Composite preform, method of manufacturing the same, composite container, and method of manufacturing the same
The composite preform and container design with a UV laser printed layer on a non-bonded plastic member addresses the limitations of conventional blow molding by ensuring clear printed layers and facilitating easy recycling, enhancing functional properties and reducing manufacturing costs.
Patent Information
- Application Number
- JP2023062235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional biaxial stretch blow molding methods for plastic containers limit the means to impart various functions and properties such as barrier and heat retention, and existing composite containers face issues with printed layers being damaged during blow molding.
A composite preform and container design featuring a plastic member with a UV laser printing layer that is not bonded to the container body, allowing for clear display of printed layers and preventing damage during blow molding, while enabling separate recycling of the container body.
The solution enables clear display of printed layers without damage and allows for easy separation and recycling of the container body, reducing manufacturing costs and maintaining the integrity of the plastic member.
Smart Images

Figure 2024148790000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composite preform and a method for manufacturing the same, and a composite container and a method for manufacturing the same. [Background technology]
[0002] Recently, plastic bottles have become common as bottles for containing liquid contents such as food and beverages. Plastic bottles are manufactured by inserting a preform into a mold and subjecting it to biaxial stretch blow molding.
[0003] In conventional biaxial stretch blow molding, a preform containing a single-layer material such as PET or PP, a multi-layer material, or a blended material is molded into a container shape. However, in conventional biaxial stretch blow molding, the preform is generally simply molded into a container shape. Therefore, when it is desired to give the container various functions and properties (barrier properties, heat retention, etc.), the means are limited, for example, by changing the material constituting the preform.
[0004] In response to this, the present applicant has proposed in Patent Document 1 a composite container that can be endowed with various functions and properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-128858 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present embodiment provides a composite preform and a manufacturing method thereof, as well as a composite container and a manufacturing method thereof, which can clearly display a printed layer applied to a plastic part after blow molding and suppress damage to the plastic part during printing. [Means for solving the problem]
[0007] The embodiments of the present disclosure relate to the following [1] to [9].
[0008] [1] A composite preform comprising a preform and a plastic member provided in intimate contact with the outside of the preform without being bonded thereto, the plastic member having a UV laser printed layer on the outer surface thereof.
[0009] [2] The composite preform according to [1], wherein the UV laser printed layer is a foamed or carbonized layer.
[0010] [3] The composite preform according to [1] or [2], wherein the thickness of the UV laser printing layer is 5 μm or more and 30 μm or less.
[0011] [4] A composite container comprising a container body and a plastic member that is in intimate contact with the outside of the container body without being bonded, and a UV laser printed layer is present on the outer surface of the plastic member.
[0012] [5] The composite container according to [4], wherein the UV laser printed layer is a foamed or carbonized layer.
[0013] [6] The composite container according to [4], wherein the thickness of the UV laser printed layer is 5 μm or more and 30 μm or less.
[0014] [7] A method for manufacturing a composite preform, comprising the steps of: preparing a plastic member; preparing a preform; attaching the plastic member to the outside of the preform without gluing it; and applying UV laser printing to the outer surface of the plastic member.
[0015] [8] A method for manufacturing a composite preform, comprising the steps of: preparing a plastic member having a UV laser printed layer on its outer surface; preparing a preform; and affixing the plastic member to the outside of the preform without gluing it.
[0016] [9] A method for manufacturing a composite container, comprising the steps of: preparing a composite preform described in any one of [1] to [3]; heating the composite preform and inserting it into a blow molding die; and blow molding the composite preform in the blow molding die, thereby expanding the preform and the plastic member of the composite preform as a unit. Effect of the Invention
[0017] According to an embodiment of the present disclosure, it is possible to clearly display a printed layer applied to a plastic member after blow molding, and to prevent damage to the plastic member during printing. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a partial vertical sectional view showing a composite container according to one embodiment. [Diagram 2] FIG. 2 is a horizontal cross-sectional view (cross-sectional view taken along line II-II in FIG. 1) showing a composite container according to one embodiment. [Diagram 3] FIG. 3 is a partially enlarged cross-sectional view showing a composite container according to one embodiment (a cross-sectional view taken along line III-III in FIG. 1). [Figure 4] FIG. 4 is a partial vertical cross-sectional view showing a composite preform according to one embodiment. [Diagram 5] FIG. 5 is a horizontal cross-sectional view (cross-sectional view taken along line VV in FIG. 4) showing a composite preform according to one embodiment. [Figure 6] FIG. 6 is a partially enlarged cross-sectional view (cross-sectional view taken along line VI-VI in FIG. 4) showing the outer surface of the composite preform according to the embodiment. [Figure 7] 7(a) to (d) are perspective views showing various plastic members. [Figure 8] 8(a) to 8(g) are schematic diagrams showing a manufacturing method for a composite container according to one embodiment. [Figure 9] 9(a) to 9(h) are schematic diagrams showing a manufacturing method for a composite container according to a modified example. [Figure 10] 10(a) to 10(f) are schematic diagrams showing a manufacturing method for a composite container according to another modified example. [Figure 11] 11(a) to (g) are schematic diagrams showing a manufacturing method for a composite container according to another modified example. [Figure 12] FIG. 12 is a partially enlarged cross-sectional view showing the outer surface of a composite preform according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the drawings attached to this specification, the scale and aspect ratios are appropriately changed and exaggerated from those of the actual objects for the convenience of illustration and understanding.
[0020] An embodiment will now be described with reference to the drawings, in which: Figures 1 to 8 show an embodiment.
[0021] (Composition of composite container) First, an overview of the composite container according to the present embodiment will be described with reference to Figures 1 to 3. In this specification, "upper" and "lower" refer to the upper and lower sides, respectively, of the composite container 10A in an upright position (Figure 1).
[0022] 1 to 3 is obtained by performing biaxial stretch blow molding on a composite preform 70 (see FIG. 5) including a preform 10a and a plastic member 40a, using a blow molding die 50. The composite container 10A is obtained by expanding the preform 10a and the plastic member 40a of the composite preform 70 as a unit.
[0023] The composite container 10A comprises a container body 10 and a plastic member 40. The container body 10 is made of a plastic material and is located on the inside. The plastic member 40 is provided in close contact with the outside of the container body 10 without being bonded.
[0024] Of these, the container body 10 includes a mouth portion 11, a neck portion 13, a shoulder portion 12, a body portion 20, and a bottom portion 30. The neck portion 13 is located below the mouth portion 11. The shoulder portion 12 is located below the neck portion 13. The body portion 20 is located below the shoulder portion 12. The bottom portion 30 is located below the body portion 20.
[0025] The plastic member 40 is thinly stretched and adhered to the outer surface of the container body 10. The plastic member 40 is attached to the container body 10 in such a manner that it does not easily move or rotate.
[0026] Next, a detailed description will be given of the container body 10. The container body 10 has the mouth portion 11, the neck portion 13, the shoulder portion 12, the body portion 20, and the bottom portion 30 as described above.
[0027] Of these, the mouth portion 11 has a threaded portion 14 and a flange portion 17. The threaded portion 14 is screwed onto a cap (not shown). The flange portion 17 is provided below the threaded portion 14. The flange portion 17 protrudes laterally from the peripheral wall of the mouth portion 11. The shape of the mouth portion 11 may be a conventionally known shape. The container body 10 is filled with contents such as a liquid content, and a cap (not shown) is screwed onto the mouth portion 11 to produce a composite container containing the contents.
[0028] The neck portion 13 is located between the flange portion 17 and the shoulder portion 12. The neck portion 13 has a generally cylindrical shape with a generally uniform diameter. The shoulder portion 12 is located between the neck portion 13 and the body portion 20. The shoulder portion 12 has a shape in which the diameter gradually increases from the neck portion 13 side toward the body portion 20 side (a shape in which the area gradually increases in horizontal cross section).
[0029] The body 20 has a cylindrical shape with a generally uniform diameter as a whole. This is not a limitation, and the body 20 may have a polygonal cylindrical shape such as a rectangular cylindrical shape or an octagonal cylindrical shape. Alternatively, the body 20 may have a cylindrical shape with a non-uniform horizontal cross section from top to bottom. In this embodiment, the body 20 has a generally flat surface without any irregularities, but this is not a limitation. For example, the body 20 may have irregularities such as panels or grooves.
[0030] The bottom 30 has a recess 31 and a grounding portion 32. The recess 31 is located in the center of the bottom 30. The grounding portion 32 is provided around the recess 31. The grounding portion 32 comes into contact with the mounting surface when the composite container 10A is placed on the mounting surface. The shape of the bottom 30 is not particularly limited, and may have a conventionally known bottom shape (for example, a petaloid bottom shape, a rounded bottom shape, etc.).
[0031] The thickness of the container body 10 at the trunk 20 can be, for example, thinned to about 50 μm or more and 250 μm or less, but is not limited thereto. Furthermore, the weight of the container body 10 can be, for example, thinned to about 10 g or more and 20 g or less, but is not limited thereto. By thinning the thickness of the container body 10 in this way, the weight of the container body 10 can be reduced.
[0032] Such a container body 10 can be produced by biaxially stretching and blow molding a preform 10a (described later) produced by injection molding a synthetic resin material. The material of the container body 10 is preferably a thermoplastic resin, particularly PE (polyethylene), PP (polypropylene), PET (polyethylene terephthalate), PEN (polyethylene naphthalate), or PC (polycarbonate). The container body 10 may be colored in colors such as red, blue, yellow, green, brown, black, and white. In consideration of ease of recycling, the container body 10 is preferably colorless and transparent. In addition, the above-mentioned various resins may be blended and used. Furthermore, a deposition film such as a diamond-like carbon film or a silicon oxide thin film may be formed on the inner surface of the container body 10 in order to improve the barrier property of the container.
[0033] The container body 10 can also be formed as a multi-layered bottle of two or more layers. That is, the container body 10 may be formed as a multi-layered bottle having gas barrier properties. This multi-layered bottle is obtained by producing a preform 10a consisting of three or more layers by injection molding, and then blow molding it. The preform 10a consisting of three or more layers may contain a resin having gas barrier properties, such as MXD6, MXD6 + fatty acid salt, PGA (polyglycolic acid), EVOH (ethylene vinyl alcohol copolymer), or PEN (polyethylene naphthalate), as an intermediate layer. Note that the intermediate layer may be a resin obtained by blending the above-mentioned various resins.
[0034] The container body 10 may be manufactured by mixing an inert gas (nitrogen gas, argon gas) with a melt of a thermoplastic resin to form a foamed preform having a foam cell diameter of 0.5 μm or more and 100 μm or less, and then blow molding the foamed preform. Since such a container body 10 has foamed cells built in, the light blocking property of the entire container body 10 can be improved.
[0035] The container body 10 may be a bottle having a full capacity of, for example, 100 ml to 2000 ml, or a large bottle having a full capacity of, for example, 10 L to 60 L.
[0036] Next, a description will be given of the plastic member 40. As will be described later, the plastic member 40 (40a) is provided so as to surround the outside of the preform 10a, and is obtained by being closely attached to the outside of the preform 10a and then being biaxially stretch-blow molded together with the preform 10a.
[0037] The plastic member 40 is attached to the outer surface of the container body 10 without being glued. The plastic member 40 is in close contact with the container body 10 so that it does not move or rotate relative to the container body 10. The plastic member 40 is stretched thinly on the outer surface of the container body 10 to cover the container body 10. As shown in Fig. 2, the plastic member 40 is provided over the entire circumferential area of the container body 10 so as to surround it. The plastic member 40 has a horizontal cross section that is approximately circular.
[0038] In this case, the plastic member 40 is provided so as to cover the neck portion 13, shoulder portion 12, body portion 20, and bottom portion 30 of the container body 10, excluding the mouth portion 11. This allows the neck portion 13, shoulder portion 12, body portion 20, and bottom portion 30 of the container body 10 to be given desired functions and characteristics.
[0039] The plastic member 40 may be provided on the entire or partial area of the container body 10 except for the mouth 11. For example, the plastic member 40 may be provided so as to cover the entire shoulder 12, body 20, and bottom 30 of the container body 10, excluding the mouth 11 and neck 13. Alternatively, the plastic member 40 may be provided so as to cover the shoulder 12, body 20, and bottom 30 of the container body 10, excluding the mouth 11, neck 13, and central parts of the bottom 30.
[0040] Since the plastic member 40 is not welded or bonded to the container body 10, it can be peeled off and removed from the container body 10. Specifically, for example, the plastic member 40 can be cut off using a blade or the like, or a cutting line (not shown) can be provided in advance on the plastic member 40, and the plastic member 40 can be peeled off along this cutting line. This allows the plastic member 40 to be separated and removed from the container body 10.
[0041] Such a plastic member 40 may be one that does not have a shrinking effect relative to the preform 10a, or may be one that has a shrinking effect.
[0042] When the plastic member 40 has a shrinking effect relative to the preform 10a, the plastic member (outer shrink member) 40a is provided on the outside of the preform 10a. The plastic member 40 is obtained by heating together with the preform 10a and subjecting it to biaxial stretch blow molding.
[0043] In this embodiment, a UV laser printed layer 43 is present on the outer surface of the plastic member 40. The UV laser printed layer 43 is formed by UV laser printing in advance on the plastic member 40a before blow molding. The UV laser printed layer 43 may be a foamed or carbonized layer.
[0044] As shown in FIG. 3, the UV laser printed layer 43 includes a convex portion that is raised higher than other portions constituting the plastic member 40. The thickness T1 of the UV laser printed layer 43 may be, for example, 5 μm or more, 15 μm or more, or 20 μm or more. The thickness T1 of the UV laser printed layer 43 may be, for example, 30 μm or less, 25 μm or less, or 20 μm or less. The thickness T1 of the UV laser printed layer 43 refers to the distance between the portion of the UV laser printed layer 43 that is closest to the central axis CL of the composite container 10A and the surface of the UV laser printed layer 43. The thickness T1 of the UV laser printed layer 43 refers to the distance in a direction perpendicular to the central axis CL of the composite container 10A. The thickness T1 of the UV laser printed layer 43 is measured as follows. First, the composite container 10A is cut using a blade on a plane perpendicular to the central axis CL of the composite container 10A and including the UV laser printed layer 43. Next, the cross section is magnified and observed using a laser microscope. Using this enlarged observation image, the thickness of the UV laser printed layer 43 is measured at any ten points, and the average value of these values is taken as the thickness T1.
[0045] The UV laser printed layer 43 of the composite container 10A is formed by biaxially stretching and blow molding the UV laser printed layer 43a of the composite preform 70. In addition, the configuration of the UV laser printed layer 43 of the composite container 10A is substantially the same as the configuration of the UV laser printed layer 43a of the composite preform 70 described later, so a detailed description will be omitted here.
[0046] Examples of the plastic member 40 include polyethylene, polypropylene, polyethylene terephthalate, polyethylene naphthalate, poly-4-methylpentene-1, polystyrene, AS resin, ABS resin, polyvinyl chloride, polyvinylidene chloride, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, polyvinyl butyral, ionomer resin, diallyl phthalate resin, fluorine-based resin, polymethyl methacrylate, polyacrylic acid, polymethyl acrylate, polyacrylonitrile, polyacrylamide, polybutadiene, polybutene-1, polyisoprene, polychloroprene, ethylene propylene rubber, and butyl rubber. Examples of the resin include rubber, nitrile rubber, acrylic rubber, silicone rubber, fluororubber, nylon 6, nylon 6,6, aromatic polyamide, polycarbonate, polyethylene terephthalate ethylene, polyethylene butylene terephthalate, polynaphthalene ethylene, U polymer, liquid crystal polymer, modified polyphenylene ether, polyether ketone, polyether ether ketone, unsaturated polyester, alkyd resin, polyimide, polysulfone, polyphenylene sulfide, polyether sulfone, silicone resin, polyurethane, phenolic resin, urea resin, polyethylene oxide, polypropylene oxide, polyacetal, and epoxy resin. Among these, it is preferable to use thermoplastic non-elastic resins such as polyethylene (PE) such as low-density polyethylene (LDPE), polypropylene (PP), polyethylene terephthalate (PET), and polyethylene naphthalate (PEN). In addition, blends, multilayer structures, and partial multilayer structures of these may be used. Furthermore, various additives may be added to the material of the plastic member 40 in addition to the resin as the main component, as long as the characteristics are not impaired. Examples of additives that can be added include plasticizers, UV stabilizers, coloring inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducers, slip agents, mold release agents, antioxidants, ion exchange agents, and color pigments. Also, by mixing an inert gas (nitrogen gas, argon gas) into the molten thermoplastic resin, a foamed material having a foam cell diameter of 0.5 μm to 100 μm is used, and this foamed preform is molded, thereby improving the light blocking properties.
[0047] The plastic member 40 may be made of a material having a light barrier property that blocks invisible light such as ultraviolet light. In this case, the light barrier property of the composite container 10A can be improved and the content liquid can be prevented from being deteriorated by ultraviolet light or the like without using a multi-layer preform or a preform containing a blended material as the preform 10a. Such a material may be a blended material, or a material in which a light-shielding resin is added to PET, PE, or PP. A foamed member having a foam cell diameter of 0.5 μm or more and 100 μm or less, which is produced by mixing an inert gas (nitrogen gas, argon gas) with a melt of a thermoplastic resin, may also be used.
[0048] The plastic member 40 may be made of a material (material with low thermal conductivity) with higher cold insulation or heat insulation than the plastic material constituting the container body 10 (preform 10a). In this case, it is possible to make it difficult for the temperature of the content liquid to be transmitted to the surface of the composite container 10A without increasing the thickness of the container body 10 itself. This improves the cold insulation or heat insulation of the composite container 10A. In addition, when a user grasps the composite container 10A, it is prevented that the composite container 10A becomes difficult to hold due to being too cold or too hot. Such materials include foamed polyurethane, polystyrene, PE (polyethylene), PP (polypropylene), phenolic resin, polyvinyl chloride, urea resin, silicone, polyimide, melamine resin, etc. It is preferable to mix hollow particles into a resin material containing these resins. The average particle diameter of the hollow particles is preferably 1 μm or more and 200 μm or less, and more preferably 5 μm or more and 80 μm or less. The term "average particle size" means the volume average particle size, and is measured using a particle size distribution / particle size distribution measuring device (Nanotrack particle size distribution measuring device, manufactured by Nikkiso Co., Ltd.). The hollow particles may be organic hollow particles made of resin or inorganic hollow particles made of glass, but organic hollow particles are preferred because of their excellent dispersibility. Examples of resins constituting organic hollow particles include styrene resins such as crosslinked styrene-acrylic resins, (meth)acrylic resins such as acrylonitrile-acrylic resins, phenolic resins, fluorine resins, polyamide resins, polyimide resins, polycarbonate resins, and polyether resins. Also usable are commercially available hollow particles such as Ropeake HP-1055, Ropeake HP-91, Ropeake OP-84J, Ropeake Ultra, Ropeake SE, and Ropeake ST (manufactured by Rohm and Haas Co., Ltd.), Nipol MH-5055 (manufactured by Zeon Corporation), SX8782, and SX866 (manufactured by JSR Corporation). The content of the hollow particles is preferably 0.01 parts by mass or more and 50 parts by mass or less, and more preferably 1 part by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the resin material contained in the plastic member 40.
[0049] The plastic member 40 may be made of a material that is less slippery than the plastic material that constitutes the container body 10 (preform 10a). In this case, the user can easily grip the composite container 10A without changing the material of the container body 10.
[0050] The plastic member 40 may be colored in a color such as red, blue, yellow, green, brown, black, or white, and may be transparent or opaque.
[0051] Furthermore, the thickness of the plastic member 40 can be, for example, about 5 μm or more and 500 μm or less in a state where it is attached to the container body 10, although it is not limited thereto.
[0052] (Composite preform composition) Next, the configuration of the composite preform according to this embodiment will be described with reference to Figs.
[0053] As shown in Figs. 4 and 5, the composite preform 70 includes a preform 10a made of a plastic material, and a bottomed cylindrical plastic member 40a provided on the outside of the preform 10a.
[0054] Among these, the preform 10a has a mouth portion 11a, a body portion 20a, and a bottom portion 30a. The mouth portion 11a corresponds to the mouth portion 11 of the container body 10 described above, and has approximately the same shape as the mouth portion 11. The body portion 20a is connected to the mouth portion 11a, and the bottom portion 30a is connected to the body portion 20a. The body portion 20a corresponds to the neck portion 13, the shoulder portion 12, and the body portion 20 of the container body 10 described above, and has an approximately cylindrical shape. The bottom portion 30a corresponds to the bottom portion 30 of the container body 10 described above, and has an approximately hemispherical shape.
[0055] The plastic member 40a is attached to the outer surface of the preform 10a without being bonded. The plastic member 40a is in close contact with the preform 10a so that it does not move or rotate relative to the preform 10a, or so that it does not fall under its own weight. The plastic member 40a is provided over the entire circumferential area of the preform 10a so as to surround it, and has a circular horizontal cross section.
[0056] In this case, the plastic member 40a covers the entire body 20a and the entire bottom 30a. The plastic member 40a may be provided on the entire or partial area other than the mouth 11a. For example, the plastic member 40a may cover the entire body 20a and the bottom 30a except for the portion corresponding to the neck 13 of the container body 10 and the mouth 11a. Alternatively, the plastic member 40a may cover the body 20a except for the bottom 30.
[0057] Such a plastic member 40a may be one that does not have a shrinking effect relative to the preform 10a, or may be one that has a shrinking effect.
[0058] When the plastic member 40a has a shrinking function, the plastic member 40a may be one that shrinks (e.g., thermally shrinks) relative to the preform 10a when an external action (e.g., heat) is applied to it. Alternatively, the plastic member 40a may be one that itself has shrinkability or elasticity and can shrink without the application of an external action.
[0059] The plastic member 40a may be, for example, a direct blow tube produced by direct blow molding, a sheet molded tube produced by sheet molding, an extrusion tube produced by extrusion molding, an injection molded tube produced by injection molding, an inflation molded tube produced by inflation molding, etc. The method for molding the plastic member 40a is not limited to this, and molding methods other than those mentioned above may also be used.
[0060] The plastic member 40a may be colored in a color such as red, blue, yellow, green, brown, black, or white, and may be transparent or opaque. It is preferable that the plastic member 40a absorbs the UV laser light used to form the UV laser printed layer 43a.
[0061] In this embodiment, a UV laser printed layer 43a is present on the outer surface of the plastic member 40a. The UV laser printed layer 43a is formed by previously applying UV laser printing. In this specification, UV laser printing refers to printing that modifies the outer surface of the plastic member 40a by applying external energy by UV (ultraviolet) laser light. The wavelength of the UV laser light may be, for example, 300 nm or more, or 340 nm or more. The wavelength of the UV laser light may be, for example, 400 nm or less, or 370 nm or less. As an example, a UV laser light with a wavelength of 355 nm may be used.
[0062] The UV laser printed layer 43a may be a foamed or carbonized layer. The UV laser printed layer 43a may be foamed or carbonized by applying external energy by UV laser light to the resin constituting the plastic member 40a. Whether the UV laser printed layer 43a is foamed or carbonized can be adjusted by the output and scan speed of the UV laser light. When the UV laser printed layer 43a is a foamed layer, the UV laser printed layer 43a may be formed by reacting the UV laser light with a pigment in the resin constituting the plastic member 40a. When the plastic member 40a is a dark color such as black or brown, the foamed UV laser printed layer 43a may be a light color such as gray or white. This makes it easier to see the UV laser printed layer 43a from other parts of the plastic member 40a. When the UV laser printed layer 43a is a carbonized layer, the UV laser printed layer 43a may be formed by carbonizing the resin constituting the plastic member 40a with the UV laser light. When the plastic member 40a is a light color such as gray or white, the carbonized UV laser printed layer 43a may be a dark color such as black or brown, which makes it easier to see the UV laser printed layer 43a from other parts of the plastic member 40a.
[0063] The UV laser printed layer 43a may be a layer that imparts aesthetic or decorative appearance to the plastic member 40a. The UV laser printed layer 43a may be formed on the entire outer surface of the plastic member 40a, or may be formed on a part of the outer surface of the plastic member 40a. UV laser printing for forming the UV laser printed layer 43a is performed on the plastic member 40a before biaxial stretch blow molding. In this case, the UV laser printing may be performed on the plastic member 40a in a state where it is attached to the preform 10a. Alternatively, the UV laser printing may be performed on the plastic member 40a before it is attached to the preform 10a.
[0064] As shown in FIG. 6, the UV laser printed layer 43a includes a convex portion that is raised higher than other portions constituting the plastic member 40a. The thickness T2 of the UV laser printed layer 43a may be, for example, 5 μm or more, 15 μm or more, or 20 μm or more. The thickness T2 of the UV laser printed layer 43a may be, for example, 30 μm or less, 25 μm or less, or 20 μm or less. The thickness T2 of the UV laser printed layer 43a refers to the distance between the portion of the UV laser printed layer 43a that is closest to the central axis CL of the preform 10a and the outermost surface of the UV laser printed layer 43a. The thickness T2 of the UV laser printed layer 43a refers to the distance in a direction perpendicular to the central axis CL of the composite container 10A. The thickness T2 of the UV laser printed layer 43a is measured as follows. First, the preform 10a is cut using a blade on a plane perpendicular to the central axis CL of the preform 10a and including the UV laser printed layer 43a. Next, this cross section is magnified and observed with a laser microscope. Using this magnified observation image, the thickness of the UV laser printed layer 43a is measured at any 10 points, and the average value of these values is defined as the thickness T2.
[0065] By providing the UV laser printed layer 43a on the plastic member 40a, images and characters can be displayed on the composite container 10A without providing a separate label or the like to the container body 10 after blow molding. In particular, the UV laser printed layer 43a may be provided in an area of the plastic member 40a with a high stretch ratio. Even in this case, it is possible to suppress the occurrence of cracks in the plastic member 40a starting from the UV laser printed layer 43 during stretching during blow molding. One or more UV laser printed layers 43a may be provided. Items displayed on the UV laser printed layer 43a may include text information such as the name of the content liquid, the manufacturer, and the names of raw materials, in addition to designs and product names.
[0066] Other printed layers may be formed on the plastic member 40a. When other printed layers are formed, the other printed layers may be formed by a printing method such as an inkjet method, a gravure printing method, an offset printing method, or a flexographic printing method. This printing may be performed on the plastic member 40a before it is attached to the preform 10a, or may be performed in a state where the plastic member 40a is provided on the outside of the preform 10a. Any ink may be used for printing, but it is preferable to use a highly extensible ink so that the UV laser printed layer 43 is clearly displayed even after it is stretched by biaxial stretch blow molding. Examples of such highly extensible ink include UV curable ink and EB curable ink.
[0067] Next, the shape of the plastic member 40a will be described.
[0068] As shown in FIG. 7(a), the plastic member 40a may be formed in a cylindrical shape with a bottom as a whole, and may have a cylindrical (tubular) body 41 and a bottom 42 connected to the body 41. This plastic member 40a has no joints. A UV laser printed layer 43a is not formed on the outer surface of the plastic member 40a. The UV laser printed layer 43a is formed after the plastic member 40a is attached to the preform 10a. In this case, the bottom 42 of the plastic member 40a covers the bottom 30a of the preform 10a, so that various functions and characteristics such as barrier properties can be imparted to the bottom 30 as well as the body 20 of the composite container 10A. Examples of such a plastic member 40a include the above-mentioned direct blow tube, sheet molding tube, and injection molding tube. The bottom 42 may be closed by thermocompression bonding the end of a tubular plastic member.
[0069] As shown in FIG. 7(b), the plastic member 40a may be formed in a circular tube shape (bottomless cylindrical shape) as a whole, and may have a cylindrical (tube-shaped) body 41. This plastic member 40a has no seams. The UV laser printed layer 43a is not formed on the outer surface of the plastic member 40a. The UV laser printed layer 43a is formed after the plastic member 40a is attached to the preform 10a. In this case, the plastic member 40a may be, for example, the above-mentioned blow tube, extrusion tube, inflation molding tube, or sheet molding tube.
[0070] As shown in Fig. 7(c), the plastic member 40a may be formed in a cylindrical shape with a bottom as a whole, and may have a cylindrical body 41 and a bottom 42 connected to the body 41. This plastic member 40a has no seams. A UV laser printed layer 43a is formed on the outer surface of the plastic member 40a. That is, the UV laser printed layer 43a is formed before the plastic member 40a is attached to the preform 10a.
[0071] As shown in Fig. 7(d), the plastic member 40a may be formed in a circular tube shape as a whole and have a cylindrical body 41. This plastic member 40a has no seams. A UV laser printed layer 43a is formed on the outer surface of the plastic member 40a. That is, the UV laser printed layer 43a is formed before the plastic member 40a is attached to the preform 10a.
[0072] (Method of manufacturing composite preform and composite container) Next, a manufacturing method (blow molding method) for the composite container 10A according to this embodiment will be described with reference to FIGS. 8(a) to (g).
[0073] First, a preform 10a made of a plastic material is prepared (see FIG. 8(a)). In this case, the preform 10a may be produced by injection molding using, for example, an injection molding machine (not shown). Alternatively, a preform that is generally used in the past may be used as the preform 10a.
[0074] Next, a plastic member 40a is provided so as to surround the outside of the preform 10a (see FIG. 8(b)). The plastic member 40a is adhered to the outside of the preform 10a without being bonded. At this time, the plastic member 40a, which has an inner diameter equal to or slightly smaller than the outer diameter of the preform 10a, may be pressed against the preform 10a to adhere to the outer surface of the preform 10a.
[0075] Next, the outer surface of the plastic member 40a is UV laser printed to form a UV laser printed layer 43a. At this time, UV laser light (for example, wavelength 355 nm) is irradiated from the outside of the plastic member 40a. The UV laser light is irradiated from a laser light irradiation device 58. The UV laser light scans the outer surface of the plastic member 40a to generate a predetermined image or character. The irradiated UV laser light modifies the outer surface of the plastic member 40a. The UV laser light does not substantially reach the preform 10a. The UV laser light foams or carbonizes the resin material that constitutes the plastic member 40a, thereby forming the UV laser printed layer 43a. The UV laser printed layer 43a becomes a convex portion that is raised higher than other parts of the plastic member 40a.
[0076] In this manner, the composite preform 70 shown in Figures 4 to 6 is obtained. The composite preform 70 has a preform 10a and a plastic member 40a that is in close contact with the outside of the preform 10a without being bonded. A UV laser printed layer 43a is present on the outer surface of the plastic member 40a.
[0077] In this manner, the plastic member 40a is attached in advance to the outside of the preform 10a to produce the composite preform 70. This makes it possible to carry out a series of steps for producing the composite preform 70 (FIGS. 8(a)-(c)) and a series of steps for producing the composite container 10A by blow molding (FIGS. 8(d)-(g)) in separate locations (such as factories).
[0078] Next, the composite preform 70 is heated by the heating device 51 (see FIG. 8(d)). At this time, the composite preform 70 is heated uniformly in the circumferential direction by the heating device 51 while rotating with the mouth portion 11a facing downward. The heating temperature of the preform 10a and the plastic member 40a in this heating process may be, for example, 90°C to 130°C.
[0079] Next, the composite preform 70 heated by the heating device 51 is sent to the blow molding die 50 (see FIG. 8(e)).
[0080] The composite container 10A is molded using this blow molding die 50. In this case, the blow molding die 50 is composed of a pair of body dies 50a, 50b, which are separated from each other, and a bottom die 50c (see FIG. 8(e)). In FIG. 8(e), the pair of body dies 50a, 50b are open from each other, and the bottom die 50c is raised upward. In this state, the composite preform 70 is inserted between the pair of body dies 50a, 50b.
[0081] 8(f), after the bottom die 50c is lowered, the pair of body dies 50a, 50b are closed, and the pair of body dies 50a, 50b and the bottom die 50c form a sealed blow molding die 50. Next, air is forced into the preform 10a, and the composite preform 70 is subjected to biaxial stretch blow molding.
[0082] As a result, the container body 10 is obtained from the preform 10a in the blow molding die 50. During this time, the body dies 50a, 50b are heated to 30°C to 80°C, and the bottom die 50c is cooled to 5°C to 25°C. At this time, the preform 10a and the plastic member 40a of the composite preform 70 are expanded as a unit in the blow molding die 50. As a result, the preform 10a and the plastic member 40a are integrally shaped into a shape corresponding to the inner surface of the blow molding die 50. In this way, the container body 10 and the plastic member 40 provided on the outer surface of the container body 10 are obtained.
[0083] Thereafter, as shown in FIG. 8(g), the pair of body molds 50a, 50b and the bottom mold 50c are separated from each other, and the composite container 10A is removed from the blow molding mold 50. The composite container 10A includes a container body 10 and a plastic member 40. A UV laser printed layer 43 is present on the outer surface of the plastic member 40. The UV laser printed layer 43 corresponds to the UV laser printed layer 43a described above. The UV laser printed layer 43 is produced by stretching the UV laser printed layer 43a together with the plastic member 40a. In this manner, the composite container 10A shown in FIGS. 1 to 3 is obtained.
[0084] In this embodiment, as described above, a UV laser printed layer 43a is formed on the outer surface of the plastic member 40a. This allows a printed layer of characters, symbols, images, etc. to be clearly displayed on the outer surface of the plastic member 40 after blow molding. The UV laser printed layer 43a is formed by UV laser light. The UV laser light foams or carbonizes the outer surface of the plastic member 40a. Therefore, the UV laser printed layer 43a rises higher than other parts of the plastic member 40a. This prevents the plastic member 40a from being damaged by the energy of the laser light. As a result, when the plastic member 40a expands during blow molding, it is possible to prevent the UV laser printed layer 43a from being cracked or damaged.
[0085] On the other hand, in a comparative example, when the printed layer is formed by a carbon dioxide laser or a YAG laser (see FIG. 12), the printed layer destroys the outer surface of the plastic member 40a. Therefore, when the plastic member 40a expands during blow molding, cracks may form in the printed layer, causing damage to the plastic member 40a.
[0086] Furthermore, according to this embodiment, since the UV laser printed layer 43 is provided on the plastic member 40, there is no need to apply a label using a labeler after filling the composite container 10A with the content liquid and sealing it. This makes it possible to reduce the manufacturing cost for producing the final product. In addition, it is possible to prevent a decrease in yield when producing the final product due to a malfunction of the labeler or the like.
[0087] Furthermore, according to this embodiment, the plastic member 40 provided with the UV laser printed layer 43 can be separated and removed from the container body 10, so the colorless and transparent container body 10 can be recycled in the same manner as in the conventional case. On the other hand, as a comparative example, when the UV laser printed layer 43 is provided on the container body 10, there is a concern that recycling of the container body 10 may become difficult.
[0088] Furthermore, according to this embodiment, when producing the composite container 10A, a general blow molding device can be used as is, so there is no need to prepare new molding equipment for producing the composite container 10A. Moreover, since the plastic member 40a is provided on the outside of the preform 10a, there is no need to prepare new molding equipment for molding the preform 10a.
[0089] (Modification of the manufacturing method of the composite container) Next, modified examples of the manufacturing method (blow molding method) for the composite container 10A according to the present embodiment will be described with reference to Figures 9(a) to (h). In the modified examples shown in Figures 9(a) to (h), the plastic member 40a acts to contract relative to the preform 10a, and other configurations are substantially the same as those shown in Figures 8(a) to (g). In Figures 9(a) to (h), the same parts as those in Figures 8(a) to (g) are given the same reference numerals and detailed descriptions are omitted.
[0090] First, a preform 10a made of a plastic material is prepared (see FIG. 9(a)).
[0091] Next, the plastic member 40a is prepared, and the plastic member 40a is loosely inserted onto the outside of the preform 10a (see FIG. 9(b)).
[0092] Next, the preform 10a and the plastic member 40a are heated by a first heating device 55 (see FIG. 9(c)). At this time, the heating temperature of the preform 10a and the plastic member 40a may be, for example, 50° C. to 100° C. As the plastic member 40a is heated, it thermally shrinks and comes into close contact with the outside of the preform 10a.
[0093] Next, a UV laser printing layer 43a is formed by applying UV laser printing to the outer surface of the plastic member 40a (see FIG. 9(d)). At this time, a laser light irradiation device 58 irradiates UV laser light from the outside of the plastic member 40a. The UV laser printing process may be performed in a manner substantially similar to that of FIG. 8(c) described above. This results in a composite preform 70 having the preform 10a and the plastic member 40a in close contact with the outside of the preform 10a.
[0094] In this manner, the plastic member 40a is heated and adhered in advance to the outside of the preform 10a using the first heating device 55 to produce the composite preform 70. This allows a series of steps for producing the composite preform 70 (FIGS. 9(a)-(e)) and a series of steps for producing the composite container 10A by blow molding (FIGS. 9(f)-(h)) to be carried out in separate locations (such as factories).
[0095] Next, the composite preform 70 is heated by the second heating device 51 (see FIG. 9(e)). At this time, the composite preform 70 is heated uniformly in the circumferential direction by the second heating device 51 while rotating with the mouth portion 11a facing downward. The heating temperature of the preform 10a and the plastic member 40a in this heating process may be, for example, 90°C to 130°C.
[0096] Next, the composite preform 70 heated by the second heating device 51 is sent to the blow molding die 50 (see FIG. 9(f)).
[0097] The composite preform 70 is molded using this blow molding die 50. In substantially the same manner as in the above-mentioned cases of Fig. 8(a) to (g), a composite container 10A including a container body 10 and a plastic member 40 provided on the outer surface of the container body 10 is obtained (see Fig. 9(f) to (h)).
[0098] (Another modified example of the manufacturing method of the composite container) Next, another modified example of the manufacturing method (blow molding method) for the composite container 10A according to this embodiment will be described with reference to Figures 10(a) to (f). In the modified example shown in Figures 10(a) to (f), UV laser printing is performed on the plastic member 40a before it is attached to the preform 10a, and the other configurations are substantially the same as those shown in Figures 8(a) to (g). In Figures 10(a) to (f), the same parts as those in Figures 8(a) to (g) are given the same reference numerals and detailed description will be omitted.
[0099] First, a preform 10a made of a plastic material is prepared (see FIG. 10(a)).
[0100] Next, a plastic member 40a on which a UV laser printed layer 43a has been formed in advance is prepared. Then, the plastic member 40a on which the UV laser printed layer 43a has been formed is provided so as to surround the outside of the preform 10a (see FIG. 10(b)). The plastic member 40a is adhered to the outside of the preform 10a without being bonded. This results in a composite preform 70 having the preform 10a and the plastic member 40a adhered to the outside of the preform 10a.
[0101] Next, the composite preform 70 is heated by the second heating device 51 (see FIG. 10(c)). At this time, the composite preform 70 is heated uniformly in the circumferential direction by the second heating device 51 while rotating with the mouth portion 11a facing downward. The heating temperature of the preform 10a and the plastic member 40a in this heating process may be, for example, 90°C to 130°C.
[0102] Next, the composite preform 70 heated by the second heating device 51 is sent to the blow molding die 50 (see FIG. 10(d)).
[0103] The composite preform 70 is molded using this blow molding die 50. In substantially the same manner as in the above-mentioned cases of Fig. 8(a) to (g), a composite container 10A including a container body 10 and a plastic member 40 provided on the outer surface of the container body 10 is obtained (see Fig. 10(d) to (f)).
[0104] (Another modified example of the manufacturing method of the composite container) Next, another modified example of the manufacturing method (blow molding method) for the composite container 10A according to this embodiment will be described with reference to Figs. 11(a) to (g). In the modified example shown in Figs. 11(a) to (g), UV laser printing is performed on the plastic member 40a before it is attached to the preform 10a. Also, the plastic member 40a has the effect of shrinking relative to the preform 10a. The rest of the configuration is substantially the same as the embodiment shown in Figs. 8(a) to (g). In Figs. 11(a) to (g), the same parts as those in Figs. 8(a) to (g) are given the same reference numerals and detailed description will be omitted.
[0105] First, a preform 10a made of a plastic material is prepared (see FIG. 11(a)).
[0106] Next, a plastic member 40a on which a UV laser printed layer 43a has been formed in advance is prepared. Then, the plastic member 40a on which the UV laser printed layer 43a has been formed is loosely inserted onto the outside of the preform 10a (see FIG. 11(b)).
[0107] Next, the preform 10a and the plastic member 40a are heated by a first heating device 55 (see FIG. 11(c)). At this time, the heating temperature of the preform 10a and the plastic member 40a may be, for example, 50°C to 100°C. By heating the plastic member 40a, the plastic member 40a thermally shrinks and comes into close contact with the outside of the preform 10a. This results in a composite preform 70 having the preform 10a and the plastic member 40a in close contact with the outside of the preform 10a.
[0108] In this manner, the plastic member 40a is heated and adhered to the outside of the preform 10a in advance using the first heating device 55 to produce the composite preform 70. This allows a series of steps for producing the composite preform 70 (FIGS. 11(a)-(d)) and a series of steps for producing the composite container 10A by blow molding (FIGS. 11(e)-(g)) to be carried out in separate locations (such as factories).
[0109] Next, the composite preform 70 is heated by the second heating device 51 (see FIG. 11(d)). At this time, the composite preform 70 is heated uniformly in the circumferential direction by the second heating device 51 while rotating with the mouth portion 11a facing downward. The heating temperature of the preform 10a and the plastic member 40a in this heating process may be, for example, 90°C to 130°C.
[0110] Next, the composite preform 70 heated by the second heating device 51 is sent to the blow molding die 50 (see FIG. 11(f)).
[0111] The composite preform 70 is molded using this blow molding die 50. In substantially the same manner as in the above-mentioned cases of Fig. 8(a) to (g), a composite container 10A including a container body 10 and a plastic member 40 provided on the outer surface of the container body 10 is obtained (see Fig. 11(e) to (g)).
[0112] The present disclosure is not limited to the above-described embodiments and modifications, and can be embodied by modifying the components without departing from the spirit of the present disclosure. In addition, various inventions can be formed by appropriately combining the multiple components disclosed in the above-described embodiments and modifications. Some components may be deleted from all the components shown in each embodiment and modification.
Claims
1. In the composite preform, A preform and A plastic member provided in intimate contact with the outer side of the preform without being bonded thereto; A composite preform having a UV laser printed layer on an outer surface of the plastic member.
2. The composite preform of claim 1 , wherein the UV laser printed layer is a foamed or carbonized layer.
3. The composite preform according to claim 1 , wherein the UV laser printing layer has a thickness of 5 μm or more and 30 μm or less.
4. In composite containers, A container body; a plastic member provided in intimate contact with the outside of the container body without being bonded thereto; A composite container having a UV laser printed layer on the outer surface of the plastic member.
5. The composite container of claim 4 , wherein the UV laser printed layer is a foamed or carbonized layer.
6. The composite container according to claim 4 , wherein the UV laser printed layer has a thickness of 5 μm or more and 30 μm or less.
7. In the method for producing a composite preform, Providing a plastic member; Preparing a preform; providing the plastic member on the outer side of the preform in intimate contact with the outer side without bonding; and applying UV laser printing to the outer surface of the plastic member.
8. In the method for producing a composite preform, Providing a plastic component having a UV laser printed layer on an outer surface thereof; Preparing a preform; and providing the plastic member on the outside of the preform in intimate contact with the outside of the preform without bonding.
9. Providing a composite preform according to claim 1; heating the composite preform and inserting it into a blow mold; and a step of blow molding the composite preform in the blow molding die, thereby expanding the preform and the plastic member of the composite preform as a single unit.
Citation Information
Patent Citations
Blow molding method, complex preform, composite container, inside label member, and plastic-made member