Manufacturing method of silicon carbide semiconductor device
By employing ion implantation and controlled oxide film thickness manipulation, the method addresses substrate warping in silicon carbide semiconductor manufacturing, reducing defects and improving manufacturing stability.
Patent Information
- Application Number
- JP2023062418
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
Smart Images

Figure 2024148882000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a silicon carbide semiconductor device. [Background technology]
[0002] Conventionally, a method for manufacturing a silicon carbide semiconductor device is known that reduces the amount of warpage of a wafer that occurs in an electrode formation step to a value that does not affect the manufacturing process (see Patent Document 1 below). Also known is a method for manufacturing a silicon carbide semiconductor device that includes a step of forming an ion implantation region that controls warpage of a SiC epitaxial substrate (see Patent Document 2 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5550738 [Patent Document 2] Patent No. 6272488 Summary of the Invention [Problem to be solved by the invention]
[0004] Conventionally, when an impurity layer is formed only by ion implantation, there is a problem that warpage of the substrate causes transportation failure, stage chuck failure, patterning failure, etc. in the manufacturing equipment. The present invention aims to provide a manufacturing method for a silicon carbide semiconductor device that can reduce or mitigate warpage of a silicon carbide semiconductor substrate and reduce or suppress the occurrence of transportation failure, stage chuck failure, patterning failure, etc. in the manufacturing equipment. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems and achieve the object of the present invention, the method for manufacturing a silicon carbide semiconductor device according to the present invention has the following features. First, a first step is performed to prepare a silicon carbide semiconductor substrate having a first semiconductor layer of a first conductivity type having a lower impurity concentration than a starting substrate provided on the front surface side of the starting substrate of a first conductivity type. Next, a second step is performed to form a first semiconductor region of a second conductivity type in the first semiconductor layer by ion implantation. Next, after the first semiconductor region is formed, a third step is performed to restore the warp of the silicon carbide semiconductor substrate. Next, a fourth step is performed to form a second semiconductor layer of a second conductivity type in the first semiconductor layer by ion implantation. Next, a fifth step is performed to form a third semiconductor layer of a first conductivity type in a surface layer of the second semiconductor layer by ion implantation. Next, a sixth step is performed to activate the first semiconductor region, the second semiconductor layer, and the third semiconductor layer formed by ion implantation. Next, a seventh step is performed in which a trench that penetrates the third semiconductor layer and the second semiconductor layer to reach the first semiconductor layer is formed at a position facing the first semiconductor region in the depth direction. Next, an eighth step is performed in which a gate electrode is formed inside the trench via a gate insulating film. Next, a ninth step is performed in which a first electrode is formed in contact with the third semiconductor layer and the second semiconductor layer. Next, a tenth step is performed in which a second electrode is formed on the back surface of the starting substrate. The process of returning the warp is a process of forming an oxide film on the silicon carbide semiconductor substrate, the film thickness of which is thicker on the C-face than on the Si-face.
[0006] Moreover, the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, is characterized in that it further includes an eleventh step of performing a process for removing the warpage of the silicon carbide semiconductor substrate after the fifth step and before the seventh step.
[0007] Furthermore, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, in the second step, a second semiconductor region of a second conductivity type is further formed between the trenches in the first semiconductor layer by ion implantation.
[0008] Moreover, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, a difference in oxide film thickness between the Si-face and the C-face is not less than 200 nm and not more than 1000 nm.
[0009] Moreover, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the treatment for straightening the warp is performed until an amount of warp of the silicon carbide semiconductor substrate is reduced to less than 100 μm.
[0010] Moreover, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the treatment for removing the warpage is performed after each ion implantation. Effect of the Invention
[0011] According to the method for manufacturing a silicon carbide semiconductor device of the present invention, it is possible to reduce or mitigate warping of a silicon carbide semiconductor substrate, and to reduce or suppress the occurrence of transport defects, stage chuck defects, patterning defects, and the like within the manufacturing equipment. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view showing a configuration of a silicon carbide semiconductor device according to an embodiment; [Diagram 2] 1 is a flowchart outlining a method for manufacturing a silicon carbide semiconductor device according to an embodiment. [Diagram 3] 1A to 1C are cross-sectional views (part 1) illustrating schematic diagrams of a silicon carbide semiconductor device according to an embodiment during manufacture. [Figure 4] 5A to 5C are cross-sectional views (part 2) illustrating schematic diagrams of a silicon carbide semiconductor device according to the embodiment during manufacture. [Diagram 5] 5A to 5C are cross-sectional views (part 3) illustrating schematic configurations of the silicon carbide semiconductor device according to the embodiment during manufacture. [Figure 6] 4 is a cross-sectional view (part 4) illustrating a schematic diagram of a silicon carbide semiconductor device according to the embodiment during manufacture. FIG. [Figure 7] 5 is a cross-sectional view (part 5) illustrating a schematic diagram of a silicon carbide semiconductor device according to the embodiment during manufacture. FIG. [Figure 8] 6 is a cross-sectional view illustrating a silicon carbide semiconductor device according to the embodiment during its manufacture (part 6). FIG. [Figure 9] 7 is a cross-sectional view illustrating a silicon carbide semiconductor device according to the embodiment during its manufacture (part 7). FIG. [Figure 10] 1 is a graph showing the relationship between the difference in oxide film thickness between the Si surface and the C surface and the amount of wafer warpage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A preferred embodiment of the method for manufacturing a silicon carbide semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p. Note that in the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations are omitted. In addition, in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and adding "-" before the index represents a negative index. In addition, the description of "same" or "equivalent" should include up to 5% in consideration of variations in manufacturing.
[0014] (Embodiment) First, a conventional method for manufacturing a semiconductor device will be described. Conventionally, in a trench MOSFET, an impurity layer is formed as follows. + On the front surface of the starting substrate + A first buffer layer and an n-type silicon carbide epitaxial layer are deposited. Next, n-type impurities are ion-implanted to form an n-type high concentration region. Next, p-type impurities are ion-implanted to form a first p-type high concentration region. + Type base region and second p+ Next, an n-type silicon carbide layer is epitaxially grown. Next, a p-type base region is formed by ion implantation of p-type impurities. Next, an n-type silicon carbide layer is epitaxially grown. Next, a p-type base region is formed by ion implantation of n-type impurities. + Next, p-type source regions are formed by ion implantation of p-type impurities. ++ A mold contact region is formed. After this, an activation process is performed and a trench is formed. In this way, an impurity layer is formed by combining ion implantation and epitaxial growth.
[0015] On the other hand, epitaxial growth can cause defects in the substrate, which can degrade the characteristics of the semiconductor device. In addition, epitaxial growth equipment requires process control and maintenance costs. For this reason, development is underway for silicon carbide semiconductor devices that do not use epitaxial growth, but instead form an impurity layer using only ion implantation, combining normal energy ion implantation (up to 900 KeV) with high-acceleration ion implantation (acceleration of 1 MeV or higher), which can implant impurities deeper.
[0016] In the manufacture of semiconductor devices, when an impurity layer is formed by ion implantation, a problem occurs in that the semiconductor substrate warps. In silicon carbide semiconductor devices, which have an extremely small diffusion coefficient of impurities, ions are implanted at high acceleration and high concentration, which can have a particularly large effect and cause warping of several hundred micrometers or more. Conventionally, semiconductor devices have been manufactured by combining ion implantation and epitaxial growth, so that the warping is canceled out by the difference in the warping direction, and the warping is kept to about several tens of micrometers. However, when an impurity layer is formed only by ion implantation, the warping of the substrate is not alleviated. In that case, there is a problem that it causes transportation failure, stage chuck failure, patterning failure, etc. in the manufacturing device.
[0017] A method for manufacturing a semiconductor device according to an embodiment that solves the above-mentioned problems will be described below. The semiconductor device according to the present invention is configured using a wide band gap semiconductor. In the embodiment, a silicon carbide semiconductor device fabricated (manufactured) using, for example, silicon carbide (SiC) as a wide band gap semiconductor will be described using a trench MOSFET 50 as an example. FIG. 1 is a cross-sectional view showing a structure of a silicon carbide semiconductor device according to the embodiment. FIG. 1 shows only an active region of the trench MOSFET 50 through which a main current flows.
[0018] As shown in FIG. 1, the silicon carbide semiconductor device according to the embodiment has n + The first main surface (front surface) of the starting substrate 1, for example, the (0001) surface (Si surface), is + A first n-type buffer layer 16 - A silicon carbide epitaxial layer 2 is deposited.
[0019] n + The starting substrate 1 is, for example, a silicon carbide single crystal substrate doped with nitrogen (N). + The mold buffer layer 16 has a thickness of, for example, 1 μm or more and 5 μm or less, and a nitrogen concentration of 1×10 17 / cm 3 More than 1×10 18 / cm 3 It is a highly doped layer doped at a high concentration of n + The buffer layer 16 is a 1n - This promotes the recombination of holes from the n-type silicon carbide epitaxial layer 2. + The concentration of holes reaching the starting mold substrate 1 is controlled to suppress the occurrence of stacking faults and their area expansion.
[0020] 1st n - The silicon carbide epitaxial layer 2 is + The starting substrate 1 is doped with a lower impurity concentration, for example, nitrogen. - The 1n-type drift layer - The n-type silicon carbide epitaxial layer 2 + The surface side opposite to the mold starting substrate 1 side is the 2nth -A 2n-th type silicon carbide layer 6 is formed. - The silicon carbide layer 6 is + The starting substrate 1 is lower than the first n - The n-type high-concentration drift layer is doped with, for example, nitrogen at a higher impurity concentration than the n-type silicon carbide epitaxial layer 2. + Starting substrates 1 and n - A silicon carbide epitaxial layer 2 and a second n - The p-type silicon carbide layer 6 and a p-type base layer 3 (described later) together constitute a silicon carbide semiconductor substrate.
[0021] n + A back electrode (drain electrode) is provided on the second main surface (back surface, i.e., the back surface (C surface) of the silicon carbide semiconductor base) of the mold starting substrate 1. The back electrode constitutes a drain electrode. A drain electrode pad 14 is provided on the surface of the back electrode.
[0022] A trench gate structure is formed on the first main surface side (p-type base layer 3 side) of the silicon carbide semiconductor substrate. + A second n-type insulating layer is formed on the surface opposite to the starting substrate 1 side through the p-type base layer 3. - The gate insulating film 9 is formed on the bottom and side walls of the trench 18 along the inner wall of the trench 18, and the gate electrode 10 is formed on the inside of the gate insulating film 9 in the trench 18. The gate electrode 10 is formed by the gate insulating film 9. - Type silicon carbide epitaxial layer 2, 2n - The gate electrode 10 is insulated from the p-type silicon carbide layer 6 and the p-type base layer 3. A part of the gate electrode 10 may protrude from above the trench 18 (the source electrode pad 15 side) towards the source electrode pad 15.
[0023] 1st n - The n-type silicon carbide epitaxial layer 2 and the n-th - The inside of the first silicon carbide layer 6 is + Type region 4 and 2p + A mold region 5 is selectively provided. +The type region 4 reaches a position deeper on the drain side than the bottom of the trench 18. + The lower end (drain side end) of the mold region 4 is located closer to the drain side than the bottom of the trench 18. + The mold region 4 is provided between the trenches 18. As shown in FIG. + The type region 4 is a p ++ The p-type contact region 8 is in contact with the p ++ It is also possible for the first p-type contact region 8 not to be in contact with the first p-type contact region 8. + The upper surface of the mold region 4 is the 2nth - The second insulating layer 4 is provided on the surface layer of the p-type silicon carbide layer 6 and is in contact with the lower surface of the p-type base layer 3 .
[0024] 2nd p. + The lower end of the mold region 5 is located closer to the drain side than the bottom of the trench 18. + The mold region 5 is formed at a position facing the bottom of the trench 18 in the depth direction z. + The width of the mold region 5 is wider than the width of the trench 18. The bottom of the trench 18 is the second p + The p-type region 5 may extend between the p-type base layer 3 and the second p + The 2nth mold region 5 is sandwiched between - The second p + It is not necessary for the second p + The upper surface of the mold region 5 may be located closer to the drain side or the source side than the bottom of the trench 18. + Type region 4 and 2p + The mold region 5 is doped with, for example, aluminum (Al).
[0025] 1st p. + A part of the mold region 4 is extended to the trench 18 side to form a second p + In this case, the first p + A part of the mold region 4 is the first p + Type region 4 and 2p + In the direction x in which the mold regions 5 are arranged (hereinafter referred to as the first direction) and in the direction y perpendicular to the direction x (hereinafter referred to as the second direction), -The first p-type silicon carbide layers 6 may be arranged alternately in a plane layout. + Part of type region 4 and 2p + It is sufficient that a part of the mold region 5 is connected at least at one or more places. + Type 5 and 1n regions - Holes generated when avalanche breakdown occurs at the junction of the silicon carbide epitaxial layer 2 can be efficiently evacuated to the source electrode 13, and the load on the gate insulating film 9 is reduced, thereby improving reliability.
[0026] 1st n - A p-type base layer 3 is provided on the first main surface side of the silicon carbide epitaxial layer 2. The impurity concentration of the p-type base layer 3 is, for example, + The impurity concentration of the p-type base layer 3 may be lower than that of the n-type region 4. This makes it possible to prevent a decrease in breakdown voltage due to punch-through by suppressing the spread of the depletion layer in the p-type base layer 3 even if the concentration is reduced to lower the threshold voltage. + Type source region 7 and p ++ A contact region 8 is selectively provided. + Type source region 7 and p ++ The mold contact regions 8 abut each other.
[0027] Although FIG. 1 illustrates only two trench MOS structures, more trench MOS gate (insulated gate made of metal-oxide-semiconductor) structures may be arranged in parallel.
[0028] The interlayer insulating film 11 is provided on the entire first main surface side of the silicon carbide semiconductor substrate so as to cover the gate electrode 10 embedded in the trench 18. The source electrode 13 is connected to the n-type + Type source region 7 and p ++The source electrode 13 is in contact with the type contact region 8. The source electrode 13 is electrically insulated from the gate electrode 10 by an interlayer insulating film 11. On the source electrode 13, a source electrode pad 15 is provided.
[0029] (Method of Manufacturing Silicon Carbide Semiconductor Device According to an Embodiment) Next, a method for manufacturing a silicon carbide semiconductor device according to an embodiment will be described. Fig. 2 is a flowchart showing an outline of the method for manufacturing a silicon carbide semiconductor device according to an embodiment. Figs. 3 to 9 are cross-sectional views each showing a schematic state during the manufacturing process of a silicon carbide semiconductor device according to an embodiment.
[0030] First, as shown in Figure 3, we have a n-type silicon carbide + A first conductive type starting substrate (a first conductive type starting substrate) 1 is - A silicon carbide epitaxial layer (first semiconductor layer of a first conductivity type) 2 and + A silicon carbide semiconductor substrate 30 having a type buffer layer 16 deposited thereon is prepared (first step). + The starting substrate has a diameter of 150 mm. The silicon carbide semiconductor substrate 30 may be purchased or may be manufactured by + Purchase a substrate containing only the starting substrate 1 and grow n + The first n-type buffer layer 16 and - The n-type silicon carbide epitaxial layer 2 may be formed to form the above-mentioned silicon carbide semiconductor substrate 30. In this case, + On the first main surface of the starting substrate 1, an n-type impurity such as nitrogen (N) is doped into a silicon carbide n-type semiconductor layer. + The n-type buffer layer 16 is then epitaxially grown. + A first n-type buffer layer 16 is formed on the buffer layer 16 by doping with n-type impurities, such as nitrogen atoms, and the first n-type buffer layer 16 is formed on the buffer layer 16 by doping with n-type impurities, such as nitrogen atoms. - A silicon carbide epitaxial layer 2 is grown.
[0031] Next, the 1nth -A resist mask (not shown) having desired openings is formed on the surface of the silicon carbide epitaxial layer 2 by photolithography. Then, as shown in FIG. 4, p-type impurities, for example, aluminum atoms, are implanted by ion implantation to form a first n-type silicon carbide epitaxial layer. - A first p-type silicon carbide epitaxial layer 2 is formed to a depth of about 0.6 μm. + A second semiconductor region of a second conductivity type (a second semiconductor region of a second conductivity type) 4, + The second conductive type region (first semiconductor region) 5 is, for example, 3×10 18 / cm 3 (Step S1: second process) Next, the resist mask for ion implantation is removed.
[0032] Next, a first warping back process is performed to straighten the warp of the silicon carbide semiconductor substrate 30 (step S2: third process). By the ion implantation in step S1, the silicon carbide semiconductor substrate 30 warps in a convex mountain shape on the front surface, for example, a warp of about 150 μm occurs. + Type area 4, 2nd p + Since the mold region 5 is formed in a deep region, high-acceleration ion implantation (1 MeV or more) is performed. As a result, the silicon carbide semiconductor substrate 30 becomes significantly warped in a mountain shape, and a warping reduction process must be performed to reduce the amount of warping of the silicon carbide semiconductor substrate 30. In the warping reduction process, for example, the amount of wafer warping of the silicon carbide semiconductor substrate 30 is reduced to less than 100 μm. The amount of wafer warping is the difference in height between the highest and lowest parts of the silicon carbide semiconductor substrate 30.
[0033] Fig. 10 is a graph showing the relationship between the difference in oxide film thickness between the Si surface and the C surface and the amount of wafer warpage. In Fig. 10, the vertical axis shows the amount of wafer warpage in μm. The horizontal axis shows the difference in oxide film thickness between the Si surface and the C surface in nm. The silicon carbide semiconductor substrate 30 has a front surface (Si surface) and a back surface (C surface), and between the Si surface and the C surface, the C surface is more easily oxidized. For this reason, when the silicon carbide semiconductor substrate 30 is oxidized, a difference occurs in the growth rate of the oxide film between the Si surface and the C surface, and the C surface is oxidized to a greater extent than the Si surface, resulting in a difference in oxide film thickness.
[0034] 10, wafer warpage occurs due to the difference in oxide film thickness between the Si surface and the C surface. The C surface of silicon carbide semiconductor substrate 30 is oxidized more thickly, so a concave warpage occurs on the front surface. In this way, the oxide film thickness between the Si surface and the C surface causes warpage in the direction opposite to the warpage of silicon carbide semiconductor substrate 30 caused by ion implantation, so that it is possible to return silicon carbide semiconductor substrate 30 to its original warpage.
[0035] For this reason, in the embodiment, in the first warpage recovery process, the silicon carbide semiconductor substrate 30 is oxidized so that the oxide film thickness difference is 200 nm or more and 1000 nm or less. According to FIG. 10, the wafer warpage amount is 20 μm or more and 100 μm or less, and the amount of warpage of the silicon carbide semiconductor substrate 30 caused by ion implantation is reduced, and the amount of warpage of the silicon carbide semiconductor substrate 30 can be reduced to less than 100 μm. For example, when the oxide film thickness difference is about 600 nm, a concave warpage occurs on the front surface of about 60 μm according to FIG. 10. Therefore, the amount of warpage of 150 μm, which is a convex mountain-shaped warpage on the front surface formed by ion implantation, is reduced to 90 μm (150-60), and the amount of warpage of the silicon carbide semiconductor substrate 30 is less than 100 μm. In addition, it is not necessary to remove the oxide film formed here.
[0036] In addition, oxidation can be performed by dry (O2) oxidation or pyrogenic (H2O) oxidation, but the difference in oxidation rate is greater with pyrogenic oxidation than with dry oxidation, and pyrogenic oxidation can increase the difference in oxide film thickness and the amount of wafer warpage. Also, the higher the oxidation temperature, the smaller the difference in oxidation rate, but oxidation does not progress below 1000°C, so the oxidation temperature must be 1000°C.
[0037] In step S1, a second p + The formation of the mold region 5 is necessary, but the first p between the trenches 18 + The mold region 4 may not be formed. In this case, the second p + After the mold region 5 is formed, the first warping removal process is carried out in step S2.
[0038] Next, the 1nth- A resist mask (not shown) having desired openings is formed by photolithography on the surface of the silicon carbide epitaxial layer 2. Then, as shown in FIG. 5, a second n-type epitaxial layer having a thickness of about 0.7 μm and doped with n-type impurities such as nitrogen by ion implantation is formed. - The silicon carbide layer 6 is, for example, 2×10 17 / cm 3 (Step S3) Next, the resist mask for ion implantation is removed.
[0039] Next, n - A resist mask (not shown) having a desired opening is formed by photolithography on the surface of the silicon carbide epitaxial layer 2. Then, as shown in FIG. 6, a p-type base layer (second semiconductor layer of the second conductivity type) 3 having a thickness of about 0.5 μm is formed by ion implantation with, for example, 3×10 17 / cm 3 (Step S4: fourth process) Next, the resist mask for ion implantation is removed.
[0040] Next, a resist mask (not shown) having desired openings is formed by photolithography on the surface of the p-type base layer 3. Then, as shown in FIG. + The source layer (third semiconductor layer of the first conductivity type) 7 is, for example, 1×10 19 / cm 3 (Step S5: fifth process) Next, the resist mask for ion implantation is removed.
[0041] Next, an ion implantation mask having a predetermined opening is formed, and n + A p-type impurity such as aluminum is ion-implanted into a part of the p-type source layer 7 and a part of the p-type base layer 3, so that, as shown in FIG. ++ The contact area 8 is, for example, 1×10 20 / cm 3 (Step S6) Next, the resist mask for ion implantation is removed.
[0042] Next, a second warping back process is performed to return the warp of the silicon carbide semiconductor substrate 30 to its original shape (step S7). Since ions are implanted only on the front surface side by ion implantation, the silicon carbide semiconductor substrate 30 warps in a convex mountain shape on the front surface, for example, a warp of about 120 μm occurs. For this reason, in the embodiment, in the second warping back process, the silicon carbide semiconductor substrate 30 is oxidized so that the oxide film thickness difference is 200 nm or more and 1000 nm or less, and the amount of warp of the silicon carbide semiconductor substrate 30 is reduced to less than 100 μm. For example, when the oxide film thickness difference is about 300 nm, a concave warp of about 30 μm occurs on the front surface according to FIG. 10. For this reason, the amount of warp of 120 μm of the convex mountain shape on the front surface formed by ion implantation is reduced to 90 μm (120-30), and the amount of warp of the silicon carbide semiconductor substrate 30 becomes less than 100 μm. The oxide film formed here is removed before the next activation process is carried out.
[0043] If the amount of warping of silicon carbide semiconductor substrate 30 caused by ion implantation does not affect the next process or subsequent processes, the second warping back process in step S7 does not need to be performed. - A silicon carbide layer 6, a p-type base layer 3, and an n + Type source layer 7 and p ++ The mold contact region 8 is implanted by normal accelerated ion implantation, but since warping occurs in each step, it is preferable to carry out a second warping recovery process.
[0044] In the embodiment, the first p + Type 4 and 2p + After the mold region 5 is formed, a first warping process is performed. ++ Although the second warping treatment is performed after the formation of the mold contact region 8, the warping treatment may be performed after each ion implantation. In addition, if the amount of warping of the silicon carbide semiconductor substrate 30 caused by the ion implantation does not affect the next process or subsequent processes, the warping treatment does not need to be performed.
[0045] Next, a heat treatment is performed in an inert gas atmosphere at about 1750° C. to activate the impurity regions formed by ion implantation (step S8: sixth step). The ion implantation regions may be activated all at once by a single heat treatment, or may be activated by performing a heat treatment each time an ion implantation is performed. The order of steps S8 and S9 may be reversed. That is, the activation process may be performed after the trench 18 is formed. In this case, a mask for forming a trench is formed on the oxide film formed in the second warping back process, and is removed together with the mask for forming a trench before the activation process.
[0046] Next, n + A trench forming mask having a predetermined opening is formed by photolithography on the surface of the source region 7. The mask is then made of, for example, an oxide film. Next, as shown in FIG. + The second p + A trench 18 is formed so as to reach the mold region 5 (step S9: seventh step). Next, the trench forming mask is removed.
[0047] Since it is preferable that the amount of warping of the silicon carbide semiconductor substrate 30 is small and the front surface of the silicon carbide semiconductor substrate 30 is flat when the trenches 18 are formed, the second warping reduction treatment is performed before the formation of the trenches 18. Since the activation treatment eliminates the warping of the silicon carbide semiconductor substrate 30, it is preferable to perform the activation treatment before the formation of the trenches 18.
[0048] Next, n + Type source region 7 and p ++ A gate insulating film 9 is formed along the surface of the contact region 8 and the bottom and sidewalls of the trench 18. This gate insulating film 9 may be formed by thermal oxidation at a temperature of about 1300° C. in a gas atmosphere containing oxygen. Also, this gate insulating film 11 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).
[0049] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 9. This polycrystalline silicon layer may be formed so as to fill the trench 18. This polycrystalline silicon layer is patterned by photolithography and left inside the trench 18 to form the gate electrode 10 (eighth step).
[0050] Next, an insulating film is formed on the surface of the gate electrode 10. For example, annealing is performed in an oxygen atmosphere at 1000°C to form a thermal oxide film. Next, the surface is protected with a protective film, for example, formed of a photoresist. Next, the insulating film formed on the back surface, the gate electrode, and the gate insulating film are all removed by dry etching. Next, the protective film formed on the surface is removed in an ashing and stripping process. This time, ashing in oxygen plasma and stripping using an SPM were performed.
[0051] Next, for example, phosphorus glass is deposited to a thickness of about 1 μm so as to cover the gate insulating film 9 and the gate electrode 10, forming an interlayer insulating film 11. Next, the interlayer insulating film 11 and the gate insulating film 10 are patterned by photolithography. + Type source region 7 and p ++ A contact hole is formed to expose the n-type contact region 8. Next, a conductive film, such as nickel, which becomes the source electrode (first electrode) 13 is formed in the contact hole and on the interlayer insulating film 11 by, for example, a sputtering method (step 9). Next, a heat treatment at about 700° C. is performed to selectively react the conductive film with silicon carbide, and then the unreacted conductive film is selectively removed to leave the source electrode 13 only in the contact hole, and the n-type contact region 8 is formed. + Type source region 7 and p ++ The contact region 8 is brought into contact with a source electrode 13 .
[0052] Next, a metal film to become the source electrode pad 15 is formed, for example, by sputtering, on the source electrode 13 and the interlayer insulating film 11 on the front surface of the silicon carbide semiconductor substrate. At this time, a barrier metal (not shown) made of titanium or titanium nitride may be formed first. The thickness of the portion of the electrode pad on the interlayer insulating film 11 may be, for example, 5.5 μm. The electrode pad may be formed of aluminum containing 1% silicon (Al-Si), for example. Next, the metal film is selectively removed to form the source electrode pad 15.
[0053] Next, n + After the front surface of the mold starting substrate 1 is covered with a protective film (not shown) for protection, + The starting substrate 1 is polished from the back side to form a n + The starting mold substrate 1 may be thinned to the product thickness.
[0054] Next, n + On the second main surface of the starting substrate 1, a conductive film that will become a drain electrode (not shown), such as a molybdenum film and a nickel film, is successively formed by, for example, a sputtering method. Then, a heat treatment such as laser annealing is performed to form a n + The starting mold substrate 1 and a conductive film are reacted to form an ohmic junction, thereby forming a drain electrode.
[0055] Next, on the surface of the drain electrode, films of, for example, titanium, nickel and gold are formed in this order as a drain electrode pad (second electrode) 14 (tenth step) In this manner, the silicon carbide semiconductor device shown in FIG.
[0056] As described above, according to the embodiment, an oxide film having a difference in thickness between the Si surface and the C surface is formed by oxidizing a silicon carbide semiconductor substrate. This reduces the amount of warping of the silicon carbide semiconductor substrate caused by ion implantation, and can reduce the amount of warping of the silicon carbide semiconductor substrate to less than 100 μm. This can reduce or suppress the occurrence of transport defects, stage chuck defects, patterning defects, and the like in a manufacturing device.
[0057] In the above, the present invention can be modified in various ways without departing from the spirit of the present invention, and in each of the above-mentioned embodiments, for example, the dimensions and impurity concentrations of each part are variously set according to the required specifications, etc. Also, in each of the embodiments, the first conductivity type is n-type and the second conductivity type is p-type, but the present invention is similarly valid even if the first conductivity type is p-type and the second conductivity type is n-type. [Industrial Applicability]
[0058] INDUSTRIAL APPLICABILITY As described above, the method for manufacturing a silicon carbide semiconductor device according to the present invention is useful for power semiconductor devices used in power conversion devices such as inverters, power supply devices for various industrial machines, igniters for automobiles, and the like. [Explanation of symbols]
[0059] 1n + Starting substrate 2 1stn - Silicon carbide epitaxial layer 3 p-type base layer 4 1st p. + type area 5 2nd p. + type area 6 2nd n - mold silicon carbide layer 7 n + Type Source Area 8 p ++ Mold Contact Area 9 Gate insulating film 10 Gate electrode 11 Interlayer insulating film 13 Source electrode 14 Drain electrode pad 15 Source electrode pad 16n + Mold Buffer Layer 18 Trench 30 Silicon carbide semiconductor substrate 50 Trench MOSFET
Claims
1. A first step of preparing a silicon carbide semiconductor substrate having a first conductivity type starting substrate and a first semiconductor layer having a lower impurity concentration than the starting substrate provided on a front surface side of the first conductivity type starting substrate; a second step of forming a first semiconductor region of a second conductivity type in the first semiconductor layer by ion implantation; A third step of performing a process for removing warpage of the silicon carbide semiconductor substrate after forming the first semiconductor region; a fourth step of forming a second semiconductor layer of a second conductivity type in the first semiconductor layer by ion implantation; a fifth step of forming a third semiconductor layer of a first conductivity type on a surface layer of the second semiconductor layer by ion implantation; a sixth step of activating the first semiconductor region, the second semiconductor layer, and the third semiconductor layer formed by ion implantation; a seventh step of forming a trench penetrating the third semiconductor layer and the second semiconductor layer to reach the first semiconductor layer at a position opposite to the first semiconductor region in a depth direction; an eighth step of forming a gate electrode inside the trench via a gate insulating film; a ninth step of forming a first electrode in contact with the third semiconductor layer and the second semiconductor layer; A tenth step of forming a second electrode on a rear surface of the starting substrate; Including, a silicon carbide semiconductor device manufacturing method comprising the steps of: forming an oxide film having a thickness greater on a C-face than on a Si-face of the silicon carbide semiconductor substrate;
2. After the fifth step and before the seventh step, The method for manufacturing a silicon carbide semiconductor device according to claim 1 , further comprising an eleventh step of performing a process for straightening out the warp of the silicon carbide semiconductor substrate.
3. 2 . The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein in the second step, a second semiconductor region of a second conductivity type is further formed between the trenches in the first semiconductor layer by ion implantation.
4. 2 . The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein a difference in oxide film thickness between the Si-face and the C-face is not less than 200 nm and not more than 1000 nm.
5. 2 . The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein the treatment for straightening the warp is performed until an amount of warp of the silicon carbide semiconductor substrate is reduced to less than 100 μm.
6. 2 . The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein the process of removing the warp is performed after each ion implantation. 3 .
Citation Information
Patent Citations
Decoding method of adaptability forecasting type differential pulse code and its unit
JP1980050738A
Electron beam machining method
JP1987072488A