Nitride semiconductor device

The nitride semiconductor device addresses the trade-off between on-resistance and off-state characteristics by strategically positioning the p-type layer and controlling sidewall angles, resulting in improved performance and reliability.

JP2024148579AActive Publication Date: 2024-10-18PANASONIC HOLDINGS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023061829
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Conventional nitride semiconductor devices face a trade-off between reducing on-resistance and maintaining off-state characteristics due to the extension of the depletion layer affecting the two-dimensional electron gas channel, leading to inadequate performance in both areas.

Method used

The nitride semiconductor device is designed with a specific configuration that includes a p-type nitride semiconductor layer positioned away from the two-dimensional electron gas channel to minimize channel narrowing while maintaining electric field relaxation during the off-state, achieved by controlling the angles and positions of the sidewall surfaces of the opening, allowing for precise etching and improved reliability.

Benefits of technology

This configuration enables both reduced on-resistance and good off-state characteristics by effectively managing the depletion layer, enhancing the device's performance and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148579000001_ABST
    Figure 2024148579000001_ABST
Patent Text Reader

Abstract

To achieve both satisfactory off-characteristics and reduction in on-resistance.SOLUTION: A nitride semiconductor device 1 comprises: a substrate 10; a drift layer 12; a p-type first ground layer 14; a second ground layer 16; a gate opening 40 penetrating the second ground layer 16 and the first ground layer 14 and reaching the drift layer 12; an electron travel layer 22 and an electron supply layer 24 which are provided successively from a lower side so as to cover a top face of the second ground layer 16 and the gate opening 40; a gate electrode 34; a source electrode 32; and a drain electrode 36. Regarding a sidewall part 40b of the gate opening 40, in a case where a position of the sidewall part 40b between a lower end PL and an upper end PH of the first ground layer 14 is defined as a first end P1, a first angle α1 formed by a dashed line VL1 connecting the lower end PL and the first end P1 with respect to a principal surface 10a is larger than a second angle α2 formed by a dashed line VL2 connecting the lower end PL and the upper end PH with respect to the principal surface 10a.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to nitride semiconductor devices. [Background technology]

[0002] Nitride semiconductors, such as GaN, are wide-gap semiconductors with bandgaps of 3.4 eV and 6.2 eV for GaN and AlN at room temperature, respectively. Nitride semiconductors have the advantage of a large dielectric breakdown field and a high electron saturation drift velocity compared to compound semiconductors such as GaAs or Si semiconductors. For this reason, research and development of power transistors using nitride semiconductors, which are advantageous for achieving high output and high voltage resistance, is currently being actively conducted.

[0003] In addition, in the AlGaN / GaN heterostructure, spontaneous polarization and piezoelectric polarization on the (0001) surface generate a high concentration of two-dimensional electron gas (2DEG) at the heterointerface, and the density of 2DEG is 1×10 13 cm -2 The sheet carrier concentration can be increased by 100%.

[0004] Patent Document 1 discloses a vertical nitride semiconductor device. In the nitride semiconductor device disclosed in Patent Document 1, a GaN electron transit layer and an AlGaN electron supply layer are formed in this order in an opening that penetrates a p-type underlayer and reaches a drift layer. A two-dimensional electron gas channel generated at an AlGaN / GaN heterointerface formed on the side wall of the opening is opened and closed by a gate voltage to realize a transistor operation. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6511645 Summary of the Invention [Problem to be solved by the invention]

[0006] In conventional nitride semiconductor devices, when a transistor is turned on, a depletion layer extends from the p-type underlayer into the electron transport layer. This narrows the two-dimensional electron gas channel in the electron transport layer, which makes it difficult to sufficiently reduce the on-resistance. On the other hand, if the p-type underlayer is separated from the channel to such an extent that it is not affected by the extended depletion layer, the electric field during the off-state cannot be sufficiently alleviated, and the off-state breakdown voltage decreases. Thus, in conventional nitride semiconductor devices, there is a trade-off between reducing the on-resistance and maintaining the off-state characteristics.

[0007] The present disclosure provides a nitride semiconductor device that can achieve both good off-characteristics and reduced on-resistance. [Means for solving the problem]

[0008] A nitride semiconductor device according to one aspect of the present disclosure includes a substrate, a first nitride semiconductor layer provided above the substrate, a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer, a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer, a first opening that penetrates the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaches the first nitride semiconductor layer, an electron transit layer and an electron supply layer provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening, and a gate electrode provided above the gate electrode, a source electrode provided at a distance from the gate electrode, and a drain electrode formed below the substrate, wherein a sidewall portion of the first opening is parallel to a direction in which the gate electrode and the source electrode are arranged when a position between a lower end and an upper end of the first p-type nitride semiconductor layer on the sidewall portion of the first opening is defined as a predetermined position, and in a cross section perpendicular to a main surface of the substrate, a first angle that a first line segment connecting the lower end and the predetermined position forms with the main surface is greater than a second angle that a second line segment connecting the lower end and the upper end forms with the main surface.

[0009] A nitride semiconductor device according to another aspect of the present disclosure includes a substrate, a first nitride semiconductor layer provided above the substrate, a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer, a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer, a first opening that penetrates the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaches the first nitride semiconductor layer, an electron transport layer and an electron supply layer that are provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening, and a gate electrode provided above the electron supply layer so as to cover the first opening; a second opening at a position away from the gate electrode, penetrating the electron supply layer, the electron transit layer and the second nitride semiconductor layer and reaching the first p-type nitride semiconductor layer; a source electrode provided to cover the second opening and electrically connected to the first p-type nitride semiconductor layer; and a drain electrode formed below the substrate, wherein a sidewall portion of the first opening has at least one step between an upper end and a lower end of the first p-type nitride semiconductor layer. Effect of the Invention

[0010] The nitride semiconductor device according to the present disclosure can achieve both good off-state characteristics and reduced on-state resistance. [Brief description of the drawings]

[0011] [Figure 1A] FIG. 1A is a cross-sectional view of a nitride semiconductor device according to a first embodiment. [Figure 1B] FIG. 1B is an enlarged cross-sectional view of a portion of FIG. 1A. [Figure 2A] FIG. 2A is a cross-sectional view for explaining channel narrowing in a nitride semiconductor device according to a comparative example. [Figure 2B] FIG. 2B is a cross-sectional view for illustrating the effect of the nitride semiconductor device according to the first embodiment. [Figure 3A] FIG. 3A is a cross-sectional view of a nitride semiconductor device according to a modification of the first embodiment. [Figure 3B] FIG. 3B is an enlarged cross-sectional view of a portion of FIG. 3A. [Figure 4] FIG. 4 is a cross-sectional view of a nitride semiconductor device according to the second embodiment. [Diagram 5] FIG. 5 is a cross-sectional view of a nitride semiconductor device according to a modification of the second embodiment. [Figure 6] FIG. 6 is a cross-sectional view of a nitride semiconductor device according to the third embodiment. [Figure 7A] FIG. 7A is a cross-sectional view of a nitride semiconductor device according to the fourth embodiment. [Figure 7B] FIG. 7B is an enlarged cross-sectional view of a portion of FIG. 7A. [Figure 8] FIG. 8 is a cross-sectional view of a nitride semiconductor device according to the fifth embodiment. [Figure 9A] FIG. 9A is a cross-sectional view of a nitride semiconductor device according to the sixth embodiment. [Figure 9B] FIG. 9B is an enlarged cross-sectional view of a portion of FIG. 9A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (Summary of the Disclosure) In order to solve the above problems, nitride semiconductor devices according to several aspects of the present disclosure have the following configuration.

[0013] A nitride semiconductor device according to a first aspect of the present disclosure includes a substrate, a first nitride semiconductor layer provided above the substrate, a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer, a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer, a first opening penetrating the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaching the first nitride semiconductor layer, an electron transit layer and an electron supply layer provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening, and the electron supply layer so as to cover the first opening. a gate electrode provided above a layer, a source electrode provided at a distance from the gate electrode, and a drain electrode formed below the substrate, wherein when a position between a lower end and an upper end of the first p-type nitride semiconductor layer on the sidewall of the first opening is defined as a predetermined position, the sidewall of the first opening is parallel to a direction in which the gate electrode and the source electrode are arranged, and in a cross section perpendicular to a main surface of the substrate, a first angle that a first line segment connecting the lower end and the predetermined position forms with the main surface is greater than a second angle that a second line segment connecting the lower end and the upper end forms with the main surface.

[0014] As a result, in the upper portion away from the bottom surface of the first opening, the first p-type nitride semiconductor layer can be kept away from the channel of the two-dimensional electron gas, thereby suppressing an increase in the resistance of the channel. In the lower portion close to the bottom surface of the first opening, the first p-type nitride semiconductor layer is kept close to the gate electrode, thereby mitigating the electric field during the off state and improving the breakdown voltage. In this way, the nitride semiconductor device according to this embodiment can achieve both good off characteristics and reduced on-resistance.

[0015] In a nitride semiconductor device according to a second aspect of the present disclosure, in the nitride semiconductor device according to the first aspect, the sidewall portion includes a first sidewall surface which is a section from the lower end to a first end located at the predetermined position, a second sidewall surface which is a section from a second end located between the first end and the upper end in a planar view to the upper end, and a third sidewall surface which is located between the first end and the second end and has a different slope from both the first sidewall surface and the second sidewall surface.

[0016] This makes it possible to place the second sidewall surface located in the upper part of the first p-type nitride semiconductor layer even farther away from the channel, thereby reducing the on-resistance.

[0017] A nitride semiconductor device according to a third aspect of the present disclosure is the nitride semiconductor device according to the second aspect, wherein the third sidewall surface is parallel to the primary surface.

[0018] As a result, the third sidewall surface can be the bottom surface of the opening formed by, for example, etching. This allows the first opening to be formed easily and accurately by, for example, two-stage etching. For example, it becomes easier to form the first opening according to design values, which can improve the reliability and yield of nitride semiconductor devices.

[0019] In a nitride semiconductor device according to a fourth aspect of the present disclosure, in the nitride semiconductor device according to the second or third aspect, a first inclination angle that is an angle that the first sidewall surface makes with respect to the main surface is different from a second inclination angle that is an angle that the second sidewall surface makes with respect to the main surface.

[0020] This allows the inclination angle of one of the first sidewall surface and the second sidewall surface to be increased, thereby shortening the unit cell length of the nitride semiconductor device. By shortening the unit cell length, more cells can be arranged in the same area, thereby further reducing the on-resistance. Note that a cell refers to the smallest unit configuration that operates as a transistor.

[0021] A nitride semiconductor device according to a fifth aspect of the present disclosure is the nitride semiconductor device according to the fourth aspect, wherein the first tilt angle is smaller than the second tilt angle.

[0022] This makes it more difficult for channel narrowing to occur in the upper portion of the channel within the first opening, which makes it possible to shorten the unit cell length while simultaneously achieving good off-state characteristics and reduced on-state resistance.

[0023] A nitride semiconductor device according to a sixth aspect of the present disclosure is the nitride semiconductor device according to the fifth aspect, wherein the second tilt angle is not less than 70° and not more than 90°.

[0024] As a result, when the inclination angle of the second sidewall surface located above the first sidewall surface is 70° or more and 90° or less, the effect of shortening the unit cell length becomes greater, and the on-resistance can be further reduced while maintaining good off-characteristics.

[0025] A nitride semiconductor device according to a seventh aspect of the present disclosure is the nitride semiconductor device according to any one of the second to sixth aspects, wherein the first p-type nitride semiconductor layer includes an AlGaN layer, and the third sidewall surface is a part of an upper surface of the AlGaN layer.

[0026] This allows the use of dry etching conditions that stop the etch at the AlGaN layer, stabilizing the shape and depth of the step, and making it easier to form the first opening according to the design values, thereby improving the reliability and yield of nitride semiconductor devices.

[0027] A nitride semiconductor device according to an eighth aspect of the present disclosure is a nitride semiconductor device according to any one of the first to seventh aspects, wherein the first nitride semiconductor layer is made of two or more layers having different impurity concentrations, and among the two or more layers, the uppermost layer has the lowest impurity concentration.

[0028] This promotes electric field relaxation during the off-state, resulting in better off-state characteristics.

[0029] A nitride semiconductor device according to a ninth aspect of the present disclosure is the nitride semiconductor device according to any one of the first to eighth aspects, further comprising a second p-type nitride semiconductor layer provided between the gate electrode and the electron supply layer.

[0030] This makes it possible to raise the potential of the conduction band edge of the channel and increase the threshold voltage. Therefore, for example, a normally-off type field effect transistor (FET) can be realized. In addition, the second p-type nitride semiconductor layer and the first p-type nitride semiconductor layer can optimize the electric field relaxation during the off state, thereby improving the off characteristics.

[0031] A nitride semiconductor device according to a tenth aspect of the present disclosure is the nitride semiconductor device according to any one of the first to ninth aspects, further comprising a second opening at a position away from the gate electrode, penetrating the electron supply layer, the electron transit layer and the second nitride semiconductor layer and reaching the first p-type nitride semiconductor layer, and the source electrode is provided in the second opening and electrically connected to the first p-type nitride semiconductor layer.

[0032] This allows the two-dimensional electron gas exposed on the sidewall of the second opening to come into contact with the source electrode, thereby reducing the on-resistance. Also, the first p-type nitride semiconductor layer can be strongly fixed to the source potential, thereby enhancing the electric field relaxation effect during the off-state and improving the off-state characteristics.

[0033] In a nitride semiconductor device according to an eleventh aspect of the present disclosure, in the nitride semiconductor device according to any one of the second to tenth aspects, the third side wall surface is a section from the first end to the second end.

[0034] This makes it possible to suppress an increase in channel resistance and reduce on-resistance while maintaining good off-state characteristics. In addition, by limiting the step to one step, the first opening can be easily formed. Since highly accurate mask alignment is no longer necessary and the first opening can be easily formed according to the design values, the reliability and yield of nitride semiconductor devices can be improved.

[0035] In a nitride semiconductor device according to a twelfth aspect of the present disclosure, in the nitride semiconductor device according to any one of the second to tenth aspects, the sidewall portion includes a plurality of the third sidewall surfaces, and further includes one or more fourth sidewall surfaces that connect two adjacent third sidewall surfaces and have a different slope from any of the plurality of third sidewall surfaces.

[0036] This makes it possible to suppress an increase in the resistance of the channel and reduce the on-resistance while maintaining good off-state characteristics.

[0037] In a nitride semiconductor device according to a thirteenth aspect of the present disclosure, in the nitride semiconductor device according to the first aspect, the sidewall portion includes a first sidewall surface which is a section from the lower end to a first end located at the predetermined position, and a second sidewall surface which is a section from the first end to the upper end.

[0038] This makes it possible to achieve both good off-state characteristics and reduced on-state resistance.

[0039] A nitride semiconductor device according to a fourteenth aspect of the present disclosure includes a substrate, a first nitride semiconductor layer provided above the substrate, a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer, a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer, a first opening penetrating the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaching the first nitride semiconductor layer, an electron transit layer and an electron supply layer provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening, a gate electrode provided above the electron supply layer so as to cover the first opening; a second opening at a position away from the gate electrode, penetrating the electron supply layer, the electron transit layer and the second nitride semiconductor layer to reach the first p-type nitride semiconductor layer; a source electrode provided to cover the second opening and electrically connected to the first p-type nitride semiconductor layer; and a drain electrode formed below the substrate, wherein a sidewall portion of the first opening has at least one step between an upper end and a lower end of the first p-type nitride semiconductor layer.

[0040] As a result, by providing a step on the end face of the first p-type nitride semiconductor layer on the side of the first opening, the first p-type nitride semiconductor layer can be kept away from the channel of the two-dimensional electron gas in the upper part away from the bottom surface of the first opening, and an increase in the resistance of the channel can be suppressed. Also, in the lower part close to the bottom surface of the first opening, the first p-type nitride semiconductor layer is kept close to the gate electrode, so that the electric field during the off-state can be relaxed and the breakdown voltage can be improved. In this way, the nitride semiconductor device according to this embodiment can achieve both good off-state characteristics and reduced on-state resistance.

[0041] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0042] The embodiments described below are all comprehensive or specific examples. The numerical values, shapes, materials, components, component arrangements and connection forms, steps, and step sequences shown in the following embodiments are merely examples and are not intended to limit the present disclosure. Furthermore, among the components in the following embodiments, components that are not described in the independent claims are described as optional components.

[0043] In addition, each figure is a schematic diagram and is not necessarily illustrated precisely. Therefore, for example, the scales in each figure do not necessarily match. In addition, in each figure, substantially the same configurations are given the same reference numerals, and duplicated explanations are omitted or simplified.

[0044] Furthermore, in this specification, terms indicating the relationship between elements, such as parallel or perpendicular, terms indicating the shape of elements, such as rectangle or trapezoid, and numerical ranges are not expressions that only express a strict meaning, but are expressions that include a substantially equivalent range, for example, a difference of about a few percent.

[0045] In this specification and the drawings, the x-axis, y-axis, and z-axis indicate the three axes of a three-dimensional Cartesian coordinate system. When the planar shape of the substrate is rectangular, the x-axis and y-axis are directions parallel to a first side of the rectangle and a second side perpendicular to the first side, respectively. The z-axis is the thickness direction of the substrate. In this specification, the "thickness direction" of the substrate refers to a direction perpendicular to the main surface of the substrate. The thickness direction is the same as the stacking direction of the semiconductor layers, and is also referred to as the "vertical direction". The direction parallel to the main surface of the substrate may be referred to as the "horizontal direction".

[0046] In addition, the side of the substrate on which the gate electrode and source electrode are provided (the positive side of the z-axis) is regarded as the "upper" or "upper side", and the side of the substrate on which the drain electrode is provided (the negative side of the z-axis) is regarded as the "lower" or "lower side".

[0047] In this specification, the terms "upper" and "lower" do not refer to the upward (vertically upward) and downward (vertically downward) directions in absolute spatial recognition, but are used as terms defined by the relative positional relationship based on the stacking order in the stacked structure. Further, the terms "upper" and "lower" are applicable not only when two components are spaced apart from each other and there is another component between the two components, but also when the two components are arranged in close contact with each other and the two components are in contact with each other.

[0048] In this specification, "plan view" refers to the view from a direction perpendicular to the main surface of the substrate of the nitride semiconductor device, that is, the view of the main surface of the substrate from the front, unless otherwise specified.

[0049] In this specification, ordinal numbers such as "first" and "second" do not mean the number or order of components, unless otherwise specified, but are used for the purpose of avoiding confusion and distinguishing between components of the same type.

[0050] In this specification, AlGaN represents ternary mixed crystal Al x Ga 1-x N (0 < x < 1). Hereinafter, the multi-component mixed crystal is abbreviated with the arrangement of the respective component symbols, for example, AlInN, GaInN, etc. For example, Al x Ga 1-x-y In y N (0 < x < 1, 0 < y < 1, and 0 < x + y < 1), which is abbreviated as AlGaInN.

[0051] (Embodiment 1) [Configuration] First, the configuration of the nitride semiconductor device according to Embodiment 1 will be described with reference to FIGS. 1A and 1B.

[0052] Fig. 1A is a cross-sectional view of a nitride semiconductor device 1 according to the present embodiment. Fig. 1B is a partially enlarged cross-sectional view of Fig. 1A. Specifically, Fig. 1B shows a portion in the vicinity of a sidewall portion 40b of a gate opening 40 in Fig. 1A. In each cross-sectional view, in order to ensure ease of viewing, the electron transit layer 22 is not shaded with diagonal lines to indicate a cross section.

[0053] 1A, the nitride semiconductor device 1 of the present embodiment is a so-called vertical field effect transistor (FET). Specifically, in the nitride semiconductor device 1, a current flows between the drain electrode 36 and the source electrode 32 in a direction perpendicular to the main surface 10a of the substrate 10.

[0054] The nitride semiconductor device 1 is a device having a stacked structure of semiconductor layers containing nitride semiconductors such as GaN and AlGaN as the main component. Note that "A contains B as the main component" means that the content of B in A is 50% or more.

[0055] The nitride semiconductor device 1 according to the present embodiment is a normally-off type FET. In the nitride semiconductor device 1, for example, the source electrode 32 is grounded (i.e., the potential is 0 V), and a positive potential is applied to the drain electrode 36. The potential applied to the drain electrode 36 is, for example, not limited to, 100 V or more and 1200 V or less. When the nitride semiconductor device 1 is in an off state, 0 V or a negative potential (for example, −5 V) is applied to the gate electrode 34. When the nitride semiconductor device 1 is in an on state, a positive potential (for example, +5 V) is applied to the gate electrode 34. The nitride semiconductor device 1 may be a normally-on type FET.

[0056] 1A, the nitride semiconductor device 1 includes a substrate 10, a drift layer 12, a first underlayer 14, a second underlayer 16, an electron transit layer 22, an electron supply layer 24, a threshold adjustment layer 28, a source opening 30, a source electrode 32, a gate electrode 34, a drain electrode 36, and a gate opening 40. At the interface between the electron transit layer 22 and the electron supply layer 24, a two-dimensional electron gas (2DEG) 26 that functions as a channel is generated.

[0057] Each of the components of the nitride semiconductor device 1 will be described in detail below.

[0058] The substrate 10 is made of a nitride semiconductor, and has principal surfaces 10a and 10b facing each other as shown in Fig. 1A. The principal surface 10a is the principal surface (upper surface) on the side where the drift layer 12 is formed. Specifically, the principal surface 10a approximately coincides with the c-plane. The principal surface 10b is the principal surface (lower surface) on the side where the drain electrode 36 is formed. The planar shape of the substrate 10 is, for example, rectangular, but is not limited thereto.

[0059] The substrate 10 has a thickness of, for example, 300 μm and a carrier concentration of 1×10 18 cm -3 n + The substrate is made of n-type GaN. Note that n-type and p-type refer to the conductivity type of the semiconductor. + The n-type represents a state in which a semiconductor is heavily doped with n-type dopants. - The term "type" refers to a state in which a semiconductor is doped with a low concentration of n-type dopants, i.e. lightly doped. + Type and p - The same is true for types. n-type, n + Type and n - The p-type is an example of the first conductivity type. + Type and p - The n-type is an example of a second conductivity type. The second conductivity type is a conductivity type of the opposite polarity to the first conductivity type. + Type and n - In some cases, the type is not distinguished and is referred to as n-type.+ Type and p - Sometimes it is referred to as p-type without distinguishing the type.

[0060] The substrate 10 does not have to be a nitride semiconductor substrate, but may be, for example, a silicon (Si) substrate, a silicon carbide (SiC) substrate, or a zinc oxide (ZnO) substrate.

[0061] The drift layer 12 is an example of a first nitride semiconductor layer provided above the substrate 10. The drift layer 12 is, for example, a n-type nitride semiconductor layer having a thickness of 8 μm. - The drift layer 12 is a film made of GaN. The donor concentration of the drift layer 12 is 1×10 15 cm -3 More than 1×10 17 cm -3 As an example, 16 cm -3 The carbon concentration (C concentration) of the drift layer 12 is 1×10 15 cm -3 More than 2×10 17 cm -3 The following is the result.

[0062] The drift layer 12 is provided, for example, in contact with the main surface 10a of the substrate 10. The drift layer 12 is formed on the main surface 10a of the substrate 10 by crystal growth such as a metal organic vapor phase epitaxy (MOVPE) method or a hydride vapor phase epitaxy (HVPE) method.

[0063] The first underlayer 14 is an example of a first p-type nitride semiconductor layer provided above the drift layer 12. The first underlayer 14 is also called a p-type block layer. The first underlayer 14 has a thickness of 400 nm and a carrier concentration of 1×10 17 cm -3The first underlayer 14 is a film made of p-type GaN, which is a p-type GaN film having a p-type conductivity. The first underlayer 14 is provided in contact with the upper surface of the drift layer 12. The first underlayer 14 is formed on the drift layer 12 by crystal growth, for example, by MOVPE, HVPE, or the like.

[0064] Although the first underlayer 14 is formed by crystal growth, it may be formed, for example, by implanting magnesium (Mg) into a deposited undoped GaN (i-GaN) film. Undoping will be described later.

[0065] The first underlayer 14 suppresses leakage current between the source electrode 32 and the drain electrode 36. For example, when a reverse voltage is applied to the pn junction formed by the first underlayer 14 and the drift layer 12, specifically, when the drain electrode 36 has a higher potential than the source electrode 32, a depletion layer extends to the drift layer 12. This allows the nitride semiconductor device 1 to withstand high voltage. In this embodiment, the drain electrode 36 has a higher potential than the source electrode 32 in both the off state and the on state, except in the case of reverse conduction. This allows the nitride semiconductor device 1 to withstand high voltage.

[0066] 1A, in this embodiment, the first underlayer 14 is in contact with the source electrode 32. Therefore, the first underlayer 14 is fixed to the same potential as the source electrode 32.

[0067] The second underlayer 16 is an example of a second nitride semiconductor layer provided above the first underlayer 14. The second underlayer 16 is a high-resistance layer having a higher resistance than the first underlayer 14. The second underlayer 16 is, for example, a film made of undoped GaN (i-GaN) having a thickness of 200 nm. The second underlayer 16 is provided in contact with the first underlayer 14. The second underlayer 16 is formed on the first underlayer 14 by crystal growth, for example, by MOVPE, HVPE, or the like.

[0068] The second underlayer 16 is assumed to be an undoped semiconductor layer, but may be an insulating layer or a semi-insulating layer. Here, "undoped" means that it is not doped with a dopant such as Si or Mg that changes the polarity of GaN to n-type or p-type. In this embodiment, the second underlayer 16 is doped with carbon (C). Specifically, the carbon concentration of the second underlayer 16 is higher than the carbon concentration of the first underlayer 14.

[0069] For example, the carbon concentration of the second underlayer 16 is 3×10 17 cm -3 That's it, but 1×10 18 cm -3 In this case, the concentration of silicon (Si) or oxygen (O) serving as an n-type impurity is lower than the carbon concentration. For example, the silicon concentration or oxygen concentration of the second underlayer 16 is 5×10 16 cm -3 Below, 2×10 16 cm -3 It may be the following.

[0070] The second underlayer 16 may be formed by ion implantation of magnesium (Mg), iron (Fe), boron (B), etc., other than carbon. Other ion species may be used as long as they can increase the resistance of GaN.

[0071] Here, if the nitride semiconductor device 1 does not include the second underlayer 16, a parasitic npn structure, i.e., a parasitic bipolar transistor, consisting of the electron transit layer 22, the p-type first underlayer 14, and the n-type drift layer 12, is present between the source electrode 32 and the drain electrode 36. Therefore, when the nitride semiconductor device 1 is in an off state, if a current flows through the p-type first underlayer 14, the parasitic bipolar transistor may be turned on, which may reduce the breakdown voltage of the nitride semiconductor device 1. In this case, the nitride semiconductor device 1 is likely to malfunction. In this embodiment, the high-resistance second underlayer 16 is provided, which suppresses the formation of a parasitic npn structure and suppresses malfunction of the nitride semiconductor device 1.

[0072] The second underlayer 16 may be provided below the first underlayer 14 and between the first underlayer 14 and the drift layer 12. Alternatively, the second underlayer 16 may be provided either above or below the first underlayer 14.

[0073] In addition, a layer for suppressing diffusion of p-type impurities such as Mg from the first underlayer 14 may be provided on the upper surface of the second underlayer 16. For example, an AlGaN layer having a thickness of 20 nm may be provided on the second underlayer 16.

[0074] The gate opening 40 is an example of a first opening that penetrates the second underlayer 16 and the first underlayer 14 and reaches the drift layer 12. The gate opening 40 has a bottom portion 40a and a sidewall portion 40b.

[0075] 1A, the bottom 40a is located below the lower surface of the first underlayer 14. The lower surface of the first underlayer 14 corresponds to the interface between the first underlayer 14 and the drift layer 12. The bottom 40a is parallel to the main surface 10a of the substrate 10, for example.

[0076] The sidewall portion 40b is a part of the surface of each of the drift layer 12, the first foundation layer 14, and the second foundation layer 16. As shown in Fig. 1A, the sidewall portion 40b has a step. The specific shape of the sidewall portion 40b will be described later with reference to Fig. 1B.

[0077] The electron transit layer 22 is an example of a first regrown layer provided to cover the upper surface of the second underlayer 16 and the gate opening 40. Specifically, a part of the electron transit layer 22 is provided along the bottom 40a and the sidewall 40b of the gate opening 40, and the other part of the electron transit layer 22 is provided on the upper surface of the second underlayer 16. The electron transit layer 22 is, for example, a film made of undoped GaN with a thickness of 150 nm. Note that although the electron transit layer 22 is assumed to be undoped, it may be made n-type by Si doping or the like.

[0078] The electron transit layer 22 is in contact with the drift layer 12 at the bottom 40a and the sidewall 40b of the gate opening 40. The electron transit layer 22 is in contact with each of the first underlayer 14 and the second underlayer 16 at the sidewall 40b of the gate opening 40. Furthermore, the electron transit layer 22 is in contact with the upper surface of the second underlayer 16. The electron transit layer 22 is formed by crystal regrowth after the gate opening 40 is formed.

[0079] The electron transit layer 22 has a channel region. Specifically, a two-dimensional electron gas 26 that serves as a channel is generated near the interface between the electron transit layer 22 and the electron supply layer 24. The two-dimensional electron gas 26 functions as the channel of the electron transit layer 22. In FIG. 1A, the two-dimensional electron gas 26 is diagrammatically illustrated by a dashed line. The two-dimensional electron gas 26 is bent along the interface between the electron transit layer 22 and the electron supply layer 24, i.e., along the inner surface of the gate opening 40.

[0080] 1A, an AlN layer with a thickness of about 1 nm is provided as a second regrown layer between the electron transit layer 22 and the electron supply layer 24. This makes it possible to suppress alloy scattering, improve channel mobility, and reduce on-resistance. Note that the regrown AlN layer is not necessarily required.

[0081] The electron supply layer 24 is an example of a third regrown layer provided so as to cover the upper surface of the second underlayer 16 and the gate opening 40. The electron transit layer 22 and the electron supply layer 24 are provided in this order from the substrate 10 side. The electron supply layer 24 is formed to a shape that conforms to the upper surface of the electron transit layer 22 and to a substantially uniform thickness. The electron supply layer 24 is, for example, a film made of undoped AlGaN having a thickness of 20 nm. The electron supply layer 24 is formed by crystal regrowth following the step of forming the electron transit layer 22.

[0082] The electron supply layer 24 has a larger band gap than the electron transit layer 22. Therefore, an AlGaN / GaN heterointerface is formed between the electron supply layer 24 and the electron transit layer 22. As a result, a two-dimensional electron gas 26 is generated in the electron transit layer 22. The electron supply layer 24 supplies electrons to a channel region (i.e., the two-dimensional electron gas 26) formed in the electron transit layer 22.

[0083] The threshold adjustment layer 28 is an example of a second p-type nitride semiconductor layer provided between the electron supply layer 24 and the gate electrode 34. Specifically, the threshold adjustment layer 28 is formed in a shape that follows the upper surface of the electron supply layer 24 and with a substantially uniform thickness.

[0084] The threshold adjustment layer 28 has a thickness of, for example, 100 nm and a carrier concentration of 1×10 17 cm -3 The threshold adjustment layer 28 is a nitride semiconductor layer made of p-type GaN or AlGaN, which is a p-type nitride semiconductor layer. The threshold adjustment layer 28 is formed by regrowth using the MOVPE method or the HVPE method following the step of forming the electron supply layer 24, and then patterning.

[0085] The provision of the threshold adjustment layer 28 raises the potential of the conduction band edge of the channel portion. This makes it possible to increase the threshold voltage of the nitride semiconductor device 1. This allows the nitride semiconductor device 1 to be realized as a normally-off type FET. In other words, when a potential of 0 V is applied to the gate electrode 34, the nitride semiconductor device 1 can be turned off. The threshold adjustment layer 28 does not necessarily have to be provided.

[0086] Moreover, the threshold adjustment layer 28 may be an insulating layer made of SiN and / or SiO2 instead of a p-type AlGaN layer. Even in this case, it is possible to realize a normally-off operation by suppressing the gate current and shifting the threshold in the positive direction.

[0087] The gate electrode 34 is provided above the electron supply layer 24 so as to cover the gate opening 40. Specifically, the gate electrode 34 is disposed above the threshold adjustment layer 28 and overlaps with the gate opening 40 in a plan view. Specifically, the gate electrode 34 is provided in contact with the upper surface of the threshold adjustment layer 28 so as to cover the gate opening 40. The gate electrode 34 is formed, for example, in a shape that follows the upper surface of the threshold adjustment layer 28 and with a substantially uniform film thickness. Alternatively, the gate electrode 34 may be formed so as to fill a recess in the upper surface of the threshold adjustment layer 28.

[0088] The gate electrode 34 is formed using a conductive material such as a metal. For example, the gate electrode 34 is formed using palladium (Pd). The gate electrode 34 may be made of a material that is ohmic-connected to the p-type GaN layer. For example, nickel (Ni)-based material, tungsten silicide (WSi), gold (Au), etc. may be used. The gate electrode 34 is formed by patterning a conductive film formed by, for example, sputtering or deposition after the threshold adjustment layer 28 is formed, after the source opening 30 is formed, or after the source electrode 32 is formed.

[0089] The source opening 30 is an example of a second opening that penetrates the electron supply layer 24, the electron transit layer 22, and the second underlayer 16 at a position away from the gate electrode 34, and reaches the first underlayer 14. The source opening 30 is disposed at a position away from the gate electrode 34 in a plan view.

[0090] 1A, the bottom 30a is located below the lower surface of the second underlayer 16. The lower surface of the second underlayer 16 corresponds to the interface between the second underlayer 16 and the first underlayer 14. The bottom 30a is parallel to the main surface 10a of the substrate 10, for example.

[0091] 1A, the source opening 30 is formed so that the opening area is constant regardless of the distance from the substrate 10. Specifically, the sidewall portion 30b of the source opening 30 is perpendicular to the bottom portion 30a. That is, the cross-sectional shape of the source opening 30 is rectangular.

[0092] Alternatively, the source opening 30 may be formed so that the opening area increases as it is farther from the substrate 10. Specifically, the sidewall 30b of the source opening 30 may be inclined obliquely. For example, the cross-sectional shape of the source opening 30 may be an inverted trapezoid, more specifically, an inverted isosceles trapezoid. In this case, the inclination angle of the sidewall 30b with respect to the bottom 30a may be, for example, in the range of 30° to 60°. Since the sidewall 30b is inclined obliquely, the contact area between the source electrode 32 and the electron transit layer 22 (the two-dimensional electron gas 26) increases, so that an ohmic connection is easily made. The two-dimensional electron gas 26 is exposed to the sidewall 30b of the source opening 30, and is connected to the source electrode 32 at the exposed portion.

[0093] The source opening 30 is not necessarily required. By providing the source opening 30, the ohmic contact resistance with the two-dimensional electron gas 26 (channel) can be reduced. Also, the first underlayer 14 and the source electrode 32 can be electrically connected.

[0094] The source electrode 32 is disposed apart from the gate electrode 34. In this embodiment, the source electrode 32 is provided along the inner surface of the source opening 30. Specifically, the source electrode 32 is connected to each of the electron supply layer 24, the electron transit layer 22, and the first underlayer 14. The source electrode 32 is ohmic-connected to each of the electron transit layer 22 and the electron supply layer 24. The source electrode 32 is in contact with the two-dimensional electron gas 26 (channel) at the sidewall portion 30b of the source opening 30. This makes it possible to reduce the contact resistance between the source electrode 32 and the two-dimensional electron gas 26 (channel).

[0095] The source electrode 32 is formed using a conductive material such as a metal. For example, a material that can be ohmic-connected to the n-type GaN layer by heat treatment, such as Ti / Al, can be used as the material for the source electrode 32. The source electrode 32 is formed by patterning a conductive film formed by, for example, sputtering or vapor deposition.

[0096] The drain electrode 36 is provided below the substrate 10. That is, the drain electrode 36 is provided on the opposite side to the drift layer 12. Specifically, the drain electrode 36 is provided in contact with the major surface 10b of the substrate 10.

[0097] The drain electrode 36 is formed using a conductive material such as a metal. As with the material of the source electrode 32, the material of the drain electrode 36 may be, for example, a material that forms an ohmic connection with n-type GaN, such as Ti / Al. The drain electrode 36 is formed by patterning a conductive film formed by, for example, sputtering or vapor deposition.

[0098] [Characteristic configuration] Next, a main characteristic configuration of the nitride semiconductor device 1 according to the present embodiment will be described with reference to FIG. 1B.

[0099] [Edge shape of first base layer] 1B shows a cross section (xz plane) parallel to the direction in which the gate electrode 34 and the source electrode 32 are arranged (x-axis direction) and perpendicular to the main surface 10a of the substrate 10. In FIG. 1B, a bottom end PL, a first end P1, a second end P2, and a top end PH, which represent positions on the surface of the first underlayer 14, are shown.

[0100] The bottom end PL, the first end P1, the second end P2, and the top end PH are all located in a portion of the surface of the first underlayer 14 that constitutes the sidewall portion 40b of the gate opening 40. In other words, the bottom end PL, the first end P1, the second end P2, and the top end PH are all located within the contact surface between the first underlayer 14 and the electron transit layer 22.

[0101] In a plan view, the lower end PL, the first end P1, the second end P2, and the upper end PH are arranged in this order in a direction from the bottom 40a of the gate opening 40 toward the opening end (i.e., the upper end). As shown in FIG. 1B, the first end P1 is located above the lower end PL. The second end P2 is located below the upper end PH. In this embodiment, the first end P1 and the second end P2 are located at the same height.

[0102] 1B shows two dashed dotted lines VL1 and VL2. The dashed dotted line VL1 is an extension of a first line segment connecting the lower end PL and the first point P1. The dashed dotted line VL2 is an extension of a second line segment connecting the lower end PL and the upper end PH. An angle α1 that the dashed dotted line VL1 makes with the main surface 10a is larger than an angle α2 that the dashed dotted line VL2 makes with the main surface 10b.

[0103] By satisfying α1>α2, it is possible to achieve both good off-characteristics and reduced on-resistance in the nitride semiconductor device 1. The principle behind this will be described with reference to Figures 2A and 2B, in comparison with a comparative example.

[0104] 2A is a cross-sectional view for explaining channel narrowing of a nitride semiconductor device 1x according to a comparative example. In FIG. 2A, the side surface of the first underlayer 14x of the sidewall portion 40bx of the gate opening 40x is a flat inclined surface. Therefore, the side surface of the first underlayer 14x and the two-dimensional electron gas 26 (channel) are approximately parallel to each other. As a result, as shown in FIG. 2A, a depletion layer extends from the side surface of the first underlayer 14x toward the two-dimensional electron gas 26 (channel) in the electron transit layer 22 during on-state. This depletion layer narrows most of the inclined portion of the two-dimensional electron gas 26, resulting in high on-resistance.

[0105] FIG. 2B is a cross-sectional view for explaining the channel narrowing of the nitride semiconductor device 1 according to the present embodiment. In contrast to the comparative example shown in FIG. 2A, in the present embodiment, by satisfying α1>α2, as shown in FIG. 1B, the upper end PH is located closer to the source electrode 32 than the dashed-dotted line VL1, that is, in the direction in which the opening of the gate opening 40 is widened. As a result, while keeping the distance between each of the lower end PL and the first end P1 of the first underlayer 14 and the two-dimensional electron gas 26 short, the distance between the upper end PH of the first underlayer 14 and the two-dimensional electron gas 26 can be secured long. Therefore, as shown in FIG. 2B, the depletion layer extending from the first underlayer 14 into the electron transit layer 22 narrows only a part of the slope of the two-dimensional electron gas 26. As is clear from comparison with FIG. 2A, the slope of the two-dimensional electron gas 26 has an increased portion that is not narrowed by the depletion layer, so that the on-resistance can be reduced.

[0106] In addition, the lower end PL and the first end P1 of the first underlayer 14 are located on the bottom 40a side of the gate opening 40, as in the comparative example. The distance between the lower part of the first underlayer 14 and the threshold adjustment layer 28 functioning as a part of the gate electrode 34 is the same as in the comparative example. Therefore, as in the comparative example, good off characteristics can be maintained with respect to electric field relaxation during off-state. In addition, as in the comparative example, the contact area between the first underlayer 14 and the drift layer 12 can be secured large, as in the comparative example, and therefore the breakdown voltage due to the expansion of the depletion layer due to the pn junction between the first underlayer 14 and the drift layer 12 can also be secured.

[0107] As described above, the nitride semiconductor device 1 according to the present embodiment can achieve both good off-characteristics and reduced on-resistance.

[0108] In the present embodiment, specifically, sidewall portion 40b is formed to satisfy α1>α2 by having a step between the lower end PL and the upper end PH of first underlayer 14. Specifically, as shown in FIG. 1A and FIG. 1B, sidewall portion 40b includes inclined surfaces 41 and 42 and an intermediate surface 43.

[0109] The inclined surface 41 is an example of a first sidewall surface, and is a section from the lower end PL of the first underlayer 14 to the first end P1 on the sidewall portion 40b of the gate opening 40. The inclined surface 41 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β1 is an example of a first inclination angle, and is the angle that the inclined surface 41 makes with respect to the main surface 10a.

[0110] The inclined surface 42 is an example of a second sidewall surface, and is a section from the second end P2 to the upper end PH of the first underlayer 14 on the sidewall portion 40b of the gate opening 40. The inclined surface 42 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β2 is an example of a second inclination angle, and is the angle that the inclined surface 42 makes with the main surface 10a.

[0111] In this embodiment, the inclination angle β2 is equal to the inclination angle β1. For example, the inclination angles β1 and β2 are 20° or more and 80° or less. Alternatively, the inclination angles β1 and β2 may be 30° or more and 45° or less. The larger the inclination angles β1 and β2 are, the shorter the unit cell length can be. The unit cell length corresponds to, for example, the center-to-center distance (pitch) of the source electrodes 32 arranged on either side of the gate opening 40. The smaller the inclination angles β1 and β2 are, the closer the inclined surfaces 41 and 42 are to the c-plane, and the better the film quality of the electron transit layer 22 and the like formed along the inclined surfaces 41 and 42 by crystal regrowth can be.

[0112] The intermediate surface 43 is an example of a third sidewall surface, and is a section from the first end P1 to the second end P2 of the first underlayer 14 on the sidewall portion 40b of the gate opening 40. The intermediate surface 43 has a different inclination from both the inclined surfaces 41 and 42. Specifically, the intermediate surface 43 is a plane parallel to the main surface 10a of the substrate 10. The intermediate surface 43 may be inclined with respect to the main surface 10a.

[0113] The intermediate surface 43 is located, for example, at approximately the center in the thickness direction of the first underlayer 14. Alternatively, the intermediate surface 43 may be located below the center in the thickness direction of the first underlayer 14. This can further reduce the region where the channel is constricted, thereby further reducing the on-resistance.

[0114] Such a stepped gate opening 40 is formed by performing etching in two separate steps. Specifically, the drift layer 12, the first underlayer 14, and the second underlayer 16 are formed in this order on the entire main surface 10a of the substrate 10, and then a first resist mask patterned into a predetermined shape is formed and etching is performed. In the first etching, the first underlayer 14 is not penetrated. As a result, the inclined surface 42 and the intermediate surface 43 are formed.

[0115] Next, a second resist mask having an opening smaller than that of the first resist mask is formed, and a second etching is performed. In the second etching, the first underlayer 14 is penetrated and the surface portion of the drift layer 12 is removed. This forms the inclined surface 41 and the bottom portion 40a. In this way, a step is formed in the first underlayer 14 by performing etching in two stages.

[0116] In this way, in the upper part of the stepped first underlayer 14, the distance between the first underlayer 14 and the slope of the two-dimensional electron gas 26 is increased. Therefore, as shown in FIG. 2B, the narrowed channel region can be shortened, and the on-resistance can be reduced. In addition, in the lower part of the stepped first underlayer 14, the distance to the threshold adjustment layer 28 can be kept short, allowing appropriate electric field relaxation. Therefore, good off characteristics can be maintained.

[0117] The inclined surfaces 41 and 42 do not have to be flat. At least one of the inclined surfaces 41 and 42 may be a concave or convex curved surface. When the inclined surfaces are curved, the inclination angles β1 and β2 can be defined as the angle between the main surface 10a and a line segment connecting the lower end and the upper end of each inclined surface. In this case, β1 may be larger or smaller than α1.

[0118] [End position of threshold adjustment layer] In this embodiment, the threshold voltage of the transistor can be adjusted depending on whether the threshold adjustment layer 28 completely covers the gate opening 40 or only partially covers it. That is, the threshold voltage can be adjusted depending on the position of the end of the threshold adjustment layer 28. Note that if the threshold adjustment layer 28 is not provided, the position of the end of the gate electrode 34 corresponds to the position of the end of the threshold adjustment layer 28.

[0119] When the end position of the threshold adjustment layer 28 is located inside the upper end of the sidewall portion 40b of the gate opening 40 in a plan view, the threshold voltage of the transistor is determined only by the inclined portion (specifically, the portion along the sidewall portion 40b) of the two-dimensional electron gas 26. In such a configuration, the carrier concentration of the flat portion of the two-dimensional electron gas 26 (specifically, the portion located above the second underlayer 16) can be increased, thereby reducing the on-resistance.

[0120] When the end position of the threshold adjustment layer 28 is located outside the upper end of the sidewall portion 40b of the gate opening 40 in a plan view, the threshold voltage of the transistor is determined by the larger of the threshold voltage of the slope portion or the flat portion of the two-dimensional electron gas 26. For example, if the threshold voltage of the transistor is to be determined by the flat portion, it is necessary to make only the threshold voltage of the slope portion small (for example, a negative voltage).

[0121] In this case, the film thickness Gx1 of the electron transit layer 22 in the direction parallel to the main surface 10a of the substrate 10 is set to be larger than the film thickness Gz of the electron transit layer 22 in the direction perpendicular to the main surface 10a of the substrate 10. This allows the distance between the first underlayer 14 and the sloped portion of the two-dimensional electron gas 26 to be larger than the distance between the first underlayer 14 and the flat portion of the two-dimensional electron gas 26. This allows the influence of the depletion layer extending from the first underlayer 14 in the sloped portion of the two-dimensional electron gas 26 to be reduced compared to the flat portion, so that the threshold voltage of the sloped portion can be selectively reduced. Therefore, the threshold voltage of the transistor can be determined by the flat portion of the two-dimensional electron gas 26.

[0122] [Thickness of electron transport layer] 1A, the electron transit layer 22 has a thickness Gx2 in a direction parallel to the main surface 10a of the substrate 10 that is greater than a thickness Gz in a direction perpendicular to the main surface 10a of the substrate 10. The thickness Gx2 is the distance between the upper end of the gate opening 40 and the electron supply layer 24 in a direction parallel to the main surface 10a. By increasing the thickness Gx2, the distance between the two-dimensional electron gas 26 generated along the sidewall portion 40b of the gate opening 40 and the first underlayer 14 can be increased, thereby suppressing a decrease in carrier concentration.

[0123] In general, in a vertical FET, GaN crystal is grown so that the c-plane of the GaN crystal is parallel to the main surface 10a of the substrate 10. At this time, the polarization of the two-dimensional electron gas 26 is smaller in the portion inclined with respect to the c-plane than in the portion parallel to the c-plane, and the carrier concentration is therefore lower. That is, the carrier concentration of the two-dimensional electron gas 26 is lower in the portion along the sidewall portion 40b of the gate opening 40 than in the flat portion. Therefore, the inclined portion of the two-dimensional electron gas 26 is easily affected by the constriction effect of the depletion layer extending from the first underlayer 14, and the on-resistance can be further reduced by moving the inclined portion away from the first underlayer 14.

[0124] Furthermore, if the thickness of the electron transit layer 22 in the direction perpendicular to the main surface 10a of the substrate 10 is small, the depth of the source opening 30 for contacting the source electrode 32 with the first underlayer 14 can be made shallow. A shallower source opening 30 not only shortens the process time but also improves the coverage of the source electrode 32 to be formed later. This makes it possible to reduce the on-resistance while facilitating the process.

[0125] In this way, since the film thickness Gx2 of the electron transit layer 22 in the direction parallel to the main surface 10a of the substrate 10 is greater than the film thickness Gz in the direction perpendicular to the main surface 10a of the substrate 10, it is possible to reduce the on-resistance while facilitating the process.

[0126] [Variations] Next, a modified example of the nitride semiconductor device according to the present embodiment will be described with reference to Figures 3A and 3B. The following description will focus on the differences from the first embodiment, and description of the commonalities will be omitted or simplified.

[0127] Fig. 3A is a cross-sectional view of a nitride semiconductor device 2 according to a modified example of the present embodiment. Fig. 3B is an enlarged cross-sectional view of a portion of Fig. 3A. Specifically, Fig. 3B shows a portion near a sidewall portion 40b of a gate opening 40 in Fig. 3A.

[0128] 3A and 3B, in nitride semiconductor device 2 according to this modification, inclination angle β1 of inclined surface 41 is different from inclination angle β2 of inclined surface 42. Specifically, inclination angle β1 is smaller than inclination angle β2. For example, inclination angle β1 is not less than 30° and not more than 45°. Inclination angle β2 is not less than 70° and not more than 90°.

[0129] Even when the inclination angle β1 is smaller than the inclination angle β2, as shown in FIG. 3B, α1>α2 is satisfied as long as the upper end PH is located below the dashed-dotted line VL1. This makes it possible to shorten the unit cell length of the nitride semiconductor device 2 while maintaining good off-characteristics and suppressing an increase in on-resistance. Reducing the unit cell length makes it possible to arrange more cells in the same area. Therefore, the on-resistance can be further reduced.

[0130] The inclination angle β1 may be larger than the inclination angle β2. Even in this case, since α1>α2 is satisfied, it is possible to achieve both good off-state characteristics and reduced on-state resistance.

[0131] The inclined surfaces 41 and 42 are formed so that the end shape of the resist mask when etching is performed is transferred to them. Therefore, when etching is performed in two stages, the inclination angles of the ends of the resist mask are made different, so that the inclination angle β1 of the inclined surface 41 and the inclination angle β2 of the inclined surface 42 can be made different. For example, the end shapes of the resist mask can be made different by adjusting conditions such as whether or not the resist mask is baked, the temperature, and the time.

[0132] Also, when a step is provided in the first underlayer 14, that is, when the intermediate surface 43 is provided, α1>α2 does not necessarily have to be satisfied. Specifically, in FIG. 3B, α1≦α2 may be satisfied by the upper end PH being located on the dashed line VL1 or above the dashed line VL1. In this case, not only the lower part but also the upper part of the inclined part of the two-dimensional electron gas 26 is constricted, but the constriction in the middle part is suppressed. Therefore, compared with the comparative example shown in FIG. 2A, the region where the two-dimensional electron gas 26 is constricted is narrowed, so that the on-resistance can be reduced. The off-characteristics are the same as those of the comparative example, so that good off-characteristics can be maintained. In this way, when a step is provided in the first underlayer 14, good off-characteristics and reduced on-resistance can be achieved at the same time even if α1≦α2.

[0133] (Embodiment 2) Next, a second embodiment will be described.

[0134] The second embodiment is different from the first embodiment in that the p-type first underlayer includes an AlGaN layer. The following description will focus on the differences from the first embodiment, and descriptions of the commonalities will be omitted or simplified.

[0135] Fig. 4 is a cross-sectional view of a nitride semiconductor device 101 according to the present embodiment. As shown in Fig. 4, the nitride semiconductor device 101 according to the present embodiment differs from the nitride semiconductor device 1 according to the first embodiment in that a first underlayer 114 is provided instead of the first underlayer 14.

[0136] The first underlayer 114 includes a p-type AlGaN layer 114c. Specifically, the first underlayer 114 includes p-type GaN layers 114a and 114b and a p-type AlGaN layer 114c. The AlGaN layer 114c is provided between the GaN layer 114a and the GaN layer 114b. The AlGaN layer 114c can be formed at a desired position with a desired thickness by changing the supply gas to that for forming a film by epitaxial growth.

[0137] The AlGaN layer 114c functions as an etch stopper layer. That is, the first dry etching condition for forming the gate opening 40 can be such that the etch rates of the GaN layer 114b and the AlGaN layer 114c are different.

[0138] Specifically, dry etching conditions are used that result in an extremely low etching rate for the AlGaN layer 114c compared to the etching rate for the GaN layer 114b. This allows the intermediate surface 43 in the first underlayer 114 to become the upper surface of the AlGaN layer 114c. Even if the actual etching rate for the GaN layer 114b differs from the expected rate due to variations within the wafer, stable etching is possible.

[0139] The height of each of the inclined surfaces 41 and 42 can be determined in advance depending on the position of the AlGaN layer 114c in the first underlayer 114. This makes it possible to stabilize the shape and depth of the steps. By stabilizing the shape of the steps, a highly reliable nitride semiconductor device 101 can be realized.

[0140] The AlGaN layer 114c may have a thickness of, for example, about 5 nm as long as it functions as an etch stopper. The AlGaN layer 114c may be made of undoped AlGaN.

[0141] Also in this embodiment, as in the modified example of the first embodiment, the inclination angle β1 of the inclined surface 41 and the inclination angle β2 of the inclined surface 42 may be different.

[0142] Fig. 5 is a cross-sectional view of a nitride semiconductor device 102 according to a modification of the present embodiment. As shown in Fig. 5, in the nitride semiconductor device 102 according to this modification, the first underlayer 114 includes an AlGaN layer 114c, and the inclination angle of the inclined surface 41 and the inclination angle of the inclined surface 42 are different. For example, the inclination angle of the inclined surface 41 is not less than 30° and not more than 45°. The inclination angle of the inclined surface 42 is not less than 70° and not more than 90°.

[0143] This makes it possible to shorten the unit cell length of the nitride semiconductor device 102 while simultaneously achieving good off-characteristics and reduced on-resistance. Also, it is possible to stabilize the shape and depth of the step in the first underlayer 114. Therefore, by stabilizing the shape, it is possible to realize a highly reliable nitride semiconductor device 102.

[0144] (Embodiment 3) Next, a third embodiment will be described.

[0145] The third embodiment is different from the first embodiment in that the bottom of the threshold adjustment layer is located lower than the lower end of the first underlayer. The following description will focus on the differences from the first embodiment, and the description of the commonalities will be omitted or simplified.

[0146] Fig. 6 is a cross-sectional view of a nitride semiconductor device 201 according to the present embodiment. As shown in Fig. 6, the nitride semiconductor device 201 according to the present embodiment differs from the nitride semiconductor device 1 according to the first embodiment in that it includes a gate opening 240 instead of the gate opening 40.

[0147] The bottom 240a of the gate opening 240 is formed by largely removing the surface portion of the drift layer 12. Since the bottom 240a is closer to the substrate 10, the bottom of the threshold adjustment layer 28 is closer to the drain electrode 36 than the bottom of the first underlayer 14 (i.e., the bottom end PL).

[0148] When a high voltage is applied to the drain electrode 36 during off-state, an electric field is applied to each of the pn junctions formed between the p-type threshold adjustment layer 28 located in the gate opening 240 and the electron supply layer 24 and electron transit layer 22, and the pn junctions formed between the p-type first underlayer 14 and the drift layer 12. In general, the gate opening 240 is formed by dry etching, and therefore the etched surface at the end of the first underlayer 14 is easily damaged. Therefore, the pn junction formed between the first underlayer 14 and the drift layer 12 near the gate opening 240 may have a low dielectric breakdown field strength.

[0149] On the other hand, the pn junction formed between the threshold adjustment layer 28 and the electron supply layer 24 and the electron transit layer 22 is formed by crystal growth, and therefore no etching damage occurs. In other words, it is easy to obtain an ideal value of the dielectric breakdown field strength. Therefore, by placing the bottom of the threshold adjustment layer 28 closer to the drain electrode 36 than the bottom of the first underlayer 14, the pn junction formed between the threshold adjustment layer 28 and the electron supply layer 24 and the electron transit layer 22 can receive more of the field strength during the off state. This makes it possible to reduce the off-leak current and obtain high voltage resistance characteristics.

[0150] In the present embodiment, the first underlayer 14 may include an AlGaN layer 114c that functions as an etch stopper, similarly to the second embodiment.

[0151] (Embodiment 4) Next, a fourth embodiment will be described.

[0152] The fourth embodiment is different from the first embodiment in that two steps are provided in the first underlayer. The following description will focus on the differences from the first embodiment, and the description of the commonalities will be omitted or simplified.

[0153] Fig. 7A is a cross-sectional view of a nitride semiconductor device 301 according to this embodiment. Fig. 7B is an enlarged cross-sectional view of a portion of Fig. 7A. Specifically, Fig. 7B shows a portion near a sidewall portion 340b of a gate opening 340 in Fig. 7A.

[0154] 7A, nitride semiconductor device 301 according to the present embodiment differs from nitride semiconductor device 1 according to the first embodiment in that it includes a gate opening 340 instead of gate opening 40. Sidewall portion 340b of gate opening 340 has two steps. Specifically, sidewall portion 340b includes inclined surfaces 341, 342, and 344, and intermediate surfaces 343a and 343b.

[0155] The inclined surface 341 is an example of a first sidewall surface, and is a section from the lower end PL of the first underlayer 14 to the first end P1 on the sidewall portion 340b of the gate opening 340. The inclined surface 341 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β1 is an example of a first inclination angle, and is the angle that the inclined surface 341 makes with respect to the main surface 10a.

[0156] The inclined surface 342 is an example of a second sidewall surface, and is a section from the second end P2 to the upper end PH of the first underlayer 14 on the sidewall portion 340b of the gate opening 340. The inclined surface 342 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β2 is an example of a second inclination angle, and is the angle that the inclined surface 342 makes with the main surface 10a.

[0157] The intermediate surfaces 343a and 343b are each an example of a third sidewall surface, and are located between the first end P1 and the second end P2. Specifically, the intermediate surface 343a is the section from the first end P1 to the third end P3 of the first underlayer 14. The intermediate surface 343b is the section from the fourth end P4 to the second end P2 of the first underlayer 14.

[0158] Intermediate surfaces 343a and 343b have different inclinations from both inclined surfaces 341 and 342. Specifically, intermediate surfaces 343a and 343b are planes parallel to main surface 10a of substrate 10. At least one of intermediate surfaces 343a and 343b may be inclined with respect to main surface 10a.

[0159] The inclined surface 344 is an example of a fourth sidewall surface, and connects two adjacent intermediate surfaces 343a and 343b. Specifically, the inclined surface 344 is a section from the third end P3 to the fourth end P4 of the first underlayer 14. The inclined surface 344 has a different inclination from both the intermediate surfaces 343a and 343b. Specifically, the inclined surface 344 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β4 is an example of a fourth inclination angle, and is the angle that the inclined surface 344 makes with respect to the main surface 10a.

[0160] In this embodiment, the inclination angles β1, β2, and β4 are equal to each other. For example, the inclination angles β1, β2, and β4 are 20° or more and 80° or less. Alternatively, the inclination angles β1, β2, and β4 may be 30° or more and 45° or less. The unit cell length can be shortened as at least one of the inclination angles β1, β2, and β4 becomes larger. Note that, as at least one of the inclination angles β1, β2, and β4 becomes smaller, the inclined surface 41, 42, or 44 approaches the c-plane, and therefore the film quality of the electron transit layer 22 formed along the inclined surface 41, 42, or 44 by crystal regrowth can be improved.

[0161] The bottom end PL, the first end P1, the second end P2, the third end P3, the fourth end P4, and the top end PH are all located in a portion of the surface of the first underlayer 14 that constitutes the sidewall portion 340b of the gate opening 340. In other words, the bottom end PL, the first end P1, the second end P2, the third end P3, the fourth end P4, and the top end PH are all located within the contact surface between the first underlayer 14 and the electron transit layer 22.

[0162] In a plan view, the lower end PL, the first end P1, the third end P3, the fourth end P4, the second end P2, and the upper end PH are arranged in this order in a direction from the bottom 40a of the gate opening 340 toward the opening end (i.e., the upper end). As shown in FIG. 7B, the first end P1 and the third end P3 are located above the lower end PL. The second end P2 and the fourth end P4 are located below the upper end PH and above the first end P1 and the third end P3. In this embodiment, the first end P1 and the third end P3 are located at the same height. The fourth end P4 and the second end P2 are located at the same height. When the side wall portion 340b has a plurality of steps, the first end P1 is the upper end of the inclined surface 341 closest to the lower end, and the second end P2 is the lower end of the inclined surface 342 closest to the upper end. Both the third end P3 and the fourth end P4 are located below the dashed-dotted line VL1. Note that the fourth end P4 is located above the dashed-dotted line VL2, but may be located below the dashed-dotted line VL2.

[0163] As described above, the sidewall portion 340b including the two intermediate surfaces 343a and 343b is formed by etching the gate opening 340 in three separate steps. The sidewall portion 340b may have three or more steps (specifically, intermediate surfaces). By performing etching in stages a number of times equal to the number of steps plus one, the sidewall portion 340b having multiple steps can be formed.

[0164] This allows the film thickness of the first underlayer 14 to be reduced stepwise toward the bottom 40a, and the off-characteristics can be maintained more stably than when there is only one step.

[0165] In this embodiment, α1>α2 is satisfied. As a result, the nitride semiconductor device 301 can achieve both good off-characteristics and reduced on-resistance. In this embodiment, at least two of the inclination angles β1, β2, and β4 may be different from each other. For example, by increasing one of the inclination angles β1, β2, and β4, the unit cell length can be shortened, and the on-resistance can be further reduced.

[0166] In the present embodiment, the first underlayer 14 may include an AlGaN layer 114c that functions as an etch stopper, as in the second embodiment. In this case, the AlGaN layer 114c may be included in multiple layers for each step. Alternatively, the first underlayer 14 may include only one AlGaN layer 114c for forming the lowest step (specifically, the intermediate surface 343a).

[0167] As in the third embodiment, the bottom of the threshold adjustment layer 28 may be located lower than the bottom of the first underlayer 14.

[0168] (Embodiment 5) Next, a fifth embodiment will be described.

[0169] The fifth embodiment is different from the first embodiment in that the drift layer includes a plurality of layers. The following description will focus on the differences from the first embodiment, and description of the commonalities will be omitted or simplified.

[0170] 8 is a cross-sectional view of a nitride semiconductor device 401 according to the present embodiment. As shown in FIG. 8, the nitride semiconductor device 401 according to the present embodiment differs in that it includes a drift layer 412 instead of the drift layer 12.

[0171] The drift layer 412 includes a plurality of layers 412a and 412b having different impurity concentrations. Here, the drift layer 412 is shown to be made up of two layers, but may be made up of three or more layers. The layer 412b is the uppermost layer among all the layers included in the drift layer 412. The upper surface of the layer 412b is in contact with the lower surface of the first underlayer 14.

[0172] The impurity concentration of layer 412b is the lowest among all layers included in drift layer 412. Here, the impurity concentration specifically refers to a donor concentration, and is the concentration of Si or O. This promotes electric field relaxation of the pn junction formed between first underlayer 14 and drift layer 412 during the off state, and good off characteristics are obtained.

[0173] In the present embodiment, the first underlayer 14 may include an AlGaN layer 114c functioning as an etch stopper, similar to the second embodiment. Also, the bottom of the threshold adjustment layer 28 may be located lower than the bottom of the first underlayer 14, similar to the third embodiment. Also, the first underlayer 14 may have a plurality of steps, similar to the fourth embodiment.

[0174] (Embodiment 6) Next, a sixth embodiment will be described.

[0175] The sixth embodiment is different from the first embodiment in that the side wall portion does not have a step. The following description will focus on the differences from the first embodiment, and description of the commonalities will be omitted or simplified.

[0176] Fig. 9A is a cross-sectional view of a nitride semiconductor device 501 according to this embodiment. Fig. 9B is an enlarged cross-sectional view of a portion of Fig. 9A. Specifically, Fig. 9B shows a portion near a sidewall portion 540b of a gate opening 540 in Fig. 9A.

[0177] 9A, nitride semiconductor device 501 according to the present embodiment differs from nitride semiconductor device 1 according to the first embodiment in that it includes gate opening 540 instead of gate opening 540. Sidewall 540b of gate opening 540 does not have a step. Sidewall 540b includes two inclined surfaces with different inclinations. Specifically, sidewall 540b includes inclined surfaces 41 and 542. Inclined surface 41 is the same as in the first embodiment.

[0178] The inclined surface 542 is an example of a second sidewall surface, and is a section from the second end P2 to the upper end PH of the first underlayer 14 on the sidewall portion 540b of the gate opening 540. The inclined surface 542 is a plane inclined with respect to the main surface 10a of the substrate 10. The inclination angle β2 is an example of a second inclination angle, and is the angle that the inclined surface 542 makes with respect to the main surface 10a.

[0179] In the present embodiment, the first end P1 and the second end P2 are located at the same position. Therefore, the inclined surface 41 and the inclined surface 542 are continuous. The inclination angle β1 of the inclined surface 41 is larger than the inclination angle β2 of the inclined surface 542. This satisfies α1>α2, so that it is possible to achieve both good off characteristics and reduced on-resistance, similar to the first embodiment.

[0180] (Other embodiments) Although the nitride semiconductor device according to one or more aspects has been described based on the embodiments, the present disclosure is not limited to these embodiments. As long as it does not deviate from the gist of the present disclosure, various modifications conceivable by a person skilled in the art to the present embodiment and forms constructed by combining components of different embodiments are also included within the scope of the present disclosure.

[0181] For example, in a plan view, the end of the threshold adjustment layer 28 may coincide with the end of the gate opening 40. Alternatively, in a plan view, the end of the threshold adjustment layer 28 may be provided inside the gate opening 40.

[0182] In addition, for example, in the above embodiment, the source opening 30 is provided so as to reach the first underlayer 14, but this is not limiting. For example, the source opening 30 may be an opening that reaches the electron transit layer 22, and the source electrode 32 may be connected to the electron transit layer 22 and not connected to the first underlayer 14.

[0183] Furthermore, each of the above embodiments can be modified, substituted, added, omitted, and the like in various ways within the scope of the claims or their equivalents. [Industrial Applicability]

[0184] INDUSTRIAL APPLICABILITY Nitride semiconductor devices according to the present disclosure can be used as power transistors used in power supply circuits, inverter circuits, and the like of equipment. [Explanation of symbols]

[0185] 1, 2, 101, 102, 201, 301, 401, 501 Nitride Semiconductor Devices 10 Substrate 10a, 10b main surface 12, 412 Drift layer 14, 114 First base layer 16 Second Undercoat Layer 22 Electron transport layer 24 Electron supply layer 26 Two-dimensional electron gas 28 Threshold adjustment layer 30 Source opening 30a, 40a, 240a bottom 30b, 40b, 340b, 540b side wall 32 Source electrode 34 Gate electrode 36 Drain electrode 40, 240, 340, 540 gate openings 41, 42, 341, 342, 344, 542 inclined surfaces 43, 343a, 343b intermediate surfaces 114a, 114b GaN layers 114c AlGaN layer 412a, 412b layers P1 first terminal P2 second terminal P3 third terminal P4 fourth terminal PH upper end PL lower end VL1, VL2 dashed lines

Claims

1. A substrate; a first nitride semiconductor layer provided above the substrate; a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer; a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer; a first opening that penetrates the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaches the first nitride semiconductor layer; an electron transit layer and an electron supply layer provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening; a gate electrode provided above the electron supply layer so as to cover the first opening; a source electrode provided apart from the gate electrode; a drain electrode formed below the substrate; The side wall of the first opening has when a position between a lower end and an upper end of the first p-type nitride semiconductor layer on a sidewall portion of the first opening is defined as a predetermined position, in a cross section parallel to a direction in which the gate electrode and the source electrode are arranged and perpendicular to a main surface of the substrate, a first angle formed by a first line segment connecting the lower end and the predetermined position with the main surface is larger than a second angle formed by a second line segment connecting the lower end and the upper end with the main surface; Nitride semiconductor devices.

2. The side wall portion is a first side wall surface that is a section from the lower end to a first end located at the predetermined position; a second side wall surface that is a section from a second end located between the first end and the upper end to the upper end in a plan view; a third side wall surface located between the first end and the second end and having a slope different from both the first side wall surface and the second side wall surface, The nitride semiconductor device of claim 1 .

3. The third side wall surface is parallel to the main surface. The nitride semiconductor device of claim 2 .

4. a first inclination angle that is an angle that the first sidewall surface forms with respect to the main surface is different from a second inclination angle that is an angle that the second sidewall surface forms with respect to the main surface; The nitride semiconductor device of claim 2 .

5. The first tilt angle is smaller than the second tilt angle. The nitride semiconductor device of claim 4.

6. The second inclination angle is equal to or greater than 70° and equal to or less than 90°. The nitride semiconductor device of claim 5 .

7. the first p-type nitride semiconductor layer includes an AlGaN layer; The third sidewall surface is a part of the upper surface of the AlGaN layer. The nitride semiconductor device according to any one of claims 2 to 6.

8. the first nitride semiconductor layer is composed of two or more layers having different impurity concentrations, and among the two or more layers, a top layer has a lowest impurity concentration; The nitride semiconductor device according to any one of claims 1 to 6.

9. a second p-type nitride semiconductor layer provided between the gate electrode and the electron supply layer; The nitride semiconductor device according to any one of claims 1 to 6.

10. a second opening that is disposed at a position away from the gate electrode, passes through the electron supply layer, the electron transit layer and the second nitride semiconductor layer, and reaches the first p-type nitride semiconductor layer; the source electrode is provided in the second opening and is electrically connected to the first p-type nitride semiconductor layer. The nitride semiconductor device according to any one of claims 1 to 6.

11. The third side wall surface is a section from the first end to the second end. The nitride semiconductor device according to any one of claims 2 to 6.

12. The side wall portion is The third sidewall surface includes a plurality of third sidewall surfaces, and further including at least one fourth side wall surface that connects two adjacent third side wall surfaces and has a slope different from that of any of the third side wall surfaces. The nitride semiconductor device according to any one of claims 2 to 6.

13. The side wall portion is a first side wall surface that is a section from the lower end to a first end located at the predetermined position; a second side wall surface that is a section from the first end to the upper end, The nitride semiconductor device of claim 1 .

14. A substrate; a first nitride semiconductor layer provided above the substrate; a first p-type nitride semiconductor layer provided above the first nitride semiconductor layer; a second nitride semiconductor layer provided above the first p-type nitride semiconductor layer; a first opening that penetrates the second nitride semiconductor layer and the first p-type nitride semiconductor layer and reaches the first nitride semiconductor layer; an electron transit layer and an electron supply layer provided in this order from below so as to cover an upper surface of the second nitride semiconductor layer and the first opening; a gate electrode provided above the electron supply layer so as to cover the first opening; a second opening that is located at a position away from the gate electrode, passes through the electron supply layer, the electron transit layer and the second nitride semiconductor layer, and reaches the first p-type nitride semiconductor layer; a source electrode provided to cover the second opening and electrically connected to the first p-type nitride semiconductor layer; a drain electrode formed below the substrate; a sidewall portion of the first opening has at least one step between an upper end and a lower end of the first p-type nitride semiconductor layer; Nitride semiconductor devices.

Citation Information

Patent Citations

  • Heterojunction transistor, and method of fabricating heterojunction transistor

    JP2011077400A

  • Semiconductor device, power source circuit, and computer

    JP2021145113A

  • Nitride semiconductor device

    US20210167061A1

  • Semiconductor device, power supply circuit, and computer

    US20210288175A1

  • Nitride semiconductor device

    US20230387286A1