Desulfurization method of molten pig iron
By controlling the impeller position in the desulfurization process to enhance the incorporation of the desulfurization agent into hot metal, the method addresses inefficiencies in sulfur removal, improving efficiency and reducing slag generation and environmental impact.
Patent Information
- Application Number
- JP2023061687
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing desulfurization methods using KR equipment do not fully utilize the added quicklime, leading to inefficiencies in sulfur removal, which results in excessive slag generation and reduced steel productivity, along with environmental impacts.
Control the impeller position in the desulfurization process by adjusting the relative position h/H to optimize the incorporation of the desulfurization agent into the hot metal, promoting deeper penetration and extended floating time, thereby enhancing desulfurization efficiency.
Increased desulfurization efficiency reduces the amount of quicklime required, decreases slag generation, improves steel productivity, and minimizes environmental impact.
Smart Images

Figure 2024148503000002 
Figure 2024148503000003 
Figure 2024148503000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for removing sulfur (desulfurization) from molten iron in the steelmaking industry. [Background technology]
[0002] Molten iron (hot metal) obtained by reducing iron ore contains impurities, and steel with a desired composition is produced by removing unnecessary components from the hot metal and adding necessary elements. As a method for desulfurizing hot metal, a method (mechanical stirring method) has been known in which a desulfurizing agent such as quicklime is added to the hot metal, and the desulfurizing agent is diffused into the hot metal and reacted with the hot metal by stirring with an impeller. Such a method in which an impeller is immersed in the hot metal and rotates to stir the hot metal is usually called the KR (Kanbara Reactor) method, and the equipment is called the KR equipment. Patent Documents 1 to 3 disclose methods for desulfurizing hot metal using the KR method. Hereinafter, unless otherwise specified, "desulfurization" simply means desulfurization of hot metal.
[0003] The desulfurization method using the KR method is briefly explained. Figure 1 shows a cross-sectional view of the state of molten iron in a vessel (also called a molten iron vessel or ladle), with molten iron (molten iron) 2 contained in the molten iron vessel (ladle) 1. The surface position of the molten iron when stationary is indicated by dotted line 6 in Figure 1. First, prior to the start of the desulfurization process, an impeller is inserted into the stationary molten iron and begins to rotate. When the impeller is rotated, a vortex is generated in the molten iron, and centrifugal force causes the peripheral parts to rise and the center of the molten iron (the impeller shaft) to become depressed, resulting in the molten iron at position 4 in Figure 1.
[0004] After that, the desulfurization agent is added to start the desulfurization process. Immediately after the start of the desulfurization process (the initial stage of the process), the temperature of the added desulfurization agent is low, so it does not turn into slag but floats on the surface of the molten pig iron. The desulfurization agent becomes hot as it is stirred by the rotation of the impeller and repeatedly comes into contact with the high-temperature molten pig iron, and is mixed with slag containing SiO2 (hereinafter sometimes referred to as molten pig iron slag) that has been mixed in from the molten pig iron container and with components that promote a low melting point (e.g. Al2O3, FeO) that are mixed into the desulfurization agent to form low-melting point complex oxides such as CaO-SiO2-Al2O3-FeO. Some of these oxides and other materials liquefy at approximately 800°C or higher and incorporate solids such as quicklime to become slag, a mixture of solid and liquid, which turns into slag (liquefaction).
[0005] The slag-formed desulfurization agent becomes pseudo-particles, which are entrained in the vortex of the molten iron, are thrown outward by the rotational energy of the impeller and diffuse into the molten iron, and then float to the surface of the molten iron by the molten iron flow. In this way, the entire desulfurization agent is entrained in the molten iron, and there is no more remaining desulfurization agent on the molten iron surface. As this process is repeated and the desulfurization of the desulfurization agent progresses, the liquid phase of the pseudo-particles approaches CaO saturation, improving the desulfurization ability, and desulfurization progresses through this liquid phase. As desulfurization progresses, the sulfur in the molten iron reacts with quicklime to produce calcium sulfide, which becomes slag (dotted line 5 in Figure 1) and is separated from the molten iron. By repeating this process, the sulfur can be removed from the molten iron. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-247910 A [Patent Document 2] JP 2007-262501 A [Patent Document 3] JP 2010-185114 A Summary of the Invention [Problem to be solved by the invention]
[0007] Desulfurization treatment using KR equipment generally shows high desulfurization efficiency, but several proposals have been made to further increase the desulfurization efficiency. Patent Document 1 proposes that even higher desulfurization efficiency can be obtained by setting the ratio of the bath depth to the inner diameter of the treatment vessel to 1.2 to 2.0. Patent Document 2 proposes that even higher desulfurization efficiency can be obtained by making the recess depth of the molten pig iron at the vortex center larger than the sum of the immersion depth of the impeller, which is the distance from the still molten iron surface to the upper end of the impeller, and the height of the impeller. Patent Document 3 proposes that even higher desulfurization efficiency can be obtained by setting the ratio of the immersion depth of the impeller to the recess depth of the molten pig iron at the vortex center to 0.6 to 0.8.
[0008] However, even if these methods are used, the total amount of quicklime added does not contribute to the desulfurization of the molten pig iron, and there is room for further improvement in desulfurization efficiency. If the desulfurization efficiency is improved, the amount of quicklime added can be reduced, and the amount of slag generated can be reduced accordingly. Reducing the amount of slag generated can reduce the amount of iron (Fe) taken out of the molten pig iron together with the slag, thereby improving the productivity of steel from iron ore. Furthermore, reducing the amount of slag generated leads to a reduction in the environmental load. For these reasons, there is a demand for further improvement in desulfurization efficiency. An object of the present invention is to further improve the desulfurization efficiency in desulfurization treatment using KR equipment. [Means for solving the problem]
[0009] When observing the desulfurization process using KR equipment, it is observed that the desulfurization agent floats on the surface of the molten pig iron immediately after it is added. At this time, most of the desulfurization agent is not absorbed into the molten pig iron, so it is thought that the added desulfurization agent does not exert a sufficient desulfurization effect. Eventually, it is observed that the desulfurization agent turns into slag and begins to be absorbed into the vortex of the molten pig iron.
[0010] The inventors then realized that if the time required for the desulfurization agent to turn into slag in the early stage of the desulfurization process and the time it takes for the desulfurization agent to be incorporated into the molten iron flow could be shortened, the desulfurization efficiency could be increased, and that the desulfurization agent that has turned into slag and been incorporated into the molten iron flow could be allowed to penetrate deep into the molten iron and have enough time to rise to the surface. As a result of this development, they obtained the following findings.
[0011] (A) It was found that if the impeller is immersed deep from the beginning and starts rotating, the desulfurization agent stays on the surface of the molten pig iron outside the vortex, slowing down the slag formation, while the desulfurization agent that gets into the center of the vortex stays around the impeller axis and does not diffuse to the surroundings. It was also found that if the impeller position is too shallow, it splashes the molten pig iron near the surface.
[0012] (a) On the other hand, when the impeller position is shallow, the mixed molten pig iron slag and partially liquefied desulfurization agent diffuse shallowly into the molten pig iron and rise to the surface of the molten pig iron in a short time, promoting the conversion of the desulfurization agent remaining on the surface of the molten pig iron to slag, so the conversion progresses quickly and the converted desulfurization agent diffuses into the molten pig iron on the vortex. However, although the time required for conversion to slag was shortened, the desulfurization rate after the converted desulfurization agent diffuses into the molten pig iron on the vortex tended to be low.
[0013] (c) Simulations using a water model and numerical calculations revealed that the desulfurization agent does not reach the deep parts of the molten iron vessel (ladle) when the impeller position is shallow. It is estimated that the desulfurization agent therefore does not diffuse to the deep parts of the molten iron vessel (ladle), resulting in a decrease in the desulfurization rate. On the other hand, when the impeller position is deep, the desulfurization agent reaches the deep parts of the ladle and diffuses to the deep parts of the molten iron vessel (ladle). However, when the impeller position is too deep, the desulfurization agent that enters the center of the vortex is not entrained in the impeller as much, and remains around the impeller axis.
[0014] (e) From the above findings, it was found that by making the impeller position shallow when adding the desulfurization agent, the mixed molten pig iron slag and partially liquefied desulfurization agent diffuse shallowly into the molten pig iron and rise to the surface of the molten pig iron in a short time, promoting the conversion of the desulfurization agent remaining on the surface of the molten pig iron to slag, and then by making the impeller position deep, the desulfurization agent is carried by the vortex of the molten pig iron and diffuses to the depths of the molten pig iron container (ladle), thereby lengthening the time for the slag to rise to the surface of the molten pig iron (desulfurization reaction time during floating), thereby increasing the desulfurization rate, and thereby the desulfurization efficiency throughout the entire KR process can be improved.
[0015] (E) It was found that the slag formation status of the desulfurization agent can be evaluated from the temperature distribution on the molten pig iron surface because when the slag formation progresses and the entire desulfurization agent is taken into the vortex of the molten pig iron and starts to float, the temperature of the desulfurization agent rises and the difference with the molten pig iron temperature becomes small (within 100℃). Therefore, it was found that it is good to observe the temperature distribution on the molten pig iron surface and control the impeller position to be deeper when the low temperature part reaches a specified area ratio (about 30%).
[0016] The present invention has been made based on these findings, and the gist of the present invention is as follows.
[0017] [1] A molten iron desulfurization method for performing a desulfurization treatment by stirring molten iron in a vessel by rotation of an impeller and introducing a desulfurization agent into the molten iron, When the distance from the surface position of the molten iron when the molten iron is stationary in the vessel (the reference position of the molten iron surface) to the deepest position of the depression in the molten iron surface caused by stirring the molten iron is H, and the distance to the top end of the impeller is h, A molten metal desulfurization method, characterized in that the impeller position is controlled by changing the relative position h / H of the impeller in accordance with the progress of desulfurization treatment. [2] The method for desulfurizing molten iron according to [1], further comprising: evaluating the progress of the desulfurization treatment based on an area ratio of the desulfurizing agent not converted into slag on the surface of the molten iron; and controlling an impeller position based on the evaluation. [3] The method for desulfurizing molten iron according to [2], wherein the area ratio of the unslag-formed desulfurizing agent on the surface of the molten iron is evaluated based on a temperature distribution on the surface of the molten iron. [4] The molten metal desulfurization method according to any one of [1] to [3], wherein the relative position h / H of the impeller is controlled so as to monotonically increase as the desulfurization treatment progresses. [5] The molten metal desulfurization method according to any one of [1] to [3], wherein the relative position h / H of the impeller is controlled so as to increase in a step function as the desulfurization treatment progresses. [6] The molten iron desulfurization method according to [4], further comprising controlling an impeller position so that a relative position h / H of the impeller at the start of desulfurization treatment is 0.40 or more and 0.49 or less, and a relative position h / H of the impeller when an area ratio of unslag-formed desulfurization agent on the surface of the molten iron is 20% is 0.50 or more and 0.60 or less. [7] The molten iron desulfurization method according to [5], wherein the impeller position is controlled so that the relative position h / H of the impeller at the start of desulfurization treatment is 0.40 or more and 0.49 or less, and the relative position h / H of the impeller when the area ratio of the unslag-formed desulfurization agent on the surface of the molten iron is 20% is 0.50 or more and 0.60 or less. [8] The molten iron desulfurization method according to [7], further comprising changing an impeller position so that the impeller relative position h / H becomes 0.50 or more and 0.60 or less when the impeller relative position h / H is 0.40 or more and 0.49 or less from the start of desulfurization treatment and when an area ratio of unslag-formed desulfurization agent on the surface of the molten iron is 20% or more and 40% or less. Effect of the Invention
[0018] According to the present invention, the efficiency of desulfurization of molten iron can be increased. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the state of molten iron in a molten iron vessel. [Diagram 2] Figure 2 is a conceptual diagram showing the relationship between the impeller relative position h / H and the progress of the desulfurization process, particularly the area ratio (%) below the boundary temperature for evaluating the non-slag sulfurizing agent. Figure 2(a) shows an example of a conventional sulfurization process, Figure 2(b) shows an example of a case where the impeller relative position h / H is controlled by a monotonically increasing function, and Figure 2(c) shows an example of a case where the impeller relative position h / H is controlled by a step function. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention can be used to remove sulfur components from molten iron (hot metal). For example, the present invention can be used to remove sulfur components from molten iron (hot metal) obtained by reducing iron ore in a blast furnace. The present invention can also be applied to remove excess sulfur from molten iron (this molten iron is sometimes called molten iron) melted in an electric furnace.
[0021] [Desulfurization equipment] The present invention can be applied to a molten pig iron desulfurization method in which molten pig iron in a vessel (which may also be called a molten pig iron vessel or ladle) is stirred by the rotation of an impeller and a desulfurization agent is added to the molten pig iron to perform desulfurization. There are no particular limitations on the type of desulfurization device as long as it stirs the molten pig iron by the rotation of an impeller, but generally, a mechanical stirring desulfurization device or a KR facility is applicable.
[0022] [Relative position of impeller h / H] Figure 1 shows a cross-sectional view of the state of molten pig iron in a molten pig iron vessel. Molten iron (molten pig iron) 2 is contained in the molten pig iron vessel 1. The surface position 6 of the molten pig iron 2 when the molten pig iron is stationary (when the molten pig iron is stationary) is shown by a dotted line. The molten pig iron is stirred by the rotation of the impeller 3, and a vortex is generated as the impeller rotates. When the vortex is viewed in cross section, the molten pig iron position 4 forms a depression 7 centered on the impeller axis (solid line in Figure 1). The vertical distance between the deepest position of the depression 7 of this molten pig iron position (usually located on the impeller axis) and the molten pig iron surface reference position is defined as H (depression depth). The vertical distance between the top of the impeller and the molten pig iron surface reference position is defined as h (impeller depth). At this time, the ratio of h to H (impeller relative position) is used as an index to show how deep the impeller is located in relation to the depression in the molten iron (the depression caused by the vortex). In other words, when h / H=1, the top end of the impeller is at the deepest part of the depression caused by the vortex. In other words, this means that the entire impeller is just submerged in the molten iron. When h / H exceeds 1, this indicates that the entire impeller is submerged in the molten iron. Conversely, when h / H is less than 1, this indicates that part or all of the impeller is at least above the depression in the molten iron.
[0023] [Impeller position control]
[0024] As mentioned above, by making the impeller position relatively shallow at the beginning of the desulfurization process, a strong stirring flow can be formed on the surface, and the desulfurization agent can be promoted. This is thought to be because the mixed hot metal slag and the partially liquefied desulfurization agent diffuse shallowly into the hot metal and float to the surface of the hot metal in a short time, promoting the slag formation of the remaining desulfurization agent. When the desulfurization agent turns into slag, it is taken into the hot metal as mentioned above, so by deepening the impeller position accordingly, the stirring flow reaches a deep position in the hot metal, promoting the diffusion of the desulfurization agent. For this reason, it is recommended to make the impeller position shallow at the start of the desulfurization process and deepen the relative position of the impeller as the desulfurization process progresses. In other words, it is recommended to control the impeller position by changing the impeller relative position h / H according to the progress of the desulfurization process.
[0025] Furthermore, the position of the molten iron when a vortex is occurring (line 4 in Figure 1) naturally changes with changes in the impeller rotation speed, etc. In this case, the deepest position of the molten iron depression may be measured directly, may be estimated by measuring the molten iron position, or may be estimated from a molten iron flow calculation. The impeller top position h can be easily obtained from the impeller shape and the impeller shaft position, so the impeller relative position h / H can be obtained on an as-needed basis.
[0026] [Evaluation of the progress of desulfurization treatment] The progress of the desulfurization process, especially in the initial stage, can be evaluated by the state of slag formation of the desulfurization agent added onto the molten iron. When the desulfurization agent is first added, it exists on the surface of the molten iron due to the difference in specific gravity. As the temperature of the desulfurization agent rises, the slag-formed desulfurization agent is gradually absorbed into the molten iron, so the progress of the slag formation of the desulfurization agent can be evaluated by the area ratio of the unslag-formed desulfurization agent on the molten iron surface.
[0027] There is no particular limitation on the means for evaluating whether the desulfurization agent has been slag-formed. For example, it can be evaluated from the surface temperature distribution of the molten pig iron. The surface temperature of the molten pig iron is usually 1250 to 1350°C (although rare, it may be 1150 to 1450°C depending on the composition). In contrast, the temperature of the desulfurization agent before it is slag-formed and taken into the vortex of the molten pig iron is low, and it floats on the surface of the molten pig iron.
[0028] On the other hand, the desulfurization agent, which has turned into slag and started to be drawn into the vortex of the molten iron, reaches a high temperature close to the molten iron temperature, and as a result of the desulfurization agent being drawn into the molten iron, the surface of the molten iron is exposed. Therefore, the progress of desulfurization can be grasped by measuring the temperature distribution on the molten iron surface. There is no need to measure the temperature distribution precisely, and it is sufficient to binarize the temperature by using a predetermined temperature as the boundary temperature. The boundary temperature may be, for example, "molten iron temperature -100°C" or "molten iron temperature -200°C" based on the molten iron temperature.
[0029] Also, for example, a temperature of 950°C to 1150°C, which is below the lower limit of the molten iron temperature of about 1150°C, may be set as the boundary temperature. When binarized, the part below the boundary temperature is displayed dark and the part above the boundary temperature is displayed bright, and the progress of the desulfurization process can be grasped by measuring the area ratio of the dark parts. Normally, as time passes, that is, as the desulfurization process progresses, the area ratio of the desulfurization agent that is not slag-ified decreases. For example, the initial stage of the desulfurization process can be determined until the area ratio of the part (dark part) below the boundary temperature becomes 40% in the temperature distribution measurement (i.e., when the area ratio of the part (dark part) below the boundary temperature becomes 40% or more). The initial stage of the desulfurization process can be appropriately set. Preferably, the initial stage of the desulfurization process can be determined until the area ratio of the part (dark part) below the boundary temperature becomes 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or 0%.
[0030] Alternatively, the evaluation may simply be based on the desulfurization time. In this case, it is also advisable to measure the time until slag formation and determine the initial time of the desulfurization in advance. For example, for a given amount of molten pig iron and sulfurizing agent, the time until the area ratio of the part below the boundary temperature becomes 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or 0% may be measured, and the initial time of the desulfurization may be predicted based on the actual amount of molten pig iron and amount of sulfurizing agent.
[0031] [Impeller position control] As described above, it is preferable that the impeller position is made deeper as the desulfurization process progresses. Therefore, it is preferable to control the impeller relative position h / H so that it increases as the desulfurization process progresses from the start of the desulfurization process. There is no particular limitation on the way in which the impeller relative position is made larger. It is preferable to control the impeller relative position so that it monotonically increases as a function of the progress of the desulfurization process (for example, the temperature distribution on the surface of the molten pig iron or the desulfurization process time). "Monotonically increasing" means that it does not decrease as the desulfurization process progresses, that is, it is maintained or increases. For example, when the impeller relative position h / H is a function of the area ratio of the high-temperature portion (the portion at or above the boundary temperature) on the surface of the molten pig iron, it may be a continuous function such as a linear function, a quadratic function, or a multi-order function whose first-order differential value is positive or zero.
[0032] Alternatively, the impeller relative position h / H may be a step function that increases stepwise with the progress of the desulfurization process (e.g., the desulfurization process time). For example, the impeller relative position h / H may be set to a relatively small value at the beginning of the desulfurization process, and when the area ratio occupied by the unslag-formed desulfurization agent (unslag-formed desulfurization agent area ratio) reaches a predetermined value, the impeller relative position h / H may be changed to a large value, so that the control may be performed using a single-step function. Of course, the control may be performed using a multi-step function.
[0033] In conventional desulfurization processes, the impeller relative position h / H was operated to be constant at about 0.50 to 0.60 (see, for example, FIG. 2(a)). In light of this, it is advisable to control the impeller relative position h / H to be 0.50 to 0.60 when the desulfurization process has progressed to a certain extent (when the initial stage of the desulfurization process ends, for example, when the area ratio of the non-slag desulfurization agent becomes 20%).
[0034] Therefore, at the start of the desulfurization process, the impeller relative position h / H can be controlled to be smaller than that, thereby promoting the slagification (liquefaction) of the desulfurization agent and shortening the time to start entrainment. However, if the impeller relative position h / H is too small (i.e., too shallow), spitting occurs, in which the molten iron splashes outside the vessel, so the impeller relative position h / H should be 0.40 or more. Preferably, it should be 0.41 or more, 0.42 or more, or 0.43 or more. The upper limit of the impeller relative position h / H at the start of the desulfurization process should be less than 0.50, at which the time to start entrainment of the desulfurization agent becomes significantly longer, and is preferably 0.49 or less, 0.48 or less, 0.47 or less, or 0.46 or less (see, for example, FIG. 2(b)).
[0035] After the molten iron is entrained in the vortex flow due to the slag conversion (liquefaction) of the desulfurization agent (i.e., after the initial stage of the desulfurization process ends and a steady state is reached), the desulfurization agent can be dispersed to the depth of the molten iron vessel (ladle) by increasing the impeller relative position h / H to the same extent as in conventional operation. The desulfurization agent can be diffused toward the depth of the molten iron vessel by setting the impeller relative position h / H to 0.50 or more. It is preferable that the impeller relative position h / H is 0.51 or more, 0.52 or more, 0.53 or more, or 0.54 or more. However, if the impeller relative position h / H exceeds 0.60, the desulfurization agent cannot be dispersed in the molten iron by the impeller and tends to remain on the surface of the molten iron, so the impeller relative position h / H needs to be 0.60 or less, and preferably 0.59 or less, 0.58 or less, or 0.57 or less. As mentioned above, in the steady state of desulfurization, the desulfurization agent turns to slag and moves on the surface of the molten iron toward the center of the vortex (moving to the center), is diffused into the molten iron by the impeller (internal diffusion), and floats to the surface of the molten iron with the molten iron flow (floating). Desulfurization of the molten iron progresses by repeating this cycle of (moving to the center) ⇒ (internal diffusion) ⇒ (floating). At this time, if the impeller is positioned too deep, the transition from (moving to the center) ⇒ (internal diffusion) does not work well, and desulfurization efficiency decreases.
[0036] As a control method, as described above, the monotonically increasing function control or the one-stage or multi-stage step function control with respect to the progress of the desulfurization treatment is preferable. Therefore, the monotonically increasing function control or the one-stage or multi-stage step function control may be adopted in which the impeller relative position h / H is 0.40 to 0.49 at the start of the desulfurization treatment and the impeller relative position h / H is 0.50 to 0.60 when the non-slag desulfurization agent area ratio becomes small (for example, when the non-slag desulfurization agent area ratio becomes 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or 0%) (for example, see FIG. 2(c)).
[0037] For example, when controlling with a monotonically increasing function (e.g., FIG. 2(b)), the impeller relative position h / H is gradually increased, and when the non-slag desulfurization agent area ratio (area ratio of the dark area) reaches 20%, the impeller relative position h / H is controlled to be 0.50 to 0.60. When controlling with a one-step function (e.g., FIG. 2(c)), the impeller relative position h / H is changed to be 0.50 to 0.60 when the non-slag desulfurization agent area ratio (area ratio of the dark area) is between 40% and 20%, and the impeller relative position h / H is controlled to be 0.50 to 0.60 when the non-slag desulfurization agent area ratio (area ratio of the dark area) reaches 20%. EXAMPLES
[0038] [Example 1] An example will be shown in which the impeller relative position h / H in an actual KR facility is controlled by monotonically increasing function control and one-step step function control. In this example, the impeller position is controlled in the initial stage of desulfurization treatment until the non-slag desulfurization agent area ratio reaches 30%. That is, in the case of monotonically increasing function control, the impeller relative position h / H is set to 0.40 to 0.49 at the start of desulfurization treatment, and the impeller relative position h / H is set to 0.50 to 0.60 when the non-slag desulfurization agent area ratio reaches 20% (see FIG. 2(b), for example). In the case of the one-stage step function control, the impeller relative position h / H was set to 0.40 to 0.49 from the start of the desulfurization process until the non-slag desulfurization agent area ratio reached 30% (initial stage of the desulfurization process), and when the non-slag desulfurization agent area ratio reached 30%, the impeller was moved so that the impeller relative position h / H became 0.50 to 0.60. Thereafter, the impeller relative position h / H was controlled to be constant until the end of the desulfurization process (see, for example, Figure 2(c)).
[0039] The non-slag desulfurization agent area ratio was evaluated by binarizing the molten iron surface temperature with the boundary temperature set at 1000°C as described above, and calculating the area ratio of the area of the part (dark area) below 1000°C. The impeller rotation speed was kept constant, and the shape of the depression caused by the molten iron vortex was calculated from the molten iron properties, vessel shape, impeller shape, and impeller rotation speed. The calculated maximum depth of the depression and the actual measurement of the molten iron surface position around the impeller confirmed that the calculated maximum depth of the depression was appropriate.
[0040] The following three test levels, 11 to 13, were tested using an actual machine. Test level 11 (conventional example): As a comparative example, the impeller position was controlled to maintain the impeller relative position h / H = 0.56 from the start to the end of desulfurization treatment, as in conventional operation (see Figure 2(a)). Test level 12: When h / H is controlled to increase monotonically, from h / H = 0.42 at the start of desulfurization treatment to h / H = 0.5 to 0.6 when the non-slag desulfurization agent area ratio is 20% (see Figure 2(b)). Test level 13: When h / H is 0.42 at the start of desulfurization treatment, and h / H is step function controlled so that it becomes 0.56 when the non-slag desulfurization agent area ratio is 30% (see Figure 2(c)).
[0041] The desulfurization efficiency was compared using the desulfurization reaction efficiency K_CaO (see formula 1) obtained by measuring the sulfur content in the molten pig iron before and after the desulfurization process and dividing the logarithm of the ratio by the amount of quicklime added as a desulfurization agent per unit of the amount of molten pig iron. The results are shown as a relative evaluation with the desulfurization reaction efficiency in the conventional method set at 1. JPEG2024148503000001.jpg1383...Formula 1 Test level 11: Desulfurization reaction efficiency K_CaO=1.0 Test level 12: Desulfurization reaction efficiency K_CaO=1.55 Test level 13: Desulfurization reaction efficiency K_CaO=1.46
[0042] [Example 2] In the impeller position control using the one-stage step function control performed in Example 1, the impeller relative position h / H at the beginning of the desulfurization process was set to 0.43 to 0.49, and the impeller relative position h / H after the non-slag desulfurization agent area ratio reached 30% was set to the following three levels, and the change in desulfurization reaction efficiency was determined. Test level 21: The impeller relative position h / H is kept at the initial stage of desulfurization treatment. Test level 22: When the impeller relative position h / H is set to 0.50 to 0.60. (Same as the one-stage step function control in Example 1) Test level 23: When impeller relative position h / H is 0.61 to 0.68.
[0043] The desulfurization reaction efficiency obtained after the test is shown as a relative evaluation with the conventional desulfurization treatment being set at 1, as in Example 1. Test level 21: Desulfurization reaction efficiency K_CaO=1.10 Test level 22: Desulfurization reaction efficiency K_CaO=1.46 Test level 23: Desulfurization reaction efficiency K_CaO=0.96
[0044] From the above, it was confirmed once again that after the non-slag desulfurization agent area ratio reaches 30%, that is, when the desulfurization process reaches a steady state, it is preferable to set the impeller relative position h / H to 0.50 to 0.60. This confirmed the effect that by making the impeller relative position h / H smaller in the early stage of the desulfurization process, that is, by making the impeller position shallower, the desulfurization efficiency is improved compared to the conventional method. [Industrial Applicability]
[0045] The present invention can be utilized in the steel industry. [Explanation of symbols]
[0046] 1 Molten metal container (pot) 2 Molten iron (molten iron) 3 Impeller 4 Hot metal position (vortex) 5 Slag surface 6 Hot metal surface reference position 7 Molten iron recess
Claims
1. A molten iron desulfurization method for performing a desulfurization treatment by stirring molten iron in a vessel by rotation of an impeller and introducing a desulfurization agent into the molten iron, When the distance from the surface position of the molten iron when the molten iron is stationary in the vessel (the reference position of the molten iron surface) to the deepest position of the depression in the molten iron surface caused by stirring the molten iron is H, and the distance from the top end of the impeller is h, A method for desulfurizing molten metal, comprising controlling an impeller position by changing a relative position h / H of the impeller in accordance with the progress of desulfurization treatment.
2. 2. The method for desulfurizing molten iron according to claim 1, further comprising the step of evaluating the progress of the desulfurization treatment based on an area ratio of the desulfurizing agent not converted into slag on the surface of the molten iron, and controlling an impeller position based on the evaluation.
3. 3. The method for desulfurizing molten iron according to claim 2, wherein the area ratio of the unslag-formed desulfurizing agent on the surface of the molten iron is evaluated based on a temperature distribution on the surface of the molten iron.
4. The molten metal desulfurization method according to any one of claims 1 to 3, wherein the relative position h / H of the impeller is controlled so as to monotonically increase as the desulfurization treatment progresses.
5. The molten metal desulfurization method according to any one of claims 1 to 3, wherein the relative position h / H of the impeller is controlled to increase in a step function as the desulfurization treatment progresses.
6. 5. The method for desulfurizing molten iron according to claim 4, wherein the impeller position is controlled so that a relative position h / H of the impeller at the start of desulfurization treatment is 0.40 or more and 0.49 or less, and a relative position h / H of the impeller when an area ratio of unslagified desulfurizing agent on the surface of the molten iron is 20% is 0.50 or more and 0.60 or less.
7. 6. The method for desulfurizing molten iron according to claim 5, wherein the impeller position is controlled so that a relative position h / H of the impeller at the start of desulfurization treatment is 0.40 or more and 0.49 or less, and a relative position h / H of the impeller when an area ratio of unslagified desulfurizing agent on the surface of the molten iron is 20% is 0.50 or more and 0.60 or less.
8. 8. The method for desulfurizing molten iron according to claim 7, wherein the impeller position is changed so that the relative position h / H of the impeller becomes 0.50 or more and 0.60 or less when the relative position h / H of the impeller is 0.40 or more and 0.49 or less from the start of desulfurization treatment and when an area ratio of unslagified desulfurizing agent on the surface of the molten iron is 20% or more and 40% or less.
Citation Information
Patent Citations
Method for stirring molten iron
JP2001247910A
Method for stirring molten metal using impeller
JP2007262501A
Method for desulfurizing molten iron
JP2010185114A