Method for coproducing epoxy resin and dialkyl carbonate, method for producing epoxy resin composition, method for producing diphenyl carbonate, and method for producing polycarbonate resin
The direct reaction of polycarbonate resin with epihalohydrin and metal alkoxide co-produces epoxy resin and dialkyl carbonate, addressing the limitations of conventional recycling methods by providing efficient production of industrially useful products for polycarbonate resin recycling.
Patent Information
- Application Number
- JP2023062925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional chemical recycling methods for polycarbonate resin yield dihydroxy compounds like bisphenol A and dialkyl carbonate, which are not suitable for industrial use and require further processing steps.
A method involving the direct reaction of polycarbonate resin with epihalohydrin in the presence of metal alkoxide to co-produce epoxy resin and dialkyl carbonate, followed by blending a curing agent to form an epoxy resin composition and converting dialkyl carbonate to diphenyl carbonate for polycarbonate production.
This method efficiently produces industrially useful epoxy resins and dialkyl carbonates, enabling the production of high-quality polycarbonate resins through chemical recycling, reducing the need for additional processing steps.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for simultaneously producing an epoxy resin and a dialkyl carbonate, a method for producing an epoxy resin composition containing the obtained epoxy resin, a method for producing diphenyl carbonate from the obtained dialkyl carbonate, and a method for producing a polycarbonate resin from the obtained diphenyl carbonate. [Background technology]
[0002] Polycarbonate resin has excellent mechanical properties, electrical properties, heat resistance, cold resistance, transparency, etc., and is a material used for various applications. The demand for polycarbonate resin is increasing, and the amount of discarded polycarbonate resin is also increasing accordingly. Therefore, it is becoming important to reuse the discarded polycarbonate resin.
[0003] Under these circumstances, a method has been disclosed in which an aromatic polycarbonate resin is decomposed with an aqueous metal hydroxide solution to obtain an aqueous solution of an alkali metal salt of an aromatic dihydroxy compound, and the aromatic dihydroxy compound is recovered from the aqueous solution (see Patent Document 1).
[0004] Also, a method for recovering dialkyl carbonates in addition to recovering aromatic dihydroxy compounds has been proposed (see Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2006 / 114893 [Patent Document 2] Japanese Patent Application Publication No. 10-259151 [Patent Document 3] JP 2002-212335 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described in the above Patent Documents 1 to 3, in conventional chemical recycling techniques for discarded polycarbonate resins, only dihydroxy compounds such as bisphenol A, or dihydroxy compounds such as bisphenol A and dialkyl carbonates are recovered, and in order to obtain industrially useful chemical products, further processes such as polycondensation and functionalization are required. The present invention provides a new production method that can provide industrially useful epoxy resins and dialkyl carbonates. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors in order to provide the above-mentioned new production method, they have found that an epoxy resin and a dialkyl carbonate can be directly produced by decomposing a polycarbonate resin and an epihalohydrin in the presence of a metal alkoxide. That is, the present invention relates to the following inventions.
[0008] [1] A method for simultaneously producing an epoxy resin and a dialkyl carbonate from a polycarbonate resin, comprising: A method for simultaneously producing an epoxy resin and a dialkyl carbonate, comprising: a reaction step of reacting a polycarbonate resin with an epihalohydrin in the presence of a metal alkoxide to obtain an epoxy resin and a dialkyl carbonate. [2] The method according to [1], wherein the polycarbonate resin is an aromatic polycarbonate resin. A method for the co-production of epoxy resin and dialkyl carbonate. [3] The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to [1] or [2], wherein in the reaction step, 1 to 20 moles of the epihalohydrin are reacted per mole of carbonate groups contained in the polycarbonate resin. [4] The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to any one of [1] to [3], wherein in the reaction step, 1 to 10 moles of the metal alkoxide are used per mole of carbonate groups contained in the polycarbonate resin. [5] The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to any one of [1] to [4], wherein the epoxy resin obtained by the reaction step has an epoxy equivalent of 50 to 10,000 g / eq. [6] A method for producing an epoxy resin composition, comprising a step of blending a curing agent with the epoxy resin obtained by the simultaneous production method according to any one of [1] to [5]. [7] The method for producing an epoxy resin composition according to [6], further comprising mixing 0.1 to 1,000 parts by mass of the curing agent with respect to 100 parts by mass of the epoxy resin. [8] The method for producing an epoxy resin composition according to [6] or [7], wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, mercaptan compounds, cationic polymerization initiators, and organic phosphines. [9] A method for producing a cured epoxy resin product, comprising a step of curing an epoxy resin composition obtained by the production method according to any one of [6] to [8].
[10] A method for producing diphenyl carbonate, comprising a step of reacting the dialkyl carbonate obtained by the simultaneous production method according to any one of [1] to [5] with phenol.
[11] A method for producing a polycarbonate resin, comprising: a step of polymerizing the diphenyl carbonate obtained by the production method according to
[10] through an ester exchange reaction. Effect of the Invention
[0009] The present invention provides a new production method capable of providing an industrially useful epoxy resin and dialkyl carbonate, a method for producing an epoxy resin composition containing the obtained epoxy resin, a method for producing diphenyl carbonate from the obtained dialkyl carbonate, and a method for producing a polycarbonate resin from the obtained diphenyl carbonate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following description, and can be modified as desired without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values before and after the "~" are included.
[0011] One aspect of the present invention is a method for co-producing an epoxy resin and a dialkyl carbonate from a polycarbonate resin, comprising the steps of: The method for simultaneously producing an epoxy resin and a dialkyl carbonate includes a reaction step of reacting a polycarbonate resin with an epihalohydrin in the presence of a metal alkoxide to obtain an epoxy resin and a dialkyl carbonate.
[0012] In this specification, the term "co-production method" means that an epoxy resin and a dialkyl carbonate, which are industrially useful, are recovered together by chemically recycling a polycarbonate resin. This method has a different objective from the method for obtaining a dihydroxy compound such as bisphenol A and a dialkyl carbonate, which have been recovered in the conventional chemical recycling of a polycarbonate resin.
[0013] <Reaction process> The reaction step is a step of reacting a polycarbonate resin with epihalohydrin in the presence of a metal alkoxide to obtain an epoxy resin and a dialkyl carbonate. In this step, by reacting a polycarbonate resin with epihalohydrin in the presence of a metal alkoxide, it is possible to provide an extremely efficient chemical recycling method that can simultaneously obtain an industrially useful epoxy resin and a dialkyl carbonate.
[0014] (Polycarbonate resin) The polycarbonate resin includes a polymer containing a carbonate bond (-OC(=O)-O-). Although there is no limitation on the polycarbonate resin, it is preferable to use an aromatic polycarbonate resin in terms of availability of raw materials and usefulness of the epoxy resin to be produced.
[0015] The aromatic polycarbonate resin may be a polycarbonate resin containing a structural unit derived from an aromatic dihydroxy compound. Examples of the aromatic dihydroxy compound include bisphenols such as bisphenol A, bisphenol C, bisphenol F, bisphenol E, bisphenol Z, bisphenol S, bisphenol AD, bisphenol acetophenone, bisphenol trimethylcyclohexane, bisphenol fluorene, tetramethyl bisphenol A, tetramethyl bisphenol F, tetra-t-butyl bisphenol A, and tetramethyl bisphenol S; biphenol, tetramethyl biphenol, dimethyl biphenol, and tetra-t-butyl bisphenol; Examples of phenolic compounds include biphenols such as tylbiphenol; benzenediols such as hydroquinone, methylhydroquinone, dibutylhydroquinone, resorcin, and methylresorcin (here, "benzenediols" are compounds having one benzene ring, and two hydroxyl groups are directly bonded to the benzene ring); dihydroanthrahydroquinones such as dihydroanthrahydroquinone; dihydroxydiphenyl ethers such as dihydroxydiphenyl ether; thiodiphenols such as thiodiphenol; dihydroxynaphthalenes such as dihydroxynaphthalene; and dihydroxystilbenes such as dihydroxystilbene. The aromatic polycarbonate resin may be a homopolymer using one of these aromatic dihydroxy compounds alone, or a copolymer using two or more of them.
[0016] Among the above-mentioned aromatic dihydroxy compounds, those having bisphenol A or bisphenol C as the main structural unit are particularly preferred from the viewpoints of reactivity, ease of availability of raw materials, and versatility of the resulting epoxy resin. These aromatic polycarbonates may be used alone or in combination of two or more.
[0017] Further, the polycarbonate resin is not limited to a polycarbonate resin alone, and may be a composition containing one or more resins other than polycarbonate, such as polyester resins, polyarylate resins, etc. When a composition containing a resin other than polycarbonate resin is used, the polycarbonate resin composition preferably contains 50% by mass or more of the polycarbonate resin, more preferably 70% by mass or more, and even more preferably 90% by mass or more.
[0018] From the viewpoint of chemical recycling, the raw polycarbonate resin preferably contains used polycarbonate resin (hereinafter sometimes abbreviated as "waste polycarbonate") that is treated as waste plastic. When using waste polycarbonate as the raw polycarbonate resin, it is preferable that the waste polycarbonate is washed, crushed, pulverized, or the like in advance. In addition, when using waste plastics containing polycarbonate resin, It is preferable to remove substances other than polycarbonate resin contained in the plastic. Examples of a method for removing substances other than polycarbonate resin include a method in which waste plastic is dissolved in epihalohydrin and, if necessary, an organic solvent, and then filtered to remove substances other than polycarbonate resin.
[0019] (epihalohydrin) Examples of epihalohydrin include epichlorohydrin, β-methylepichlorohydrin, epibromohydrin, etc. Among these, epichlorohydrin is particularly preferred from the viewpoints of reactivity, availability of raw materials, and versatility of the resulting epoxy resin. These epihalohydrins can be used alone or in combination.
[0020] The amount of epihalohydrin used in the reaction step is not particularly limited, but is preferably 1 to 20 moles, more preferably 3 to 16 moles, and particularly preferably 6 to 14 moles per mole of carbonate bond in the raw material polycarbonate resin. If the amount of epihalohydrin used is equal to or more than the lower limit, it is preferable in that undesirable side reactions such as crosslinking reactions can be suppressed. In addition, if the amount of epihalohydrin used is equal to or less than the upper limit, it is preferable in that industrial production efficiency is improved.
[0021] (Metal alkoxide) The reaction step is carried out in the presence of a metal alkoxide. Examples of the metal in the metal alkoxide include alkali metals such as lithium, sodium, potassium, rubidium, and cesium, and alkaline earth metals such as magnesium, calcium, strontium, and barium. Examples of the alkoxide include methoxide, ethoxide, propoxide, and glycoxide. The alcohol of the metal alkoxide is not particularly limited, and may be a monoalcohol or a polyol such as a glycol-based compound, but is preferably a monoalcohol. Examples of the monoalcohol include methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, and t-butanol. Examples of the polyol include ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, cyclohexanedimethanol, and glycerin. The glycol compound is a compound in which one hydroxyl group is bonded to each of two carbon atoms of an alkyl group having two or more carbon atoms, and examples of the glycol compound include ethylene glycol and propylene glycol. Metal alkoxides may be used alone or in combination of two or more. Among these, sodium methoxide is preferred from the viewpoint of industrial availability.
[0022] In the reaction step, the metal alkoxide is continuously supplied within the reaction time, and is preferably 1 to 10 moles, more preferably 2.4 to 8 moles, and particularly preferably 3 to 6 moles per mole of carbonate group contained in the polycarbonate resin. When the amount of metal alkoxide used is equal to or more than the above lower limit, the reaction rate of the decomposition reaction and the epoxy group formation reaction can be sufficiently ensured, which is preferable from the viewpoint of the quality and production efficiency of the obtained epoxy resin. In addition, when the amount is equal to or less than the above upper limit, it is preferable from the viewpoint of suppressing excessive reaction and side reactions such as crosslinking reaction.
[0023] In the reaction step, the reaction temperature is preferably 30 to 100° C. in order to ensure a sufficient reaction rate, and the reaction time is preferably 10 to 360 minutes, more preferably 20 to 300 minutes, and particularly preferably 30 to 240 minutes in order to allow the reaction to proceed sufficiently.
[0024] After the reaction is completed, a post-treatment step may be carried out as necessary. As a post-treatment step, insoluble by-product salts are filtered off. After removing the unreacted epihalohydrin by distillation under reduced pressure, the desired epoxy resin and dialkyl carbonate are obtained.
[0025] In addition, in the reaction step, catalysts such as quaternary ammonium salts such as tetramethylammonium chloride and tetraethylammonium bromide; tertiary amines such as benzyldimethylamine and 2,4,6-tris(dimethylaminomethyl)phenol; imidazoles such as 2-ethyl-4-methylimidazole and 2-phenylimidazole; phosphonium salts such as ethyltriphenylphosphonium iodide; and phosphines such as triphenylphosphine may be used.
[0026] In addition, in the reaction step, inert organic solvents such as alcohols such as ethanol and isopropanol; glycols such as ethylene glycol, diethylene glycol, propylene glycol, and polyethylene glycol; ketones such as acetone and methyl ethyl ketone; ethers such as dioxane and ethylene glycol dimethyl ether; glycol ethers such as propylene glycol monomethyl ether; aprotic polar solvents such as dimethyl sulfoxide and dimethylformamide; and aromatic hydrocarbon solvents such as toluene and xylene may be used.
[0027] Furthermore, if the epoxy resin obtained as above has too much saponifiable halogen, it can be reprocessed to obtain a purified epoxy resin with a sufficiently reduced amount of saponifiable halogen. That is, the crude epoxy resin obtained by the reaction is redissolved in an inert organic solvent such as isopropyl alcohol, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, dioxane, methoxypropanol, or dimethyl sulfoxide, and an alkali metal hydroxide or metal alkoxide is added as a solid or aqueous solution to carry out a ring-closing reaction at a temperature of about 30 to 120°C, more preferably 40 to 110°C, and even more preferably 50 to 100°C for 0.1 to 8 hours, more preferably 0.3 to 7 hours, and even more preferably 0.5 to 6 hours. Then, the excess alkali metal hydroxide or metal alkoxide and secondary salts are removed by a method such as water washing, and the organic solvent is distilled off under reduced pressure and / or steam distillation is carried out to obtain an epoxy resin with a reduced amount of hydrolyzable halogen. If the reaction temperature is too low or the reaction time is too short, the ring-closing reaction may not proceed, whereas if the reaction temperature is too high or the reaction time is too long, the reaction may proceed, but may result in problems such as high molecular weight, high epoxy equivalent, and high viscosity.
[0028] (Obtained epoxy resin) The epoxy equivalent of the epoxy resin obtained through the reaction step is preferably 50 to 10,000 g / eq, more preferably 100 to 5,000 g / eq, and particularly preferably 150 to 3,000 g / eq, as measured according to JIS K7236. When the epoxy equivalent of the obtained epoxy resin is within the above range, the crosslink density increases when cured with various curing agents, and a cured product having excellent chemical resistance and the like can be obtained.
[0029] (Obtained dialkyl carbonate) The dialkyl carbonate obtained through the reaction process can be used as a raw material for producing polycarbonate by the melting method. It is preferable that the dialkyl carbonate is recovered by distillation. Therefore, the alkyl of the dialkyl carbonate is preferably an alkyl having 10 or less carbon atoms, more preferably an alkyl having 6 or less carbon atoms, and particularly preferably an alkyl having 4 or less carbon atoms. Specifically, dimethyl carbonate, diethyl carbonate, and dibutyl carbonate are particularly preferable. The dialkyl carbonate thus obtained is preferably converted to diphenyl carbonate by transesterification with phenol and used as a raw material for the production of polycarbonate by a melting method. The diphenyl carbonate can be produced by a known method for producing diphenyl carbonate from dialkyl carbonate (for example, JP-A-3-291257). For example, diphenyl carbonate can be produced by a method in which dialkyl carbonate and phenol are used as raw materials, an ester exchange reaction is carried out to obtain an alkylphenyl carbonate, and the alkylphenyl carbonate is then subjected to a disproportionation reaction to obtain diphenyl carbonate. As a catalyst for this ester exchange reaction, a known catalyst used for producing diphenyl carbonate can be used. For example, an organic titanium catalyst such as tetraphenoxytitanium can be used.
[0030] <Epoxy resin composition> The epoxy resin obtained above can be mixed with a curing agent to produce an epoxy resin composition. In addition, other epoxy compounds, curing accelerators, other components, etc. can be appropriately mixed into the epoxy resin composition as necessary.
[0031] (hardening agent) A curing agent is a substance that contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound. In this specification, even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound.
[0032] The amount of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 100 parts by mass or less, further preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, based on 100 parts by mass of the epoxy resin.
[0033] When the epoxy resin composition contains an epoxy compound other than the above epoxy resin, the amount of the curing agent is preferably 0.1 to 1000 parts by mass, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, based on 100 parts by mass of the total epoxy resin components as solids. The more preferable amount of the curing agent is as described below according to the type of the curing agent.
[0034] In this specification, "solid content" means the components excluding the solvent, and includes not only solid epoxy compounds but also semi-solid and viscous liquid substances. Moreover, "total epoxy resin components" means the sum of the above epoxy resins and other epoxy resins described below.
[0035] In the method for producing an epoxy resin composition, it is preferable to use, as the curing agent, at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, cationic polymerization initiators, and organic phosphines.
[0036] Examples of polyfunctional phenols include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; catechol, resorcin, hydroquinone, and dihydroxynaphthalenes; and compounds in which the hydrogen atoms bonded to the aromatic rings of these compounds are substituted with non-interfering substituents such as halogen groups, alkyl groups, aryl groups, ether groups, ester groups, and organic substituents containing hetero elements such as sulfur, phosphorus, and silicon. Further examples include novolaks and resols which are polycondensates of these phenols, or monofunctional phenols such as phenol, cresol, and alkylphenols with aldehydes.
[0037] Examples of polyisocyanate compounds include tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, Examples of the polyisocyanate compound include xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, lysine triisocyanate, etc. Further examples include polyisocyanate compounds obtained by reacting these polyisocyanate compounds with compounds having at least two active hydrogen atoms such as amino groups, hydroxyl groups, carboxyl groups, water, etc., and trimers to pentamers of the above polyisocyanate compounds.
[0038] Examples of the amine compounds include aliphatic primary, secondary, and tertiary amines, aromatic primary, secondary, and tertiary amines, cyclic amines, guanidines, and urea derivatives. Specific examples include triethylenetetramine, diaminodiphenylmethane, diaminodiphenyl ether, metaxylenediamine, dicyandiamide, 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.
[0039] Examples of the acid anhydride compound include phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and condensates of maleic anhydride and unsaturated compounds.
[0040] Examples of the imidazole-based compound include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, benzimidazole, etc. Although the imidazole-based compound also functions as a curing accelerator, which will be described later, in the present invention it is classified as a curing agent.
[0041] Examples of the amide-based compounds include dicyandiamide and its derivatives, polyamide resins, and the like.
[0042] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. - , BF4 - , AsF6 - , PF6 - , CF3SO3 2- , B(C6F5)4 - and an aromatic cation component containing an atom of iodine, sulfur, nitrogen, phosphorus, etc. Diaryliodonium salts and triarylsulfonium salts are particularly preferred.
[0043] Examples of organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine. Examples of phosphonium salts include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate. Examples of tetraphenylboron salts include 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate.
[0044] The above curing agents may be used either individually or in combination of two or more of the same or different types.
[0045] When polyfunctional phenols, amine compounds, or acid anhydride compounds are used as the curing agent, it is preferable to use them in such a manner that the equivalent ratio of the functional groups in the curing agent (hydroxyl groups of polyfunctional phenols, amino groups of amine compounds, or acid anhydride groups of acid anhydride compounds) to the total epoxy groups in the epoxy resin composition is in the range of 0.8 to 1.5. When polyisocyanate compounds are used, it is preferable to use them in such a range that the equivalent ratio of the number of isocyanate groups in the polyisocyanate compounds to the number of hydroxyl groups in the epoxy resin composition is in the range of 1:0.01 to 1:1.5. When imidazole compounds are used, it is preferable to use them in the range of 0.5 to 10 parts by mass with respect to 100 parts by mass of the total epoxy resin components as solid contents in the epoxy resin composition. When amide compounds are used, it is preferable to use them in the range of 0.1 to 20% by mass with respect to the total amount of the total epoxy resin components and amide compounds as solid contents in the epoxy resin composition. When a cationic polymerization initiator is used, it is preferably used in the range of 0.01 to 15 parts by mass based on 100 parts by mass of all epoxy resin components as solid contents in the epoxy resin composition.When an organic phosphine is used, it is preferably used in the range of 0.1 to 20% by mass based on the total amount of all epoxy resin components as solid contents in the epoxy resin composition and the organic phosphines.
[0046] In addition to the curing agents listed above, the epoxy resin composition may also contain, as a curing agent, for example, a mercaptan compound, an organic acid dihydrazide, a boron halide amine complex, etc. These curing agents may be used alone or in combination of two or more.
[0047] (Other epoxy resins) In the method for producing an epoxy resin composition, epoxy resins other than the above-mentioned epoxy resins (sometimes referred to as "other epoxy resins" in this specification) can be used. Examples of the other epoxy resins include glycidyl ether type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, tetrabromobisphenol A type epoxy resins, and other polyfunctional phenol type epoxy resins, epoxy resins obtained by hydrogenating the aromatic rings of the above-mentioned aromatic epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, linear aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. The above-mentioned other epoxy resins may be used alone or in combination of two or more.
[0048] When the epoxy resin composition contains the above-mentioned epoxy resin and other epoxy resins, the ratio of the other epoxy resins in the total epoxy resin components as solids in the epoxy resin composition is preferably 1% by mass or more, more preferably 5% by mass or more, and on the other hand, is preferably 99% by mass or less, more preferably 95% by mass or less. By having the ratio of the other epoxy resins be equal to or more than the lower limit, the physical property improvement effect by blending the other epoxy resins can be sufficiently obtained. On the other hand, by having the ratio of the other epoxy resins be equal to or less than the upper limit, the effect of chemical recyclability by the epoxy resins can be sufficiently obtained.
[0049] The epoxy resin composition may be diluted by blending a solvent in order to appropriately adjust the viscosity of the epoxy resin composition when handling it, such as when forming a coating film. The solvent is used to ensure the handleability and workability in molding the epoxy resin composition, and there is no particular limit to the amount used. As described above, in the present invention, the terms "solvent" and "solvent" are used separately depending on the form of use, but the same or different types of solvents may be used independently.
[0050] As the solvent, one or more of the organic solvents exemplified as reaction solvents used in the production of epoxy resins can be used.
[0051] The epoxy resin composition may contain other components in addition to the components listed above. Examples of other components include curing accelerators (excluding those corresponding to the above-mentioned curing agents), coupling agents, flame retardants, antioxidants, light stabilizers, plasticizers, reactive diluents, pigments, inorganic fillers, organic fillers, etc. The other components listed above may be used in appropriate combinations depending on the desired physical properties of the epoxy resin composition.
[0052] [Cured product] The epoxy resin composition can be cured to obtain a cured product. The term "curing" used here means intentionally curing an epoxy compound by heat and / or light, and the degree of curing can be controlled depending on the desired physical properties and applications.
[0053] The method of curing the epoxy resin composition to produce a cured product varies depending on the components and amounts of the components in the epoxy resin composition and the form of the compounded product, but typically includes heating conditions of 5 seconds to 180 minutes at 50 to 200° C. This heating is preferably performed in two stages, consisting of a primary heating at 50 to 160° C. for 5 seconds to 30 minutes and a secondary heating at 90 to 200° C., which is 40 to 120° C. higher than the primary heating temperature, for 1 minute to 150 minutes, in order to reduce poor curing.
[0054] When producing a cured product as a semi-cured product, the curing reaction of the epoxy resin composition may be allowed to proceed to an extent that allows the shape to be maintained by heating, etc. When the epoxy resin composition contains a solvent, most of the solvent is removed by techniques such as heating, reducing pressure, and air drying, but 5% by mass or less of the solvent may remain in the semi-cured product.
[0055] The dialkyl carbonate obtained together with the epoxy resin by the above method can be reacted with phenol to give diphenyl carbonate, which can be polymerized by transesterification to give polycarbonate resin. The production of the diphenyl carbonate and the production of the polycarbonate resin can be carried out according to a conventional method. EXAMPLES
[0056] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples. Note that the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples. The epoxy equivalent of the epoxy resin obtained in the following examples was measured in accordance with JIS K 7236.
[0057] [analysis] The production of the epoxy resin was confirmed by high performance liquid chromatography according to the following procedure and conditions. Equipment: JASCO RHPLC, JASCO 03150-3M Unifinepak C18 3μm 150mm×3.0mmID Method: Gradient method ·Analysis temperature: 40℃ ·Eluent composition: Solution A: Acetonitrile Solution B: Distilled water At 0 min of analysis time, the ratio of liquid A: liquid B was 30:70 (volume ratio, the same applies below), and gradually changed to liquid A: liquid B = 100:0 from 0 to 25 min of analysis time. ·Flow rate: 0.40mL / min Detection wavelength: 280nm
[0058] The production and quantification of dialkyl carbonate were carried out by gas chromatography according to the following procedure and conditions. Equipment: AGILENT TECHNOLOGIES 7820GC SYSTEM AGILENT HP-1 30m×0.25mm 0.25μm Detection method: FID Vaporizer temperature: 230℃ Detector temperature: 300℃ From 0 to 5 minutes of analysis time, the column temperature was kept at 50°C, from 5 to 30 minutes of analysis time, the column temperature was gradually increased to 280°C, and from 30 to 40 minutes of analysis time, the column temperature was maintained at 280°C.
[0059] [Method of manufacturing tetraphenoxytitanium] (Reference example 1) 200 parts by weight of phenol and 100 parts by weight of toluene were charged into a 500 mL three-neck flask equipped with a receiver and a distillation tube, and the flask was replaced with nitrogen flow. The flask was immersed in a 100 ° C oil bath to obtain a homogeneous solution. 57 parts by weight of tetraisopropoxytitanium were added thereto. When the internal temperature of the bottom of the flask was maintained at 100 ° C, distillation of the generated isopropyl alcohol began. After that, the internal temperature was gradually raised to 116 ° C, and 80 parts by weight of a distillate, which is a mixture of isopropyl alcohol and toluene, was distilled. 50 parts by weight of hexane was added to the obtained residue, and the mixture was cooled to room temperature and crystallized. The precipitated red crystals were obtained by filtration and dried in a rotary evaporator equipped with an oil bath at an oil bath temperature of 140 ° C and a pressure of 50 Torr to obtain 60 parts by weight of tetraphenoxytitanium.
[0060] [Production and evaluation of epoxy resin] Example 1 A separable flask reactor equipped with a thermometer, a dropping funnel, a stirrer, a nitrogen inlet tube, and a cooling tube was charged with 75 parts by weight of 7027J (Mitsubishi Chemical's bisphenol A type polycarbonate resin) and 327 parts by weight of epichlorohydrin (12 moles per mole of carbonate bond in polycarbonate), and heated to 100°C to dissolve the polycarbonate resin, and then cooled to about 40°C under a nitrogen gas atmosphere. Then, 136 parts by weight of a 28% sodium methoxide methanol solution (sodium methoxide was supplied so that the amount of sodium methoxide was 2.4 moles per mole of carbonate bond in polycarbonate) was continuously dropped while the temperature was raised to 65°C, and the reaction was carried out for 120 minutes. Then, 230 parts by weight of water was added, and the water layer separated from the oil and water was separated to remove salts generated by the reaction from the resin solution, residual sodium methoxide, etc., and the reaction was stopped.
[0061] The temperature of the reaction solution obtained was gradually raised, and the pressure in the system was reduced. The system was held at 150°C and 5mmHg for 30 minutes, and methanol, excess epichlorohydrin, and dimethyl carbonate were completely distilled out of the system. The amount of the distillate was 287 parts by mass. After that, the system was returned to normal pressure while nitrogen was sealed in the system, and 150 parts by weight of methyl isobutyl ketone was added to obtain a methyl isobutyl ketone solution of crude resin. 100 parts by weight of water was added to this solution to separate the aqueous layer, and then the aqueous layer removed with 100 parts by weight of water was repeatedly washed with water several times until it became neutral, and a methyl isobutyl ketone solution of epoxy resin was obtained. The methyl isobutyl ketone was distilled out of this solution under heating and reduced pressure, and the system was held at 150°C and 5mmHg for 30 minutes to completely remove the methyl isobutyl ketone, and a liquid epoxy resin was obtained. The epoxy equivalent of the obtained epoxy resin was 198g / eq.
[0062] Example 2 A portion of the distillate obtained in Example 1 was extracted and analyzed by gas chromatography, which revealed that it was 10% by mass of methanol, 5% by mass of dimethyl carbonate, and 69% by mass of epichlorohydrin (the remaining components were estimated to be water). In order to remove water from the distillate, 287 parts by weight of the distillate and 100 parts by weight of molecular sieves 3A (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were fed into an eggplant-shaped flask and allowed to stand overnight. Thereafter, 205 parts by weight of the supernatant were decanted and placed in a distillation apparatus equipped with a thermometer, a distillation tube, a stirrer, an oil bath, and a pressure regulator. The pressure was gradually reduced from normal pressure to 20 kPa to distill off a mixture of dimethyl carbonate and methanol, and 30 parts by weight of fraction A was obtained.
[0063] The obtained fraction A (30 parts by weight) and anisole (100 parts by weight) were placed in a distillation apparatus equipped with a thermometer, a distillation tube, a stirrer, an oil bath, and a pressure regulator. The internal temperature was set to 80° C., and 20 parts by weight of fraction B, mainly composed of methanol, was distilled off to obtain 110 parts by weight of bottom residue. The bottom residue was extracted and subjected to gas chromatography, revealing that it contained 8% by mass (110 parts by weight×8% by mass=9 parts by weight) of dimethyl carbonate. To 110 parts by weight of the resulting bottoms, 100 parts by weight of phenol and 1 part by weight of the tetraphenoxytitanium obtained in Reference Example 1 were added. Thereafter, the internal temperature was raised to 100° C., and methanol was distilled off. Next, the internal temperature was lowered from 100° C. to 200° C., and the pressure was gradually lowered from normal pressure to 10 kPa, whereby phenol and dimethyl carbonate were distilled off, and then 0.5 parts by weight of diphenyl carbonate was distilled off.
[0064] Example 3 In a 45 mL glass reaction vessel equipped with a stirrer and a distillation tube, 10 parts by weight of bisphenol A (manufactured by Mitsubishi Chemical Group), 10 parts by weight of the diphenyl carbonate obtained in Example 2, and 18×10 parts of a 400 ppm cesium carbonate aqueous solution were added. -6 The glass reaction vessel was depressurized to about 100 Pa, and then the pressure was returned to atmospheric pressure with nitrogen. This operation was repeated three times to replace the inside of the reaction vessel with nitrogen. Thereafter, the reaction vessel was immersed in an oil bath at 220° C. to dissolve the contents. The stirrer rotation speed was set to 100 revolutions per minute, and the pressure in the reaction tank was reduced from 101.3 kPa to 13.3 kPa absolute pressure over a period of 40 minutes while distilling off phenol produced as a by-product in the oligomerization reaction of bisphenol A and diphenyl carbonate in the reaction tank.
[0065] The pressure inside the reaction vessel was then maintained at 13.3 kPa, and the transesterification reaction was carried out for 80 minutes while further distilling off phenol. Thereafter, the temperature outside the reaction vessel was raised to 290° C., and the pressure inside the reaction vessel was reduced from 13.3 kPa to 399 Pa in absolute pressure over a period of 40 minutes, and the distilled phenol was removed outside the system. Thereafter, the absolute pressure of the reaction vessel was reduced to 30 Pa, and the polycondensation reaction was carried out. When the agitator of the reaction vessel reached a predetermined stirring power, the polycondensation reaction was terminated. The time from raising the temperature to 290°C to completing the polymerization was 120 minutes. Next, the reaction vessel was restored to an absolute pressure of 101.3 kPa with nitrogen, and then the pressure was increased to a gauge pressure of 0.2 MPa, and the polycarbonate resin was extracted from the reaction vessel to obtain a polycarbonate resin.
Claims
1. A method for co-producing epoxy resin and dialkyl carbonate from polycarbonate resin, comprising: A method for simultaneously producing an epoxy resin and a dialkyl carbonate, comprising: a reaction step of reacting a polycarbonate resin with an epihalohydrin in the presence of a metal alkoxide to obtain an epoxy resin and a dialkyl carbonate.
2. 2. The method for co-producing epoxy resin and dialkyl carbonate according to claim 1, wherein the polycarbonate resin is an aromatic polycarbonate resin.
3. 2. The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to claim 1, wherein in the reaction step, 1 to 20 moles of the epihalohydrin are reacted per mole of carbonate groups contained in the polycarbonate resin.
4. 2. The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to claim 1, wherein the reaction step uses 1 to 10 moles of the metal alkoxide per mole of carbonate groups contained in the polycarbonate resin.
5. The method for simultaneously producing an epoxy resin and a dialkyl carbonate according to claim 1, wherein the epoxy resin obtained by the reaction step has an epoxy equivalent of 50 to 10,000 g / eq.
6. A method for producing an epoxy resin composition, comprising: blending a curing agent with the epoxy resin obtained by the simultaneous production method according to any one of claims 1 to 5.
7. The method for producing an epoxy resin composition according to claim 6, wherein 0.1 to 1000 parts by mass of the curing agent is mixed with 100 parts by mass of the epoxy resin.
8. 7. The method for producing an epoxy resin composition according to claim 6, wherein the curing agent is at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, mercaptan compounds, cationic polymerization initiators and organic phosphines.
9. A method for producing a cured epoxy resin product, comprising: a step of curing the epoxy resin composition obtained by the method according to claim 6.
10. A method for producing diphenyl carbonate, comprising the step of reacting the dialkyl carbonate obtained by the co-production method according to any one of claims 1 to 5 with phenol.
11. A method for producing a polycarbonate resin, comprising: a step of polymerizing the diphenyl carbonate obtained by the production method according to claim 10 through a transesterification reaction.
Citation Information
Patent Citations
Production of carbonic acid dialkyl ester and bisphenol from polycarbonate
JP1998259151A
Method for useful substance recovery from waste plastic consisting essentially of polycarbonate resin
JP2002212335A
Method for producing aqueous solution of alkali metal salt of aromatic dihydroxy compound from waste aromatic polycarbonate
WO2006114893A1
Cited By
Method for producing epoxy resin, method for producing epoxy resin composition, and method for producing cured product