Operation method of electric furnace

By introducing resin-coated iron materials into an electric furnace with controlled ratios and timings, the nitrogen concentration in molten steel is reduced, addressing odor issues and achieving efficient denitrification.

JP2024149195APending Publication Date: 2024-10-18NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023062926
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methods for reducing nitrogen concentration in molten steel in electric furnaces, such as blowing gas into the molten steel, require large-scale equipment and can generate unpleasant odors due to the thermal decomposition of synthetic resin-coated materials.

Method used

A method for operating an electric furnace that involves introducing synthetic resin-coated iron materials into the furnace body while using a conveying device to preheat them with exhaust gas, controlling the ratio of resin-coated to resin-free materials and their feeding speeds to minimize odor generation and nitrogen absorption.

Benefits of technology

Reduces nitrogen concentration in molten steel during tapping while effectively suppressing the generation of off-flavors and odors, utilizing a controlled mixture and timing of resin-coated and resin-free iron materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149195000001_ABST
    Figure 2024149195000001_ABST
Patent Text Reader

Abstract

To provide an operation method of an electric furnace capable of reducing the nitrogen concentration of molten steel at the time of tapping while suppressing the generation of an offensive odor.SOLUTION: An operation method of an electric furnace 1 comprises charging a synthetic resin-adhered iron material A into a furnace together with a synthetic non-resin-adhered iron material N as an iron source 16 by a conveying device 15. The synthetic resin-adhered iron material A is conveyed into the furnace 10 with the synthetic non-resin-adhered iron material N placed thereon. A ratio WA / (WA+WN) of an input weight WA of the synthetic resin-adhered iron material A to the total value WA+WN of the input weight WA of the synthetic resin-adhered iron material A and an input weight WN of the synthetic non-resin-adhered iron material N is 0.05 to 0.25. A ratio SA / (SA+SN) of a charging speed SA during charging the synthetic resin-adhered iron material A to the total value SA+SN of the charging speed SA during charging the synthetic resin-adhered iron material A and a charging speed SN during charging the synthetic non-resin-adhered iron material N is 0.25 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for operating an electric furnace in which ferrous material is melted by arcs from electrodes to produce molten steel, and more particularly to a method for removing nitrogen from molten steel. [Background technology]

[0002] In general, in electric arc furnaces, the contact between the arc and the atmosphere causes a nitrogen absorption reaction in the molten steel, which increases the nitrogen concentration in the molten steel. Therefore, in order to remove the nitrogen from the molten steel, the injection of a large amount of gas into the molten steel by bottom injection has been considered. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2-217788 Summary of the Invention [Problem to be solved by the invention]

[0004] In order to inject a large amount of gas into molten steel, it is necessary to introduce a large-scale facility. The inventors have conducted various studies to determine whether it is possible to remove nitrogen from molten steel during the operation of an electric furnace by a method other than injecting gas into molten steel. As a result, they have come to the idea that when iron materials with synthetic resins attached thereto, such as painted steel sheets and / or steel sheets with plastic materials, are charged into the body of an electric furnace, the nitrogen in the molten steel can be removed by the large amount of gas generated by the thermal decomposition of the synthetic resins (coatings and / or plastic materials) due to the heat of the molten steel in the furnace.

[0005] However, as described in the above-mentioned Patent Document 1, there is a concern that the use of synthetic resin-coated iron materials in a Consteel-type electric furnace may result in the generation of an unpleasant odor.

[0006] The present invention has been made to solve the above-mentioned problems, and one of its objects is to provide a method for operating an electric furnace that can reduce the nitrogen concentration of molten steel at the time of tapping while suppressing the generation of nasty odors. [Means for solving the problem]

[0007] In one embodiment, the method of operating an electric furnace according to the present invention is a method of operating an electric furnace in which iron materials are continuously fed into the furnace body of a Consteel type electric furnace by a conveying device, and the iron materials are melted by an arc from an electrode to produce molten steel. The electric furnace is configured to introduce exhaust gas from within the furnace body into the conveying device to heat the iron materials by the exhaust gas, and includes feeding synthetic resin-adhered iron materials (A) together with synthetic resin-free iron materials (N) into the furnace body by the conveying device, and the synthetic resin-adhered iron materials (A) are transported into the furnace body with the synthetic resin-free iron materials (N) placed on top of them, and the weight (W) of the synthetic resin-adhered iron materials (A) fed is determined by the following formula: A ) and the weight of the synthetic resin-free iron material (N) (W N ) and the sum (W A +W N The weight of synthetic resin-coated iron material (A) added to the A ) ratio (W A / (W A +W N )) is set to be 0.05 or more and 0.25 or less, and the feeding speed (S A ) and the feeding speed (S N ) and the sum (S A +S N ) during feeding of the synthetic resin-coated iron material (A) (S A ) ratio (S A / (S A +S N )) is set to be less than 0.25. Effect of the Invention

[0008] According to one embodiment of the method for operating an electric furnace of the present invention, the synthetic resin-adhering iron material (A) is transported into the furnace body with the synthetic resin-free iron material (N) placed on top of it, and the input weight (WA ) and the weight of the synthetic resin-free iron material (N) (W N ) and the sum (W A +W N The weight of synthetic resin-coated iron material (A) added to the A ) ratio (W A / (W A +W N )) is set to be 0.05 or more and 0.25 or less, and the feeding speed (S A ) and the feeding speed (S N ) and the sum (S A +S N ) during feeding of the synthetic resin-coated iron material (A) (S A ) ratio (S A / (S A +S N ) is set to 0.25 or less, it is possible to reduce the nitrogen concentration of the molten steel at the time of tapping while suppressing the generation of unpleasant odors. [Brief description of the drawings]

[0009] [Figure 1] 1 is an explanatory diagram showing an example of an electric furnace for carrying out a method for operating an electric furnace according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described with reference to the drawings. The present invention is not limited to each embodiment, and the components can be modified without departing from the gist of the present invention. In addition, various inventions can be formed by appropriately combining multiple components disclosed in each embodiment. For example, some components may be deleted from all the components shown in the embodiments. Furthermore, components of different embodiments may be appropriately combined.

[0011] Fig. 1 is an explanatory diagram showing an example of an electric furnace 1 for carrying out a method for operating an electric furnace 1 according to an embodiment of the present invention. The method for operating an electric furnace 1 according to an embodiment of the present invention can be carried out in the electric furnace 1 shown in Fig. 1. The configuration of this electric furnace 1 is merely an example for the purpose of explanation, and does not limit the configuration of the electric furnace 1 used in the method for operating an electric furnace 1 according to the present embodiment.

[0012] The electric furnace 1 includes a furnace body 10, a conveying device 15, an electrode 20, an oxygen blowing nozzle 30, and a carbonaceous material blowing nozzle 35.

[0013] The furnace body 10 includes a furnace bottom 11, a side wall 12, and a furnace cover 13. Shaped and irregular furnace body refractories (not shown) are arranged on at least a portion of the furnace bottom 11 and the side wall 12. A portion of the furnace bottom 11 and the side wall 12 may be water-cooled.

[0014] The conveying device 15 is for conveying the iron material 16 toward the furnace body 10. The electric furnace 1 of this embodiment is called a Consteel type, and is configured so that the iron material 16 is continuously fed into the furnace body 10 by the conveying device 15. The electric furnace 1 is also configured so that the exhaust gas 10a in the furnace body 10 is introduced into the conveying device 15 to heat (preheat) the iron material 16 with the exhaust gas 10a. That is, the conveying device 15 also serves as a discharge passage for the exhaust gas 10a. Although not shown in detail, the conveying device 15 has an exterior body forming a sealed passage and a conveyor arranged in the lower part of the exterior body. The iron material 16 is placed on the conveyor and conveyed toward the furnace body 10. The upper part of the exterior body forms a discharge passage for the exhaust gas 10a, and while the iron material 16 is conveyed toward the furnace body 10, heat is exchanged between the exhaust gas 10a in the upper part of the exterior body and the iron material 16 in the lower part of the exterior body, so that the iron material 16 is preheated. By preheating the iron material 16, the unit electricity consumption for melting the iron material 16 can be reduced.

[0015] Auxiliary materials can be further added to the inside of the furnace body 10. The auxiliary materials may include, but are not limited to, CaO, SiO2, and MgO. The auxiliary materials may be added through an inlet (not shown) provided in the furnace cover 13.

[0016] The electrodes 20 generate an arc between the iron material 16 charged into the furnace bottom 11 and molten steel M obtained by melting the iron material 16. Although FIG. 1 illustrates a case in which three electrodes 20 are used, the number of electrodes 20 is arbitrary. The electric furnace 1 may be of an AC type or a DC type. In the electric furnace 1, the iron material 16 is melted by the arc from the electrodes 20 to produce molten steel M.

[0017] The oxygen blowing nozzle 30 is for blowing oxygen into the furnace body 10. The carbonaceous material blowing nozzle 35 is for blowing carbonaceous material into the furnace body 10. The carbonaceous material may be blown using an inert gas such as Ar or CO2 as a carrier gas. Each of the oxygen blowing nozzle 30 and the carbonaceous material blowing nozzle 35 may be in contact with the slag S during melting, or may not be in contact with the slag S. In FIG. 1, one oxygen blowing nozzle 30 and one carbonaceous material blowing nozzle 35 are illustrated, but a plurality of oxygen blowing nozzles 30 and a plurality of carbonaceous material blowing nozzles 35 may be provided.

[0018] An electric furnace operation has a melting period and a heat-up period. During the melting period, the iron material 16 charged into the furnace body 10 is melted by an arc. During the heat-up period, the molten steel M composed of the molten iron material 16 is heated to a predetermined temperature. The iron material 16 is continuously charged into the furnace body 10 from the beginning to the end of the melting period. After the molten steel M is heated to a predetermined temperature in the heat-up period, the furnace body 10 is tilted and the steel is tapped. The period from the charging of the iron material 16 to the tapping is called 1Ch (charge). Tapping is completed with some of the molten steel M remaining, and charging of the iron material 16 begins at the same time as the start of current flow to the electrodes 20 in the next Ch.

[0019] Here, the present inventors have investigated various methods other than the method of injecting gas into the molten steel M to lower the nitrogen concentration (hereinafter, sometimes expressed as [%N], where the nitrogen concentration is expressed in mass %) of the molten steel M at the time of tapping, and have decided to adopt a method of charging synthetic resin into the electric furnace 1. It is believed that if synthetic resin is thermally decomposed in the molten steel M at about 1600°C to 1700°C, the generated gas bubbles will take in nitrogen in the molten steel M while rising in the molten steel M and release it into the gas phase on the surface of the molten steel M, that is, denitrification will proceed.

[0020] Various synthetic resins are conceivable, but from the viewpoint of thermally decomposing the synthetic resin in the molten steel M, a method was adopted in which the synthetic resin-adhered iron material A is introduced into the furnace body 10 as the iron material 16 by the transport device 15. The synthetic resin-adhered iron material A is a steel plate having a layer or member containing synthetic resin attached thereto. For example, the synthetic resin-adhered iron material A can be a painted steel plate and / or a steel plate with a plastic material. The painted steel plate is a steel plate having a coating film at least partially containing synthetic resin. The painted steel plate can be scrap, such as an automobile steel plate and / or a steel plate for home appliances. The plastic material-adhered steel plate is a steel plate to which a plastic material (part) as a synthetic resin is attached or incorporated. The plastic material-adhered steel plate can be scrap, such as a machine equipment. The synthetic resin-adhered iron material A may have a certain size, or may be fragmented scrap. The synthetic resin-adhered iron material A may be fragmented to a size that can be transported by the transport device 15 and can be covered by the synthetic resin-free iron material N as described later.

[0021] As described above, if synthetic resin is thermally decomposed in molten steel M, it is presumed that the gas bubbles generated by the thermal decomposition will take in nitrogen in the molten steel M while rising in the molten steel M, and this nitrogen will be released into the gas phase above the molten steel M, thereby promoting denitrification of the molten steel M. In order to add synthetic resin to the molten steel M, it is sufficient to add synthetic resin attached to iron material. That is, synthetic resin can be added to the molten steel M by adding painted steel sheets that can be obtained from scrap of home appliances such as refrigerators and automobiles, or steel sheets with plastics that can be obtained from scrap of machinery and equipment.

[0022] The amount of synthetic resin attached to (contained in) the synthetic resin-coated iron material A should be 0.1% or more by weight relative to the weight of the iron, and preferably 0.3% or more. In the case of a typical coated steel plate, it is about 0.3 to 0.4%. The upper limit is about 5%, and preferably 3% or less.

[0023] As described above, in the Consteel type electric furnace 1, the conveying device 15 also serves as a discharge passage for the exhaust gas 10a in the furnace body 10. For this reason, when the synthetic resin-adhered iron material A is simply conveyed by the conveying device 15, the synthetic resin in the synthetic resin-adhered iron material A is thermally decomposed in the conveying device, generating gas. Since the temperature in the conveying device 15, particularly in the conveying device 15 away from the furnace body 10, is lower than in the furnace body 10 or in the molten steel M (about several hundred degrees Celsius), the gas generated by thermal decomposition here does not completely react with the oxygen in the surrounding air, and may have an unpleasant odor. In order to suppress the decomposition of the synthetic resin in the conveying device 15, the synthetic resin-adhered iron material A is put into the furnace body 10 by the conveying device 15 together with the synthetic resin-free iron material N, and the synthetic resin-adhered iron material A is conveyed into the furnace body 10 with the synthetic resin-free iron material N placed on top. The high-temperature exhaust gas 10a passes through the upper part of the conveying device 15. By placing the iron material N without synthetic resin on the iron material A with synthetic resin, heat exchange between the exhaust gas 10a and the iron material A with synthetic resin can be suppressed.

[0024] The synthetic resin-free iron material N is an iron material 16 to which synthetic resin is not attached, that is, iron material 16 that is not painted and to which no plastic material is attached. As the synthetic resin-free iron material N, scrap that is selected to have no synthetic resin attached or scrap of known origin can be used. For example, scrap generated in a steelworks can be used as the synthetic resin-free iron material N.

[0025] The inventor investigated the nitrogen concentration ([%N]) of the molten steel M at the time of tapping while changing various conditions for feeding the iron material N not adhered to synthetic resin and the iron material A adhered to synthetic resin. Aand the weight of the synthetic resin-free iron material N W N The sum of W A +W N Weight of synthetic resin-coated iron material A added W A Ratio of W A / (W A +W N ) is 0.05 or more and 0.25 or less, and the feeding speed S A and the feeding speed S during feeding of the synthetic resin-free iron material N N The sum of S A +S N The feeding speed S of synthetic resin-coated iron material A during feeding A Ratio of S A / (S A +S N It has been found that by setting the ratio of the nitrogen concentration in the molten steel M to 0.25 or less, it is possible to reduce the generation of unpleasant odors while lowering the nitrogen concentration in the molten steel M at the time of tapping. That is, the method of operating the electric furnace 1 according to the embodiment of the present invention includes charging the synthetic resin-adhered iron material A together with the synthetic resin-free iron material N as the iron material 16 into the furnace body 10 by the transport device 15, the synthetic resin-adhered iron material A is transported into the furnace body 10 with the synthetic resin-free iron material N placed thereon, and the charged weight W of the synthetic resin-adhered iron material A is A and the weight of the synthetic resin-free iron material N W N The sum of W A +W N Weight of synthetic resin-coated iron material A (W A ) ratio W A / (W A +W N ) is set to be 0.05 or more and 0.25 or less, and the feeding speed S A and the feeding speed S during feeding of the synthetic resin-free iron material N N The sum of S A +S N The feeding speed S of synthetic resin-coated iron material A during feeding A Ratio of S A / (S A +S N ) is set to 0.25 or less. As will be shown later as an example, the ratio W A / (W A +W NBy making the ratio S 0.05 or more, the amount of gas generated by vaporization of synthetic resin can be secured sufficiently, and the nitrogen concentration of molten steel M at the time of tapping can be reduced. A / (S A +S N By making the ratio S 0.25 or less, the synthetic resin of the synthetic resin-coated iron material A can be reduced in contact with the high-temperature exhaust gas 10a in the conveying device 15, and the generation of unpleasant odors can be suppressed. A / (S A +S N ) is less than 0.25, so the ratio W A / (W A +W N ) is automatically capped at 0.25.

[0026] Furthermore, the inventors investigated the nitrogen concentration ([%N]) of molten steel M at the time of tapping while changing various conditions for feeding the synthetic resin-free iron material N and the synthetic resin-adhered iron material A, and found that the effect of suppressing nitrogen absorption can be increased by feeding the synthetic resin-adhered iron material A in the latter half of the period in which the iron material 16 is fed into the furnace body 10. That is, in the method of operating the electric furnace 1 according to the embodiment of the present invention, it is preferable that the synthetic resin-adhered iron material A is fed in the latter half of the period in which the iron material 16 is fed into the furnace body 10. In other words, the synthetic resin-free iron material N is fed in the first half of the period in which the iron material 16 is fed into the furnace body 10, and the above-mentioned ratio W A / (W A +W N In order to achieve this, it is preferable to charge the entire amount of synthetic resin-adhered iron material A to be charged together with synthetic resin-free iron material N in the latter half of the charging period of iron material 16.

[0027] In addition, the ratio W A / (W A +W N ) is the weight W of synthetic resin-free iron material N per channel N (ton) and the input weight W of synthetic resin-coated iron material A A For example, if a total of 100 tons of synthetic resin-free iron material N and synthetic resin-adhered iron material A are put into the furnace body 10 during 1Ch, and the synthetic resin-adhered iron material A is 3 tons, the ratio W A / (W A +WN ) is 0.03.

[0028] ratio S A / (S A +S N ) is the charging speed S of the synthetic resin-adhered iron material A and the synthetic resin-free iron material N charged into the furnace body 10 of the electric furnace 1 through the conveying device 15. A ,S N (ton / min). A ,S N is the average injection speed in a predetermined period shorter than the entire injection period, and can be, for example, the average injection speed per minute. When the average injection speed fluctuates, each injection speed S A ,S N can be the maximum value of the average input speed during a predetermined period (for example, per minute) during the input of the synthetic resin-adhered iron material A. For example, when the synthetic resin-adhered iron material A is input at a speed of about 0.075 ton / min and the synthetic resin-free iron material N is input at a speed of about 2.425 ton / min, the ratio S A / (S A +S N ) is 0.03. As described above, when the synthetic resin-coated iron material A is charged in the latter half of the charging period of the iron material 16 into the furnace body 10, the ratio S A / (S A +S N The ratio S can be calculated from the feeding speed (ton / min) of both the synthetic resin-coated iron material A and the synthetic resin-free iron material N in the latter half of the feeding period. A / (S A +S N ) corresponds to the blending ratio of synthetic resin-adhered iron material A and synthetic resin-non-adhered iron material N in the conveying device 15, and can also be said to correspond to the weight ratio or presence ratio of synthetic resin-adhered iron material A and synthetic resin-non-adhered iron material N in the conveying device 15 when both synthetic resin-adhered iron material A and synthetic resin-non-adhered iron material N are fed.

[0029] In addition, if the input speed of the synthetic resin-adhered iron material A is always constant during the input period of the synthetic resin-adhered iron material A, and the input speed of the synthetic resin-free iron material N is always constant during the input period of the synthetic resin-free iron material N, the ratio W A / (W A +W N ) is the ratio S throughout the entire input period. A / (S A +S N Specifically, as in Test Examples No. 1 to 6 described later, when both the synthetic resin-free iron material N and the synthetic resin-adhered iron material A are input over the entire period, the ratio S A / (S A +S N ) is the ratio W A / (W A +W N ) is the same value. In addition, as in the test examples No. 7 and 8 described later, when synthetic resin-coated iron material A is input only for a certain period, the ratio S A / (S A +S N ) is the ratio W A / (W A +W N ) is higher than the ratio S of the period during which synthetic resin-coated iron material A is fed (half of the total period) when the total amount of synthetic resin-coated iron material A is fed in half the period. A / (S A +S N ) is the ratio W A / (W A +W N In other words, the ratio S A / (S A +S N ) is the average value of the ratio W A / (W A +W N ) and the other half of the period is 0, so the ratio W A / (W A +W N ) is the same value.

[0030] The charging period of the iron material 16 into the furnace body 10 may be a charging period for every 1Ch. The charging period of the synthetic resin-adhered iron material A may be 50% or more of the entire charging period (the entire charging period in 1Ch).

[0031] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. EXAMPLES

[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0033] The inventor produced molten steel M while changing the feeding conditions of synthetic resin-adhered iron material A as shown in the test examples No. 1 to 8 in the table below. The basic conditions are as follows. That is, a total of 100 tons of synthetic resin-free iron material N and synthetic resin-adhered iron material A were continuously fed into the furnace body 10, which held about 60 tons ([%N] = 0.0045) of molten steel from the previous Ch, at a speed of about 2.5 tons / min for about 40 minutes. As synthetic resin-free iron material N, iron scraps not coated with synthetic resin generated in a steelworks were used, and as synthetic resin-adhered iron material A, scraps of plastic-adhered iron obtained when crushing machinery and equipment were used. Since it is scrap, it is difficult to strictly manage the amount of attached resin, but even at the very least, the scrap had synthetic resin attached to it at a weight ratio of 0.1% or more to the weight of iron. CaO, SiO2, and MgO are charged into the furnace body 10 as auxiliary materials, and the scrap is melted by applying an arc from the electrode 20 installed above the center of the furnace to produce molten steel M. At the same time, oxygen (3000 Nm3) is introduced into the slag S (approximately 70 kg / ton of molten steel) from the side wall 12. 3 / hr) and carbonaceous material powder (60 kg / min) were injected. At the end of the treatment, the temperature of molten steel M reached about 1650°C. The main components of slag S were CaO, SiO2, MgO and FeO.

[0034] While scrap (iron material N without synthetic resin and iron material A with synthetic resin) was being charged, the presence or absence of peculiar odors was investigated around electric furnace 1. 10 channel operation was carried out under similar conditions, and if an peculiar odor was generated for even 1 channel, it was judged to be "present with peculiar odor." In addition, molten steel M was sampled at the time of tapping and the nitrogen concentration ([%N]) of molten steel M was measured. 10 channel operation was carried out under similar conditions, and the average [%N] obtained was calculated. The results are shown in the table below.

[0035] [Table 1]

[0036] In addition, the "Ratio (W A / (W A +W N )) is the weight W of synthetic resin-coated iron material A A and the weight of the synthetic resin-free iron material N W N The sum of W A +W N Weight of synthetic resin-coated iron material A (W A ) ratio.

[0037] The loading order indicates the order in which the synthetic resin-adhered iron material A is placed on the conveyor of the transport device 15. "First" means that the synthetic resin-adhered iron material A is placed on the conveyor of the transport device 15 first, and then the synthetic resin-free iron material N is placed on top of the synthetic resin-adhered iron material A. "Simultaneous" means that the synthetic resin-adhered iron material A and the synthetic resin-free iron material N are placed simultaneously in a mixed state on the conveyor of the transport device 15. In short, the "loading order" indicates the "way in which" the synthetic resin-adhered iron material A and the synthetic resin-free iron material N are placed on the conveyor of the transport device 15.

[0038] "Feeding speed S A " is the feeding speed S during feeding of the synthetic resin-coated iron material A. A (ton / min) and "Feeding speed S N " is the feeding speed S during feeding of the synthetic resin-free iron material N. N (ton / min). A / (S A +S N) is the input speed S A and the input speed S N The sum of S A +S N The feeding speed S of synthetic resin-coated iron material A during feeding A The ratio of each input speed S A ,S N is the maximum value of the average feeding speed per minute during feeding of the synthetic resin-coated iron material A. A ,S N The fluctuation of each input speed S A ,S N was equal to the average input rate over the entire input period.

[0039] 0% of the "input period" represents the start of the input of iron material 16, and 100% represents the completion of the input of iron material 16. "0 to 100%" means that synthetic resin-coated iron material A is input throughout the entire input period of iron material 16, "0 to 50%" means that the entire amount of synthetic resin-coated iron material A is input in the first half of the input period of iron material 16, and "50 to 100%" means that the entire amount of synthetic resin-coated iron material A is input in the second half of the input period of iron material 16.

[0040] More specifically, in Test Example No. 1, synthetic resin-adhered iron material A was fed continuously for about 40 minutes at a feeding rate of about 0.075 ton / min and synthetic resin-free iron material N was fed continuously at a feeding rate of about 2.425 ton / min.

[0041] Similarly, in test example No. 2, synthetic resin-adhered iron material A was fed continuously at a feeding rate of about 0.125 ton / min and synthetic resin-free iron material N was fed continuously at a feeding rate of about 2.375 ton / min for about 40 minutes. In test samples No. 3 and No. 6, the synthetic resin-adhered iron material A was fed continuously for about 40 minutes at a feeding rate of about 0.3 ton / min, and the synthetic resin-free iron material N was fed continuously at a feeding rate of about 2.2 ton / min. In test example No. 4, synthetic resin-adhered iron material A was fed continuously for about 40 minutes at a feeding rate of about 0.625 ton / min and synthetic resin-free iron material N was fed continuously at a feeding rate of about 1.875 ton / min. In test example No. 5, synthetic resin-adhered iron material A was fed continuously at a feeding rate of about 0.75 ton / min and synthetic resin-free iron material N was fed continuously at a feeding rate of about 1.75 ton / min for about 40 minutes.

[0042] In addition, in test example No. 7, during the first 20 minutes of the iron material 16 feeding period, synthetic resin-adhered iron material A was continuously fed at a feeding rate of approximately 0.6 tons / min and synthetic resin-free iron material N was continuously fed at a feeding rate of approximately 1.9 tons / min, and during the last 20 minutes, only synthetic resin-free iron material N was continuously fed at a rate of approximately 2.5 tons / min. Similarly, in test example No. 8, during the first 20 minutes of the feeding period, only synthetic resin-free iron material N was fed continuously at a rate of approximately 2.5 tons / min, and during the last 20 minutes, synthetic resin-free iron material A was fed continuously at a rate of approximately 0.6 tons / min and synthetic resin-free iron material N was fed continuously at a rate of approximately 1.9 tons / min.

[0043] In the evaluation column, cases where there is no abnormal odor and the tapping [%N] (the [%N] of molten steel M at the time of tapping) is 0.0050 or less are indicated with a circle, and other cases are indicated with an x.

[0044] In the test examples No. 1 to 5, the synthetic resin-adhered iron material A was transported into the furnace body 10 with the synthetic resin-free iron material N placed on top, and the ratio W A / (W A +W N ) and S A / (S A +S N In other words, the supply sequence and supply period were not changed in Test Examples Nos. 1 to 5.

[0045] As in Test Example No. 1, the ratio W A / (W A +W N When the ratio W was less than 0.05, the [%N] of the molten steel M at the time of tapping was as high as 0.0061%. A / (W A +W N When the ratio W is 0.05 or more, the target [%N] of molten steel M at the time of tapping is achieved at 0.0050 or less. Whether the denitrification reaction by gas proceeds sufficiently depends on the ratio WA / (W A +W N ) is related to the ratio W A / (W A +W N It was confirmed that the nitrogen concentration of the molten steel M at the time of tapping can be reduced by setting the ratio of M to 0.05 or more.

[0046] On the other hand, as in Test Example No. 5, the ratio W A / (W A +W N ) and S A / (S A +S N When the ratio S ) exceeded 0.25, an unpleasant odor was generated around the electric furnace 1 when the iron material 16 was fed. Whether or not an unpleasant odor was generated is related to the instantaneous proportion of the iron material A with synthetic resin attached thereto in the conveying device 15, and the proportion of the iron material A with synthetic resin attached thereto is particularly important in the case of the ratio S A / (S A +S N ) is related to the ratio S A / (S A +S N When the ratio S exceeds 0.25, the height of the synthetic resin-coated iron material A increases, and the synthetic resin of the synthetic resin-coated iron material A has more opportunities to come into contact with the high-temperature exhaust gas 10a. A / (S A +S N It was confirmed that the generation of unpleasant odors can be suppressed by keeping the ratio of odors to odor components below 0.25.

[0047] From these results, it was found that the synthetic resin-adhered iron material A was transported into the furnace body 10 with the synthetic resin-free iron material N placed on top, and the ratio W A / (W A +W N ) is 0.05 or more and the ratio S A / (S A +S N It was confirmed that by setting the ratio of nitrogen concentration in the molten steel M at the time of tapping to 0.25 or less, it is possible to reduce the generation of unpleasant odors while lowering the nitrogen concentration in the molten steel M at the time of tapping.

[0048] Test Examples No. 3 and 6 are examples in which the order of putting in the synthetic resin-coated iron material A is changed. When the synthetic resin-coated iron material A is put on the conveyor first as in Test Example No. 3, and the synthetic resin-free iron material N is put on top of it, it is considered that the high-temperature exhaust gas 10a in the conveyor 15 is unlikely to come into contact with the synthetic resin of the synthetic resin-coated iron material A, and therefore the synthetic resin is unlikely to vaporize and emit an unpleasant odor. On the other hand, when the synthetic resin-coated iron material A and the synthetic resin-free iron material N are put on the conveyor at the same time as in Test Example No. 6, the synthetic resin-coated iron material A and the synthetic resin-free iron material N may sometimes be placed on top of the synthetic resin-free iron material N, which is considered to have generated an unpleasant odor. From these results, it was confirmed that the generation of an unpleasant odor can be suppressed by putting the synthetic resin-free iron material N on top of the synthetic resin-coated iron material A.

[0049] Test Examples Nos. 3, 7, and 8 are examples in which the period during which synthetic resin-adhered iron material A was charged was changed. When the entire amount of synthetic resin-adhered iron material A was charged in the first half (0-50%) as in Test Example No. 7, the [%N] of molten steel M at the time of tapping reached the target value of 0.0050% or less, but was higher than when synthetic resin-adhered iron material A was charged throughout the entire period (0-100%) as in Test Example No. 3. This is thought to be because when the entire amount of synthetic resin-adhered iron material A was charged in the first half (0-50%) as in Test Example No. 7, nitrogen absorption from the arc occurred even after the charging of synthetic resin-adhered iron material A was completed, and nitrogen was also mixed in from synthetic resin-free iron material N. On the other hand, when the entire amount of synthetic resin-adhered iron material A was charged in the second half (50-100%) as in Test Example No. 8, the [%N] of molten steel M at the time of tapping was lower than that of Test Example No. 3, in which synthetic resin-adhered iron material A was charged throughout the entire period. This is because, when the entire amount of synthetic resin-coated iron material A is charged in the latter half (50-100%) as in Test Example No. 8, the [%N] of the molten steel M may rise in the first half, but the denitrification reaction proceeds more efficiently due to the large amount of gas generated from the synthetic resin-coated iron material A charged in the latter half than when the synthetic resin-coated iron material A is charged over the entire period. From these results, it was confirmed that it is preferable to charge the synthetic resin-coated iron material A in the latter half of the charging period of the iron material 16 into the furnace body 10. [Explanation of symbols]

[0050] 1: Electric furnace 10:Furnace body 10a: Exhaust gas 15: Transport device 16: Iron 20: Electrode

Claims

1. A method for operating an electric furnace of a Consteel type, in which iron materials are continuously fed into a furnace body of the electric furnace by a conveying device and the iron materials are melted by an arc from an electrode to produce molten steel, the electric furnace being configured to introduce exhaust gas from within the furnace body into the conveying device and heat the iron materials with the exhaust gas, The method includes feeding the synthetic resin-adhered iron material (A) together with the synthetic resin-free iron material (N) into the furnace body as the iron material by the conveying device; The synthetic resin-adhered iron material (A) is transported into the furnace body with the synthetic resin-free iron material (N) placed thereon, The weight of the synthetic resin-coated iron material (A) (W A ) and the input weight (W N ) and the sum (W A +W N The weight of the synthetic resin-coated iron material (A) added to the A ) ratio (W A / (W A +W N ) is set to be 0.05 or more and 0.25 or less, The feeding speed (S A ) and the feeding speed (S N ) and the sum (S A +S N The feeding speed (S A ) ratio (S A / (S A +S N ) is set to be 0.25 or less. How to operate an electric furnace.

2. The synthetic resin-adhered iron material (A) is charged in the latter half of the charging period of the iron material into the furnace body. The method for operating an electric furnace according to claim 1.

Citation Information

Patent Citations

  • The continuous steelmaking method and device

    JP1986502899A

  • Smelting of scrap in electric arc furnace and electric arc furnace therefor

    JP1990217788A

  • Method and device for continuous preheating of scrap

    JP1994128657A

  • Melting equipment and treatment method using the same

    JP2002156186A