Alloy steel, electrolytic corrosion prevention component and method for producing the same
The alloy steel with controlled elemental composition and surface treatment forms a hardened oxide layer, addressing the limitations of existing methods by maintaining high hardness and dimensional stability for high-precision, high-load applications.
Patent Information
- Application Number
- JP2023062440
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing methods for imparting insulation and wear resistance to steel parts using ceramics or surface oxidation face issues such as reduced strength, toughness, and high material costs, while surface oxidation methods result in dimensional changes and softening, compromising their use in high-load environments.
An alloy steel with specific elemental compositions (C: 0.01-1.0%, Si: 0.2-4.0%, Mn: 0.2-2.0%, Cr: 1.0-9.0%, Mo: 1.5-6.0%, Al: 0.01-5.0%) is treated to form a hardened layer with a surface oxide film, ensuring hardness above 55 HRC and minimal dimensional change during oxidation.
The alloy steel maintains high hardness and dimensional stability, enabling the production of high-precision parts with improved wear resistance and insulation properties, suitable for high-load environments.
Abstract
Description
[Technical field]
[0001] The present invention relates to an alloy steel containing chromium, molybdenum, etc., an electrolytic corrosion prevention part using the same, and a method for manufacturing the same. [Background technology]
[0002] Conventionally, when manufacturing parts that require insulation using steel, measures to impart insulation have been taken by replacing part of the part with insulating ceramics such as alumina, or by covering the surface of the part with a resin such as PPS (see Patent Document 1).
[0003] Alternatively, some steel materials manufactured with a specified composition can be heated at high temperatures to form an insulating oxide layer on the surface of the part, thereby giving the part insulating properties (see Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-236259 A [Patent Document 2] JP 2013-199674 A [Patent Document 3] JP 2004-84767 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when some of the parts disclosed in Patent Document 1 were replaced with resin and added, there were problems with the wear resistance and strength being insufficient compared to steel. Also, ceramics lacked toughness compared to steel, and there were problems with workability. In addition, the material costs of all of these materials were higher than steel, which increased the cost of the entire part.
[0006] On the other hand, as disclosed in Patent Document 2, when the surface of a steel material is oxidized to impart insulating properties to the parts, this is advantageous in terms of cost, but the hardness of conventional alloy steel is below 50HRC (HRC: Rockwell hardness C scale), and it is difficult to use such steel for long periods of time as parts in high-load environments that require wear resistance, fatigue strength, and the like.
[0007] This is because the carbon content, which contributes greatly to the hardness of alloy steel, is extremely low. In addition, the temperature required to form the oxide layer is in the high range of about 980 to 1220°C, so even if the material had high hardness before treatment, it may soften.
[0008] Even if high hardness could be achieved by heating to about 1200°C for both quenching and oxidation, the dimensions would vary greatly before and after the treatment. Therefore, in order to manufacture high-precision parts, grinding or other processes would be required after oxidation, and the oxide layer that had been so carefully formed would be ground away.
[0009] Furthermore, the material disclosed in Patent Document 3 describes a method for oxidizing the surface of the steel material to provide insulating properties to the parts, but does not disclose any information on the hardness or strength of the material, nor does it include any special consideration of this. In addition, the oxide layer is formed by immersion in an acid solution, which poses problems such as a decrease in material strength due to hydrogen embrittlement and a burden on the natural environment.
[0010] Therefore, an objective of the present invention is to provide an alloy steel that can maintain high strength (or hardness) while having electrical insulation between adjacent metal products, an electrolytic corrosion prevention part using the same, and a method for manufacturing the electrolytic corrosion prevention part. [Means for solving the problem]
[0011] In order to solve the above-mentioned problems, the invention relates to an alloy steel containing, by weight, 0.01-1.0% C, 0.2-4.0% Si, 0.2-2.0% Mn, 1.0-9.0% Cr, 1.5-6.0% Mo, 0.01-5.0% Al, with the balance being Fe and unavoidable impurities, and a hardened layer is provided on the surface of the alloy steel.
[0012] Alternatively, the alloy steel may further contain, by weight, 0.01 to 1.2% V, or 0.01 to 2.0% W.
[0013] This hardened layer may be either a carburized layer or a carbonitrided layer, in which case the surface hardness of the carburized layer or the carbonitrided layer may be 58 HRC or more on the Rockwell C scale.
[0014] Next, the invention of an electrolytic corrosion prevention part is an electrolytic corrosion prevention part in which an oxide film is coated on a hardened layer formed on an alloy steel using the above-mentioned alloy steel invention.
[0015] In the method for manufacturing the electrolytic corrosion prevention part, an oxide film is formed on the surface of the above-mentioned alloy steel at a temperature range of 500° C. to 600° C. In this case, the oxide film may be formed on the surface of the alloy steel in an atmosphere containing at least either oxygen or water vapor. Effect of the Invention
[0016] The alloy steel of the present invention has a specific composition and can form an insulating oxide layer (oxide film) on the surface of the steel while maintaining a hardness exceeding 55HRC (Rockwell hardness C scale). The electrolytic corrosion prevention part of the present invention can achieve a hardness exceeding 55HRC by subjecting the alloy steel to heat treatment by quenching and tempering, and then by carrying out finish processing to ensure the dimensional accuracy of the part and then carrying out an oxidation heat treatment, even if an insulating oxide film is formed, the dimensional change of the part due to the oxidation treatment can be kept relatively small. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The content of each element contained in the alloy steel according to one embodiment of the present invention will be described. The chemical composition of the alloy steel of the present invention satisfies the following conditions: (1) the composition range allows an insulating oxide layer to be formed on the surface, (2) the composition range does not allow conductive precipitate particles (such as carbides) of a size large enough to penetrate the oxide layer to be formed, and (3) the composition range is such that the alloy steel is resistant to softening even when subjected to oxidation treatment after quenching and tempering, and has a hardness exceeding 55HRC.
[0018] The range of C (carbon) is set to 0.01 to 1.0% by weight. If the C content exceeds this range, the toughness of the alloy steel may decrease, and the carbides in the matrix structure may become coarse. In addition, the hot workability of the alloy steel may deteriorate. On the other hand, if the C content is less than this range, the hardness will be 55HRC or less.
[0019] The content of silicon (Si) is set to 0.2-4.0% by weight. If the amount of silicon exceeds this range, the toughness of the alloy steel may decrease, or the hot workability may deteriorate. On the other hand, if the amount of silicon falls below this range, the insulating property of the oxide layer formed on the surface may decrease, or the machinability may deteriorate.
[0020] The Mn (manganese) content is set to the range of 0.2 to 2.0% by weight. If it exceeds this range, the workability may deteriorate. On the other hand, if it is below this range, the raw materials must be carefully selected, which may result in higher material costs.
[0021] Cr (chromium) should be in the range of 1.0 to 9.0% by weight. If it exceeds this range, the oxide layer of the alloy steel becomes thin and the insulating properties of the oxide layer decrease. If it falls below this range, the insulating properties of the oxide layer of the alloy steel decrease.
[0022] Mo (molybdenum) is in the range of 1.5 to 6.0% by weight. If it exceeds this range, the carbides may become coarse or the toughness of the alloy steel may decrease. On the other hand, if it is below this range, the hardness after oxidation treatment may become 55HRC or less.
[0023] The content of aluminum (Al) is set to the range of 0.01 to 5.0% by weight. If the content exceeds this range, the hardness after oxidation treatment may become 55HRC or less, or non-metallic inclusions may increase, causing a decrease in fatigue strength. On the other hand, if the content falls below this range, the insulating properties of the oxide layer may decrease.
[0024] V (vanadium) may be contained within the range of 0.01 to 1.2% by weight. If the content exceeds this range, the carbides may become coarse or the toughness of the alloy steel may decrease. Furthermore, W (tungsten) may be contained within the range of 0.01 to 2.0% by weight.
[0025] In addition, a hardened layer, either a carburized layer or a carbonitrided layer, is formed on the surface of the alloy steel of the present invention. The surface hardness of this carburized layer or carbonitrided layer is preferably 58HRC or more on the Rockwell C scale.
[0026] Next, an embodiment of the present invention will be described, which is an electrolytic corrosion prevention part using an alloy steel and a manufacturing method thereof. In the invention of the electrolytic corrosion prevention part using an alloy steel of the present invention, an oxide film is formed on the surface of the alloy steel, which is the base material.
[0027] Furthermore, even if the alloy steel, which has been quenched and tempered in advance, is heat treated again at a temperature range of 500°C or higher and 600°C or lower, the alloy steel has sufficient temper softening resistance characteristics and can fully ensure a hardness of more than 55HRC.
[0028] In addition, in the above-mentioned oxidation heat treatment process, the alloy steel is heat-treated in an atmosphere containing either oxygen or water vapor, or in an atmosphere containing both oxygen and water vapor, thereby forming an oxide film on the surface of the alloy steel.
[0029] In this case, it is desirable to carry out the treatment after the final processing such as molding or cutting of the electrolytic corrosion prevention part. This is because even if heat treatment is carried out in an oxygen atmosphere after the final processing, the heating temperature is relatively low at 500 to 600°C, and the dimensional change of the electrolytic corrosion prevention part is very small.
Claims
1. An alloy steel comprising, by weight, 0.01-1.0% C, 0.2-4.0% Si, 0.2-2.0% Mn, 1.0-9.0% Cr, 1.5-6.0% Mo, 0.01-5.0% Al, with the balance being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
2. The alloy steel according to claim 1, further comprising, by weight percent, V: 0.01 to 1.2%.
3. The alloy steel according to claim 2, further comprising, by weight percent, W: 0.01 to 2.0%.
4. The alloy steel according to claim 1, characterized in that the hardened layer is either a carburized layer or a carbonitrided layer.
5. The alloy steel according to claim 2, characterized in that the hardened layer is either a carburized layer or a carbonitrided layer.
6. The alloy steel according to claim 3, characterized in that the hardened layer is either a carburized layer or a carbonitrided layer.
7. 5. The alloy steel according to claim 4, wherein the surface hardness of the carburized or carbonitrided layer is 58 HRC or more on the Rockwell C scale.
8. 6. The alloy steel according to claim 5, wherein the surface hardness of the carburized or carbonitrided layer is 58 HRC or more on the Rockwell C scale.
9. 7. The alloy steel according to claim 6, wherein the surface hardness of the carburized or carbonitrided layer is 58 HRC or more on the Rockwell C scale.
10. 10. An electrolytic corrosion prevention part using the alloy steel according to claim 1, wherein the hardened layer is coated with an oxide film.
11. 11. The method for producing an electrolytic corrosion prevention part according to claim 10, wherein the oxide film is formed on the alloy steel at a temperature in the range of 500° C. to 600° C.
12. The method for producing an electrolytic corrosion-preventing part according to claim 11, characterized in that the oxide film is formed on the surface of the alloy steel in an atmosphere containing at least either oxygen or water vapor.
Citation Information
Patent Citations
Roller bearing
JP2004084767A
Insulating rolling bearing for electrical corrosion prevention
JP2009236259A
Stainless steel material with good insulation and method for producing the same
JP2013199674A