Wiring board

The wiring board design with distinct buildup sections and specific metal layer configurations addresses the issue of reduced contact area between insulating and conductor layers, enhancing adhesion and reducing wiring loss for improved signal transmission.

JP2024148520AInactive Publication Date: 2024-10-18IBIDEN CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023061717
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The contact area between the insulating layer and the seed layer in existing wiring boards becomes smaller due to undercutting, leading to missing wiring.

Method used

A wiring board design with multiple buildup sections, each having different wiring densities, where the first buildup section has a conductor layer with a smaller minimum wiring width and interval than the second buildup section, and includes a laminated structure with specific metal layers to enhance adhesion between the insulating and conductor layers.

Benefits of technology

Improves adhesion between the insulating and conductor layers, reducing the risk of wiring loss and enhancing signal transmission characteristics by maintaining a stable contact area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148520000001_ABST
    Figure 2024148520000001_ABST
Patent Text Reader

Abstract

To improve a quality of a wiring board containing a plurality of conductive layers of which a wiring density is different.SOLUTION: A wiring board 1 of an embodiment, includes a first surface and a second surface, and contains: a first built-up part 10; and a second built-up part 20. The first built-up part 10 is laminated to the first surface side in the second built-up part 20. A minimum width W1 of wiring 12w contained in a conductive layer 12 of the first built-up part 10 is smaller than a minimum width W2 of wiring 22w contained in a conductive layer 22a of the second built-up part 20. A minimum gap G1 between each wiring 12w is smaller than a minimum gap G2 between each wiring 22w. A conductive pattern contained in the conductive layer 12 contains: a first metal layer 121; a second metal layer 122; and a third metal layer 123 that are laminated. In a cross section of the conductive pattern of the conductive layer 12, the width of the first metal layer 121 is larger than the width of the second metal layer 122, and the width of the third metal layer 123 is larger than the width of the first metal layer 121.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wiring board. [Background technology]

[0002] Patent Document 1 discloses a method for producing a printed wiring board by a semi-additive process including copper etching. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-5341 A Summary of the Invention [Problem to be solved by the invention]

[0004] In a wiring board manufactured by the method disclosed in Patent Document 1, there is a concern that the contact area between the insulating layer and the seed layer is reduced due to undercutting, which may cause wiring to be missing. [Means for solving the problem]

[0005] The wiring board of the present invention has a first surface and a second surface opposite to the first surface, and includes a first buildup section including laminated insulating layers and conductor layers, and a second buildup section including laminated insulating layers and conductor layers, the first buildup section is laminated on the first surface side of the second buildup section, a minimum wiring width of wiring included in the conductor layer of the first buildup section is smaller than a minimum wiring width of wiring included in the conductor layer of the second buildup section, a minimum wiring interval between wiring included in the conductor layer of the first buildup section is smaller than a minimum wiring interval between wiring included in the conductor layer of the second buildup section, a conductor pattern included in the conductor layer of the first buildup section includes a first metal layer, a second metal layer laminated on the second surface side of the first metal layer, and a third metal layer laminated on the second surface side of the second metal layer, and in a cross section of the conductor pattern along a lamination direction of the first buildup section and the second buildup section, a width of the first metal layer is larger than a width of the second metal layer, and a width of the third metal layer is larger than a width of the first metal layer.

[0006] According to an embodiment of the present invention, in a wiring board including a plurality of conductor layers having different wiring densities, the adhesion between the insulating layer and the conductor layer may be improved, and loss of wiring may be suppressed. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a wiring board according to an embodiment of the present invention. [Diagram 2] An enlarged view of part II in Figure 1. [Diagram 3] An enlarged view of part III in FIG. [Figure 4A] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; [Figure 4B] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; [Figure 4C] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4D] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4E] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4F] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4G] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4H] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4I] FIG. 4 is an enlarged cross-sectional view of a portion of an example of a wiring substrate according to an embodiment during a manufacturing process. [Figure 4J] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; [Figure 4K] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; [Figure 4L] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; [Figure 4M] 1 is a cross-sectional view showing an example of a wiring substrate according to an embodiment in a manufacturing process; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] <Structure of wiring board according to embodiment> A wiring board according to an embodiment will be described with reference to the drawings. FIG. 1 shows a cross-sectional view of a wiring board 1, which is an example of a wiring board according to an embodiment. FIG. 2 shows an enlarged view of part II in FIG. 1. The wiring board 1 is merely an example of the wiring board according to this embodiment. The number and thickness of each of the conductor layers and insulating layers in the wiring board according to this embodiment, and the conductor patterns included in each conductor layer are not limited to the number and thickness of each of the conductor layers and insulating layers included in the wiring board 1 of FIG. 1, and the conductor patterns. In addition, in each drawing referred to in the following description, a specific portion may be drawn enlarged so that the disclosed embodiment can be easily understood, and the components may not be drawn in exact proportion to each other in terms of size and length.

[0009] As shown in FIG. 1 and FIG. 2, the wiring board 1 has two surfaces (a first surface 1F and a second surface 1B opposite to the first surface 1F) perpendicular to the thickness direction of the wiring board 1. The wiring board 1 includes a first buildup section 10 and a second buildup section 20. The first buildup section 10 is laminated on the first surface 1F side of the second buildup section 20. The lamination direction of the first buildup section 10 and the second buildup section 20 is the thickness direction of the wiring board 1. The first buildup section 10 and the second buildup section 20 overlap each other entirely. The wiring board 1 of FIG. 1 further includes a third buildup section 30 laminated on the second surface 1B side of the wiring board 1 in the second buildup section 20, and a solder resist 40 covering the surface of the third buildup section 30. The wiring board of this embodiment may be a coreless wiring board that does not include a core layer, like the wiring board 1 of FIG. 1.

[0010] In the description of the wiring board 1 of this embodiment, the first surface 1F of the wiring board 1 is also referred to as the "top" or "upper side", and the second surface 1B of the wiring board 1 is also referred to as the "bottom" or "lower side". In addition, the surface of each component facing the first surface 1F of the wiring board 1 is also referred to as the "top surface", and the surface facing the second surface 1B of the wiring board 1 is also referred to as the "bottom surface".

[0011] The first buildup section 10 has a first surface 10F which is a surface common to the first surface 1F of the wiring board 1, and a second surface 10B which is a surface opposite to the first surface 1F. The first buildup section 10 includes conductor layers 12 (first conductor layers) and insulating layers 11 (first insulating layers) which are alternately laminated. Each conductor layer 12 is formed on the lower surface of the insulating layer 11 adjacent thereto above. The first buildup section 10 further includes a conductor layer 12a which is the conductor layer in the first buildup section 10 closest to the first surface 1F of the wiring board 1.

[0012] Conductive layer 12a is embedded in insulating layer 11 at the portion of first buildup section 10 closest to first surface 1F of wiring board 1, and has an upper surface exposed to first surface 1F. The exposed upper surface of conductor layer 12a and the upper surface of insulating layer 11 in which conductor layer 12a is embedded form the first surface 1F of wiring board 1.

[0013] The first surface 1F of the wiring board 1 includes one or more component regions (component region Ea1 and component region Ea2 in the example of FIG. 1) on which mounted components (component E1 and component E2 in the example of FIG. 1) are mounted when the wiring board 1 is used. The first surface 1F of the wiring board 1 can be a component mounting surface that is at least partially covered by mounted components such as component E1 and component E2 when the wiring board 1 is used.

[0014] Each of the conductor layers 12 and 12a includes an arbitrary conductor pattern. The conductor layer 12 includes wiring 12w (see FIG. 2) as a conductor pattern. The conductor layer 12a constituting the component mounting surface in the first build-up section 10 includes a component mounting pad 12p made of a conductor pad. The component mounting pad 12p is embedded in the insulating layer 11 constituting the first surface 1F of the wiring board 1, and one surface of the component mounting pad 12p is exposed to the first surface 1F. The exposed surface of the component mounting pad 12p can be connected to an electrode of a mounted component by, for example, a conductive bonding material (not shown) such as solder. The exposed surface of the component mounting pad 12p may be formed with a surface treatment layer (not shown) made of a plating layer containing, for example, nickel, palladium, and gold.

[0015] Examples of the components E1 and E2 that can be mounted on the wiring board 1 include electronic components such as active components such as semiconductor integrated circuit devices and transistors. As some examples, the components E1 and E2 can be integrated circuit devices such as logic chips, processing devices such as MPUs (Micro Processor Units), and memory devices such as HBMs (High Bandwidth Memory).

[0016] The first buildup section 10 further includes via conductors 13 (first via conductors) that penetrate each insulating layer 11. The via conductors 13 are formed in openings 13a that penetrate each insulating layer 11. Each via conductor 13 connects the lower conductor layer 12 of each insulating layer 11 including the via conductor 13 to the upper conductor layer 12 or conductor layer 12a. Each via conductor 13 is formed integrally with the conductor layer 12 that is in contact with it at an end portion on the second surface 1B side of the wiring board 1.

[0017] The second buildup section 20 has a first surface 20F which is the surface on the first surface 1F side of the wiring board 1, and a second surface 20B which is the surface opposite to the first surface 20F. The first surface 20F of the second buildup section 20 faces the second surface 10B of the first buildup section 10. The second buildup section 20 includes conductive layers 22 and insulating layers 21 (second insulating layers) which are alternately stacked, and via conductors 23 (second via conductors) which penetrate each insulating layer 21. The second buildup section 20 further includes a conductive layer 22a (second conductor layer) which is the conductive layer closest to the first surface 20F of the second buildup section 20, and a via conductor 23a. The via conductor 23a is formed integrally with the conductive layer 22a, and penetrates the insulating layer 11 in the first buildup section 10 which is closest to the second buildup section 20. A first surface 20F of the second buildup section 20 is formed by the top surface of the insulating layer 21 that is located closest to the first buildup section 10 among the multiple insulating layers 21, and the top surface of the conductor layer 22a.

[0018] On the other hand, the second surface 20B of the second buildup section 20 is constituted by the lower surfaces of the insulating layer 21 and the conductor layer 22 which are closest to the second surface 1B of the wiring board 1 in the second buildup section 20. In the wiring board 1 of FIG. 1, the second surface 20B of the second buildup section 20 faces the surface (upper surface) of the third buildup section 30 facing the first surface 1F of the wiring board 1.

[0019] Each of the conductor layers 22 and 22a includes an arbitrary conductor pattern. The conductor layer 22a includes wiring 22w (see FIG. 2) as a conductor pattern. Each of the conductor layers 22 and 22a is formed on the lower surface of the insulating layer 21 or insulating layer 11 adjacent to the upper side of the conductor layer 22 or 22a. Each of the via conductors 23 connects the lower conductor layer 22 of the insulating layer 21 through which the via conductor 23 penetrates to the upper conductor layer 22 or conductor layer 22a. The via conductor 23a connects the conductor layer 22a to the conductor layer 12 of the first buildup section 10.

[0020] The third buildup section 30 includes an insulating layer 31 (third insulating layer), a conductor layer 32 (third conductor layer), and a via conductor 33 (third via conductor), which are stacked together. The conductor layer 32 includes an arbitrary conductor pattern, such as a conductor pad 32p. The via conductor 33 connects the conductor layer 32 and the conductor layer 22 included in the second buildup section 20.

[0021] The solder resist 40 is formed on the surface of each of the insulating layer 31 and the conductor layer 32 on the second surface 1B side of the wiring board 1. An opening 41 is formed in the solder resist 40, and the conductor pad 32p is exposed in the opening 41. The solder resist 40 is formed using, for example, a photosensitive polyimide resin or an epoxy resin.

[0022] 1, second side 1B of wiring board 1 consists of the surface of solder resist 40 on the second side 1B side of wiring board 1 and the exposed surface of conductor layer 32 exposed from solder resist 40. However, the wiring board of this embodiment does not necessarily include third buildup portion 30 and / or solder resist 40. The second side of a wiring board in an embodiment that does not include third buildup portion 30 consists of second side 20B of second buildup portion 20, or solder resist formed on second side 20B of second buildup portion 20 and an exposed portion of second side 20B from the solder resist.

[0023] The second surface 1B of the wiring board 1 can be a connection surface to be connected to an external element when the wiring board 1 itself is mounted on an external element such as an external wiring board (for example, a motherboard of an electric device). In the example of Fig. 1, the conductor pad 32p of the third buildup section 30 can be connected to an arbitrary board, electric component, mechanical component, or the like.

[0024] The insulating layers 11, 21, and 31 may be formed using a thermosetting insulating resin such as an epoxy resin, a bismaleimide triazine resin (BT resin), and a phenol resin. The insulating layers 11, 21, and 31 may be formed using a thermoplastic insulating resin such as a fluororesin, a liquid crystal polymer (LCP), a fluoroethylene resin (PTFE), a polyester resin (PE), or a modified polyimide resin (MPI). The insulating layers 11, 21, and 31 may contain the same insulating resin or different insulating resins.

[0025] The insulating layers 11, 21, and 31 may contain a core material (reinforcing material) made of glass fiber or the like. In the example of FIG. 1, the insulating layer 31 contains a core material 31a. The core material 31a may impart appropriate rigidity to the wiring board 1. The core material 31a may be, for example, glass fiber or aramid fiber. On the other hand, each insulating layer that does not contain a core material such as glass fiber may facilitate the formation of fine wiring on its surface or increase adhesion with the conductor layer. In the example of FIG. 1, neither the insulating layer 11 nor the insulating layer 21 contains a core material.

[0026] Although omitted in FIG. 1, the insulating layers 11, 21, and 31 may further include inorganic particles added as a filler to the insulating resin constituting each of the insulating layers 11, 21, and 31. Each insulating layer containing inorganic particles is given, for example, a low thermal expansion coefficient and high thermal conductivity. In the wiring board 1 of this embodiment, as shown in FIG. 2, the insulating layer 11 of the first buildup section 10 contains a plurality of inorganic particles 5 and the insulating resin 110 such as the epoxy resin described above. The content of the inorganic particles 5 in the insulating layer 11 is, for example, 75 wt % or more. In the example of FIG. 2, the insulating layer 21 included in the second buildup section 20 contains inorganic particles 6. The inorganic particles 5 and the inorganic particles 6 are fine particles made of, for example, silica (SiO2), alumina, or mullite.

[0027] In the example of FIG. 2, the maximum particle size of the inorganic particles 5 is smaller than the maximum particle size of the inorganic particles 6. The "particle size" of each of the inorganic particles 5 and 6 is the longest distance between two points on the surface of each inorganic particle. For example, the maximum particle size of the inorganic particles 5 is 1 μm or less, and the average particle size of the inorganic particles 5 is 0.5 μm or less. On the other hand, the maximum particle size of the inorganic particles 6 is, for example, 4 μm or less. When the particle size of the inorganic particles 5 and 6 is small, short circuit defects due to leak paths along the inorganic particles are unlikely to occur even between wirings arranged at fine intervals in the conductor layer in contact with each insulating layer. In addition, it may be easy to form a fine via conductor. The first build-up section 10 including the inorganic particles 5 having a smaller particle size has good reliability regarding insulation between wirings and may include wirings arranged at a fine pitch.

[0028] The conductor layers 12, 12a, 22, 22a, and conductor layer 32, and the via conductors 13, 23, 23a, and via conductor 33 may be formed using a metal having suitable electrical conductivity, such as copper or a copper alloy. Although each of these conductor layers and each of the via conductors is depicted as a single layer in Fig. 1, each of the conductor layers and each of the via conductors may have a multi-layer structure, such as the conductor layer 12 and the conductor layer 22a shown in Fig. 2. In the wiring board 1 of this embodiment, at least the conductor layer 12 of the first buildup section 10 has a multi-layer structure of three or more layers.

[0029] That is, the conductor layer 12 and the via conductor 13 include a first metal layer 121, a second metal layer 122, and a third metal layer 123, as shown in FIG. 2. In each conductor layer 12, the first metal layer 121 is formed closest to the first surface 1F (see FIG. 1) of the wiring board 1. The second metal layer 122 is stacked on the surface (lower surface) of the first metal layer 121 and is in contact with the lower surface of the first metal layer 121. The third metal layer 123 is stacked on the surface (lower surface) of the second metal layer 122 and is in contact with the lower surface of the second metal layer 122. Therefore, the conductor pattern such as the wiring 12w included in the conductor layer 12 of the first build-up section 10 includes the first metal layer 121, the second metal layer 122 stacked on the second surface 1B (see FIG. 1) side of the first metal layer 121, and the third metal layer 123 stacked on the second surface 1B side of the second metal layer 122.

[0030] On the other hand, in the wiring board 1 of FIG. 1, the conductor layers 22, 22a of the second buildup section 20 may be composed of a fourth metal layer 224 and a fifth metal layer 225, as in the conductor layer 22a shown in FIG. 2. The fourth metal layer 224 is formed on the conductor layer 22a on the first buildup section 10 side. The fifth metal layer 225 is formed on the fourth metal layer 224 on the second surface 1B side of the wiring board 1. Although not shown, the via conductors 23, 23a of the second buildup section 20 and the conductor layer 32 and the via conductor 33 of the third buildup section 30 may also have a two-layer structure similar to the conductor layer 22a illustrated in FIG. 2. The conductor layer 32 may further have a structure including a layer made of a metal foil in contact with the lower surface of the insulating layer 31.

[0031] The fourth metal layer 224 covers a part of the lower surface of the insulating layer 11 or the insulating layer 21 on the first surface 1F side of the wiring board 1 in each conductor layer such as the conductor layer 22a. The fifth metal layer 225 entirely covers the surface of the fourth metal layer 224 opposite to the first buildup section 10 side. As an example, the fifth metal layer 225 may be an electrolytic plating film layer formed by electrolytic plating. The fourth metal layer 224 may be a seed layer of the electrolytic plating film layer constituting the fifth metal layer 225. The fourth metal layer 224 is formed by any method. As an example, the fourth metal layer 224 may be an electroless plating film formed by a wet process.

[0032] As shown in FIG. 1, the via conductors 13, 23, 23a, and 33 all have a tapered shape that narrows from the second surface 1B to the first surface 1F of the wiring board 1. Because the via conductors 13, 23, 23a, and 33 have such a tapered shape, the conductor layer on the first surface 1F side, which may be a component mounting surface, may include wiring arranged at a finer pitch. The shape of the horizontal cross section (cross section perpendicular to the thickness direction of the wiring board 1) of each of the via conductors 13, 23, 23a, and 33 is not necessarily limited to a circle. "Diameter narrowing" simply means that the distance between the longest two points on the circumference of each via conductor in the horizontal cross section (hereinafter, this distance is also referred to as the "width" of each via conductor) becomes smaller.

[0033] The via conductors 13 included in the first buildup section 10 have, for example, an aspect ratio (distance between the upper surface of the lower conductor layer 12 to which the via conductor 13 is connected and the lower surface of the upper conductor layer 12 or conductor layer 12a / width of the via conductor 13 on the upper surface of the lower conductor layer 12) of 0.5 or more and 1.0 or less. The first buildup section 10 may include wiring arranged at a fine pitch and via conductors 13 that are unlikely to break and have low conductor resistance. The width of each of the via conductors 13 on the upper surface of the lower conductor layer 12 is, for example, about 10 μm. On the other hand, the width of each of the via conductors 23 in the second buildup section 20 on the upper surface of the lower conductor layer 22 is about 50 μm.

[0034] As shown in FIG. 2, the wiring 12w included in the conductor layer 12 of the first buildup section 10 has a wiring width W1 as its width. The wiring 12w has a wiring interval G1 as the interval between adjacent wirings 12w. The wiring width W1 is the smallest wiring width among the widths of the wirings included in the conductor layer 12. The wiring interval G1 is the smallest wiring interval among the intervals between the wirings included in the conductor layer 12. On the other hand, the wiring 22w included in the conductor layer 22 of the second buildup section 20 has a wiring width W2 as its width. The wiring 22w has a wiring interval G2 as the interval between adjacent wirings 22w. The wiring width W2 is the smallest wiring width among the widths of the wirings included in the conductor layer 22. The wiring interval G2 is the smallest wiring interval among the intervals between the wirings included in the conductor layer 22a.

[0035] The "wiring width" of each wiring such as wiring 12w included in each conductor layer of the first buildup section 10 is the width of each wiring in the third metal layer 123 (the maximum width if the width of the third metal layer 123 changes in the thickness direction of each wiring). The "wiring spacing" between each wiring such as wiring 12w included in each conductor layer of the first buildup section 10 is the spacing between the third metal layers 123 of each wiring (the minimum spacing if the spacing between the third metal layers 123 changes in the thickness direction of each wiring). Similarly, the "wiring width" and "wiring spacing" of each wiring such as wiring 22w included in each conductor layer of the second buildup section 20 are the width of each wiring in the second metal layer 222 and the spacing between the fifth metal layers 225, respectively.

[0036] 2, the wiring width W1 is smaller than the wiring width W2. Also, the wiring interval G1 is smaller than the wiring interval G2. That is, the conductor layer 12 has a minimum wiring width for the wirings included in the conductor layer 12 that is smaller than the minimum wiring width of the wirings included in the conductor layer 22a, and has a minimum wiring interval that is smaller than the minimum wiring interval between the wirings included in the conductor layer 22a. Thus, in the wiring board of the embodiment, the conductor layer 12 that constitutes the first buildup section 10 together with the insulating layer 11 can be a conductor layer that includes wiring that is arranged according to a wiring rule different from that of the wirings included in the second buildup section 20.

[0037] In the wiring board 1 of the embodiment, the first buildup section 10 may be a laminate of such a conductor layer 12 and an insulating layer 11. The wiring board 1 of the embodiment, which includes the first buildup section 10 including a conductor layer whose minimum wiring width and minimum wiring spacing are smaller than those of the conductor layer of the second buildup section 20 together with the second buildup section 20, may include fine wiring only in the necessary conductor layer. And the wiring board 1 of the embodiment may include, as another conductor layer, a conductor layer including wiring having a wider width or spacing, i.e., wiring that is easier to form.

[0038] In the wiring board 1 of the embodiment, the minimum wiring width of the wiring included in the conductor layer 12, such as the wiring 12w, may be, for example, 1 μm or more and 3 μm or less, and the minimum wiring spacing between the wirings included in the conductor layer 12 may be, for example, 1 μm or more and 3 μm or less. When the first buildup section 10 is formed of the conductor layer 12 including wiring arranged at such a fine pitch, wiring having more suitable characteristics corresponding to the electrical signals carried by the wiring in the first buildup section 10 may be provided. Furthermore, the density of the wiring in the first buildup section 10 may be high, and therefore a small wiring board 1 may be obtained.

[0039] On the other hand, the minimum wiring width of the wiring included in the conductor layers such as conductor layer 22a and conductor layer 22 constituting second buildup section 20 may be about 4 μm, for example, and the minimum wiring spacing may be about 6 μm, for example. Forming the conductor layers of second buildup section 20 may be relatively easy.

[0040] In addition, in the wiring board 1 of the embodiment, the aspect ratio of each wiring such as the wiring 12w included in the conductor layer 12 of the first buildup section 10 can be, for example, 2.0 or more and 4.0 or less. Wires having such an aspect ratio can have low conductor resistance for a small wiring width, and can therefore serve as a signal transmission path with low insertion loss. For example, signals can be transmitted between components mounted on the wiring board 1 with little transmission loss. In addition, a desired characteristic impedance can be easily obtained, and therefore the insertion loss can be further reduced.

[0041] In the example of FIG. 1 and FIG. 2, the thickness of the conductor layer 12 is different from the thickness of the conductor layer 22 and the conductor layer 22a. The thickness of the insulating layer 11 is different from the thickness of the insulating layer 21. Thus, in this embodiment, the first buildup section 10 may be a laminate of an insulating layer and a conductor layer having a thickness different from that of the conductor layer of the second buildup section 20. Also, in this embodiment, the first buildup section 10 may be a laminate of an insulating layer and a conductor layer having a thickness different from that of the insulating layer of the second buildup section 20. Also, as described above, the particle size of the inorganic particles 5 contained in the insulating layer 11 is different from the particle size of the inorganic particles 6 contained in the insulating layer 21. Therefore, in this embodiment, the first buildup section 10 may be a laminate of an insulating layer made of a material different from that of the insulating layer of the second buildup section 20 and a conductor layer.

[0042] As an example, the thickness of a conductor layer included in the first buildup section 10, such as the conductor layer 12, may be 4 μm or more and 7 μm or less. This is less likely to leave etching residue during manufacturing, and may be advantageous for arranging wiring 12w and the like that are arranged at fine intervals. The thickness of the insulating layer 11 included in the first buildup section 10 may be, for example, about 7.5 to 10 μm. On the other hand, the thickness of a conductor layer included in the second buildup section 20, such as the conductor layers 22 and 22a, may be 10 μm or more and less than 20 μm. Furthermore, the thickness of an insulating layer included in the second buildup section 20, such as the insulating layer 21, may be 20 μm or more and less than 100 μm.

[0043] The surface of the conductor layer 12 of the first buildup section 10 on the second buildup section 20 side (the second surface 1B side of the wiring board 1) may be a polished surface having a polished finish. In the example of FIG. 1, the surface on the second surface 1B side of all four conductor layers 12 is a polished surface. The polished surface may have a surface roughness lower than that of a plating film formed by metal deposition as it is. Therefore, it is considered that the deterioration of signal transmission characteristics and the increase of voltage drop are unlikely to occur in the wiring included in each conductor layer 12 having a polished surface. For example, the polished surface that each conductor layer 12 has as the surface on the second surface 1B side may have an arithmetic mean roughness of 0.3 μm or less. When such a surface roughness is obtained, the above-mentioned effects on transmission characteristics may be obtained.

[0044] Although not shown, in the wiring board 1 of FIG. 1, the wiring width of the wiring of the conductor layer 32 included in the third buildup section 30 is larger than the wiring width of the wiring included in the second buildup section 20, such as the wiring 22w. The wiring interval of the wiring of the conductor layer 32 is larger than the wiring interval of the wiring included in the second buildup section 20. The insulating layer 31 and the conductor layer 32 in the third buildup section 30 are both formed thicker than the insulating layer 21 and the conductor layers 22, 22a in the second buildup section 20. For example, the thickness of the insulating layer 31 is about 100 μm or more and 200 μm or less. The thickness of the conductor layer 32 is about 20 μm. The width of the via conductor 33 formed in the insulating layer 31 (the width at the top surface of the conductor layer 32) is about 100 μm.

[0045] As shown in FIG. 2, the lower surface 11a, which is the surface (insulating layer surface) of the insulating layer 11 constituting the first buildup section 10 facing the second buildup section 20, is composed substantially of resin 110. The inorganic particles 5 are not substantially exposed from the lower surface 11a of the insulating layer 11, or are only slightly exposed. In addition, the lower surface 11a of the insulating layer 11 is preferably not intentionally roughened in the manufacturing process of the wiring board 1, as described later. Therefore, the lower surface 11a of the insulating layer 11 is a smooth surface substantially free of recesses. For example, the arithmetic mean roughness (Ra) of the lower surface 11a of the insulating layer 11 is 0.02 μm or more and 0.06 μm or less. Necessary adhesion is ensured between the insulating layer 11 and the conductor layer 12 or conductor layer 22a formed on the lower surface 11a, and good high-frequency signal transmission characteristics and insulation between adjacent wirings may be obtained in the wiring included in the conductor layer 12 or conductor layer 22a.

[0046] As shown in FIG. 2, in the wiring board 1 of this embodiment, the inorganic particles 5 include first inorganic particles 51 and second inorganic particles 52. The first inorganic particles 51 are substantially spherical in shape. The first inorganic particles 51 are inorganic particles that are entirely embedded in the resin 110 constituting each insulating layer 11, among the inorganic particles 5. On the other hand, the second inorganic particles 52 are inorganic particles that are exposed on the inner wall surface of the insulating layer 11 exposed in the opening 13a. The second inorganic particles 52 form the inner wall surface of the insulating layer 11 exposed in the opening 13a. The second inorganic particles 52 are spherically decapitated in shape.

[0047] Fig. 3 shows an enlarged view of part III in Fig. 2. With reference to Fig. 3 in addition to Fig. 2, the conductor layer 12 of the first buildup section 10 and the conductor pattern included in the conductor layer 12 will be further described.

[0048] The first metal layer 121 of each conductor layer 12 covers a part of the lower surface of the insulating layer 11 on the first surface 1F (see FIG. 1) side of the wiring board 1, and also covers the entire inner wall surface exposed in the opening 13a penetrating the insulating layer 11. The second metal layer 122 entirely covers the surface of the first metal layer 121 facing the second buildup section 20 (see FIG. 2, the lower side in FIG. 3). The third metal layer 123 entirely covers the surface of the second metal layer 122 facing the second buildup section 20. The opening 13a is filled with the first metal layer 121, the second metal layer 122, and the third metal layer 123. The first to third metal layers 121, 122, and 123 filling the opening 13a form a via conductor 13.

[0049] The third metal layer 123 is, for example, made of a plating film, and is preferably made of an electrolytic plating film. When the third metal layer 123 is made of an electrolytic plating film, the first metal layer 121 and the second metal layer 122 may be a seed layer of a two-layer structure that functions as a power supply layer when the third metal layer 123 is formed by electrolytic plating. In other words, the first metal layer 121 and the second metal layer 122 may be a seed layer of the electrolytic plating film that constitutes the third metal layer 123.

[0050] The first metal layer 121 and the second metal layer 122 are each formed by any method such as electroless plating or sputtering. As an example, the first metal layer 121 and the second metal layer 122 may each be a sputtering film formed by a dry process. The sputtering film may have good adhesion to resins such as epoxy resin. Therefore, the conductor layer 12 having the seed layer which is a sputtering film, i.e., the first metal layer 121 and the second metal layer 122 (particularly the first metal layer 121) which are sputtering films, is considered to be firmly adhered to the insulating layer 11 on the first surface 1F side of the wiring board 1. As described above, the conductor layer 12 may include a fine conductor pattern such as the wiring 12w. If the conductor layer 12 including the fine conductor pattern is firmly adhered to the insulating layer 11, it is considered that peeling between the conductor layer and the insulating layer in the wiring board 1 is suppressed. In other words, it is considered that missing wiring such as the wiring 12W is suppressed.

[0051] As shown in FIG. 3, in a cross section of the conductor pattern 120 of the conductor layer 12, such as the wiring 12w and the via pad 12v, the width W11 of the first metal layer 121 is larger than the width W12 of the second metal layer 122. In addition, the width W13 of the third metal layer 123 is larger than the width W11 of the first metal layer. Note that FIG. 3 shows a cross section (hereinafter, this cross section is also simply referred to as "cross section C") of the conductor pattern of the conductor layer 12 along the stacking direction of the first buildup section 10 and the second buildup section 20 (see FIG. 2). The stacking direction of the first buildup section 10 and the second buildup section 20 is also simply referred to as the "Z direction" below. The width W11 of the first metal layer 121 is the length of the first metal layer 121 in the X direction perpendicular to the Z direction in the cross section C. When the length of the first metal layer 121 in the X direction is not constant in the Z direction, the width W11 of the first metal layer 121 is the length of the first metal layer 121 in the X direction that is the largest in the Z direction. Similarly, the width W12 of the second metal layer 122 is the length of the second metal layer 122 in the X direction of the cross section C, and when the length of the second metal layer 122 in the X direction is not constant in the Z direction, the width W12 of the second metal layer 122 is the length of the second metal layer 122 in the X direction that is the largest in the Z direction. Furthermore, the width W13 of the third metal layer 121 is the length of the third metal layer 123 in the X direction of the cross section C, and when the length of the third metal layer 123 in the X direction is not constant in the Z direction, the width W13 of the third metal layer 121 is the length of the third metal layer 123 in the X direction that is the largest in the Z direction.

[0052] Since the width W11 of the first metal layer 121 is larger than the width W12 of the second metal layer 122, and the width W13 of the third metal layer 123 is larger than the width W11, the width W13 is larger than the width W12. Therefore, the width of the third metal layer 123, which is an electrolytic plating film in one example, is larger than the width of the seed layer (first metal layer 121 and second metal layer 122) of the electrolytic plating film that constitutes the third metal layer 123 in that example.

[0053] The conductor pattern 120 of the conductor layer 12, which includes such first to third metal layers 121 to 123, has a constriction N in the region of the second metal layer 122. Therefore, the conductor pattern 120 has a larger contact area with the surrounding insulating layer 11 at its side surface. Therefore, it is considered that the conductor pattern 120 is more firmly attached to the insulating layer 11 that contacts it at its side surface (X direction) than if it did not have the constriction N. The length L of the constriction N in the Z direction may be about 1 μm.

[0054] Moreover, first metal layer 121, which has width W11 larger than width W12 of second metal layer 122, has an interface with insulating layer 11 on first surface 1F side (see FIG. 1) of wiring board 1 that is larger than the interface with second metal layer 122. Since the contact area with insulating layer 11 is larger than the contact area with second metal layer 122, the peel strength between insulating layer 11, which is made of epoxy resin or the like that does not easily have high adhesion with metal, and conductor pattern 120 is improved.

[0055] Furthermore, the portion of the insulating layer 11 on the side of the conductor pattern 120 near the constriction N enters into the recess on the side of the conductor pattern 120 caused by the constriction N. This suppresses the behavior of the conductor pattern 120 in the Z direction. This makes it difficult for the conductor pattern 120 to separate from the insulating layer 11 that contacts it on the first surface 1F side of the wiring board 1. This is thought to further suppress peeling between the conductor layer 12 and the insulating layer 11.

[0056] Thus, according to the wiring board of the present embodiment, the adhesion between the conductor layer 12 and the insulating layer 11 is improved and delamination is suppressed, which is believed to suppress loss of wiring such as the wiring 12W.

[0057] 3, the width of the conductor pattern 120 in cross section C is smallest at the boundary between the second metal layer 122 and the third metal layer 123. Also, in cross section C shown in FIG. 3, the side surface S3 of the third metal layer 123 has a tapered portion T that is inclined toward the inside of the conductor pattern 120 as it approaches the second metal layer 122, and a parallel portion P that is approximately along the Z direction. The tapered portion T is formed near the interface with the second metal layer 122 and is in contact with the second metal layer 122.

[0058] In the example of FIG. 3, in the cross section C, the inclination (first angle θ1) of the tapered portion T from the lower surface (insulating layer surface) 11a facing the second buildup portion 20 side (see FIG. 2) of the insulating layer 11 is smaller than the inclination (second angle θ2) of the side surface S12 of the first metal layer 121 and the second metal layer 122 from the lower surface 11a. That is, the inclination (90°-θ1) of the tapered portion T with respect to the stacking direction (Z direction) of the first buildup portion 10 and the second buildup portion 20 is larger than the inclination (90°-θ2) of the side surface S12 of the first metal layer 121 and the second metal layer 122 with respect to the Z direction. As a result, the thinnest part of the conductor pattern 120 is separated from the lower surface 11a of the insulating layer 11 by a larger amount. Therefore, the distortion transmitted from the lower surface 11a to the thinnest part of the conductor pattern 120 due to temperature change is alleviated. Therefore, the occurrence of cracks in the conductive pattern 120 may be suppressed.

[0059] The "side surface S3 of the third metal layer 123" is a surface other than the top and bottom surfaces of the third metal layer 123, which connects the top and bottom surfaces. Similarly, the "side surface S12 of the first metal layer 121 and the second metal layer 122" is a surface other than the top and bottom surfaces of the laminate of the first metal layer 121 and the second metal layer 122, which connects the top and bottom surfaces.

[0060] The total thickness of the first metal layer 121 and the second metal layer 122 is, for example, 0.02 μm or more and 1 μm or less, preferably 0.03 μm or more and 0.5 μm or less, and more preferably 0.05 μm or more and 0.3 μm or less. The arithmetic mean roughness (Ra) of the lower surface 11a of the insulating layer 11 can be 0.02 μm or more and 0.06 μm or less, as described above. Therefore, if the total thickness of the first metal layer 121 and the second metal layer 122 is less than 0.02 μm, it may be difficult to uniformly form a seed layer made of both metal layers over the entire lower surface 11a of the insulating layer 11. In addition, if the total thickness of the first metal layer 121 and the second metal layer 122 exceeds 1 μm, it may be difficult to control the wiring width of the wiring 12w, etc., in the etching removal process of the seed layer made of both metal layers.

[0061] The thickness of the first metal layer 121 is 0.01 μm or more and 0.5 μm or less, preferably 0.02 μm or more and 0.3 μm or less, and more preferably 0.03 μm or more and 0.1 μm or less. If the thickness of the first metal layer is less than 0.01 μm, the adhesion between the conductor layer 12 and the insulating layer 11 decreases. If the thickness of the first metal layer 121 exceeds 0.5 μm, the first metal layer 121 may be formed of, for example, a copper alloy rather than pure copper as described later, and therefore a low resistance value required for the conductor pattern 120 such as the wiring 12w may not be obtained.

[0062] The thickness of the second metal layer 122 is 0.01 μm or more and 0.9 μm or less, preferably 0.02 μm or more and 0.3 μm or less, and more preferably 0.03 μm or more and 0.2 μm or less. If the thickness of the second metal layer 122 is less than 0.01 μm, the low resistance value required for the conductor pattern 120 such as the wiring 12w may not be obtained. If the thickness of the second metal layer 122 exceeds 0.9 μm, the first metal layer 121 is thin, and therefore the adhesion between the conductor layer 12 and the insulating layer 11 may decrease.

[0063] The first metal layer 121 is made of, for example, an alloy of copper and an element other than copper, that is, a copper alloy. On the other hand, the second metal layer 122 may be, for example, a copper alloy different from that of the first metal layer 121, but is preferably made of substantially only copper. The third metal layer 123 is also preferably formed of substantially only copper. The copper alloy may have a higher adhesive strength with the resin used in the insulating layer 11, such as an epoxy resin, than pure copper. Therefore, peeling of the conductor layer 12 from the insulating layer 11 is further suppressed.

[0064] The weight of copper in the copper alloy constituting the first metal layer 121 is, for example, 90% or more of the total weight of the copper alloy constituting the first metal layer 121. The conductive pattern 120 such as the wiring 12w can have a low resistance value. The copper content (atomic weight %) in the second metal layer 122 is, for example, 99.5% or more, and preferably 99.95% or more. On the other hand, the conductive layers 22, 22a, 32 and the via conductors 23, 23a, 33 (see FIG. 1) included in the second buildup section 20 or the third buildup section 30 may be formed of a metal that does not contain copper, such as nickel, or other metal having appropriate conductivity.

[0065] 3, in the insulating layer 11, some (first inorganic particles 51a) of the multiple inorganic particles 5 penetrate at least partially into the conductive pattern 120 beyond the outer edge of the third metal layer 123 around the first metal layer 121 and the second metal layer 122. The first inorganic particles 51a penetrate into a recess formed on the side surface of the conductive pattern 120 due to a constriction N of the conductive pattern 120. The first inorganic particles 51a are smaller than the first inorganic particles 51b that do not penetrate into the conductive pattern 120. The particle size of the first inorganic particles 51a can be, for example, 1.0 μm or less.

[0066] The recesses on the side surface of the conductive pattern 120 caused by the constrictions N are filled with first inorganic particles 51a having a small particle size and resin 110. The proportion of the first inorganic particles 51 in the recesses caused by the constrictions N may be greater than the proportion of the first inorganic particles 51 in the entire insulating layer 11. Therefore, the expansion coefficient of the insulating layer 11 in the recesses caused by the constrictions N may approach the expansion coefficient of the conductive pattern 120. As a result, stress that tends to concentrate in the constrictions N including the portion of the conductive pattern 120 with the minimum width may be reduced.

[0067] As shown in FIG. 3, the shape of the second inorganic particles 52 is different from the shape of the first inorganic particles 51. The second inorganic particles 52 have flat portions 52a. The flat portions 52a form inner wall surfaces 13b exposed to the openings 13a in the insulating layer 11. The inner wall surfaces 13b are formed by the flat portions 52a of the second inorganic particles 52 and the surfaces 110a of the resin 110 exposed to the openings 13a. The flat portions 52a and the surfaces 110a of the resin 110 are substantially flush with each other. The surfaces 110a of the resin 110 are not uneven. The flat portions 52a are also not uneven. For example, the arithmetic mean roughness (Ra) of the inner wall surfaces 13b may be 1.0 μm or less. The inner wall surfaces 13b are substantially smooth. A thin first metal layer 121 may be formed seamlessly on the inner wall surfaces 13b.

[0068] Next, with reference to Figures 4A to 4M, an example of a method for manufacturing the wiring board of this embodiment will be described, taking as an example the case of manufacturing the wiring board 1 illustrated in Figure 1. Unless otherwise stated, each component may be formed using any of the materials previously described for each component of the wiring board 1.

[0069] As shown in FIG. 4A, a support substrate S, which is a glass substrate as an example, is prepared. An adhesive layer AL containing an adhesive such as a photoplastic azobenzene-based polymer adhesive is formed on the surface of the support substrate S by coating, lamination, or the like. Then, a metal film 124 made of copper, nickel, or the like is formed on the adhesive layer AL by electroless plating or sputtering, or by attaching a metal foil using the adhesive layer AL. The support substrate S has a first surface Sa and a second surface Sb. In FIGS. 4B to 4M to be referred to below, the second surface Sb side is omitted from illustration, and only the first surface Sa side is shown. However, the wiring substrate 1 may also be formed on the second surface Sb side by performing the same process as that on the first surface Sa side.

[0070] As shown in FIG. 4B, a conductor layer 12a including conductor pads (component mounting pads 12p) is formed on the adhesive layer AL. In forming the conductor layer 12a, a plating resist (not shown) having openings corresponding to the formation regions of the conductor patterns to be included in the conductor layer 12a is formed on the metal film 124 shown in FIG. 4A by laminating a dry film, exposing to light, and developing. Then, the conductor layer 12a is formed by electrolytic plating using the metal film 124 as a power supply layer. Thereafter, the plating resist is removed, and further, the portion of the metal film 124 exposed by removing the plating resist is removed by etching or the like. The conductor layer 12a in the state shown in FIG. 4B is obtained.

[0071] Furthermore, an insulating layer 11 is formed to cover the conductor layer 12a. The insulating layer 11 is formed, for example, by laminating a film-like epoxy resin on the conductor layer 12a and thermocompressing it. As described above, the insulating layer 11 (as well as the insulating layer 21 and the insulating layer 31 (see FIG. 4L to FIG. 4M) formed in a later process) can be formed using a thermosetting resin such as BT resin or phenol resin, or a thermoplastic resin such as fluororesin or LCP, in addition to the epoxy resin. For example, a film-like resin containing inorganic particles 5 (see FIG. 4C) made of silica (SiO2), alumina, mullite, or the like, and the insulating resin 110 (see FIG. 4C) made of the epoxy resin, phenol resin, or the like described above is used. In the state shown in FIG. 4B, all of the inorganic particles 5 contained in the insulating layer 11 can be the first inorganic particles 51 (see FIG. 4C).

[0072] A protective film PF made of a polyethylene terephthalate (PET) film or the like is provided on the surface (lower surface) 11a of the insulating layer 11. For example, a film-like resin having the protective film PF is laminated in forming the insulating layer 11. The protective film PF may be attached to the insulating layer 11 or the film-like resin constituting the insulating layer 11 via a release agent (not shown) or the like for easy peeling off of the protective film PF.

[0073] As shown in FIG. 4C, an opening 13a is formed in the insulating layer 11 at a position where the via conductor 13 (see FIG. 1) is to be formed by irradiation with a carbon dioxide laser beam or the like. FIG. 4C and FIGS. 4D to 4I, which will be referred to below, show enlarged views of a portion corresponding to the IVC portion in FIG. 4B after the steps described in each figure are performed. The formation of the opening 13a by irradiation with a carbon dioxide laser beam or the like is performed while the surface 11a of the insulating layer 11 is protected by the protective film PF. Even if the resin 110 is scattered during the irradiation with the laser beam, the scattered resin 110 is prevented from adhering to the surface 11a of the insulating layer 11. Then, the opening 13a is formed, which penetrates the protective film PF as well as the insulating layer 11.

[0074] The inner wall surface 13b of the insulating layer 11 is formed of the resin 110 and inorganic particles 53 of the inorganic particles 5 protruding from the resin 110. By irradiating the insulating layer 11 with a laser beam, a part of the first inorganic particles 51 embedded in the resin 110 protrudes from the resin 110 to become the inorganic particles 53. The inorganic particles 53 forming the inner wall surface 13b include a part protruding from the resin 110 and a part buried in the resin 110. In order to control the shape of the inner wall surface 13b, a predetermined treatment is applied to the inner wall surface 13b. The size of the unevenness of the inner wall surface 13b is controlled by controlling the conditions for treating the inner wall surface 13b. Preferably, the part of the inorganic particles 53 protruding from the resin 110 is selectively removed by the treatment.

[0075] As a result, as shown in Fig. 4D, second inorganic particles 52 having flat portions 52a are formed. As an example, the second inorganic particles 52 are formed by treating the inner wall surface 13b of the insulating layer 11 with a chemical after irradiation with the laser light. For example, the inner wall surface 13b is treated with an etching solution having a faster etching rate for the inorganic particles 5 than for the resin 110. As an example, a permanganate solution is used.

[0076] Alternatively, the second inorganic particles 52 may be formed by treating the inner wall surface 13b with a plasma gas. The shape of the inner wall surface 13b can be controlled by controlling the conditions of the plasma treatment. As some examples, the etching rate of the inorganic particles 5 and the etching rate of the resin 110 can be controlled by adjusting conditions such as temperature, concentration, time, type and pressure of the plasma gas. For example, plasma gas such as argon, tetrafluoromethane, a mixture of tetrafluoromethane and oxygen, or sulfur hexafluoride is used.

[0077] That is, a part of the spherical first inorganic particle 51 protrudes into the opening 13a by forming the opening 13a by irradiation with a laser beam to become an inorganic particle 53 (see FIG. 4C), and the protruding part is cut off flat by the above-mentioned appropriate processing. As described later, when the first metal film 12α (see FIG. 4E) is formed as a seed layer on the inner wall surface 13b of the insulating layer 11 by, for example, sputtering in a later process, the protruding part of the inorganic particle 53 may hinder the growth of the sputtering film. A seed layer that is continuous on the inner wall surface 13b may not be formed, or a thick seed layer may be required, making it impossible to form fine wiring. Therefore, the protruding part of the inorganic particle 53 is removed to form the second inorganic particle 52 having a flat part 52a. The flat part 52a that forms the inner wall surface 13b and the surface 110a of the resin 110 are approximately flush with each other. A smooth inner wall surface 13b without unevenness is obtained.

[0078] The treatment of the inner wall surface 13b is performed in a state where the surface 11a of the insulating layer 11 is protected by the protective film PF. Therefore, the surface 11a of the insulating layer 11 is not easily eroded by, for example, chemicals or plasma gas during the treatment of the inner wall surface 13b.

[0079] After the processing of the inner wall surface 13b of the insulating layer 11, the inside of the opening 13a is cleaned as necessary. By cleaning the inside of the opening 13a, resin residues generated when the opening 13a is formed are removed. That is, the cleaning may include a desmear process. The cleaning of the inside of the opening 13a is performed by a plasma process, for example. That is, the cleaning may be performed by a dry process. The surface 11a of the insulating layer 11 is not affected by the plasma process because it is covered with the protective film PF. Therefore, at this point, no irregularities are formed on the surface 11a of the insulating layer 11. The surface 11a is not roughened. Note that if the inside of the opening 13a is sufficiently cleaned by the processing of the inner wall surface 13b in the preceding process, the cleaning of the inside of the opening 13a after the processing of the inner wall surface 13b may be omitted.

[0080] After cleaning the inside of the opening 13a (after processing the inner wall surface 13b when cleaning the inside of the opening 13a is omitted), the protective film PF is removed from the insulating layer 11. As described above, the surface 11a of the insulating layer 11 is not affected by the chemicals or plasma gas used for cleaning the inside of the opening 13a or processing the inner wall surface 13b. Therefore, the surface 11a after removing the protective film PF is flat. The flat surface 11a is cleaned as necessary. As an example, the surface 11a is dry etched. The dry etching is performed by sputtering using argon gas (argon sputtering), for example. A release agent and / or adhesive (not shown) that was present between the protective film PF and the insulating layer 11 may be removed.

[0081] As shown in FIG. 4E, a first metal film 12α is formed on the inner wall surface 13b of the insulating layer 11, on the exposed surface of the component mounting pad 12p, and on the entire surface 11a of the insulating layer 11. Furthermore, a second metal film 12β is formed on the first metal film 12α. The exposed surface of the second inorganic particle 52 on the inner wall surface 13b of the insulating layer 11 is covered with the first metal film 12α. The first metal film 12α and the second metal film 12β function as a seed layer when a third metal film 12γ (see FIG. 4G) is formed by electrolytic plating in a later process. The first metal film 12α and the second metal film 12β may be formed by electroless plating, but are preferably formed by sputtering. In particular, when the first metal film 12α is formed by sputtering, high adhesion strength between the insulating layer 11 and the first metal film 12α may be obtained.

[0082] In addition, since no irregularities are formed on the inner wall surface 13b of the insulating layer 11 and the surface 11a of the insulating layer 11 is also flat, the first metal film 12α can be formed by sputtering, which is thin but continuous. For example, the first metal film 12α has a thickness of 0.01 μm or more and 0.5 μm or less, and the second metal film 12β has a thickness of 0.01 μm or more and 0.9 μm or less.

[0083] A part of the first metal film 12α can become a first metal layer 121 (see FIG. 2) constituting the conductor layer 12 formed on the insulating layer 11. A part of the second metal film 12β can become a second metal layer 122 (see FIG. 2) constituting the conductor layer 12 together with the first metal layer 121. Therefore, the first metal film 12α is formed of an alloy of copper and an element other than copper, as described above as the material of the first metal layer 121. Also, the second metal film 12β is formed of almost only copper, or a copper alloy different from the copper alloy constituting the first metal film 12α, as described above as the material of the second metal layer 122.

[0084] As shown in FIG. 4F, a plating resist R having an opening R1 is provided on the second metal film 12β. The plating resist R is formed, for example, by laminating a dry film on the second metal film 12β, and the opening R1 is formed, for example, by a photolithography technique. The opening R1 is formed in a pattern corresponding to a conductor pattern to be included in the conductor layer 12 (see FIG. 4J) formed on the insulating layer 11. As described above, the wiring such as the wiring 12w (see FIG. 2) included in the conductor layer 12 may have a wiring width of 3 μm or less. Each opening R1 is formed with an opening width according to the wiring width to be included in each conductor pattern such as the wiring 12w formed in each opening R1. Also, as described above, the wiring of the conductor layer 12 may have an aspect ratio of 2.0 or more and 4.0 or less. Therefore, preferably, the plating resist R is formed having a thickness (height) greater than or equal to the thickness (height) of the wiring that satisfies the aspect ratio to be included in the wiring to be formed.

[0085] As shown in FIG. 4G, a third metal film 12γ made of, for example, substantially copper is formed in an opening R1 of a plating resist R by electrolytic plating using the first metal film 12α and the second metal film 12β as a power supply layer. A part of the third metal film 12γ can become a third metal layer 123 (see FIG. 2) constituting a conductor layer 12 formed on an insulating layer 11. A via conductor 13 is formed in an opening 13a of the insulating layer 11. As shown in the example of FIG. 4G, the third metal film 12γ may be formed to fill the entire opening R1 and further have a curved surface protruding from the surface (lower surface) of the plating resist R. Wiring having a desired thickness and aspect ratio can be more reliably formed.

[0086] As shown in FIG. 4H, a part of the lower surface (surface opposite to the conductor layer 12a) of the third metal film 12γ is removed by polishing. At least the protruding part of the third metal film 12γ from the lower surface of the plating resist R is removed. The third metal film 12γ is polished until the total thickness of the first metal film 12α and the second metal film 12β reaches the thickness required for the conductor layer 12 (see FIG. 4J) formed on the insulating layer 11, for example, to 7 μm or less. As in the example of FIG. 4H, a part of the lower surface side of the plating resist R may also be removed together with a part of the third metal film 12γ. The polishing of the third metal film 12γ is performed by any method, such as chemical mechanical polishing (CMP). As a result of the polishing, the lower surface of the third metal film 12γ may have an arithmetic mean roughness of 0.3 μm or less.

[0087] After polishing the third metal film 12γ, the plating resist R is removed. Then, the portion of the second metal film 12β that is not covered with the third metal film 12γ is selectively removed by quick etching or the like, and further, the portion of the first metal film 12α that is exposed from the second metal film 12β is selectively removed by, for example, quick etching or the like.

[0088] When the first metal film 12α and the second metal film 12β are formed by sputtering, the surface state of the film, such as the number of crystal defects, can be controlled by setting conditions such as the temperature during sputtering and the pressure of the rare gas collided with the target. Therefore, by selecting the sputtering conditions, the first metal film 12α and the second metal film 12β having a porous surface that is more easily etched than the third metal film 12γ formed by electrolytic plating can be formed. In addition, the first metal film 12α and the second metal film 12β formed under such conditions can be dissolved and removed in a larger amount than the third metal film 12γ in quick etching. In addition, the first metal film 12α and the second metal film 12β are formed of copper alloys different from each other at least, or the first metal film 12α is formed of a copper alloy and the second metal film 12β is formed of almost only copper. Therefore, an etching solution having a higher etching rate for the second metal film 12β than the first metal film 12α, for example, an etching solution having a higher etching rate for pure copper than a copper alloy, is used. By selecting such an etching solution, it is possible to dissolve a larger amount of second metal film 12β than the amount of first metal film 12α.

[0089] As a result of selectively removing the first and second metal films 12α and 12β, as shown in FIG. 7I, an individually separated conductor pattern 120 such as the wiring 12w and the via pad of the via conductor 13 is obtained. The conductor pattern 120 includes a first metal layer 121, a second metal layer 122, and a third metal layer 123, which are stacked in this order from the insulating layer 11 side. The first metal layer 121 and the second metal layer 122 are respectively made of the remaining portions of the first metal film 12α and the second metal film 12β (see FIG. 4H) after the selective removal. The third metal layer 123 is made of the third metal film 12γ remaining after removing a part of the third metal film 12γ (see FIG. 4H) by the polishing.

[0090] As described above, by appropriately selecting the conditions for forming first metal film 12α and second metal film 12β, which are formed by sputtering as an example, it is possible to form third metal layer 123 having a width larger than that of first metal layer 121 and second metal layer 122. In addition, by appropriately selecting an etching solution for selectively removing first metal film 12α and second metal film 12β by quick etching as described above, it is possible to form first metal layer 121 having a width larger than that of second metal layer 122.

[0091] As shown in Fig. 4J, a conductor layer 12 including predetermined conductor patterns separated from one another, such as wiring 12w, is obtained. In Fig. 4J, like Fig. 1, the conductor layer 12 is shown to have only one layer, but the conductor layer 12 is composed of a first metal layer 121, a second metal layer 122, and a third metal layer 123 shown in Fig. 4I.

[0092] As shown in Fig. 4K, three sets of insulating layers 11 and conductor layers 12, and via conductors 13 are further formed on the insulating layer 11 and conductor layer 12 formed in the steps up to Fig. 4J in the same manner as described with reference to Fig. 4B to Fig. 4I. Then, on the laminate of the conductor layer 12 and insulating layer 11 thus formed, an insulating layer 11 is further laminated in the same manner as the other insulating layers 11, and an opening 13a penetrating the insulating layer 11 is formed by irradiation with laser light or the like. The first build-up section 10 is completed.

[0093] 4L, a conductor layer 22a is formed on the underside of the first buildup section 10, and a via conductor 23a is formed in the opening 13a. The second buildup section 20 is formed by repeating the formation of the insulating layer 21, the conductor layer 22, and the via conductor 23. The conductor layer 22a, the conductor layer 22, the via conductor 23a, and the via conductor 23 are formed by any method for forming a conductor layer and a via conductor, such as a semi-additive method. The insulating layer 21 can be formed by laminating and thermocompression bonding a film-like resin, similar to the method for forming the insulating layer 11.

[0094] As shown in FIG. 4M, the insulating layer 31, the conductor layer 32, and the via conductors 33 penetrating the insulating layer 31 of the third buildup section 30 are formed on the surface (second surface 20B) of the second buildup section 20 opposite to the support substrate S side. The insulating layer 31 in FIG. 4M is formed by laminating and thermocompression bonding prepregs containing an insulating resin such as epoxy resin impregnated in a core material 31a made of glass fiber or the like. The insulating layer 31 may be formed by thermocompression bonding of a film-like resin, similar to the insulating layer 21. The conductor layer 32 and the via conductors 33 may be formed, for example, by a semi-additive method, similar to the method for forming the conductor layer 22 and the via conductors 23, or may be formed by any other method for forming a conductor layer, such as a subtractive method. The formation of the third buildup section 30 is completed.

[0095] Furthermore, a solder resist 40 is formed by depositing a photosensitive epoxy resin film or a polyimide resin film on the surfaces of the insulating layer 31 and the conductor layer 32. Then, openings 41 that define the conductor pads 32p are formed by photolithography.

[0096] Thereafter, the support substrate S is removed. For example, the adhesive layer AL is irradiated with a laser beam, and after the adhesive layer AL is softened, the support substrate S is peeled off from the conductor layer 12a and the insulating layer 11. The upper surface of the conductor layer 12a and the upper surface of the insulating layer 11 are exposed. If the adhesive layer AL remains, it is removed using an appropriate solvent. The wiring board 1 shown in FIG. 1 is completed.

[0097] The wiring board of the embodiment is not limited to those having the structure illustrated in each drawing, and the structure, shape, and material illustrated in this specification. Each build-up portion included in the wiring board of the embodiment may have any number of insulating layers and conductor layers as described above. In addition, the wiring board of the embodiment does not necessarily include a third build-up portion. The outermost insulating layer and conductor layer on the opposite side to the component mounting surface of the wiring board of the embodiment may not be formed thicker than the insulating layer and conductor layer in the second build-up portion, and the outermost insulating layer on the opposite side to the component mounting surface of the wiring board may not include a core material. The inorganic particles included in the insulating layer of the first build-up portion may not include inorganic particles that constitute the inner wall surface exposed to the opening of the insulating layer, such as the second inorganic particles. [Explanation of symbols]

[0098] 1. Wiring board 1F, 1st floor 1B 2nd side 10 First build-up section 11 Insulating layer 11a: Insulating layer surface (lower surface of insulating layer 11 facing the second buildup portion) 110 Resin 12, 12a Conductive layer 12w wiring 120 Conductor Pattern 121 First metal layer (first seed layer) 122 Second metal layer (second seed layer) 123 Third metal layer (electrolytic plating film) 20 Second Build-up Section 21 Insulating layer 22, 22a Conductor layer 22w wiring 30 Third Build-up Section 31 Insulating layer 31a Core material 32 Conductor layer 33 Via conductor 51 First inorganic particle 51a Part of the first inorganic particle C section G1 Wiring spacing between 12w wires G2 Wiring spacing between 22w wires S12 Sides of the first and second metal layers S3 Third metal layer side T Tapered side of third metal layer W1 Wiring width of 12w W11 Width of first metal layer W12 Width of second metal layer W13 Width of third metal layer W2 Wiring width of 22w θ1: Inclination of the tapered portion of the third metal layer from the bottom surface of the insulating layer 11 (first angle) θ2: Inclination of the side surfaces of the first and second metal layers from the bottom surface of the insulating layer 11 (second angle)

Claims

1. a first surface and a second surface opposite the first surface; a first buildup section including insulating layers and conductor layers stacked one on the other; a second buildup section including an insulating layer and a conductor layer stacked one on the other; A wiring board comprising: the first buildup section is laminated on the first surface side of the second buildup section, and a minimum wiring width of wiring included in a conductor layer of the first buildup section is smaller than a minimum wiring width of wiring included in a conductor layer of the second buildup section; a minimum wiring interval between wirings included in the conductor layer of the first buildup portion is smaller than a minimum wiring interval between wirings included in the conductor layer of the second buildup portion; the conductor pattern included in the conductor layer of the first buildup portion includes a first metal layer, a second metal layer laminated on the second surface side of the first metal layer, and a third metal layer laminated on the second surface side of the second metal layer, In a cross section of the conductor pattern along the stacking direction of the first buildup portion and the second buildup portion, the width of the first metal layer is larger than the width of the second metal layer, and the width of the third metal layer is larger than the width of the first metal layer.

2. 2. The wiring board according to claim 1, wherein the third metal layer is made of an electrolytic plating film, and the first metal layer and the second metal layer are seed layers for the electrolytic plating film and made of sputtering films.

3. 2. The wiring board according to claim 1, wherein the minimum wiring width and the minimum wiring spacing of the wiring included in the conductor layer of the first buildup portion are each 3 [mu]m or less.

4. 2. The wiring board according to claim 1, wherein the aspect ratio of the wiring included in the conductor layer of the first buildup portion is not less than 2.0 and not more than 4.

0.

5. 2. The wiring board according to claim 1, wherein a surface of the conductor layer of the first build-up portion is a polished surface.

6. 2. The wiring board according to claim 1, further comprising a third buildup section laminated on the second surface side of the second buildup section and including an insulating layer, a conductive layer, and a via conductor.

7. 7. The wiring board according to claim 6, wherein the insulating layer included in the third buildup section includes a core material.

8. 2. The wiring board according to claim 1, wherein the first surface is a component mounting surface.

9. 2. The wiring board according to claim 1, wherein the arithmetic mean roughness (Ra) of the surface of the insulating layer of the first buildup portion is 0.02 [mu]m or more and 0.06 [mu]m or less.

10. 2. The wiring board according to claim 1, wherein the width of the conductor pattern in the cross section is smallest at a boundary between the second metal layer and the third metal layer.

11. 2. The wiring board according to claim 1, a side surface of the third metal layer has a tapered portion that is inclined toward an inner side of the conductor pattern as it approaches the second metal layer, In the cross section, the inclination of the tapered portion from the surface of the insulating layer of the first buildup portion is smaller than the inclination of the side surfaces of the first metal layer and the second metal layer from the surface of the insulating layer.

12. 2. The wiring board according to claim 1, the insulating layer of the first buildup section includes a resin and a plurality of inorganic particles; a portion of the inorganic particles is disposed around the first metal layer and the second metal layer and is at least partially inside the conductive pattern with respect to an outer edge of the third metal layer; The particle diameter of the part of inorganic particles is 1.0 μm or less.

13. 2. The wiring board according to claim 1, the first metal layer is made of an alloy of copper and an element other than copper, The second metal layer consists essentially of copper.

14. 14. The wiring board according to claim 13, wherein a weight of copper in said alloy is 90% or more of a total weight of said alloy.

15. 2. The wiring board according to claim 1, wherein the first metal layer and the second metal layer have a total thickness of 0.02 [mu]m or more and 1 [mu]m or less.

16. 2. The wiring board according to claim 1, wherein the first metal layer has a thickness of 0.01 [mu]m or more and 0.5 [mu]m or less.

Citation Information

Patent Citations

  • Method for manufacturing printed circuit board

    JP2005005341A