rotation axis), the positions of the two points may be different distances from the rotation axis. If the distance from the rotation axis to the measurement points is the same (i.e., if they are located on a concentric circle when the molten pig iron is viewed from above), the two unknowns cannot be determined because the measurements are taken at the same distance when the molten pig iron is viewed in cross section (i.e., they are at the same position). When the diameter of the molten pig iron ladle is D, it is preferable that at least two measurement points are separated by 0.05D or more. It is preferable that the measurement points are separated by 0.06D or more, 0.07D or more, 0.08D or more, 0.09D or more, 0.10D or more, 0.12D or more, 0.14D or more, 0.16D or more, 0.18D or more, or 0.20D or more.
[0029] [Function for predicting the molten iron surface position] The surface shape of the molten iron being stirred by the impeller is symmetrical around the impeller's rotation axis, and can be expressed two-dimensionally when viewed in a cross section including the rotation axis. If it is possible to grasp only the surface shape of the molten iron while it is being stirred, there is no need for a three-dimensional analysis of the entire molten iron or a complex analysis using fluid dynamics, and calculation processing can be performed in an extremely short time.
[0030] Therefore, the shape of the molten pig iron surface during stirring was observed using a water model, a simulation, and the actual surface of the molten pig iron during stirring, and it was confirmed that the molten pig iron surface shape can be approximated by a function. The approximation function is not particularly limited, but preferably a Gaussian function, a sigmoid function, a Lorentzian function, a multi-order function, etc. can be applied. For example, one selected from the Gaussian function, the sigmoid function, the Lorentzian function, and the multi-order function, or a combination of two or more functions, may be used. It was confirmed that the Gaussian function, the sigmoid function, the Lorentzian function, the multi-order function, etc. can accurately express a curve close to the actual molten pig iron surface shape. These functions are easy to handle because the formulas themselves are not complicated, and the calculation time can be shortened. Figures 3 to 5 show examples of approximating the molten pig iron surface position using a Gaussian function, a sigmoid function, and a Lorentzian function. Since the molten pig iron surface position is axially symmetrical around the impeller rotation axis, the dashed line in the figure indicates the impeller rotation axis, and each figure shows only the right side of the impeller rotation axis. The solid line in each figure represents the molten iron surface position approximated by a function, and the dotted line (some parts overlap with the solid line and are not visible) represents the molten iron surface position actually observed. Each function is explained below.
[0031] [Gaussian function] The Gaussian function is expressed by the following equation 1.
number
[0032] The remaining unknown constants are c and d. Since there are two unknowns, c and d can be determined uniquely by substituting the position data of any two points on the molten iron surface into equation 1 as boundary conditions. When the position data (coordinates) of the two points are (x1, y1) and (x2, y2), c and d can be found as follows:
number
number
[0033] Figure 3 shows the molten pig iron surface position measured during KR treatment (desulfurization treatment) with actual molten pig iron, assuming a = 0.76 and b = 0, and the molten pig iron surface position estimated from the position data of two points on the molten pig iron surface and the Gaussian function. As can be seen from Figure 3, the actually observed molten pig iron surface position (dotted line) overlaps with the solid line to the extent that it is not visible to the naked eye.
[0034] In other words, if the position data of any two points on the molten iron surface, (x1, y1) and (x2, y2), are obtained, the constants c and d in equation 1 can be obtained from equations 2 to 5, and the molten iron surface shape can be obtained from equation 1 in combination with the previously set a and b. Then, in the obtained equation 1, x=0 becomes the molten iron surface position at the center of the molten iron swirl, so the distance H to the deepest position of the depression on the molten iron surface can be obtained.
[0035] If there are more than two points of position data for the molten iron surface (for example, there is data obtained by measuring three or four points), any two points may be selected from the position data, or the constants c and d may be determined from the acquired position data using a least squares method or the like. Although there is a possibility that accuracy may be improved by acquiring data at multiple points, it should be noted that the calculation time will be longer due to the additional calculation time required for the least squares method. As can be seen from Figure 3, even if there are only two points of data on the molten iron surface position, data useful for control can be obtained, so there is no problem if there is at least two points of position data for the molten iron surface.
[0036] [Sigmoid function] The sigmoid function is expressed by the following equation 6.
number
[0037] The remaining unknown constants are c and d. As with the Gaussian function, there are two unknowns, so c and d can be determined uniquely by substituting the position data of any two points on the molten iron surface into equation 6 as boundary conditions. When the position data (coordinates) of the two points are (x1, y1) and (x2, y2), c and d can be found as follows:
number
number
[0038] As in the case of the Gaussian function, Fig. 4 shows the molten pig iron surface position measured during KR treatment (desulfurization treatment) with actual molten pig iron, with a = 0.8 and b = 0, and the molten pig iron surface position estimated from the position data of two points on the molten pig iron surface and the sigmoid function. As in the case of the Gaussian function, as can be seen from Fig. 4, it can be confirmed that the actually observed molten pig iron surface position (dotted line) coincides with the predicted solid line to such an extent that it is not visible to the naked eye.
[0039] That is, if the position data of any two points on the molten iron surface, (x1, y1) and (x2, y2), are obtained, the constants c and d in equation 6 can be obtained from equations 7 to 10, and the molten iron surface shape can be obtained from equation 6 in combination with the previously set a and b. Then, in the obtained equation 6, x=0 becomes the molten iron surface position at the center of the molten iron swirl, so the distance H to the deepest position of the depression on the molten iron surface can be obtained.
[0040] As with the Gaussian function, if there are more than two pieces of position data on the molten iron surface (for example, there is data from measurements at three or four points), the constants c and d can be determined using the least squares method or similar from those pieces of position data, and although there is a possibility that accuracy will increase with multi-point data, it should be noted that this requires a lot of calculation time. As can be seen from Figure 4, considering that data useful for control can be obtained even with only two pieces of molten iron surface position data, there is no problem with the sigmoid function as long as there is at least two pieces of molten iron surface position data.
[0041] [Lorentz function] The Lorentz function is expressed by the following equation 11.
number
[0042] As a result of various experiments, it was confirmed that by setting a = 0.2 and b = 0.9 to 1.1, it is possible to estimate the surface shape of the molten iron being stirred within a range that does not cause problems in actual operation. The remaining unknown constants are c and d. As with the Gaussian function, there are two unknowns, so c and d can be determined uniquely by substituting the position data of any two points on the molten iron surface into equation 6 as boundary conditions. When the position data (coordinates) of the two points are (x1, y1) and (x2, y2), c and d can be found as follows:
number
number
[0043] As in the case of the Gaussian function, the molten iron surface position measured during KR treatment (desulfurization treatment) using actual molten iron, with a = 0.2 and b = 0.9 to 1.1, and the molten iron surface position estimated from the position data of two points on the molten iron surface and the Lorentz function are shown in Figure 5. As can be seen from Figure 5, as in the case of the Gaussian function, the actually observed molten iron surface position (dotted line) coincides with the predicted solid line to such an extent that it is not visible to the naked eye.
[0044] In other words, if the position data of any two points on the molten iron surface, (x1, y1) and (x2, y2), are obtained, the constants c and d in equation 11 can be obtained from equations 12 to 15, and the molten iron surface shape can be obtained from equation 11 in combination with the previously set a and b. Then, in the obtained equation 11, x=0 becomes the molten iron surface position at the center of the molten iron swirl, so the distance H to the deepest position of the depression on the molten iron surface can be obtained.
[0045] Also, as with the Gaussian and Lorentz functions, if there are more than two pieces of position data on the molten iron surface (for example, there is data from measurements at three or four points), it is advisable to determine the constants c and d using the least squares method or similar from the position data, and although there is a possibility that accuracy will increase with multi-point data, it should be noted that this requires time for calculation. As can be seen from Figure 5, considering that data useful for control can be obtained even with only two pieces of data on the molten iron surface position, there is no problem if there is at least two pieces of position data on the molten iron surface.
[0046] [Multidimensional Function] A multi-order function (for example, an nth-order function) is generally expressed by the following formula:
number
[0047] That is, in the case of a multi-order function, the more degrees of freedom the curve has, the higher the approximation accuracy is, but on the other hand, the number of constants increases, and the number of positions of the molten iron surface that serve as boundary conditions increases. In other words, in order to improve accuracy, not only is it necessary to increase the number of measurement points of the molten iron surface positions and solve the corresponding number of simultaneous equations, but the calculation time also increases with the increase in the order. Therefore, in consideration of the calculation time, a lower order is preferable. On the other hand, the approximation accuracy decreases when the order is reduced. As can be imagined from the shape of the molten iron surface during stirring, it is desirable to approximate with at least a fourth-order function. Therefore, the order of the approximation function is preferably 4 to 10. In addition, considering that it is symmetrical at x=0 (y-axis), it is recommended to set the boundary condition as follows: the first-order differential value at x=0 (y-axis) in Equation 16 is 0.
[0048] [Control method of R-dip] Using the impeller relative position (R-dip) indicated by the ratio h / H of the distance h to the upper end of the impeller and the distance H to the deepest position of the recess on the surface of the hot metal, there is no particular limitation on how to control it. It can be applied to conventional control methods (for example, the method described in Patent Document 3). No matter what kind of control method it is, since the accuracy of the R-dip value is improved by the present invention, the desulfurization efficiency improvement effect due to the control also increases accordingly.
[0049] For example, one or both of the impeller position and the impeller rotation speed can be controlled according to the impeller relative position (R-dip). As an example, the control method will be described based on FIG. 6.
[0050] [Measurement of hot metal surface position] The hot metal surface position is measured by a hot metal surface position measuring device. As described above, at least two points with different distances from the impeller shaft are measured.
[0051] [Estimation of the molten metal surface position at the center of the vortex] Based on the measured hot metal surface position as a boundary condition, the molten metal surface position at the center of the vortex of the hot metal is estimated by calculation using a function that approximates the preset hot metal surface shape. As the approximation function, for example, a Gaussian function, a sigmoid function, or a Lorentz-type function may be used.
[0052] [Calculation of R-dip] The obtained molten metal surface position at the center of the vortex is taken as the deepest position of the recess on the hot metal surface generated by stirring the hot metal, and the distance H from the hot metal surface position (hot metal surface reference position) when the hot metal in the container is stationary to the deepest position of the hot metal surface is obtained. The ratio h / H of the distance h from the hot metal surface reference position to the upper end position of the impeller and the distance H to the deepest position of the recess on the hot metal surface, that is, the impeller relative position (R-dip) is calculated.
[0053] [Comparison of R-dip] Evaluate how much the obtained R-dip (R-dip achievement) deviates from a predetermined R-dip target value (R-dip target value). For example, set an upper limit value (R-dip target upper limit value) and a lower limit value (R-dip target lower limit value) of R-dip so as to sandwich the R-dip target value. When the obtained R-dip achievement is greater than the R-dip target upper limit value or less than the R-dip target lower limit value, change one or both of the impeller rotation speed and the impeller position so that the R-dip achievement falls within the range between the R-dip target upper limit value and the target lower limit value (hereinafter, the range between these R-dip target upper limit value and target lower limit value is referred to as the "R-dip target range").
[0054] The R-dip target value, the R-dip target upper limit value, and the target lower limit value may be set according to the actual desulfurization treatment situation. If the smaller of the absolute value of the difference between the R-dip target value and the R-dip target upper limit value or the absolute value of the difference between the R-dip target value and the R-dip target lower limit value (R-dip management width) is made too small, the impeller conditions will be frequently changed, and in some cases, control may become impossible. For example, the lower limit of the ratio of the R-dip management width to the R-dip target value (R-dip management width / R-dip target value; hereinafter referred to as the management width ratio) may be set to 3%, preferably 4%, 5%, 6%, 7%, 8%, 9%, or 10%. On the other hand, if the management width ratio is made too large, the action will be delayed, and there may be cases where the desulfurization efficiency cannot be improved. It may be set according to the actual desulfurization device and the properties of the hot metal. For example, the upper limit of the management width ratio may be set to 30%, preferably 25%, 20%, 18%, 17%, 16%, or 15%.
[0055] <When R-dip deviates from the R-dip target range> When the actual R-dip (actual R-dip) becomes larger than the target upper limit of R-dip or smaller than the target lower limit of R-dip (i.e., when it falls outside the target R-dip range), an action may be taken to change either or both of the impeller rotation speed and impeller position. When the actual R-dip is between the target upper and lower limits of R-dip, it is determined that the desulfurization treatment is proceeding as planned, and therefore there is no need to take any action to change the impeller rotation speed or impeller position. Below, a description is given of the case when the actual R-dip falls outside the target R-dip range.
[0056] FIG. 6 shows an example in which only the impeller rotation speed is changed first. If the R-dip result is greater than the upper limit of the R-dip target, the rotation speed can be increased to deepen the molten metal surface position of the vortex center. This increases the distance H to the deepest position of the depression on the molten iron surface, so that R-dip=h / H can be reduced. On the other hand, if the R-dip result is less than the lower limit of the R-dip target, the rotation speed can be decreased to shallow the molten metal surface position of the vortex center. This reduces the distance H to the deepest position of the depression on the molten iron surface, so that R-dip=h / H can be increased. There is no particular limit to how much the rotation speed should be increased or decreased. Since this differs depending on the equipment conditions such as the shape of the desulfurization device and the shape of the impeller, and the properties of the molten iron, it may be set according to the desulfurization treatment conditions.
[0057] After changing the impeller speed, the molten iron surface position is measured again, and the actual R-dip is calculated based on the estimated data of the molten iron surface position of the vortex center. After that, the actual R-dip is compared with the target upper limit and lower limit of R-dip, and necessary actions are taken. Figure 6 shows a case where R-dip is calculated again after changing the impeller speed, and if the actual R-dip still does not fall within the target R-dip range, the next action is to change the impeller position. In this case, if the calculated actual R-dip is greater than the target upper limit of R-dip, the impeller position can be raised. This reduces the distance h from the reference position of the molten iron surface to the top end of the impeller, so that R-diph / H can be reduced. On the other hand, if the actual R-dip is smaller than the target lower limit of R-dip, the impeller position can be lowered. This increases the distance h to the top end of the impeller, so that R-dip=h / H can be increased. There is no particular limit on how much the impeller position is increased or decreased. Since this varies depending on equipment conditions such as the shape of the desulfurization device and the shape of the impeller, and the properties of the molten iron, it may be set according to the desulfurization treatment conditions.
[0058] After taking the above action, return to the initial response, measure the molten iron surface position again, calculate R-dip, and if R-dip does not fall within the target R-dip range, repeat the action.
[0059] In addition, while FIG. 6 shows a case where the first action when R-dip is not within the R-dip target range is to adjust the impeller rotation speed, and the second action is to adjust the impeller height, the order is not limited to this. For example, the impeller height may be adjusted first, and then the impeller rotation speed. Also, for example, the impeller rotation speed and the impeller height may be adjusted simultaneously. Furthermore, an action other than the adjustment of the impeller rotation speed or height may be taken. EXAMPLES
[0060] In the actual KR equipment, two laser length measuring devices were placed directly above the molten iron ladle to measure the position of the molten iron surface at any time. The two length measuring devices were placed at positions 0.35D and 0.44D from the impeller rotation axis when the molten iron ladle (ladle diameter D) was viewed vertically from above. The shape of the molten iron surface was approximated by a Gaussian function, a sigmoid function, and a Lorentz function from the molten iron surface positions obtained at any time from the two laser length measuring devices, and the deepest position of the depression on the molten iron surface (molten iron surface position of the vortex center) was estimated, and the estimated value was used to calculate R-dip and used for control. The target value (R-dip target value) of R-dip during desulfurization treatment was 0.45, the upper limit of R-dip target value was 0.50, and the lower limit of R-dip target value was 0.40, and the impeller position was controlled to maintain the R-dip within the target range determined by these. As a comparative example, similar to conventional operation, the preset molten iron position and the deepest position of the molten iron surface depression (molten iron surface position at the center of the vortex) H were kept constant, and the actually measured molten iron position was controlled to be R-dip = 0.45. In order to keep the test conditions (desulfurization conditions) the same, the tests were conducted using the same steel type and the same weight of molten iron.
[0061] The desulfurization efficiency was compared using the desulfurization reaction efficiency K_CaO (see Equation 21) obtained by measuring the sulfur content in the molten pig iron before and after the desulfurization process and dividing the logarithm of the ratio by the amount of quicklime added as a desulfurization agent per unit of the amount of molten pig iron. The results are shown as a relative evaluation with the desulfurization reaction efficiency in the conventional method set at 1.
number
[0062] From the above, it was confirmed that by measuring the molten iron surface position at any time, approximating the surface position with a pre-set function (Gaussian function, sigmoid function, Lorentz function) to calculate the position of the deepest part of the molten iron depression (vortex center), and applying this value to R-dip control, precise control can be achieved and desulfurization efficiency (desulfurization reaction efficiency) can be improved (increased). [Industrial Applicability]
[0063] The present invention can be used in the steel industry. [Explanation of symbols]
[0064] 1 Molten iron container (pot) 2 Molten iron (molten iron) 3 Impeller 4 Hot metal position (vortex) 5 Slag surface 6 Hot metal resting position 7 Molten iron recess 11 Hot metal surface position measuring device 12 Impeller rotating shaft 13 Observed molten iron surface position
Claims
1. A molten iron desulfurization method for performing a desulfurization treatment by stirring molten iron in a vessel by rotation of an impeller and introducing a desulfurization agent into the molten iron, When the distance from the surface position of the molten iron when the molten iron is stationary in the vessel (the reference position of the molten iron surface) to the deepest position of the depression in the molten iron surface caused by stirring the molten iron is H, and the distance from the top end of the impeller is h, measuring the positions of at least two points on the surface of the molten iron, and predicting a distance H from the measured positions on the surface of the molten iron to a deepest position of a depression on the surface of the molten iron using a preset function; A molten iron desulfurization method, characterized in that one or both of the impeller position and the impeller rotation speed are controlled in accordance with R-dip, which is expressed as the ratio h / H of the distance h to the top end of the impeller and the distance H to the deepest position of a depression in the molten iron surface.
2. 2. The molten metal desulfurization method according to claim 1, wherein the predetermined function is one or a combination of two or more functions selected from the group consisting of a Gaussian function, a sigmoid function, a Lorentz function, and a multi-order function.
3. 3. The molten metal desulfurization method according to claim 1, wherein when the R-dip is greater than a predetermined R-dip target upper limit value or smaller than a predetermined R-dip target lower limit value, one or both of the rotation speed of the impeller and the distance h to the upper end of the impeller are changed.
4. 4. The molten metal desulfurization method according to claim 3, wherein the rotation speed of the impeller is increased when the R-dip is greater than the target R-dip upper limit value, and the rotation speed of the impeller is decreased when the R-dip is smaller than the target R-dip lower limit value.
5. 4. The molten metal desulfurization method according to claim 3, wherein a distance h to an upper end of the impeller is decreased when the R-dip is greater than the target R-dip upper limit value, and the distance h to an upper end of the impeller is increased when the R-dip is smaller than the target R-dip lower limit value.
6. 5. The molten metal desulfurization method according to claim 4, wherein a distance h to an upper end of the impeller is decreased when the R-dip is greater than the target R-dip upper limit value, and the distance h to an upper end of the impeller is increased when the R-dip is smaller than the target R-dip lower limit value.
Citation Information
Patent Citations
Method for stirring molten iron
JP2001247910A
Method and apparatus for desulfurizing molten pig iron
JP2004250742A
Method for stirring molten metal using impeller
JP2007262501A
Method for desulfurizing molten iron
JP2010185114A