Semiconductor device and method of manufacturing semiconductor device
The use of MCZ wafers and proton-containing buffer layers in IGBTs forms an impurity profile that addresses the issue of MOS transistor deterioration, enhancing controllability and breakdown resistance while maintaining gate oxide film integrity.
Patent Information
- Application Number
- JP2023062638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The deterioration of MOS transistor characteristics and gate oxide film characteristics due to proton irradiation in the formation of an impurity profile in insulated gate bipolar transistors (IGBTs) using Floating Zone (FZ) wafers.
A semiconductor device and manufacturing method utilizing a silicon substrate made by the Magnetic-Applying Czochralski (MCZ) method, incorporating an n-type drift layer with higher impurity concentration towards the second surface and a buffer layer containing protons, which forms an impurity profile without proton irradiation through the MOS transistor region.
This approach suppresses the deterioration of MOS transistor characteristics and maintains the integrity of the gate oxide film, while improving controllability and breakdown resistance during dynamic operations without adversely affecting off-state voltage holding ability.
Smart Images

Figure 2024149006000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor device and a method for manufacturing a semiconductor device. [Background technology]
[0002] In Patent Document 1, N - An insulated gate bipolar transistor (IGBT) is disclosed in which the impurity concentration of the drift layer is maximized at at least one location. - The impurity concentration of the drift layer decreases from the point where the impurity concentration is maximum toward the P base layer and the P collector layer. - The portion of the drift layer where the impurity concentration is maximum contains oxygen atoms and elements lighter than oxygen. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-91853 A Summary of the Invention [Problem to be solved by the invention]
[0004] In Patent Document 1, a floating zone (FZ) wafer is used as the Si wafer. In Patent Document 1, protons are introduced into Si from the emitter electrode side where the MOS (Metal-Oxide-Semiconductor) transistor of the IGBT is formed, by proton irradiation, and an impurity profile of the drift layer is formed. Therefore, protons, which are charged particles, pass through the MOS transistor region. Therefore, there is a possibility that the MOS transistor characteristics and the gate oxide film characteristics constituting the MOS gate structure will deteriorate.
[0005] The present disclosure has been made to solve the above-mentioned problems, and has an object to provide a semiconductor device and a method for manufacturing the semiconductor device that can suppress deterioration of characteristics. [Means for solving the problem]
[0006] The semiconductor device according to the present disclosure comprises a silicon substrate having a first surface and a second surface opposite to the first surface and containing oxygen as an impurity, a first electrode provided on the first surface, and a second electrode provided on the second surface, wherein the silicon substrate comprises an n-type drift layer having a higher impurity concentration toward the second surface side, an n-type first buffer layer provided on the second surface side of the drift layer and containing protons as an impurity, and a second buffer layer provided on the second surface side of the first buffer layer.
[0007] A method for manufacturing a semiconductor device according to the present disclosure is to manufacture a semiconductor device by a magnetic-applied Czochralski (MCZ) method, form a semiconductor layer on a first surface side of a silicon wafer having an n-type drift layer, perform ion implantation on a second surface of the silicon wafer opposite to the first surface, and perform annealing to form a second buffer layer, and after forming the second buffer layer, to implant protons (H + ) and annealing the protons after the protons are implanted to form a first buffer layer. Effect of the Invention
[0008] In the semiconductor device and the method for manufacturing the semiconductor device according to the present disclosure, the impurity profile of the drift layer can be formed by combining a silicon substrate containing oxygen as an impurity or a silicon wafer manufactured by the MCZ method with an n-type first buffer layer containing protons as an impurity, thereby suppressing the deterioration of characteristics such as MOS transistor characteristics. [Brief description of the drawings]
[0009] [Figure 1] 1 is a plan view of a semiconductor device according to a first embodiment. [Figure 2A] 1 is a cross-sectional view of an IGBT according to a first embodiment. [Figure 2B] 1 is a cross-sectional view of a diode according to a first embodiment. [Figure 2C] 4 is a cross-sectional view showing another example of the diode according to the first embodiment. FIG. [Figure 3A] 5 is a diagram showing an impurity profile of the drift layer according to the first embodiment. FIG. [Figure 3B] 1A to 1C are diagrams illustrating the influence of a buffer layer on an impurity profile of a drift layer. [Figure 3C] 13 shows the results of calculation of the impurity profile of hydrogen concentration in the depth direction. [Figure 4] FIG. 13 is a diagram showing the relationship between the amount of change in impurity concentration in the drift layer and the breakdown voltage. [Diagram 5] FIG. 13 is a diagram showing the relationship between the oxygen concentration in an MCZ wafer and the impurity concentration in the drift layer. [Figure 6] FIG. 13 is a diagram showing the measured temperature dependence of static breakdown voltage in a 3.3 kV diode. [Figure 7] This figure shows the prototype results of the safe operating area in the dynamic state for a 3.3 kV IGBT and diode. [Figure 8] FIG. 13 is a diagram showing the waveform of RBSOA. [Figure 9] FIG. 1 is a diagram showing the waveform of an SCSOA. [Figure 10] FIG. 13 is a diagram showing the waveform of Recovery SOA. [Figure 11A] FIG. 11 is a diagram showing an impurity profile according to the second embodiment. [Figure 11B] FIG. 1 shows impurity profiles of various first buffer layers. [Figure 11C] FIG. 11 is a diagram showing an impurity profile of the first buffer layer according to a modification of the second embodiment. [Figure 12] FIG. 13 is a diagram showing the waveform when a 1200V diode maintains its withstand voltage. [Figure 13] FIG. 1 is a diagram showing device characteristics of a 1200V diode. [Figure 14]FIG. 13 is a diagram showing the waveform of RBSOA. [Figure 15] FIG. 13 is a diagram showing the waveform of Recovery SOA. [Figure 16A] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16B] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16C] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16D] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16E] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16F] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16G] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16H] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16I] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16J] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16K] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16L] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 16M] 11A to 11C are diagrams illustrating a method for manufacturing an IGBT according to a third embodiment. [Figure 17] 13 is a flowchart showing a method for forming a vertical structure according to the third embodiment. [Figure 18A] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18B] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18C] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18D] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18E] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18F] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18G] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18H] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 18I] 13A to 13C are diagrams illustrating a method for manufacturing a diode according to a fourth embodiment. [Figure 19] 13 is a flowchart showing a method for forming a vertical structure according to the fourth embodiment. [Figure 20] 13 is a flowchart showing a method for forming a vertical structure according to a modified example of the fourth embodiment. [Figure 21] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Figure 22] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Diagram 23] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Figure 24] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Diagram 25] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Figure 26] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Figure 27] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. [Figure 28] FIG. 13 is a cross-sectional view showing an example of a semiconductor device according to a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A semiconductor device and a method of manufacturing the semiconductor device according to each embodiment will be described with reference to the drawings. The same or corresponding components are designated by the same reference numerals, and repeated description may be omitted.
[0011] Embodiment 1 FIG. 1 is a plan view of a semiconductor device 100 according to a first embodiment. The semiconductor device 100 is, for example, a power semiconductor chip. An active cell area 1 is an area that ensures the basic performance of the power semiconductor chip. An interface area 2 is an area where the active cell area 1 and an edge termination area 3 are joined. The interface area 2 supports the breakdown resistance during dynamic operation of the power semiconductor and supports the original performance of the active cell area 1. The edge termination area 3 is provided to maintain the breakdown voltage in a static state and ensure the stability and reliability of the breakdown voltage characteristics. The edge termination area 3 further suppresses breakdown resistance failure during dynamic operation and supports the original performance of the active cell area 1.
[0012] The above regions make it possible to improve the total loss performance, improve the leakage characteristics when holding a voltage at high temperatures, guarantee reliability, improve controllability during dynamic operation, and guarantee the breakdown resistance. The total loss includes the loss in the on state, the loss at turn-on, and the loss at turn-off. The semiconductor device 100 further includes a front gate wiring portion 4 and a gate pad portion 39. For example, when the semiconductor device 100 is a diode, the front gate wiring portion 4 and the gate pad portion 39 may not be present.
[0013] FIG. 2A is a cross-sectional view of an IGBT 101 according to the first embodiment. FIG. 2B is a cross-sectional view of a diode 102 according to the first embodiment. FIG. 2C is a cross-sectional view showing another example of a diode 103 according to the first embodiment. The semiconductor device 100 is, for example, an IGBT or a diode as shown in FIGS. 2A to 2C. FIGS. 2A to 2C are cross-sectional views obtained by cutting FIG. 1 along line A-A'. The diode 102 has a pin diode structure. The diode 103 has a RFC (Relaxed Field of Cathode) diode structure. The diode of this embodiment may be a power diode or a freewheeling diode (FWD).
[0014] The semiconductor device 100 includes a silicon substrate having a first surface and a second surface opposite to the first surface, a first electrode 5 provided on the first surface, and a second electrode 21 provided on the second surface. The silicon substrate has an n-type impurity layer in which the impurity concentration is higher on the second surface side. - The semiconductor device has an n-type drift layer 15. An n-type buffer layer 16 containing protons as impurities is provided on the second surface side of the drift layer 15. A buffer layer 17 is provided on the second surface side of the buffer layer 16. Of the two types of buffer layers 16, 17, only the buffer layer 16 is in contact with the drift layer 15. Hereinafter, the first surface side may be referred to as the front side, and the second surface side may be referred to as the back side.
[0015] The drift layer 15 contains phosphorus or antimony as a dopant. The drift layer 15 has an impurity concentration C n- is 1.0×10 12 ~5.0×10 14 atoms / cm 3 The device is formed using a silicon wafer manufactured by the MCZ method. The final device thickness is t device The diameter of the MCZ wafer is 40 to 700 μm. Phosphorus or antimony is used as an n-type dopant in the manufacturing of the MCZ wafer. This reduces the impurity concentration C n-In particular, the evaporation rate of antimony is about three orders of magnitude faster than that of phosphorus. The evaporation rate of P is 1.6×10 -4 cm / sec, Sb evaporation rate is 1.3×10 -1 By using evaporation control technology that takes advantage of this characteristic to produce single crystal silicon, the impurity concentration C n- This can significantly reduce variation in the
[0016] In the diodes 102 and 103, the drift layer 15 is a region from the main junction 12 on the front side to the junction 22 on the back side. In the IGBT 101, the drift layer 15 and the semiconductor layer 11 are provided between the main junction 12 and the junction 22. The main junction 12 is a junction that has the maximum electric field strength when the depletion layer extends to the back side to hold the voltage when a reverse bias is applied in the power semiconductor. The junction 22 is the junction that the depletion layer extending from the main junction 12 to the back side first contacts when the voltage is held, and is the junction that has the second highest electric field strength when the voltage is held.
[0017] In addition, the IGBT 101 and the diodes 102 and 103 are provided with buffer layers 16 and 17. The buffer layer 16 enables low loss during off-state and improved controllability and breakdown resistance during dynamic operation. The buffer layer 17 enables stable voltage retention in the off-state.
[0018] In the IGBT 101 shown in FIG. 2A, an n-type semiconductor layer 11 is provided on the first surface side of the drift layer 15. The semiconductor layer 11 is formed deeper than the base layer 9 on the first surface side of the drift layer 15. The semiconductor layer 11 has the effect of increasing the carrier concentration on the first surface side when the IGBT is in the ON state. This allows the IGBT to have a low ON voltage. A p-type base layer 9 is provided on the first surface side of the n-type semiconductor layer 11. An n-type base layer 9 is provided on the first surface side of the base layer 9. + type emitter layer 7 and p + A molded semiconductor layer 8 is provided.
[0019] A trench 24 is formed in the first surface of the silicon substrate. The trench 24 penetrates the emitter layer 7 and the base layer 9. A gate electrode 14 is provided inside the trench 24. A first electrode 5 is provided on the gate electrode 14 with an interlayer film 6 interposed therebetween. In the IGBT 101, the first electrode 5 is an emitter electrode. A p-type collector layer 18 is provided on the second surface side of the buffer layer 17. A second electrode 21 is provided in contact with the collector layer 18. In the IGBT 101, the second electrode is a collector electrode.
[0020] In the MOS transistor section, a part of the trench 24 has the same potential as the first electrode 5, which is the emitter potential. The first electrode 5 is, for example, an aluminum wiring. This structure makes it possible to suppress the saturation current density of the IGBT, suppress oscillation in a no-load short-circuit state by controlling the capacitance characteristics, improve short-circuit resistance, and realize a low ON voltage by improving the carrier concentration on the emitter side.
[0021] In the diode 102 shown in FIG. 2B, a p-type anode layer 10 is provided on the first surface side of the drift layer 15. A first electrode 5 is provided on the anode layer 10. In the diode 102, the first electrode 5 is an anode electrode. + A cathode layer 19 of the type is provided. The cathode layer 19 is in contact with a second electrode 21. In the diode 102, the second electrode 21 is the cathode electrode.
[0022] 2C differs from diode 102 in that it further includes a p-type cathode layer 20. The cathode layer 20 is provided on the second surface side of buffer layer 17, and is aligned with cathode layer 19 in the direction along the second surface. The cathode layers 19, 20 are alternately aligned in the direction along the second surface.
[0023] The following describes examples of parameters for each diffusion layer and trench of the IGBT 101. In the following, the impurity concentration refers to the concentration of an element other than Si. The element that forms the diffusion layer is called a dopant. p-type base layer 9 Dopant: boron, peak impurity concentration: 1.0×1016 ~1.0×10 18 atoms / cm 3 Depth: deeper than the emitter layer 7 and shallower than the semiconductor layer 11 n-type semiconductor layer 11 Dopant: arsenic or phosphorus, peak impurity concentration: 1.0×10 15 ~1.0×10 17 atoms / cm 3 , depth: 0.5 to 1.0 μm deeper than the base layer 9 ·n + Type emitter layer 7 Dopants: arsenic, phosphorus, peak impurity concentration: 1.0×10 18 ~1.0×10 21 atoms / cm 3 , depth: 0.2~1.0μm p + Type semiconductor layer 8 Dopant: boron, surface impurity concentration: 1.0×10 18 ~1.0×10 21 atoms / cm -3 , depth: same as or deeper than emitter layer 7 n-type buffer layer 16 Dopant: Proton, peak impurity concentration C P,n2n ≦0.01×C P,n1 , depth X j,nb2 :X j,n1 +20~30μm n-type buffer layer 17 Dopant: arsenic or phosphorus, peak impurity concentration C p,n1 :1.0×10 15 ~5.0×10 16 atoms / cm 3 , depth X j,n1 : 1.0~30μm p-type collector layer 18 Dopant: boron, peak impurity concentration: 1.0×10 16 ~1.0×10 20 atoms / cm 3 , depth: 0.3~0.8μm Trench depth D trench : 2.0 μm to a depth deeper than the n-type semiconductor layer 11
[0024] An example of parameters of each diffusion layer of the diode 102 will be described. p-type anode layer 10 Dopant: boron, surface impurity concentration: 1.0×10 16 atoms / cm 3 Above, peak impurity: 2.0×10 16 ~1.0×10 18 atoms / cm 3 , depth: 2.0~10.0μm n-type buffer layer 16 Dopant: Proton, peak impurity concentration C P,n2n ≦0.01×C P,n1 , depth X j,nb2 :X j,n1 +20~30μm n-type buffer layer 17 Dopant: arsenic or phosphorus, peak impurity concentration C P,n1 :1.0×10 15 ~5.0×10 16 atoms / cm 3 , depth X j,n1 : 1.0~30μm ·n + Type cathode layer 19 Dopants: arsenic, phosphorus, peak impurity concentration: 1.0×10 17 ~1.0×10 19 atoms / cm 3 , depth: 0.3~0.5μm
[0025] An example of parameters of each diffusion layer of the diode 103 will be described. p-type anode layer 10 Dopant: boron, surface impurity concentration: 1.0×10 16 atoms / cm 3 Above, peak impurity: 2.0×10 16 ~1.0×10 18 atoms / cm 3 , depth: 2.0~10.0μm n-type buffer layer 16 Dopant: Proton, peak impurity concentration C P,n2n ≦0.01×C P,n1 , depth X j,nb2 :Xj,n1 +20~30μm n-type buffer layer 17 Dopant: arsenic or phosphorus, peak impurity concentration C P,n1 :1.0×10 15 ~5.0×10 16 atoms / cm 3 , depth X j,n1 : 1.0~30μm ·n + Type cathode layer 19 Dopants: arsenic, phosphorus, peak impurity concentration: 1.0×10 17 ~1.0×10 19 atoms / cm 3 , depth: 0.3~0.5μm ·p-type cathode layer 20 Dopant: boron, peak impurity concentration: 1.0×10 16 ~1.0×10 18 atoms / cm 3 , depth: 0.3~0.5μm
[0026] Hereinafter, the drift layer 15, the buffer layers 16 and 17, and the collector layer 18 in the IGBT 101 may be referred to as a vertical structure 38. Similarly, the drift layer 15, the buffer layers 16 and 17, and the cathode layer 19 in the diode 102, and the drift layer 15, the buffer layers 16 and 17, and the cathode layers 19 and 20 in the diode 103 may be referred to as a vertical structure 38.
[0027] In the MCZ wafer, impurities such as oxygen and nitrogen are introduced during the manufacture of the Si wafer. Due to oxygen atoms among these impurities, a thermal donor phenomenon occurs at a specific annealing temperature. The thermal donor phenomenon is a phenomenon in which oxygen atoms in the MCZ wafer become donors in a specific temperature range. In this embodiment, this thermal donor phenomenon is utilized to control the impurity concentration of the drift layer 15 to a characteristic impurity profile that increases from the main junction 12 toward the junction 22. This makes it possible to suppress adverse effects on the voltage holding ability in the off state, that is, on the static breakdown voltage characteristics, and to improve the controllability and breakdown resistance during dynamic operation.
[0028] Oxygen and nitrogen introduced during the manufacture of MCZ wafers exist at interstitial and substitutional sites in the silicon single crystal, respectively. i is two to three orders of magnitude higher in the MCZ wafer than in the FZ wafer. s is equivalent to that of the FZ wafer in the MCZ wafer. In this embodiment, protons are injected from the back side and diffused from the back side to the front side to utilize the thermal donor phenomenon caused by oxygen. This makes it possible to form a characteristic impurity profile in which the impurity concentration of the drift layer 15 increases from the main junction 12 toward the junction 22.
[0029] 3A to 3C show impurity profiles along the line C-C' in FIG. 2. FIG. 3A shows the impurity profile of drift layer 15 according to the first embodiment. In FIG. 3A, "new structure" shows the impurity profile of this embodiment, and "con. structure" shows the impurity profile of a comparative example. The comparative example differs from this embodiment in that an FZ wafer is used. The impurity concentration of drift layer 15 of this embodiment is higher than that of the comparative example in that the X j,MJ From junction 22 X j、n2n The impurity concentration of drift layer 15 may continue to increase from the junction between drift layer 15 and a layer provided on the first surface side of drift layer 15 to the junction between drift layer 15 and buffer layer 16.
[0030] FIG. 3B is a diagram for explaining the influence of the buffer layer 16 on the impurity profile of the drift layer 15. FIG. 3B shows the impurity profiles of the new structure and the con. structure with and without the buffer layer 16. Note that the buffer layer 17 exists in each sample shown in FIG. 3B. The horizontal axis of FIG. 3A and FIG. 3B is the t device3B, it can be seen that a profile in which the impurity concentration increases toward the second surface side can be obtained simply by combining the new structure using the MCZ wafer with the buffer layer 16.
[0031] FIG. 3C shows the calculation result of the impurity profile of hydrogen concentration in the depth direction. The buffer layer 16 is formed by implanting protons from the back side. + 1 and critical H + 2 are the critical H values for the diffusion of one and two oxygen atoms, respectively. + The hydrogen concentration is the critical H concentration for oxygen to diffuse. + concentration is 1 to 3 orders of magnitude higher.
[0032] Protons have the effect of accelerating oxygen diffusion. + The presence of protons in the drift layer 15 promotes the phenomenon of becoming a thermal donor due to oxygen. Hydrogen introduced from the back side diffuses to the front side by annealing during the formation of the buffer layer 16, which will be described later. For this reason, the back side is more likely to become a thermal donor than the front side. Therefore, the combination of oxygen in the drift layer 15 and protons in the buffer layer 16 can form an impurity profile of hydrogen element whose concentration gradually decreases toward the front side.
[0033] FIG. 4 is a diagram showing the relationship between the amount of change in impurity concentration of the drift layer 15 and the breakdown voltage. FIG. 4 shows the results of a simulation performed on a 6.5 kV IGBT. The horizontal axis shows the amount of change in impurity concentration relative to the impurity concentration of the con. structure. 100% shows the impurity concentration of the drift layer 15 of the con. structure in FIG. 3A. The vertical axis shows the static breakdown voltage (BV) at 218 K. If the amount of change is 20%, that is, if it is greater than 120% of the horizontal axis, the breakdown voltage at 218 K will be lower than the rated voltage of 6500 V. For this reason, it is preferable that the amount of change in the impurity concentration of the drift layer 15 is 20% or less relative to the impurity concentration of the drift layer 15 of the con. structure. In other words, it is preferable that the amount of change in the impurity concentration in the drift layer 15 is 20% or less.
[0034] Figure 5 shows the oxygen concentration (O) in the MCZ wafer. i and the impurity concentration C of the drift layer 15 n- When a donor layer is formed due to the thermal donor phenomenon in an MCZ wafer, the impurity concentration C n- increases. minimum[O i ] and maximum[O i ] are expressed by the relationship equations (1) and (2), respectively.
[0035]
number
[0036]
number
[0037] Here, minimum[O i ] is the minimum [O i ] value. i ] is due to thermal donor formation caused by oxygen in the MCZ wafer. n-Even if the temperature changes, the [O i ] is the limit value.
[0038] Maximum[O i ] and minimum[O i ] during the oxygen concentration O i By controlling n- Even if the oxygen concentration O in the drift layer 15 changes, the power semiconductor's basic performance, that is, its ability to hold voltage in the off state, that is, its static breakdown voltage characteristics, can be suppressed from being adversely affected. i and impurity concentration C n- is minimum[O i ]≦O i ≦maximum[O i ] is desirable.
[0039] Figure 6 shows the static breakdown voltage (BV) of a 3.3kV diode. R The new device A in FIG. 6 shows the measurement temperature dependence of the oxygen concentration in FIG. i ] and minimum[O i ]. new deviceB is the device that was controlled during [O i ] to maximum[O i The impurity profiles of the drift layer 15 of the new devices A and B are both characteristic impurity profiles shown in FIG. 3A. However, the new device B has a higher impurity concentration C due to the thermal donor phenomenon caused by oxygen than the new device A. n- This is a diode with a large increase in
[0040] As a result, new device A exhibits a withstand voltage retention capability equivalent to that of the con. device, but new device B cannot retain a rated voltage of 3,300 V, which is a 3.3 kV class, even at 298 K, and its voltage retention capability in the off state is reduced.
[0041] FIG. 7 is a diagram showing the results of a prototype of the safe operating area (SOA) in a dynamic state in a 3.3 kV IGBT and a diode. The impurity profiles of the drift layer 15 of the con. device and the new device in FIG. 7 are the same as the impurity profiles of the con. structure and the new structure in FIG. 3A, respectively. In the new device, the maximum [O i ] and minimum[O i ] between [O i In the con. device, an FZ wafer is used.
[0042] In Fig. 7, J C (break) is the maximum breaking current density of the IGBT when switching with a low load. Max. power density is the maximum breaking power density when turning off the IGBT when switching with a low load or when the diode recovers. t W is the maximum gate pulse width of the IGBT under no-load short circuit. E SC is the maximum short circuit energy of the IGBT when it is short circuited without load. dj / dt is the J A This is the slope of the waveform and the maximum slope at which it is cut off.
[0043] The new device, which has the characteristic impurity profile of the drift layer 15 of this embodiment, has a larger SOA than the con. device, whether it is an IGBT or a diode. This is the result of controlling the interaction between the carrier plasma layer inside the device and the electric field strength under dynamic conditions. The carrier plasma layer is a layer formed by conductivity modulation when electrons and holes are injected into the drift layer 15 when the device is ON. The carrier plasma layer is a neutral layer where n is the electron concentration and p is the hole concentration, and n ≒ p. Controlling this carrier plasma layer is important for improving the performance of IGBTs and diodes, which are power semiconductors.
[0044] Fig. 8 is a diagram showing the waveform of RB (Reverse-Bias) SOA. Fig. 9 is a diagram showing the waveform of SC (Short Circuit) SOA. Fig. 10 is a diagram showing the waveform of Recovery SOA. Figs. 8 and 10 show that the new device is capable of blocking even under conditions that would cause breakdown in the con. device, and has a large breakdown resistance. Fig. 9 shows the waveform at maximum blocking in short circuit mode, and shows that the new device can block under conditions with a longer pulse width than the con. device, and has a large breakdown resistance in short circuit mode.
[0045] In this way, according to this embodiment, the controllability and breakdown resistance during dynamic operation can be improved without adversely affecting the voltage holding ability in the off state. Also, in this embodiment, by combining a silicon substrate manufactured by the MCZ method containing oxygen as an impurity with a buffer layer 16 containing protons as an impurity, an impurity profile of the drift layer 15 in which the impurity concentration is higher on the second surface side can be formed. Therefore, the impurity profile of the drift layer 15 can be formed by proton irradiation without causing protons to pass through the MOS transistor region. Therefore, deterioration of the MOS transistor characteristics and the gate oxide film characteristics can be suppressed.
[0046] The concentration of carbon [Cs], another impurity element introduced during the manufacture of MCZ wafers, is 1.0×10 14 ~5.0×10 15 atoms / cm -3 This is the order.
[0047] In the present embodiment, an example has been described in which the semiconductor device 100 is an IGBT or a diode, but the semiconductor device 100 may be an RC (Reverse-Conducting)-IGBT. That is, the silicon substrate in the semiconductor device 100 may have an IGBT region and a diode region. The IGBT region may have the structure of an IGBT 101. The diode region may have the structure of either a diode 102 or a diode 103.
[0048] The above-mentioned modifications can be appropriately applied to the semiconductor device and the manufacturing method of the semiconductor device according to the following embodiments. Note that the semiconductor device and the manufacturing method of the semiconductor device according to the following embodiments have many points in common with the first embodiment, so the differences from the first embodiment will be mainly described.
[0049] Embodiment 2 11A is a diagram showing an impurity profile according to the second embodiment. FIG. 11A shows an impurity profile along the line C-C' in FIG. 2. In the present embodiment, the impurity profile of the buffer layer 16 is different from that of the first embodiment. The other configurations are the same as those of the first embodiment. The impurity concentration of the buffer layer 16 has multiple peaks in the thickness direction of the silicon substrate. The impurity concentrations of the multiple peaks become higher as they approach the buffer layer 17.
[0050] That is, the buffer layer 16 is made up of a plurality of n-type layers 2n It can also be said that it includes multiple layers n 2n Peak concentration C p,n2n is the junction X of the buffer layers 16 and 17 j,n1 to the junction X between the buffer layer 16 and the drift layer 15 j,n2n In the example of FIG. 11A, the buffer layer 16 has n=2 peaks. The peak concentration of the buffer layer 17 is C p,21 , the peak concentration of the buffer layer 16 is C from the side closer to the buffer layer 17. p,n21 , C p,n22 Then, C p,n22 <C p,n21 <C p,21 It becomes.
[0051] FIG. 11B is a diagram showing impurity profiles of various buffer layers 16. FIG. 11B shows impurity profiles along the line B-B' in FIG. 2. "new profile" is the impurity profile of this embodiment, and "C p,n22 <C p,n21 <C p,21In the profile 1, the buffer layer 16 has only one peak of impurity concentration. In the profile 2, the peak of the impurity concentration in the buffer layer 16 becomes lower as it approaches the buffer layer 17. In the profile 3, the impurity concentration in the buffer layer 16 does not have a peak and is a nearly constant impurity concentration profile.
[0052] In the case of the profile 1′, a region 37 having a lower impurity concentration than the drift layer 15 exists in the buffer layer 16. The buffer layer 16 is formed by introducing H + Region 37 is formed when H reacts with point defects in silicon to form complex defects, which become a donor layer. + does not diffuse toward the back side, and H + The H required to react with + does not exist, and H + This layer is formed due to non-reaction between the silicon and point defects in the silicon.
[0053] H + The behavior of not diffusing toward the back side is due to the oxygen concentration O i The higher the oxygen concentration, the more H is generated in the complex defects caused by oxygen in silicon. + is trapped, and H + The diffusion of oxygen is hindered. Complex defects include, for example, VO (Vacancy-Oxygen pair), C i O i (interstitial carbon-interstitial oxygen pair), V2 (di-vacancy). + is trapped, VOH, C i O i H n , V2H2.
[0054] In contrast, in the new profile corresponding to this embodiment, the impurity concentration of the buffer layer 16 has multiple peaks. As will be described later, this structure is formed by ion implantation using multiple acceleration energies.+ This is achieved by introducing H into the silicon from the back side. + Even if the back side cannot diffuse, H + This makes it possible to prevent the formation of a region 37 having a lower impurity concentration than that of drift layer 15, as shown in the new profile of FIG.
[0055] 11C is a diagram showing an impurity profile of the buffer layer 16 according to a modification of the second embodiment. As shown in new profiles 1 and 2, the buffer layer 16 may have three or more impurity concentration peaks. As shown in new profile 3, the impurity concentration peaks may be provided separately on the first surface side and the second surface side of the buffer layer 16. The horizontal axis of FIG. 11C represents the t device It is standardized in.
[0056] 12 is a diagram showing a waveform when the breakdown voltage of the diode 103 is maintained. In FIG. 12, a waveform when the breakdown voltage of a 1200V diode having the structure of the diode 103 is maintained at 298K is shown. The diode of con. profile 1' has a low concentration region 37. Therefore, the main junction X J,MJ When the depletion layer extending from the MOSFET reaches the MOSFET, the leakage current increases, which is a characteristic leakage characteristic. This results in a decrease in the breakdown voltage retention capability and a loss during off-state = V R xJ R On the other hand, according to the new profile of this embodiment, there is no sudden increase in leakage current, and it is possible to maintain the breakdown voltage.
[0057] 13 is a diagram showing the device characteristics of the diode 103. In FIG. 13, the device characteristics of a 1200 V diode having the structure of the diode 103 are shown for the con. profiles 2 and 3 shown in FIG. 11B and the new profile. The new profile of this embodiment has a lower ON voltage V F While realizing this, the leakage current JR Furthermore, the SOA can be widely secured in a dynamic state.
[0058] In the diode having the new profile of the buffer layer 16 of this embodiment, the depletion layer is formed at the main junction X during dynamic operation. J、MJ This allows carriers to remain on the back side while easing the extension of the depletion layer when it reaches the buffer layer 16. This behavior is due to the effect of controlling the interaction between the carrier plasma layer and the electric field strength during dynamic operation of the IGBT or diode.
[0059] In addition, in the snappy mode SOA, the maximum voltage during recovery operation is V snap-off This allows the voltage to be lower than the rated voltage of 1200V for the 1200V element. In this way, it is possible to suppress breakdown during dynamic operation and improve controllability, and in the case of a large current mode SOA, the breaking current density J during recovery operation is A (break) can be increased.
[0060] Fig. 14 is a diagram showing the waveform of RBSOA. Fig. 14 shows the interruption capability under L-load switching conditions for a 3.3 kV IGBT having con. profile 1 and the new profile shown in Fig. 11B. The IGBT having the new profile of this embodiment has improved interruption capability compared to con. profile 1. In other words, even in an IGBT, a dynamic SOA expansion can be achieved according to the new profile of this embodiment.
[0061] Fig. 15 is a diagram showing the waveform of Recovery SOA. Fig. 15 shows the interruption capability under L-load switching conditions for the 3.3 kV diodes having con. profile 1 and the new profile shown in Fig. 11B. The HV (High Voltage) diode having the new profile has improved interruption capability compared to con. profile 1.
[0062] Moreover, in the modified examples of the impurity profile of the buffer layer 16 of the present embodiment, new profiles 1 to 3, shown in FIG. 11C, results similar to those shown in FIGS. 13 to 15 are obtained.
[0063] In addition, the new profile of the buffer layer 16 of this embodiment alone has the effect of controlling the interaction between the carrier concentration and the electric field strength during dynamic operation of the IGBT or diode. Therefore, the buffer layer 16 of this embodiment having multiple peaks in the impurity concentration may be applied to the FZ wafer.
[0064] Embodiment 3 A method for manufacturing the IGBT 101 according to the first and second embodiments will be described. FIGS. 16A to 16M are diagrams for explaining a method for manufacturing the IGBT 101 according to the third embodiment. FIGS. 16A to 16M are cross-sectional views at a position corresponding to the line A-A' in FIG. 1. First, a semiconductor layer is formed on a first surface of a silicon wafer having an n-type drift layer 15 manufactured by the MCZ method. Specifically, as shown in FIG. 16A, after forming an oxide film 23, a base layer 9 and a semiconductor layer 11 are formed on the front side of the drift layer 15 by photolithography, etching, ion implantation, annealing, or the like. Next, as shown in FIG. 15B, an emitter layer 7 is partially formed on the front side by ion implantation and annealing.
[0065] Thereafter, as shown in FIG. 16C, a trench 24 is formed by etching. Furthermore, the etching and oxidation techniques are used in combination to clean, smooth and round the inner wall of the trench. Next, as shown in FIG. 16D, a gate oxide film 13 is formed on the inner wall of the trench. Furthermore, the trench 24 is filled with a d-poly Si film that will become the gate electrode 14. The d-poly Si film is formed by doping an n-type element such as As or phosphorus at 1×10 19 atoms / cm 3 The polysilicon film is doped to have the above-mentioned high concentration.
[0066] Next, as shown in FIGS. 16E to 16H, in order to recover the carrier lifetime of the drift layer 15, a high-concentration n + A gettering layer is formed by the layer 27 and the high crystal defect density layer 28. + Layer 27 has a surface concentration of 1.0×10 20 ~1.0×10 22 cm -3 , and the depth is 1.0 to 10 μm. As a result, the carrier lifetime of drift layer 15 becomes equal to or greater than the value calculated by the following formula 3.
[0067]
number
[0068] Here, t N- is the thickness of the drift layer 15 (m), τ t is the carrier lifetime (sec) in the drift layer 15 at which the influence of the carrier lifetime on the ON voltage of the IGBT disappears. N- is the t in Figure 2 device are device parameters equivalent to
[0069] The ON voltage of the IGBT and the diode depends on the carrier lifetime of the drift layer 15. Equation (3) is an index of the carrier lifetime required to minimize the dependency. The carrier lifetime is calculated by τ t If the above settings can be made, the effect of the carrier lifetime on switching loss can be controlled to a minimum. In addition, because off-state loss is also affected by the carrier lifetime, it is possible to reduce off-state loss and suppress thermal runaway.
[0070] Next, a method for forming a gettering layer will be described in detail. First, as shown in FIG. 16E, the d-poly Si film formed on the first surface of the wafer, which will become the gate electrode 14, is removed, an oxide film 25 is formed on the surface of the d-poly Si film, and an interlayer film 6 is formed on the first surface of the wafer. Next, as shown in FIG. 16F, selective etching is performed only on the back surface of the wafer in order to expose the Si surface on the back surface of the wafer. As a result, the gate oxide film 13 and the d-poly Si film on the back surface of the wafer are removed. A solution of hydrofluoric acid or a mixed acid is used for etching. The mixed acid is, for example, a mixed solution of hydrofluoric acid, nitric acid, and acetic acid.
[0071] Next, as shown in FIG. 16G, + As a source for forming the layer 27 and the high crystal defect density layer 28, + The polysilicon 26 doped with the element forming the layer 27 is formed by the LPCVD method. The polysilicon 26 is d-poly Si. + The layer 27 is formed of an element that diffuses into Si, such as phosphorus, arsenic, or antimony. + The elements that can form the layer can be selected. Polysilicon 26 is 1x10 19 atoms / cm 3 The polysilicon 26 is a film doped with the high concentration impurities, and has a thickness of 500 nm or more. The high concentration impurities are diffused into the Si surface on the back side of the wafer by the subsequent annealing. This results in a high concentration n + During the formation of layer 27, a high density of dislocations and lattice defects is introduced, comprising a high crystal defect density layer 28.
[0072] Specifically, after the deposition of polysilicon 26, thermal annealing is performed at 900-1000°C in a nitrogen atmosphere. Next, the temperature is lowered from 900-1000°C to 500-700°C at an arbitrary rate, and thermal annealing is performed in a nitrogen atmosphere at a temperature lower than the previous annealing temperature. This causes impurities to diffuse from the d-poly Si into the Si on the back surface of the wafer where polysilicon 26 is in direct contact with the Si. As a result, as shown in FIG. 16H, a high concentration n +A layer 27 is formed. Furthermore, a high concentration n + When the layer 27 is formed, crystal defects, that is, a high crystal defect density layer 28, are generated secondarily.
[0073] The polysilicon 26 and the Si surface, which have different thermal expansion coefficients, come into direct contact with each other, and the interface, i.e., the high-concentration n + Strain occurs in the surface layer of the layer 27. As a result, + The layer 27, the high crystal defect density layer 28, and the strained layer present in the surface layer of the polysilicon 26 serve as getter sites. With this configuration, heavy metals and contaminant atoms taken into the wafer during the wafer process diffuse in the crystal lattice and move to the getter sites during the annealing at 500 to 700°C. As a result, the heavy metals and contaminant atoms can be captured.
[0074] This technology reduces the τ of the drift layer 15 that was reduced during the wafer process. t In other words, as shown in formula (3), drift layer 15 with a sufficiently long carrier lifetime can be realized so as not to affect the electrical characteristics of IGBTs of various withstand voltage classes.
[0075] In addition to the polysilicon 26, a similar effect can be obtained by forming a high crystal defect density layer on the back surface of the wafer using a laser annealing technique. This laser annealing technique is a local annealing technique that involves rapid heating and rapid cooling using a laser with a wavelength of 500 to 1000 nm. In this case, the power density of the laser annealing is set to 4 J / cm. 2 This is the end of the process. After this, annealing is performed in the same manner as in the method using polysilicon 26. That is, thermal annealing is performed in a nitrogen atmosphere at 900-1000°C, the temperature is lowered from 900-1000°C to 500-700°C at an arbitrary temperature drop rate, and then low-temperature thermal annealing is performed in a nitrogen atmosphere at 500-700°C. This allows heavy metals and contaminant atoms to move to the getter site, resulting in an improved carrier lifetime.
[0076] After the gettering layer is formed, the polysilicon 26 formed on the first surface of the wafer is removed as shown in FIG. 16I. Furthermore, as shown in FIG. 16J, the interlayer film 6 is selectively removed, and n-type GaN is formed on the first surface of the front side of the drift layer 15. + Type emitter layer 7 or p + A contact hole is formed to expose the Si surface of the type semiconductor layer 8. Next, as shown in FIG. 16K, a first electrode 5, which is an aluminum wiring film, is formed on the interlayer film 6 and in the contact hole by using a sputtering technique. The first electrode 5 has a layered structure made of an aluminum-based metal in which Si or Cu is added to Al, a barrier metal 40, and a silicide layer 41 formed by the reaction of the exposed Si with the metal. The aluminum-based metal is, for example, AlSi, AlSiCu, or AlCu. The barrier metal 40 is, for example, TiN or TiW. The silicide layer 41 is, for example, TiSi2, PtSi, or CoSi. Next, as shown in FIG. 16L, a passivation film 30 is formed on the first electrode 5. Furthermore, polysilicon 26, high concentration n-type SiO2, and the like are deposited on the first electrode 5. + Layer 27 and high crystal defect density layer 28 are removed by a polishing step and a subsequent wet etching step.
[0077] Next, as shown in FIG. 16M, a vertical structure 38 including buffer layers 16 and 17 is formed. FIG. 17 is a flowchart showing a method for forming the vertical structure 38 according to the third embodiment. On the first surface side where the vertical structure 38 is not formed, the MOS transistor structure constituting the IGBT, the aluminum wiring, and the passivation film 30 are already present. For this reason, when forming the buffer layers 16 and 17 and the collector layer 18 constituting the vertical structure 38, the first surface side is set to a temperature lower than the melting point of the first electrode 5, that is, the melting point of aluminum, 660° C. In other words, taking into consideration the temperature gradient in the device depth direction, laser annealing using a laser with a wavelength that does not transfer heat to the first surface, or annealing in a diffusion furnace at a low temperature below the metal melting point is selected.
[0078] Also, the buffer layers 16 and 17 have a thickness equal to the thickness of the device shown in FIG. deviceThis is formed after the process of forming the high concentration n + The layer 27, the high crystal defect density layer 28, and the polysilicon 26 are removed. However, the carrier lifetime of the drift layer 15 has a value that satisfies the formula (3).
[0079] 17, the front-side protective film forming step (S1) corresponds to the above-mentioned step of forming the passivation film 30. Moreover, polishing (S2) and etching (S3) correspond to the steps shown in FIG. 16L.
[0080] In the process of this embodiment, the order of forming the buffer layers 16 and 17 and the setting of the peak position of the acceleration energy when the buffer layer 16 is introduced are important. In this embodiment, as shown in Figs. 16A to 16L, after forming a semiconductor layer on the first surface side of the silicon wafer, ion implantation is performed on the second surface of the silicon wafer (S4) and annealing is performed (S5) to form the buffer layer 17. After forming the buffer layer 17, protons are implanted (S6) into a position deeper from the second surface than the buffer layer 17, and after the protons are implanted, annealing is performed (S12) to form the buffer layer 16. Hereinafter, S5 may be referred to as the first annealing step and S12 as the third annealing step. The annealing (S12) of the buffer layer 16 to the protons may be performed, for example, at 375 to 425°C for 90 minutes or more.
[0081] Furthermore, after injecting protons (S6) and before annealing the protons (S12), ion implantation is performed on the second surface and annealing is performed to form a p-type layer shallower than buffer layer 17. In the example of Fig. 17, collector layer 18 is formed as the p-type layer.
[0082] The annealing step for forming the buffer layer 17 is performed at a higher temperature than the annealing step for forming the buffer layer 16. Therefore, forming the buffer layer 17 after forming the buffer layer 16 may adversely affect the impurity profile after activation of the buffer layer 16 and the type of lattice defects introduced to form the buffer layer 16. This may adversely affect carriers in the device ON state. Therefore, it is preferable to form the buffer layer 16 after forming the buffer layer 17.
[0083] The buffer layer 16 of the second embodiment can be formed by introducing protons into Si with two or more different types of acceleration energies and doses after the activation annealing (S5) of the buffer layer 17, and then performing annealing (S12). The buffer layers 16 and 17 are formed so as to satisfy the following relationship. The peak position of the buffer layer 16 is at the junction X of the buffer layers 16 and 17. j,n1 From X j,n2n This allows the buffer layers 16 and 17 to be formed accurately without interference with each other.
[0084] The buffer layer 17 is formed using As or phosphorus as a dopant. The buffer layer 16 is formed using protons as a dopant. When injecting protons, multiple ion implantations are performed. The multiple ion implantations are performed in order from the highest acceleration energy condition, and the higher the acceleration energy, the smaller the dose. In other words, ion implantations are performed with lower acceleration energy and higher dose from the drift layer 15 side to the buffer layer 17 side in order.
[0085] The buffer layer 16 can also be formed by using a cyclotron irradiation technique other than ion implantation.
[0086] When protons are introduced into silicon, vacancies v generated during the introduction react with impurities in silicon such as oxygen and carbon to form complex defects. Hydrogen contained in the complex defects becomes a donor, which is an electron supply source. When the donor concentration increases due to an increase in the density of complex defects caused by annealing, the donor concentration increases due to the promotion of the thermal donor phenomenon caused by the ion implantation or irradiation process. As a result, a buffer layer 16 is formed, which is an n-layer caused by donorization and has a higher impurity concentration than the drift layer 15.
[0087] In this embodiment, the device performance can be improved by utilizing the complex defects formed in the buffer layer 16. On the other hand, some complex defects are lifetime killers that shorten the carrier lifetime. Therefore, the process of forming the buffer layer 16 by ion implantation and annealing techniques after the formation of the buffer layer 17 is important for removing the lifetime killer defects by controlling the complex defects formed in the buffer layer 16 and for stabilizing the profile of the buffer layer 16. Furthermore, the peak position of the buffer layer 16 can be controlled by adjusting the junction X of the buffer layers 16 and 17. j,n1 From X j,n2n By setting it to be located on the junction side, the buffer layer 17 and the layer n 21 and does not interfere with the buffer layer 17. 21 is a layer that constitutes the buffer layer 16 and is joined to the buffer layer 17. Therefore, a plurality of diffusion layers can be formed with high precision.
[0088] After the proton implantation (S6), a photolithography step (S7) and an ion implantation step (S8) are performed to form the collector layer 18. Furthermore, after the resist removal step (S9), a second annealing step (S10) is performed to form the collector layer 18. The second annealing step may be the same annealing technique as the first annealing step. For the second annealing step, laser annealing or a low-temperature annealing technique below the metal melting point may be used.
[0089] Next, the front side protective film is removed (S11), and the third annealing step for protons described above is performed (S12). Next, light etching (S13) is performed, and a metal film that is the second electrode 21 is formed by sputtering (S14). Next, an alloy layer or a silicide layer is formed at the interface between the Si surface and the metal in a fourth annealing step (S15). The second electrode 21 is a metal that contacts the collector layer 18, and is, for example, an AlSi film with an Si content of 1 to 3% or a laminated film containing Ni. The fourth annealing step is performed at a temperature of 300 to 400°C, which is lower than the temperature in the third annealing step.
[0090] According to this embodiment, a MCZ wafer with a high oxygen concentration is used, protons are injected from the back side, and H is generated by annealing. + is diffused from the back side to the front side. This makes it possible to promote the thermal donor phenomenon caused by oxygen in the silicon on the back side more than on the front side, and thus makes it possible to form a sloped impurity profile in the drift layer 15.
[0091] Embodiment 4 A method for manufacturing the diode 103 according to the first and second embodiments will be described. FIGS. 18A to 18J are diagrams for explaining a method for manufacturing the diode 103 according to the fourth embodiment. First, as shown in FIGS. 18A to 18C, an oxide film 33 is formed on the front side, and photolithography is performed on the oxide film 33. Next, ions are implanted through an opening in the oxide film 33, and annealing is performed after removing the resist used during the photolithography, thereby forming the p-layer 31 and n-layer 32 in the termination region. + The layer 34 and the anode layer 10 in the active region are formed. Then, as shown in Figure 18C, an oxide-based interlayer film 6 is formed.
[0092] Next, as shown in FIG. 18D, a high-concentration n + A getter site is formed by the layer 27, the high crystal defect density layer 28, and the strained layer present in the surface layer portion of the polysilicon 26. This makes it possible to set the carrier lifetime of the drift layer 15 so as to satisfy the formula (3).
[0093] Next, as shown in FIG. 18E, the polysilicon 26 is removed if it is present on the front side. Next, the p-layer 31 and n-layer + A contact hole is formed in the interlayer film 6 for contacting the layer 34 and the anode layer 10. Thereafter, as shown in Figures 18F and 18G, the first electrode 5 and the passivation films 35 and 36 are formed.
[0094] 19 is a flowchart showing a method for forming a vertical structure 38 according to the fourth embodiment. The method for forming the vertical structure 38 is similar to that of the third embodiment, except that cathode layers 19, 20 are formed instead of the collector layer 18. As shown in FIG. 18H, a passivation film 30 is formed as a front-side protective film (S21), and the second surface is polished (S22) and etched (S23). S24 to S26 are similar to S4 to S6 in the third embodiment.
[0095] Next, ion implantation is performed to form cathode layer 20 (S27). Next, using photolithography (S28), ion implantation is performed to form cathode layer 19 (S29), and cathode layer 19 is partially formed on the back side. S30 to S36 are the same as S9 to S15 in the third embodiment. In this way, a diode 103 as shown in FIG. 18I can be manufactured.
[0096] Fig. 20 is a flow chart showing a method for forming a vertical structure 38 according to a modification of the fourth embodiment. Fig. 20 shows a method for forming the vertical structure 38 in a diode 102. In the diode 102, since the cathode layer 20 does not exist, the ion implantation process for the cathode layer 20, the photolithography process for partially forming the cathode layer 19 on the back side, and the associated resist removal process are not present. The other processes are the same as those in the manufacturing process of the diode 103. That is, S41 to S46 are the same as S21 to S26, and S47 to S55 are the same as S28 to S36.
[0097] Embodiment 5. In this embodiment, an example will be described in which the semiconductor device 100 is an RC-IGBT. Figures 21 to 28 are cross-sectional views showing an example of the semiconductor device 100 according to embodiment 5. Figures 21 to 28 are cross-sectional views obtained by cutting FIG. 1 along line A-A'. In the semiconductor device 100 of this embodiment, the silicon substrate has an IGBT region and a diode region.
[0098] The structure of the IGBT region of the semiconductor device 100 shown in Fig. 21 is similar to the structure of the IGBT 101 of the first embodiment. In Fig. 21, the diode region includes an n-type semiconductor layer 11 provided on the first surface side of the drift layer 15, and a p-type anode layer 10 provided on the first surface side of the semiconductor layer 11. The diode region further includes a p + The diode region includes an n-type semiconductor layer 8. The diode region also includes an n-type cathode layer 19 provided on the second surface side of the buffer layer 17. The semiconductor layer 11 is formed deeper than the base layer 9 on the first surface side of the drift layer 15 in the IGBT region, and is formed deeper than the anode layer 10 on the first surface side of the drift layer 15 in the diode region.
[0099] 21 to 28 has a characteristic impurity profile similar to that of the first embodiment. n- is 1.0 × 10 12 ~5.0×10 14 atoms / cm 3 And the final t device is 40 to 700 μm.
[0100] Below are examples of parameters of the diffusion layers and trenches that configure the RC-IGBT shown in Fig. 21. Note that the anode layer 10 is the same layer as the base layer 9. p-type base layer 9 Dopant: boron, peak impurity concentration: 1.0×10 16 ~1.0×10 18 atoms / cm 3Depth: deeper than the emitter layer 7 and shallower than the semiconductor layer 11 n-type semiconductor layer 11 Dopants: arsenic, phosphorus, peak impurity concentration: 1.0×10 15 ~1.0×10 17 atoms / cm 3 , depth: 0.5 to 1.0 μm deeper than the base layer 9 ·n + Emitter Layer 7 Dopants: arsenic, phosphorus, peak impurity concentration: 1.0×10 18 ~1.0×10 21 atoms / cm 3 , depth: 0.2~1.0μm p + Type semiconductor layer 8 Dopant: boron, surface impurity concentration: 1.0×10 18 ~1.0×10 21 atoms / cm 3 Depth: same as emitter layer 7 or deeper than emitter layer 7 Trench depth D trench 2.0 μm to a depth deeper than the semiconductor layer 11 n-type buffer layer 16 Dopant: Proton, peak impurity concentration C P,n2n ≦0.01×C P,n1 , depth X j、nb2 :X j,n1 +20~30μm n-type buffer layer 17 Dopants: arsenic, phosphorus, peak impurity concentration C P,n1 :1.0×10 15 ~5.0×10 16 atoms / cm 3 , depth X j、n1 : 1.0~30μm p-type collector layer 18 Dopant: boron, peak impurity concentration: 1.0×10 16 ~1.0×10 20 atoms / cm 3 , depth: 0.3~0.8μm ·n + Cathode Layer 19 Dopants: As, phosphorus, peak impurity concentration: 1.0×10 17 ~1.0×10 19 atoms / cm 3 , depth: 0.3~0.5μm
[0101] The semiconductor device 100 in Fig. 22 differs from the semiconductor device 100 in Fig. 21 in that the semiconductor layer 8 is not present. In other words, the anode layer 10 is in contact with the first electrode 5. The other configuration is similar to that of the semiconductor device 100 in Fig. 21. In the semiconductor device 100 in Fig. 22, the efficiency of hole injection from the base layer 9 in the ON state of the diode constituting the RC-IGBT can be reduced compared to the semiconductor device 100 in Fig. 21.
[0102] Fig. 23 shows a configuration in which the structure on the first surface side is similar to that of the semiconductor device 100 in Fig. 21 and includes a cathode layer 20. The p-type cathode layer 20 is provided on the second surface side of the buffer layer 17 and is aligned with the n-type cathode layer 19 in the direction along the second surface. Fig. 24 shows a configuration in which the structure on the first surface side is similar to that of the semiconductor device 100 in Fig. 22 and includes a cathode layer 20. ·p-type cathode layer 20 Dopant: boron, peak impurity concentration: 1.0×10 16 ~1.0×10 18 atoms / cm 3 , depth: 0.3~0.5μm 23 and 24, the efficiency of electron injection from the back side of the diode constituting the RC-IGBT in the ON state can be reduced compared to the semiconductor device 100 in FIGS. 21 and 22, respectively.
[0103] In addition, in the RC-IGBT of Figure 22-24, the turn-off loss E REC and ON voltage V F The high-speed performance on the trade-off curve can be achieved without relying on carrier lifetime control using charged particles such as electron beams. REC And high V FThe adverse effect of impurities such as oxygen and carbon in MCZ wafers on diode performance becomes more pronounced when carrier lifetime control is performed using charged particles. In order to make full use of MCZ wafers, it is important to develop E that does not rely on carrier lifetime control. REC vs. V F The structures shown in FIGS. 22 to 24 are effective in improving the performance on the high-speed side of the trade-off curve.
[0104] The semiconductor device 100 in each of Figs. 25 to 28 differs from the semiconductor device 100 in Figs. 21 to 24 in that a part of the gate electrodes 14 in the IGBT region is in contact with the first electrode 5. That is, in some of the trenches 24, the gate electrodes 14 are at the same potential as the emitter potential. In the RC-IGBT, by using a MOS transistor structure, it is possible to suppress the saturation current density of the IGBT and suppress oscillation in a no-load short-circuit state by controlling the capacitance characteristics. This improves the short-circuit resistance and realizes a lower ON voltage by improving the carrier concentration on the emitter side.
[0105] The technical features described in the present embodiment may be used in appropriate combination.
[0106] Various aspects of the present disclosure are summarized below as appendices. (Appendix 1) a silicon substrate having a first surface and a second surface opposite to the first surface, the silicon substrate containing oxygen as an impurity; A first electrode provided on the first surface; a second electrode provided on the second surface; Equipped with The silicon substrate is an n-type drift layer having a higher impurity concentration toward the second surface side; an n-type first buffer layer provided on the second surface side of the drift layer and containing protons as impurities; a second buffer layer provided on the second surface side of the first buffer layer; A semiconductor device comprising: (Appendix 2) 2. The semiconductor device according to claim 1, wherein the impurity concentration of the drift layer continues to increase from a junction between the drift layer and a layer provided on the first surface side of the drift layer to a junction between the drift layer and the first buffer layer. (Appendix 3) the drift layer contains phosphorus or antimony as an impurity, 3. The semiconductor device according to claim 1, wherein the second buffer layer contains arsenic or phosphorus as an impurity. (Appendix 4) The oxygen concentration O i is expressed as follows, where Cn is the impurity concentration of the drift layer: 1.00×10 17 ln(C n )-2.84×10 18 ≦O i ≦9.40×10 16 ln(C n )-2.27×10 18 4. The semiconductor device according to claim 1, wherein the semiconductor device satisfies the above. (Appendix 5) the impurity concentration of the first buffer layer has a plurality of peaks in a thickness direction of the silicon substrate, 5. The semiconductor device according to claim 1, wherein the impurity concentrations of the plurality of peaks are higher toward the second buffer layer. (Appendix 6) a p-type base layer provided on the first surface side of the drift layer; an n-type emitter layer provided on the first surface side of the base layer; a gate electrode provided within a trench formed on the first surface of the silicon substrate and penetrating the emitter layer and the base layer; a p-type collector layer provided on the second surface side of the second buffer layer; 6. The semiconductor device according to claim 1, further comprising: (Appendix 7) 7. The semiconductor device according to claim 6, further comprising an n-type semiconductor layer formed deeper than the base layer on the first surface side of the drift layer. (Appendix 8) a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; 8. The semiconductor device according to claim 1, further comprising: (Appendix 9) The semiconductor device described in Appendix 8, further comprising a p-type cathode layer provided on the second surface side of the second buffer layer and aligned with the n-type cathode layer in a direction along the second surface. (Appendix 10) 6. The semiconductor device according to claim 1, wherein the silicon substrate has an IGBT region and a diode region. (Appendix 11) The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; an impurity diffusion layer provided on the first surface side of the anode layer and having an impurity concentration higher than that of the anode layer; 11. The semiconductor device according to claim 10, comprising: (Appendix 12) The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; Equipped with The semiconductor device described in claim 10, wherein the anode layer is in contact with the first electrode. (Appendix 13) The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; a p-type cathode layer provided on the second surface side of the second buffer layer and aligned with the n-type cathode layer in a direction along the second surface; 11. The semiconductor device according to claim 10, comprising: (Appendix 14) The IGBT region is a p-type base layer provided on the first surface side of the drift layer; an n-type emitter layer provided on the first surface side of the base layer; a plurality of gate electrodes provided within a plurality of trenches formed on the first surface of the silicon substrate and penetrating the emitter layer and the base layer; a p-type collector layer provided on the second surface side of the second buffer layer; Equipped with 14. The semiconductor device according to claim 10, wherein some of the gate electrodes are in contact with the first electrode. (Appendix 15) The IGBT region is a p-type base layer provided on the first surface side of the drift layer; an n-type semiconductor layer formed deeper than the base layer on the first surface side of the drift layer; Equipped with The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type semiconductor layer formed on the first surface side of the drift layer and deeper than the anode layer; 14. The semiconductor device according to claim 10, further comprising: (Appendix 16) forming a semiconductor layer on a first surface side of a silicon wafer produced by an MCZ method and having an n-type drift layer; forming a second buffer layer by implanting ions into a second surface of the silicon wafer opposite to the first surface and annealing the second surface; After forming the second buffer layer, protons are injected into a position deeper from the second surface than the second buffer layer; A method for manufacturing a semiconductor device, comprising the steps of: implanting the protons and then annealing the protons to form a first buffer layer. (Appendix 17) 17. The method for manufacturing a semiconductor device according to claim 16, further comprising the steps of: implanting ions into the second surface and annealing the protons, thereby forming at least one of a p-type layer and an n-type layer shallower than the second buffer layer. (Appendix 18) When the protons are implanted, multiple ion implantations are performed, 18. The method for manufacturing a semiconductor device according to claim 16, wherein the multiple ion implantations are performed in order of acceleration energy, and the higher the acceleration energy, the smaller the dose. (Appendix 19) 19. The method for manufacturing a semiconductor device according to any one of claims 16 to 18, wherein the second buffer layer contains arsenic or phosphorus as an impurity. (Appendix 20) 20. The method for manufacturing a semiconductor device according to claim 16, wherein the drift layer contains antimony as an impurity. (Appendix 21) 21. The method for producing a semiconductor device according to any one of claims 16 to 20, wherein the annealing with protons is performed at 375 to 425° C. for 90 minutes or longer. [Explanation of symbols]
[0107] 1 active cell region, 2 interface region, 3 termination region, 4 surface gate wiring portion, 5 first electrode, 6 interlayer film, 7 emitter layer, 8 semiconductor layer, 9 base layer, 10 anode layer, 11 semiconductor layer, 12 main junction, 13 gate oxide film, 14 gate electrode, 15 drift layer, 16 buffer layer, 17 buffer layer, 18 collector layer, 19 cathode layer, 20 cathode layer, 21 second electrode, 22 junction, 23 oxide film, 24 trench, 25 oxide film, 26 polysilicon, 27 high concentration n +layer, 28 high crystal defect density layer, 30 passivation film, 31 p layer, 33 oxide film, 34 n + layer, 35 passivation film, 37 region, 38 vertical structure, 39 gate pad portion, 40 barrier metal, 41 silicide layer, 100 semiconductor device, 101 IGBT, 102, 103 diode
Claims
1. a silicon substrate having a first surface and a second surface opposite to the first surface, the silicon substrate containing oxygen as an impurity; A first electrode provided on the first surface; a second electrode provided on the second surface; Equipped with The silicon substrate is an n-type drift layer having a higher impurity concentration toward the second surface side; an n-type first buffer layer provided on the second surface side of the drift layer and containing protons as impurities; a second buffer layer provided on the second surface side of the first buffer layer; A semiconductor device comprising:
2. 2. The semiconductor device according to claim 1, wherein the impurity concentration of the drift layer continues to increase from a junction between the drift layer and a layer provided on the first surface side of the drift layer to a junction between the drift layer and the first buffer layer.
3. the drift layer contains phosphorus or antimony as an impurity, 3. The semiconductor device according to claim 1, wherein the second buffer layer contains arsenic or phosphorus as an impurity.
4. The oxygen concentration O i is expressed as follows, where Cn is the impurity concentration of the drift layer: 1.00×10 17 ln(C n )-2.84×10 18 ≦O i ≦9.40×10 16 ln(C n )-2.27×10 18 3. The semiconductor device according to claim 1, wherein the above-mentioned condition is satisfied.
5. the impurity concentration of the first buffer layer has a plurality of peaks in a thickness direction of the silicon substrate, 3. The semiconductor device according to claim 1, wherein the impurity concentrations of the plurality of peaks are higher as they approach the second buffer layer.
6. a p-type base layer provided on the first surface side of the drift layer; an n-type emitter layer provided on the first surface side of the base layer; a gate electrode provided within a trench formed on the first surface of the silicon substrate and penetrating the emitter layer and the base layer; a p-type collector layer provided on the second surface side of the second buffer layer; 3. The semiconductor device according to claim 1, further comprising:
7. 7. The semiconductor device according to claim 6, further comprising an n-type semiconductor layer formed deeper than the base layer on the first surface side of the drift layer.
8. a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; 3. The semiconductor device according to claim 1, further comprising:
9. 9. The semiconductor device according to claim 8, further comprising a p-type cathode layer provided on the second surface side of the second buffer layer and aligned with the n-type cathode layer in a direction along the second surface.
10. 3. The semiconductor device according to claim 1, wherein the silicon substrate has an IGBT region and a diode region.
11. The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; an impurity diffusion layer provided on the first surface side of the anode layer and having an impurity concentration higher than that of the anode layer; The semiconductor device according to claim 10 , further comprising:
12. The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; Equipped with The semiconductor device according to claim 10 , wherein the anode layer is in contact with the first electrode.
13. The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type cathode layer provided on the second surface side of the second buffer layer; a p-type cathode layer provided on the second surface side of the second buffer layer and aligned with the n-type cathode layer in a direction along the second surface; The semiconductor device according to claim 10 , further comprising:
14. The IGBT region is a p-type base layer provided on the first surface side of the drift layer; an n-type emitter layer provided on the first surface side of the base layer; a plurality of gate electrodes provided within a plurality of trenches formed on the first surface of the silicon substrate and penetrating the emitter layer and the base layer; a p-type collector layer provided on the second surface side of the second buffer layer; Equipped with 11. The semiconductor device according to claim 10, wherein some of the gate electrodes are in contact with the first electrode.
15. The IGBT region is a p-type base layer provided on the first surface side of the drift layer; an n-type semiconductor layer formed on the first surface side of the drift layer and deeper than the base layer; Equipped with The diode region is a p-type anode layer provided on the first surface side of the drift layer; an n-type semiconductor layer formed on the first surface side of the drift layer and deeper than the anode layer; The semiconductor device according to claim 10 , further comprising:
16. forming a semiconductor layer on a first surface side of a silicon wafer manufactured by an MCZ method and having an n-type drift layer; forming a second buffer layer by implanting ions into a second surface of the silicon wafer opposite to the first surface and annealing the second surface; After forming the second buffer layer, protons are injected into a position deeper from the second surface than the second buffer layer; a step of annealing the protons after the proton implantation to form a first buffer layer;
17. 17. The method for manufacturing a semiconductor device according to claim 16, further comprising the steps of: after the protons are injected, and before the protons are annealed, performing ion implantation on the second surface and annealing to form at least one of a p-type layer and an n-type layer shallower than the second buffer layer.
18. When the protons are implanted, multiple ion implantations are performed, 18. The method for manufacturing a semiconductor device according to claim 16, wherein the plurality of ion implantations are performed in the order of acceleration energy conditions, the higher the acceleration energy, the smaller the dose.
19. 18. The method for manufacturing a semiconductor device according to claim 16, wherein the second buffer layer contains arsenic or phosphorus as an impurity.
20. 18. The method for manufacturing a semiconductor device according to claim 16, wherein the drift layer contains antimony as an impurity.
21. 18. The method for manufacturing a semiconductor device according to claim 16, wherein the annealing with protons is performed at 375 to 425° C. for 90 minutes or longer.
Citation Information
Patent Citations
Semiconductor device and semiconductor device manufacturing method
JP2015130523A
Semiconductor device and method for manufacturing semiconductor device
JP2022062443A
Semiconductor device and manufacturing method thereof
JP2022103589A
Semiconductor device and manufacturing method thereof
JP2022136627A
Semiconductor device, and its manufacturing method
JP2008091853A
Cited By
Semiconductor device
US12652813B2